Embodiment 1
[0031] A method for stripping an ultra-thin flexible cover plate, comprising the following steps:
[0032] 1) Prepare the pretreatment solution: mix 30wt% ethanol, 15wt% DMAc and 55wt% pure water to obtain a pretreatment solution, heat it to 40°C, place an ultra-thin flexible cover plate poorly coated with polyurethane material in it, adjust the ultrasonic The frequency is 2.3KHz, ultrasonic treatment for 30min;
[0033] 2) Configure the release solution: stir 50wt% pure water, 40wt% ethanol and 10wt% mixed solution, wherein the mixed solution is configured by glycerol, propylene glycol, and polyethylene glycol at a ratio of 1:2:2 to obtain a release film Process the solution, heat it to 65°C, put the ultra-thin flexible cover plate treated in step 1) in it, set the ultrasonic frequency to 2.5KHz; ultrasonic treatment for 1.5h;
[0034] 3) Cleaning: The ultra-thin flexible cover plate treated in step 2) is soaked and cleaned in 60°C pure water for 20 minutes under ultrasonic ...
Embodiment 2
[0036] A method for stripping an ultra-thin flexible cover plate, comprising the following steps:
[0037] 1) Prepare the pretreatment solution: mix 25wt% ethanol, 10wt% dichloromethane and 65wt% pure water to obtain the pretreatment solution, heat it to 40°C, place the ultra-thin flexible cover plate coated with poor epoxy resin material Among them, adjust the ultrasonic power to 2.5KHz, and ultrasonically treat for 45 minutes;
[0038] 2) Configure the release solution: stir 55wt% pure water, 35wt% ethanol and 10wt% mixed solution, wherein the mixed solution is configured by glycerol, propylene glycol, and polyethylene glycol in a ratio of 5:2:3 to obtain a release film Treat the solution, heat it to 60°C, place the ultra-thin flexible cover plate treated in step 1) in it, set the ultrasonic power to 3.0KHz, and ultrasonically treat for 1.5h;
[0039] 3) Cleaning: The ultra-thin flexible cover plate treated in step 2) is soaked and cleaned in 65°C pure water for 30 minutes ...
Embodiment 3
[0041] A method for stripping an ultra-thin flexible cover plate, comprising the following steps:
[0042] 1) Configure pretreatment solution: mix 25wt% ethanol, 15wt% acetone and 60wt% pure water to obtain a pretreatment solution, heat it to 45°C, place an ultra-thin flexible cover plate coated with poor PMMA in it, adjust the ultrasonic The power is 2.5KHz, ultrasonic treatment for 50min;
[0043] 2) Configure the stripping solution: stir 50%wt pure water, 40wt% ethanol and 10wt% mixed solution, wherein the mixed solution is configured by glycerol, propylene glycol, and polyethylene glycol in a ratio of 4:3:3, and the stripped solution is obtained. Membrane treatment solution, heated to 65°C, put the ultra-thin flexible cover plate treated in step 1) in it, set the ultrasonic power to 3.0KHz, and ultrasonically treat for 1.5h;
[0044] 3) Cleaning: The ultra-thin flexible cover plate treated in step 2) was soaked and cleaned in 70°C pure water for 25 minutes under ultrasoni...