preparation example Construction
[0025] Meanwhile, the present invention provides the preparation method of above-mentioned waterborne paint, and this preparation method specifically comprises following operation steps:
[0026] (1), preparation of 7% special silicate liquid: take and prepare the following components by weight: 928 parts of water, 2 parts by weight of industrial preservatives, and 70 parts of special silicate, mix each component and Disperse at a speed of 800r / min until uniform and particle-free to obtain a 7% special silicate solution for use;
[0027] (2) Preparation of base material: Weigh and prepare the following components by weight: 221.5 parts of water, 1 part of AMP95 multifunctional additive, 1 part of industrial preservative, 10 parts of propylene glycol, 10 parts of lauryl alcohol, silicon 250 parts of acrylic emulsion, 6 parts of 50% TT-935 thickener, and 0.5 part of mineral oil defoamer; first mix water, AMP95 multifunctional additive, industrial preservative, propylene glycol, ...
Embodiment 1
[0033] Weigh 928kg of water, 2kg of industrial preservative, and 70kg of special silicate, mix the components and disperse at a high speed of 800r / min until uniform and particle-free to obtain 1000kg of 7% special silicate solution, which is ready for use;
[0034] Weigh 221.5kg of water, 1kg of AMP95 multifunctional additive, 1kg of industrial preservative, 10kg of propylene glycol, 10kg of lauryl alcohol fat and 250kg of silicon acrylic emulsion and mix them, and stir at a low speed of 400r / min until uniform, and add 6kg of 50% TT-935 thickener, after being completely stirred evenly, add 0.5kg of mineral oil defoamer, and continue to stir until evenly to obtain 500kg of base material for use;
[0035] Weigh 490kg of water, 2kg of industrial preservatives, 4kg of anionic surfactants, 10kg of propylene glycol, 8kg of lauryl alcohol, and 2kg of mineral oil defoamers and mix them evenly at a stirring rate of 400r / min; then add 25kg of silicone Resin, stir evenly at a stirring rate...
Embodiment 2
[0038] Compared with embodiment 1, the differences in this embodiment are:
[0039] (a) Take by weighing 490kg water, 2kg industrial preservative, 4kg anionic surfactant, 10kg propylene glycol, 8kg lauryl alcohol fat, and 2kg mineral oil defoamer and mix, then adopt a stirring rate of 600r / min to stir evenly; ( b) After putting in 25kg of silicone resin, the stirring rate used is 600r / min; (c) 2kg of polyurethane thickener is added at a revolution of 900r / min; (d) after adding polyurethane thickener, use 900r / min Min stirring speed stirring 10min.
PUM