High-resilience self-healing polyurethane elastomer and method of making same
By constructing an interpenetrating dual-network structure consisting of a multi-hydrogen bond physical network and a dynamic covalent bond chemical network, the problem of simultaneously achieving high resilience, self-healing, and high tensile properties of self-healing polyurethane elastomers in flexible electronic devices was solved, realizing efficient self-healing and improved stability of the material.
Patent Information
- Application Number
- CN202610557306.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-04-24
- Publication Date
- 2026-06-16
AI Technical Summary
Existing self-healing polyurethane elastomers cannot simultaneously achieve high resilience, self-healing, and high tensile properties. The single cross-linking network leads to insufficient performance and cannot meet the comprehensive requirements of flexible electronic devices and biological interfaces.
By constructing a basic structure of polyurethane soft segments and hard segments, an ultra-strong multi-hydrogen bond physical network and a three-dimensional chemical cross-linking network are introduced to form an interpenetrating dual network structure. The multi-hydrogen bond physical cross-linking points have high strength and are reversible, while the dynamic covalent chemical network provides a stable framework. The synergistic effect achieves high resilience and self-healing.
Achieving rapid self-healing capability at room temperature enhances fatigue resistance and structural stability, significantly improving the lifespan and signal stability of flexible electronic devices, thus resolving the core contradiction of traditional self-healing polyurethane elastomers struggling to balance performance.
Smart Images

Figure CN122213358A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the fields of polymer functional materials and flexible electronic materials technology, and more specifically, to a high-resilience self-healing polyurethane elastomer and its preparation method. Background Technology
[0002] The rapid development of technologies such as flexible electronics, wearable sensing, and biomedical detection has led to applications of electronic devices and sensors that are increasingly closer to the human body or biological interfaces. These interfaces typically possess characteristics such as softness, dynamic deformation, and surface irregularities, placing high demands on the flexibility and adaptability of the adapting materials. In existing technologies, the basic substrates of electronic devices and sensors are mostly made of rigid inorganic materials such as silicon. Although these materials can meet the needs of conventional signal detection and transmission through precision molding and assembly processes, their inherent rigidity makes it difficult to achieve good compatibility with soft, dynamic, and irregular biological interfaces, easily leading to problems such as poor fit and unstable signal acquisition during dynamic monitoring.
[0003] To adapt to flexible application scenarios, polyurethane elastomers have been gradually developed as active substrate materials for flexible electronic devices and sensors. Some polyurethane elastomers have been endowed with certain self-healing properties by introducing dynamic chemical bonds or supramolecular interactions, aiming to solve the damage problems caused by mechanical friction, collision, bending and other factors during the use of flexible substrates. Among them, intrinsic self-healing polyurethane elastomers have become the mainstream research and development direction. These materials rely on their own chemical structure to achieve repair without the need for external repair agents. Their self-healing driving force mainly comes from reversible covalent bonds (such as dynamic urea bonds, transesterification bonds) or supramolecular interactions (such as hydrogen bonds): reversible covalent bonds can break and rearrange under specific stimuli to achieve structural repair of the damaged site; although the single bond force of hydrogen bonds is relatively weak, a large number of hydrogen bonds can form a hydrogen bond network, and self-repair is completed by breaking and rearranging hydrogen bonds.
[0004] Existing self-healing polyurethane elastomers suffer from the following drawbacks: a single dynamic covalent bond or hydrogen bond network cannot simultaneously achieve self-healing, high resilience, and tensile properties. Introducing a large number of dynamic covalent bonds reduces tensile and resilience performance, leading to permanent deformation and fatigue failure. Relying solely on hydrogen bonds or a single reversible covalent bond results in low self-healing efficiency and poor mechanical recovery after repair. Furthermore, while physically cross-linked networks offer fast response, they suffer from poor structural stability and are prone to segment slippage. Chemically cross-linked networks, while structurally stable, lack sufficient repair and resilience flexibility, failing to achieve a balance between high strength, high resilience, high durability, and excellent self-healing performance. Current solutions only employ a single physically cross-linked hydrogen bond network (such as pyridyl hydrogen bonds or a combination of strong and weak hydrogen bonds), failing to establish a synergistic structure where chemical and physical cross-links interpenetrate, thus failing to resolve the core contradiction between self-healing, high resilience, and high tensile strength.
