Embodiment 1
[0036] Embodiment 1: the preparation of a kind of highly selective electrochemical hydrogen sulfide sensor working electrode comprises the following steps:
[0037] S1: Add in the reactor in turn:
[0038]
[0039] The pretreatment method of VXC-72 carbon black is to use nitric acid with a mass fraction of 45% to 60% to ultrasonically treat at 50°C to 75°C for 1h to 4h, and then dry it for use;
[0040] After mixing, use a high-shear homogeneous emulsifier to disperse and emulsify, and obtain an electrode slurry in a uniform and viscous colloidal state after homogeneous emulsification for 1 hour;
[0041] S2: Coating the electrode slurry on a porous waterproof and breathable membrane made of polytetrafluoroethylene by screen printing to obtain a working electrode diaphragm;
[0042]S3: Place the coated working electrode diaphragm in the air, dry it naturally for 30 minutes, and then dry it in a vacuum drying oven at a low temperature at 50°C for 120 minutes, then transfer ...
Embodiment 2
[0044] Embodiment 2: the preparation of a kind of highly selective electrochemical hydrogen sulfide sensor working electrode comprises the following steps:
[0045] S1: Add in the reactor in turn:
[0046]
[0047] The pretreatment method of VXC-72 carbon black is to use nitric acid with a mass fraction of 45% to 60% to ultrasonically treat at 50°C to 75°C for 1h to 4h, and then dry it for use;
[0048] After mixing, use a high-shear homogeneous emulsifier to disperse and emulsify, and obtain an electrode slurry in a uniform and viscous colloidal state after homogeneous emulsification for 1 hour;
[0049] S2: Coating the electrode slurry on a porous waterproof and breathable membrane made of polytetrafluoroethylene by screen printing to obtain a working electrode diaphragm;
[0050] S3: Place the coated working electrode diaphragm in the air, dry it naturally for 30 minutes, and then dry it in a vacuum drying oven at a low temperature at 50°C for 120 minutes, then transfer...