[0030] A modification method of straw paper, specifically comprising the following steps:
[0031] Step 10: raw material preparation, 100 parts of bleached hardwood pulp, 100 parts of bleached softwood pulp, 3 parts of dispersant, 2 parts of modifier A, 180 parts of nanocellulose, 30 parts of polyester modified dimethyl polysiloxane , 1 part of defoamer, 0.5 part of modifier B and 0.8 part of stabilizer;
[0032] Step 20: wood pulp modification, the bleached hardwood pulp, bleached softwood pulp, dispersant, and modifier A prepared in step 10 are subjected to beating, deslagging and modification operations to make the fibers in the wood pulp Fine, and further modified to generate modified mixed raw pulp, the specific operation steps for modifying wood pulp are as follows:
[0033] Step 201: beating, injecting the bleached hardwood pulp and bleached softwood pulp prepared in step 10 into the stirring tank from the two feed ports of the stirring tank, and simultaneously control...
Embodiment 2
[0043] A modification method of straw paper, specifically comprising the following steps:
[0044] Step 10: raw material preparation, 120 parts of bleached hardwood pulp, 120 parts of bleached softwood pulp, 4 parts of dispersant, 3 parts of modifier A, 200 parts of nanocellulose, 35 parts of polyester modified dimethyl polysiloxane , 2 parts of defoamer, 0.8 part of modifier B and 1.0 part of stabilizer;
[0045] Step 20: wood pulp modification, the bleached hardwood pulp, bleached softwood pulp, dispersant, and modifier A prepared in step 10 are subjected to beating, deslagging and modification operations to make the fibers in the wood pulp Fine, and further modified to generate modified mixed raw pulp, the specific operation steps for modifying wood pulp are as follows:
[0046] Step 201: beating, injecting the bleached hardwood pulp and bleached softwood pulp prepared in step 10 into the stirring tank from the two feed ports of the stirring tank, and simultaneously contro...
Embodiment 3
[0056] A modification method of straw paper, specifically comprising the following steps:
[0057] Step 10: raw material preparation, 150 parts of bleached hardwood pulp, 150 parts of bleached softwood pulp, 5 parts of dispersant, 4 parts of modifier A, 220 parts of nanocellulose, 40 parts of polyester modified dimethyl polysiloxane , 3 parts of defoamer, 1.0 part of modifier B and 1.5 parts of stabilizer;
[0058] Step 20: wood pulp modification, the bleached hardwood pulp, bleached softwood pulp, dispersant, and modifier A prepared in step 10 are subjected to beating, deslagging and modification operations to make the fibers in the wood pulp Fine, and further modified to generate modified mixed raw pulp, the specific operation steps for modifying wood pulp are as follows:
[0059] Step 201: beating, injecting the bleached hardwood pulp and bleached softwood pulp prepared in step 10 into the stirring tank from the two feed ports of the stirring tank, and simultaneously contr...
PUM
| Property | Measurement | Unit |
|---|---|---|
| Length | aaaaa | aaaaa |
| Length | aaaaa | aaaaa |
| Length | aaaaa | aaaaa |