[0005] In summary, existing polyurethane elastomers for flexible electronics cannot meet the comprehensive requirements of high resilience, self-healing, mechanical strength, and signal stability. There is an urgent need to break through the limitations of single cross-linking networks and achieve synergistic improvement of multiple properties. Summary of the Invention
[0006] To address the aforementioned problems, this invention provides a high-resilience self-healing polyurethane elastomer and its preparation method. By constructing a basic structure of polyurethane soft and hard segments, ultra-strong multiple hydrogen-bonded groups are introduced via amide chain extension to form a high-density dynamic hydrogen-bonded physical network. Simultaneously, a trifunctional isocyanate crosslinking agent is introduced to construct a three-dimensional chemical crosslinking network with polyurea bonds as dynamic covalent bonds. This allows the two networks to interpenetrate and synergistically interact. The multiple hydrogen-bonded physical crosslinking points possess strength comparable to chemical crosslinking points and exhibit room-temperature dynamic reversibility, while the dynamic covalent chemical network provides a stable three-dimensional framework. This invention effectively solves the core contradiction in existing self-healing polyurethane elastomers where self-healing performance and high resilience and high tensile strength are difficult to achieve simultaneously. While ensuring excellent tensile mechanical properties and high resilience, it endows the material with rapid self-healing ability at room temperature without external stimuli, and significantly improves fatigue resistance and structural stability.
[0007] In a first aspect, the present invention provides a method for preparing a high-resilience self-healing polyurethane elastomer, characterized by comprising the following steps: S1: A secondary amine-terminated polyetheramine is reacted with diisocyanate in an organic solvent to produce an isocyanate-terminated prepolymer. S2: Add diamine and / or acylhydrazine chain extenders to the prepolymer to carry out chain extension reaction, and obtain chain extended products containing urea bonds and acylhydrazine bonds; S3: Add a trifunctional isocyanate crosslinking agent to the chain extension product to carry out a crosslinking reaction. After the reaction reaches the gelation critical point, cast and mold to obtain the high resilience self-healing polyurethane elastomer.
[0008] Through a prepolymerization reaction, secondary amine-terminated polyether amines react with diisocyanates to form linear prepolymers with active -NCO groups at the ends. The polyether soft segments impart good entropic elasticity to the material, providing the molecular chain basis for high resilience. Further, through a chain extension reaction, diamine and / or hydrazide chain extenders react with the -NCO groups at the ends of the prepolymer, achieving molecular chain growth while densely introducing urea bonds (-NH-CO-NH-) and hydrazide bonds (-CO-NH-NH-CO-) onto the polymer backbone. These functional groups contain... The continuous hydrogen bond donors and acceptors can form a high-density, high-strength multi-hydrogen bond physical cross-linking network. The strength of the physical cross-linking points is comparable to that of the chemical cross-linking points, and it has room-temperature dynamic reversibility. In the subsequent cross-linking reaction, the trifunctional isocyanate cross-linking agent reacts with the remaining -NCO groups in the chain extension product with its three active -NCO groups, bonding the linear or slightly branched polymer chains into a stable three-dimensional chemical cross-linking network. The polyurea bonds formed therein act as dynamic covalent bonds, possessing both structural stability and reversible recombination ability.
