Method for improving texturing yield of silicon wafer for solar cell
A technology of solar cells and silicon wafers, applied in chemical instruments and methods, circuits, electrical components, etc., can solve problems such as low efficiency of solar cells and poor texturing of silicon wafers, and achieve the effect of improving conversion efficiency and yield
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment
[0037] The method for improving the texturing yield of silicon wafers for solar cells in this embodiment is divided into two steps: degreasing cleaning and immersion cleaning, and takes about 48 hours in total.
[0038] The reagents used for degreasing and cleaning are shown in Table 2.
[0039] Table 2
[0040] degreasing cleaning NaOH (45%) DI water 2O2(32%) heating bubbling cycle Remark Texturing tank 4L 150L 8L 60℃ open open Add 2L-H2O2 every 2 hours
[0041] The specific implementation is as follows:
[0042] 1-1) Add 4L NaOH solution (45% mass fraction), 150L deionized water and 8L H 2 o 2 solution (32% mass fraction). Raise the temperature of the texturing tank to 60°C, and turn on the bubbling and circulation functions. The bubbling is adjusted to an appropriate size, and the bubbles are visible, but not too large to cause the solution to splash out of the tank. due to H 2 o 2 Will decompose, need to add 2LH every 2 hour...