A water-based, water-based acrylic technology, applied in coatings, anti-corrosion coatings, etc., can solve problems such as poor wetting, easy sagging, hardness of water-based coatings, imperfect abrasion resistance and water resistance, and achieve low and high baking temperatures. The effect of abrasion resistance
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0016] Based on a 100kg product, the selected raw materials include: 35kg of water-based acrylic resin, 17kg of water-based amino resin, 4kg of polyethersulfone resin, 3kg of dimethylethanolamine, 30kg of purified water, 5kg of ethylene glycol butyl ether, and 3kg of diethylene glycol butyl ether. , 2kg of ethanol, 0.2kg of defoamer, 0.4kg of leveling agent, 0.4kg of wetting agent.
[0017] Add the water-based acrylic resin and polyethersulfone resin to the ethylene glycol butyl ether and stir in the container. During the stirring process, add diethylethanolamine to adjust the pH of the solution to keep it at 7.5~8.5. Add the water-based amino resin and diethyl in sequence Glycol butyl ether, ethanol, defoamer, leveling agent and wetting agent are mixed uniformly, and then pure water is added and fully stirred to form the solution to obtain the finished product.
[0018] The finished product is tested and evaluated according to the HG / T 2594-1994 standard for various amino baking e...
Embodiment 2
[0020] Based on 100kg product, the selected raw materials include: water-based acrylic resin 38kg, water-based amino resin 15kg, polyethersulfone resin 3kg, dimethylethanolamine 3kg, purified water 29kg, ethylene glycol butyl ether 5kg, diethylene glycol butyl ether 2kg , 2kg of ethanol, 0.2kg of defoamer, 0.4kg of leveling agent, 0.4kg of wetting agent.
[0021] Add the water-based acrylic resin and polyethersulfone resin to the ethylene glycol butyl ether and stir in the container. During the stirring process, add diethylethanolamine to adjust the pH of the solution to keep it at 7.5~8.5. Add the water-based amino resin and diethyl in sequence Glycol butyl ether, ethanol, defoamer, leveling agent and wetting agent are mixed uniformly, and then pure water is added and fully stirred to form the solution to obtain the finished product.
[0022] The finished product is tested and evaluated according to the HG / T 2594-1994 standard for various amino baking enamels in the chemical indus...
Embodiment 3
[0024] Based on 100kg product, the selected raw materials include: 33kg of water-based acrylic resin, 20kg of water-based amino resin, 5kg of polyethersulfone resin, 3kg of dimethylethanolamine, 27kg of purified water, 5kg of ethylene glycol butyl ether, and 3kg of diethylene glycol butyl ether. , Ethanol 3kg, defoamer 0.2kg, leveling agent 0.4kg, wetting agent 0.4kg.
[0025] Add the water-based acrylic resin and polyethersulfone resin to the ethylene glycol butyl ether and stir in the container. During the stirring process, add diethylethanolamine to adjust the pH of the solution to keep it at 7.5~8.5. Add the water-based amino resin and diethyl in sequence Glycol butyl ether, ethanol, defoamer, leveling agent and wetting agent are mixed uniformly, and then pure water is added and fully stirred to form the solution to obtain the finished product.
[0026] The finished product is tested and evaluated according to the HG / T 2594-1994 standard for various amino baking enamels in the ...