[0009] A high-density, multi-hydrogen-bonded physical network and a dynamic covalent chemical network interweave and synergistically within the polymer matrix: the chemical network provides a stable three-dimensional framework, inhibiting permanent chain slippage and ensuring high resilience and fatigue resistance; the physical network dissipates energy through the breaking and recombination of multiple hydrogen bonds and drives molecular chain diffusion and rebonding at the damaged interface under room temperature and without external stimuli, achieving efficient self-healing. The complementary advantages of these two networks overcome the technical bottleneck of traditional self-healing polyurethane elastomers, which struggle to simultaneously achieve self-healing performance while maintaining mechanical and resilience properties.
[0010] Preferably, the diisocyanate is isophorone diisocyanate, and the molar ratio of the secondary amine-terminated polyetheramine to the diisocyanate is 1:1.05 to 1:1.5.
[0011] Preferably, the diamine and / or hydrazide chain extender is selected from one or more of diazide hydrazide, malondihydrazide, ethylenediamine, and butanediamine, and is mixed in any proportion; in the chain extension reaction, the molar ratio of the -NCO group at the end of the prepolymer to the amino group in the chain extender is 1:1.5.
[0012] Preferably, the trifunctional isocyanate crosslinking agent is trifunctional hexamethylene diisocyanate.
[0013] Preferably, the organic solvent is N,N-dimethylformamide, and its moisture content is ≤0.05%.
[0014] Preferably, the temperature conditions for the prepolymerization reaction in S1 are 25℃~60℃, and the reaction time is 4~8 hours.
[0015] Preferably, the reaction temperature of the chain extension reaction in S2 is 40~60℃ and the reaction time is 2~5 hours.
[0016] Preferably, the reaction temperature of the crosslinking reaction in S3 is 40~50℃.
[0017] Secondly, the present invention provides a high-resilience self-healing polyurethane elastomer, characterized in that it is prepared by the above-described preparation method.
[0018] Thirdly, this invention provides an application of a high-resilience self-healing polyurethane elastomer in the preparation of flexible substrates. The high-resilience self-healing polyurethane elastomer described in this invention can be used to prepare flexible substrates, particularly as a flexible support or encapsulation layer in flexible electronic devices, wearable sensors, and biomedical detection equipment. This elastomer possesses high resilience, high tensile elongation at break, and rapid self-healing capability at room temperature without external stimuli. It can achieve good adhesion to soft, dynamic, and irregular human or biological interfaces, maintaining structural integrity and signal stability even after repeated bending, stretching, or minor damage. Flexible substrates prepared with the high-resilience self-healing polyurethane elastomer can effectively overcome the defects of traditional rigid substrates, such as poor adhesion, unstable signal acquisition, and weak fatigue resistance and large permanent deformation of existing self-healing materials, significantly improving the service life and dynamic monitoring reliability of flexible electronic devices.
[0019] In summary, the present invention has at least one of the following beneficial technical effects: 1. This invention introduces super-strong multiple hydrogen bonds through amide chain extension. The physical crosslinking point strength formed by these multiple hydrogen bonds is comparable to that of chemical crosslinking points. This ensures the tensile properties and high resilience of the material through high-strength physical crosslinking, and also endows the material with excellent self-healing ability through its room temperature dynamic characteristics. Thus, it effectively solves the core technical problem that the above three properties of self-healing polyurethane elastomers in the prior art cannot be achieved at the same time.
[0020] 2. In this invention, the multiple hydrogen bond physical network provides rapid self-healing capability at room temperature without external stimulation, and the dynamic covalent bond (polyurea bond) chemical network provides a stable three-dimensional cross-linked skeleton. The two work together to inhibit chain segment slippage and permanent deformation, fundamentally improving the problem of elasticity decay and mechanical property decline caused by self-healing modification of traditional self-healing polyurethane elastomers.
