Embodiment 1
[0028] The deicing and deicing agent with low concrete corrosion rate and low freezing point described in this embodiment, its preparation raw materials include the following components:
[0029]
[0030] The preparation method of the deicing and deicing agent with low concrete corrosion rate and low freezing point described in this embodiment comprises the steps:
[0031] (1) Measure the glucose fermentation liquid according to the selected formula, then add the organic acid potassium salt, chloride salt, and potassium tartrate in the formula amount, heat up to 60-70°C and stir for 1-3h, and after all dissolve, Then add ethylene glycol monomethyl ether, stir evenly and cool to room temperature to obtain deicing agent I component, set aside;
[0032] (2) Measure epichlorohydrin, dioctyl phthalate and low-density polyethylene according to the selected formula, heat to 70-80°C and fully stir for 1-2h to make low-density polyethylene and phthalate Dioctyl ester is fully disso...
Embodiment 2
[0036] The deicing and deicing agent with low concrete corrosion rate and low freezing point described in this embodiment, its preparation raw materials include the following components:
[0037]
[0038]
[0039] The preparation method of the deicing and deicing agent with low concrete corrosion rate and low freezing point described in this embodiment comprises the steps:
[0040] (1) Measure the glucose fermentation liquid according to the selected formula, then add the organic acid potassium salt, chloride salt, and potassium tartrate in the formula amount, heat up to 60-70°C and stir for 1-3h, and after all dissolve, Then add ethylene glycol monomethyl ether, stir evenly and cool to room temperature to obtain deicing agent I component, set aside;
[0041] (2) Measure epichlorohydrin, dioctyl phthalate and low-density polyethylene according to the selected formula, heat to 70-80°C and fully stir for 1-2h to make low-density polyethylene and phthalate Dioctyl ester is...
Embodiment 3
[0045] The deicing and deicing agent with low concrete corrosion rate and low freezing point described in this embodiment, its preparation raw materials include the following components:
[0046]
[0047]
[0048] The preparation method of the deicing and deicing agent with low concrete corrosion rate and low freezing point described in this embodiment comprises the steps:
[0049](1) Measure the glucose fermentation liquid according to the selected formula, then add the organic acid potassium salt, chloride salt, and potassium tartrate in the formula amount, heat up to 60-70°C and stir for 1-3h, and after all dissolve, Then add ethylene glycol monomethyl ether, stir evenly and cool to room temperature to obtain deicing agent I component, set aside;
[0050] (2) Measure epichlorohydrin, dioctyl phthalate and low-density polyethylene according to the selected formula, heat to 70-80°C and fully stir for 1-2h to make low-density polyethylene and phthalate Dioctyl ester is ...