[0017] Select raw materials by weight percentage
[0018] Methylthiourea 10%,
[0019] 2-Methylimidazoline 10%,
[0020] Benzylquinoline Chloride 5%,
[0021] The rest is water.
[0022] Add reverse osmosis product water, methylthiourea, 2-methylimidazoline, and benzyl quinoline chloride in proportion to the container, and stir at room temperature for 2 to 3 hours to obtain the product.
Embodiment 2
[0024] Select raw materials by weight percentage
[0025] Tolylthiourea 10%,
[0026] 2-Ethylimidazoline 10%,
[0027] Benzylquinoline Chloride 5%,
[0028] The rest is water.
[0029] Add reverse osmosis product water, tolylthiourea, 2-ethylimidazoline, and benzylquinoline chloride in sequence in proportion to the container, and stir at room temperature for 2 to 3 hours to obtain the product.
Embodiment 3
[0031] Select raw materials by weight percentage
[0032] Methylthiourea 15%,
[0033] 2-Methylimidazoline 15%,
[0034] Allyl Quinoline Chloride 10%,
[0035] The rest is water.
[0036] The reverse osmosis product water, tolylthiourea, 2-methylimidazoline, and allyl quinoline chloride are sequentially added to the container in proportion, and stirred at room temperature for 2 to 3 hours to obtain the product.