[0021] 3. This invention utilizes a dual-network synergistic design of a multiple hydrogen bond physical network and a polyurea bond dynamic covalent chemical network, combined with a specifically regulated three-dimensional chemical crosslinking network, to effectively improve the fatigue resistance of the material, reduce chain segment slippage, thereby maintaining signal stability during dynamic monitoring and significantly extending the service life of flexible electronic devices. Attached Figure Description
[0022] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the description of the embodiments of this application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0023] Figure 1 This paper illustrates the interpenetrating double network structure and working mechanism of the high-resilience self-healing polyurethane elastomer provided in an embodiment of this application. Figure 2 This illustration shows a schematic diagram of the formation mechanism and three-dimensional network structure of the high-resilience self-healing polyurethane elastomer provided in an embodiment of this application; wherein... Figure 2 a is a schematic diagram of the prepolymerization reaction between SD2001 and diisocyanate; Figure 2 b is a schematic diagram of the chain extension reaction principle; Figure 2 c is a schematic diagram of the cross-linking reaction principle; Figure 3 The following diagram illustrates the load-unload cycle test results provided in an embodiment of this application. Figure 4 The following diagram illustrates the loading-unloading cycle curves under different strains provided in the embodiments of this application; Figure 5 The diagram shows the self-healing performance test results provided in the embodiments of this application. Detailed Implementation
[0024] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. The following description of at least one exemplary embodiment is merely illustrative and is in no way intended to limit the present invention or its application or use. Based on the embodiments of the present invention, any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the protection scope of the present invention. Furthermore, all other embodiments obtained by those skilled in the art without inventive effort are within the protection scope of the present invention.
[0025] Specific experimental steps or conditions are not specified in the embodiments; they can be performed according to the conventional experimental steps or conditions described in the prior art. Reagents and other instruments used, unless otherwise specified, are all commercially available conventional reagent products. Furthermore, the accompanying drawings are merely illustrative diagrams of the embodiments of the present invention and are not necessarily drawn to scale. The same reference numerals in the drawings denote the same or similar parts, and therefore, repeated descriptions of them will be omitted. Some block diagrams shown in the drawings are functional entities and do not necessarily correspond to physically or logically independent entities.
[0026] Techniques, methods, and devices known to those skilled in the art may not be discussed in detail, but where appropriate, such techniques, methods, and devices should be considered part of this specification.
[0027] In the description of this invention, it should be understood that the use of terms such as "first" and "second" to define components is merely for the purpose of distinguishing the corresponding components. Unless otherwise stated, the above terms have no special meaning and therefore should not be construed as limiting the scope of protection of this invention.
[0028] Furthermore, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0029] To enable those skilled in the art to better understand this application, the following embodiments are provided to illustrate in detail a high-resilience self-healing polyurethane elastomer and its preparation method.
[0030] Example Example 1: Preparation of a high-resilience self-healing polyurethane elastomer This embodiment provides a method for preparing a high-resilience self-healing polyurethane elastomer, the mechanism of its core structure and performance as follows: Figure 1 As shown, the specific steps are as follows.
[0031] JEFFAMINE SD2001 ® SD2001 requires no drying and can be used directly; IPDI (isophorone diisocyanate) and Tri-HDI (trifunctional hexamethylene diisocyanate) should be used in sealed containers to prevent moisture absorption and deterioration; DMF (N,N-dimethylformamide) should have a moisture content ≤0.05% to avoid side reactions between moisture and -NCO groups. Reaction apparatus: 100 mL three-necked flask, magnetic stir bar, and dropping tube, cleaned with anhydrous ethanol and dried in a 120℃ oven for 30 min, then cooled to room temperature for use.
[0032] Add 3.00 g of SD2001 and 5 mL of anhydrous DMF to a 100 mL three-necked flask after pretreatment. Place a magnetic stir bar in the flask, turn on the stirrer, and stir at a rate of 300–400 r / min for about 5 min until the SD2001 is completely dissolved and the solution becomes clear. Slowly add a measured amount of IPDI to the solution using a dropper, controlling the dropping rate to 1 drop / 2 s. The molar ratio of SD2001 to IPDI is 1:1.2 (the calculated amount of IPDI is approximately 0.89 g). After the addition is complete, stir the mixture at a constant temperature for 6 h to obtain the isocyanate-terminated prepolymer.
