Polyurethane sealing strip and preparation method thereof
A sealing strip and polyurethane technology, which is applied in the field of polyurethane products, can solve problems such as not easy to open, poor mechanical properties, wear resistance and high pressure resistance, and achieve high production efficiency, good toughness and simple processing technology.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0025] The polyurethane sealing strip is composed of component A and component B, in parts by weight, and the raw materials are as follows:
[0026] A component:
[0027]
[0028] B component:
[0029] 100LL27.5kg.
[0030] Its preparation method is as follows:
[0031] Add the raw materials of component A into the mixer, adjust the constant material temperature to 25°C, adjust the speed of the stirrer to 4250r / min and mix them evenly; pour component B, which has been preheated to 25°C, into component A and stir for 12.5s , Pour the mixed material into a mold preheated to 40°C, and demould after 7.5 minutes to obtain the product.
[0032] The product index is shown in Table 1.
[0033] Table 1 Example 1 product index
Embodiment 2
[0036] The polyurethane sealing strip is composed of component A and component B, in parts by weight, and the raw materials are as follows:
[0037] A component:
[0038]
[0039] B component:
[0040] 100LL20kg.
[0041] Its preparation method is as follows:
[0042] Add the raw materials of component A into the mixer, adjust the constant material temperature to 23°C, adjust the speed of the stirrer to 4000r / min to mix them evenly; pour component B preheated to 23°C into component A and stir for 10s, Pour the mixed material into a mold preheated to 35°C, and demould after 5 minutes to obtain the product.
[0043] Product indicators are shown in Table 2.
[0044] Table 2 embodiment 2 product index
Embodiment 3
[0047] The polyurethane sealing strip is composed of component A and component B, in parts by weight, and the raw materials are as follows:
[0048] A component:
[0049]
[0050] B component:
[0051] 100LL35kg.
[0052] Its preparation method is as follows:
[0053] Add the raw materials of component A into the mixer, adjust the constant material temperature to 27°C, and adjust the speed of the mixer to 4500r / min to mix them evenly; pour component B, which has been preheated to 27°C, into component A and stir for 15 seconds, Pour the mixed material into a mold preheated to 45°C, and demould after 10 minutes to obtain the product.
[0054] Product indicators are shown in Table 3.
[0055] Table 3 embodiment 3 product index