A technology of room temperature synthesis and quick-setting agent, which is applied in the direction of sustainable waste treatment, solid waste management, climate sustainability, etc., can solve the problems affecting the health of construction workers on site, significant concrete durability, etc., and achieve improved stability and Accelerating coagulation effect, reducing heating equipment investment, and reducing production cost
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0028] The method for synthesizing fluorine-free and alkali-free quick-setting agent at normal temperature comprises the following steps:
[0029] (1) Mix 0.33g of 2-acrylamide-2-methylpropanesulfonic acid, 0.33g of N,N-dimethylacrylamide and 98.85g of water, stir evenly and then heat up to 60°C; control the dropping rate at 0.1 ml / min, drop 0.33 g of acrylic acid and 0.15 g of ammonium persulfate solution simultaneously, react for 4 hours; obtain a stable coagulant after cooling to room temperature;
[0030] (2) Mix 55g of 60-100 mesh aluminum sulfate, 2g of 150-200 mesh aluminum hydroxide and 27.9g of water, and shear at room temperature with a high-speed disperser at a speed of 1000 rpm for 8 hours; adjust the speed to 50 RPM, then add 10g of viscosity reducer and 0.1g of dispersant in turn, and shear for 15 minutes; keep at 50 RPM, add 5g of stable coagulant and shear for 15 minutes to obtain the final alkali-free accelerator.
Embodiment 2
[0032] The method for synthesizing fluorine-free and alkali-free quick-setting agent at normal temperature comprises the following steps:
[0033] (1) Mix 2g 2-acrylamide-2-methylpropanesulfonic acid, 2g N,N-dimethylacrylamide and 93.1g water, stir well and then heat up to 40°C; control the dropping rate to 1ml / min, drop 2g acrylic acid and 0.9g sodium persulfate solution simultaneously respectively, react for 12 hours; obtain stable coagulant after being cooled to room temperature;
[0034] (2) Mix 65g 60-100 mesh aluminum sulfate, 0.1g 150-200 mesh aluminum hydroxide and 13.9g water, and cut for 3 hours with a high-speed disperser at a speed of 5000 rpm at room temperature; adjust the speed to 500 rpm, then add 15g of viscosity reducer and 1g of dispersant in turn, and shear for 5 minutes; keep at 500 rpm, add 5g of stable coagulant and shear for 5 minutes to obtain the final alkali-free accelerator.
Embodiment 3
[0036] The method for synthesizing fluorine-free and alkali-free quick-setting agent at normal temperature comprises the following steps:
[0037] (1) Mix 1g of 2-acrylamide-2-methylpropanesulfonic acid, 1g of N,N-dimethylacrylamide and 96.7g of water, stir evenly and then heat up to 50°C; control the dropping rate to 0.2ml / minute, drop 1g acrylic acid and 0.3g potassium persulfate solution simultaneously respectively, react 8 hours; Obtain stable coagulant after being cooled to room temperature;
[0038] (2) Mix 55g of 60-100 mesh aluminum sulfate, 0.1g of 150-200 mesh aluminum hydroxide and 13.9g of water, and use a high-speed disperser at room temperature to cut for 5 hours at a speed of 3000 rpm; adjust the speed to 100 rpm, then add 15g of viscosity reducer and 1g of dispersant in turn, and shear for 15 minutes; keep at 100 rpm, add 15g of stable coagulant and shear for 15 minutes to obtain the final alkali-free coagulant.