[0033] like Figure 2 As shown in a, the secondary amine group at the end of SD2001 undergoes a nucleophilic addition reaction with the isocyanate groups (-NCO) at both ends of IPDI to generate a polyurethane prepolymer with active -NCO groups retained at the end, providing reaction sites for subsequent chain extension reactions.
[0034] Adipic acid dihydrazide (ADH) was selected as the chain extender. Adipic acid dihydrazide was accurately weighed and added to 2 mL of anhydrous DMF, stirred until completely dissolved. The molar ratio of the remaining -NCO groups in the prepolymer to the chain extender was 1:1.5 (calculated, the amount of ADH used is approximately 0.58 g). The chain extender solution was slowly added dropwise to the prepolymer solution using a dropper, controlling the dropping rate at 1 drop / 3 s to avoid local temperature rises exceeding 60°C and premature cross-linking. After the chain extender was completely added, the reaction was continued at a constant temperature with stirring for 3 h to obtain a chain-extended product containing urea bonds (-NH-CO-NH-) and hydrazide bonds (-CO-NH-NH-CO-), forming a high-density dynamic hydrogen bond network on the molecular chain, such as... Figure 2 As shown in b, the -NCO group at the end of the prepolymer undergoes an addition reaction with the amino group of adipic acid dihydrazide, resulting in molecular chain extension. At the same time, urea bonds and hydrazide bonds are densely introduced, and the above functional groups can form a high-density multi-hydrogen bond network.
[0035] Tri-HDI (trifunctional hexamethylene diisocyanate) was selected as the crosslinking agent. Tri-HDI was weighed according to the prescribed amount, diluted with 2 mL of anhydrous DMF, and stirred until homogeneous. Tri-HDI reacted equimolarly with the remaining -NCO groups in the chain-extended prepolymer (calculated, the amount of Tri-HDI used was approximately 0.25 g). The reaction system temperature was maintained at 45°C. The diluted Tri-HDI solution was slowly added dropwise to the chain-extended prepolymer solution using a dropper, controlling the dropping rate at 1 drop / 3 s. After the addition was complete, stirring was continued, and the gelation process was closely monitored: when the solution viscosity increased significantly, the stirring resistance increased, and a thin filament could be drawn from the sample, this was the gelation critical point, and stirring was immediately stopped. The reaction system that reached the gelation critical point was quickly poured into a pre-treated mold (the mold was dried and cooled at 120°C), and the mold was gently shaken to remove air bubbles, yielding the high-resilience self-healing polyurethane elastomer.
[0036] like Figure 2 As shown in c, the three active -NCO groups of Tri-HDI undergo cross-linking reactions with the active sites in the chain extension product, bonding the linear or slightly branched polymer chains into a stable three-dimensional network, forming a three-dimensional chemical cross-linked network with polyurea bonds as dynamic covalent bonds. This network interpenetrates with the aforementioned high-density multiple hydrogen bond physical network, constituting an interpenetrating double network structure.
[0037] The polyurethane elastomer prepared in this embodiment has an interpenetrating dual-network structure in which a dynamic covalent chemical network and a multiple hydrogen bond physical network intersect. The dynamic covalent chemical network is composed of polyurea bonds, providing a stable three-dimensional framework. The multiple hydrogen bond physical network is formed by urea bonds and hydrazide bonds, providing room temperature dynamic reversible physical crosslinking points, and the strength of these physical crosslinking points is comparable to that of chemical crosslinking points.
[0038] Example 2: Load-Unload Cycle Performance Test In this embodiment, the polyurethane elastomer sample prepared in Example 1 was subjected to loading-unloading cycle tests under different strains to characterize its resilience and resistance to deformation.
