Antirust glycerol and preparation method thereof
A technology of anti-rust glycerin and weight percentage, which is applied in the field of corrosion inhibitors, can solve the problems that the functions and uses cannot cover various metals or multiple media, etc., and achieve the effect of strong water absorption and lower freezing point
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0022] A kind of preparation method of antirust glycerin, it is made up of following components:
[0023] Sodium molybdate 0.3 kg;
[0024] Zinc borate 0.2 kg;
[0025] Furfural 0.1 kg;
[0026] Alkanol 0.2 kg;
[0027] Ammonium benzoate 0.1 kg;
[0028] Benzotriazole 0.1 kg;
[0029] Mercaptobenzothiazole 0.2 kg;
[0030] Sodium carbonate 2.0 kg;
[0031] Glycerol 96.8 kg,
[0032] According to the above weight, add glycerin to sodium carbonate, sodium molybdate and zinc borate in the reaction kettle, heat to stir and compound, heat to 90°C, then add furfural, benzoic acid amine, alkanol, benzotriazole Stir and compound with mercaptobenzothiazole, then add activated carbon for decolorization, filter, cool to 40°C, pack, and complete the preparation process to become a 100 kg antirust glycerin product.
Embodiment 2
[0034] A kind of preparation method of antirust glycerin, it is made up of following components by weight percentage:
[0035] Sodium molybdate 0.3%;
[0036] Zinc borate 0.2%;
[0037] Furfural 0.1%;
[0038] Alkanol 0.2%;
[0039] Ammonium Benzoate 0.1%;
[0040] Benzotriazole 0.1%;
[0041] Mercaptobenzothiazole 0.2%;
[0042] Sodium carbonate 2%;
[0043] Glycerol 96.8%,
[0044] According to the above weight percentage, add glycerin to sodium carbonate, sodium molybdate and zinc borate in the reaction kettle, heat to stir and recombine, heat to 90°C, then add furfural, benzoic acid amine, alkylamino alcohol, benzotriazepam Azole and mercaptobenzothiazole are stirred and compounded, then activated carbon is added for decolorization, filtered, cooled to 40°C, packaged, and the preparation process is completed to become an antirust glycerin product.
Embodiment 3
[0046] A kind of preparation method of antirust glycerin, it is made up of following components by weight percentage:
[0047] Sodium molybdate 0.5%;
[0048] Zinc borate 0.4%;
[0049] Furfural 0.1%;
[0050] Alkanol 0.2%;
[0051] Ammonium benzoate 0.2;
[0052] Benzotriazole 0.2;
[0053] Mercaptobenzothiazole 0.2%;
[0054] Sodium carbonate 3%;
[0055] Glycerol 95.2%,
[0056] According to the above weight percentage, add glycerin to sodium carbonate, sodium molybdate and zinc borate in the reaction kettle, heat to stir and recombine, heat to 90°C, then add furfural, benzoic acid amine, alkylamino alcohol, benzotriazepam Azole and mercaptobenzothiazole are stirred and compounded, then activated carbon is added for decolorization, filtered, cooled to 40°C, packaged, and the preparation process is completed to become an antirust glycerin product.