[0039] Test method: The specimens were subjected to 100%, 200%, and 300% strain using a universal testing machine, and the stress-strain curves were recorded.
[0040] Test results: such as Figure 3 As shown, the elastomer of the present invention exhibits a high degree of fit between the loading and unloading curves and a small hysteresis loop region in loading-unloading cycles with different strains, indicating that the material can recover quickly after deformation and possesses excellent resilience and fatigue resistance.
[0041] The above results confirm that the dynamic hydrogen bond network and dynamic covalent bond network constructed in this invention are not simply superimposed, but rather form an interpenetrating dual-network structure that complements defects and synergistically enhances each other. The dynamic covalent bond network provides a stable chemical cross-linked framework, effectively inhibiting molecular chain segment slippage; the hydrogen bond network provides dynamic reversibility, ensuring rapid recovery after deformation. The synergy between the two enables the material to maintain a stable mechanical response under repeated deformation.
[0042] Example 3: Residual Strain and Rebound Performance Analysis This embodiment, based on the loading-unloading test data of Embodiment 2, quantitatively calculates the residual strain under different strains to evaluate the material's rebound rate. Using the loading-unloading cycle curves under different strains in Embodiment 2, the residual strain after each cycle is calculated, and the rebound rate is calculated using the following formula: Springback rate = (Applied strain - Residual strain) / Applied strain × 100% The results are as follows Figure 4As shown, after 100% strain loading-unloading, the residual strain is only 5%, corresponding to a springback rate of 95%; after 200% strain loading-unloading, the residual strain is 13%, corresponding to a springback rate of 93.5%; after 300% large strain loading-unloading, the residual strain is only 22%, corresponding to a springback rate still above 92.7%.
[0043] The elastomer of this invention maintains a high resilience of >92% even under a large strain of 300%, proving that relying solely on a single hydrogen bond network cannot simultaneously meet the comprehensive performance requirements of high resilience, high tensile strength, and high self-healing. However, the interpenetrating dual-network structure of this invention can simultaneously achieve a high level of synergy in elongation at break, self-healing efficiency, and resilience after 10,000 tensile cycles.
[0044] Example 4: Self-repair performance test at room temperature without external stimuli This embodiment tests the self-healing performance of the polyurethane elastomer sample prepared in Example 1 under room temperature conditions without external stimuli.
[0045] The specimen was completely cut off with a blade, ensuring close contact between the fracture surfaces. It was then left to heal at room temperature (25°C) without external stimuli for 12 hours. After repair, a tensile test was performed, and the stress-strain curve of the repaired specimen was recorded and compared with that of the original specimen. The self-healing efficiency was calculated using the following formula: Self-healing efficiency = (Tensile strength after repair / Original tensile strength) × 100% Test results are as follows Figure 5 As shown, the tensile strength of the original sample was about 1.18 MPa and the elongation at break was about 82%. After the sample was completely cut and left to stand at room temperature for 12 hours for repair, the tensile strength recovered to about 0.85 MPa, the self-repair efficiency was over 72%, the elongation at break recovered to about 60%, and the stress-strain curve after repair was highly consistent with the original curve.
[0046] The results validate the synergistic self-healing mechanism of the dual-network system. The high-density dynamic hydrogen-bonded network provides the driving force for spontaneous recombination at room temperature, enabling rapid damage healing. The dynamic covalent network acts as a stable framework, ensuring the mechanical properties and structural stability of the repaired material and avoiding the problem of significant attenuation of mechanical strength after repair by a single hydrogen-bonded network. Furthermore, combined with the high resilience data from Example 3, it further demonstrates that the interpenetrating dual-network structure of this invention can simultaneously achieve a synergistic improvement in high self-healing efficiency, high resilience rate, and high tensile properties, breaking through the technical bottleneck of resilience performance degradation caused by traditional self-healing modification of polyurethane elastomers.
[0047] In summary, the embodiments demonstrate that the interpenetrating dual-network structure of multiple hydrogen bond physical network and dynamic covalent bond chemical network constructed in this invention can successfully prepare high-resilience self-healing polyurethane elastomers. These elastomers exhibit a resilience of 95% to 92.7% under 100% to 300% strain, and a self-healing efficiency of over 72% after 12 hours of repair at room temperature without external stimulation. This achieves a synergistic improvement in high resilience, high tensile strength, and efficient self-healing performance, effectively solving the core technical problem that traditional self-healing polyurethane elastomers struggle to achieve the aforementioned properties simultaneously.
[0048] The various embodiments in this specification are described in a progressive manner, with each embodiment focusing on the differences from other embodiments. The same or similar parts between the various embodiments can be referred to each other.
[0049] Although preferred embodiments of the present application have been described, those skilled in the art, upon learning the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments as well as all changes and modifications falling within the scope of the embodiments of the present application.
[0050] Finally, it should be noted that in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or terminal device that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or terminal device. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or terminal device that includes said element.
[0051] The above provides a detailed description of a high-resilience self-healing polyurethane elastomer and its preparation method provided in this application. Specific examples have been used to illustrate the principles and implementation methods of this application. The descriptions of the above embodiments are only for the purpose of helping to understand the method and core ideas of this application. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.
Claims
1. A method for preparing a high-resilience self-healing polyurethane elastomer, characterized in that, Includes the following steps: S1: A secondary amine-terminated polyetheramine is reacted with diisocyanate in an organic solvent to produce an isocyanate-terminated prepolymer. S2: Add diamine and / or acylhydrazine chain extenders to the prepolymer to carry out chain extension reaction, and obtain chain extended products containing urea bonds and acylhydrazine bonds; S3: Add a trifunctional isocyanate crosslinking agent to the chain extension product to carry out a crosslinking reaction. After the reaction reaches the gelation critical point, cast and mold to obtain the high resilience self-healing polyurethane elastomer.
2. The method for preparing the high-resilience self-healing polyurethane elastomer according to claim 1, characterized in that, The diisocyanate is isophorone diisocyanate, and the molar ratio of the secondary amine-terminated polyetheramine to the diisocyanate is 1:1.05 to 1:1.
5.
3. The method for preparing the high-resilience self-healing polyurethane elastomer according to claim 1, characterized in that, The diamine and / or hydrazide chain extender is selected from one or more of diazide hydrazide, malondihydrazide, ethylenediamine, and butanediamine, and is mixed in any proportion; in the chain extension reaction, the molar ratio of the terminal -NCO group of the prepolymer to the amino group in the chain extender is 1:1.
5.
4. The method for preparing the high-resilience self-healing polyurethane elastomer according to claim 1, characterized in that, The trifunctional isocyanate crosslinking agent is trifunctional hexamethylene diisocyanate.
5. The method for preparing the high-resilience self-healing polyurethane elastomer according to claim 1, characterized in that, The organic solvent is N,N-dimethylformamide, and its moisture content is ≤0.05%.
6. The method for preparing the high-resilience self-healing polyurethane elastomer according to claim 1, characterized in that, The temperature conditions for the prepolymerization reaction in S1 are 25℃~60℃, and the reaction time is 4~8 hours.
7. The method for preparing the high-resilience self-healing polyurethane elastomer according to claim 1, characterized in that, The chain extension reaction in S2 is carried out at a temperature of 40-60°C for 2-5 hours.
8. The method for preparing the high-resilience self-healing polyurethane elastomer according to claim 1, characterized in that, The cross-linking reaction in S3 is carried out at a temperature of 40-50°C.
9. A high-resilience self-healing polyurethane elastomer, characterized in that, It is prepared by the preparation method according to any one of claims 1 to 8.
10. The application of the high-resilience self-healing polyurethane elastomer as described in claim 9 in the preparation of flexible substrates.