A polycarboxyl group amino modified degradable scale and salt resistant thickening agent and a preparation method thereof
Patent Information
- Application Number
- CN202611231607.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-14
- Publication Date
- 2026-09-29
AI Technical Summary
[0007]为了解决现有技术中可降解稠化剂加量过高且不具备抗盐功能和针对高矿化度条件下的阻垢功能的问题,本发明提供了一种多羧基氨基改性可降解阻垢抗盐稠化剂及其制备方法
本发明将绿色可降解高分子材料(聚环氧琥珀酸或聚琥珀酰亚胺)与增稠单体和含磺酸基的抗盐功能单体形成的耐盐增稠功能聚合物进行分子层面的接枝共聚设计,构建“多羧基氨基改性可降解主链、侧链抗盐增稠、整体兼具阻垢特性”的新型稠化剂分子结构,制备得到多羧基氨基改性可降解阻垢抗盐稠化剂。所述多羧基氨基改性可降解阻垢抗盐稠化剂具有如下优势:(1)优异的生物降解性:采用聚环氧琥珀酸或聚琥珀酰亚胺作为稠化剂的可降解主链骨架,聚环氧琥珀酸或聚琥珀酰亚胺均属于绿色可降解高分子材料,具有优良的生物降解性,当通过接枝共聚将可降解主链骨架与抗盐增稠功能聚合物链段共价结合后,形成的接枝共聚物仍保留可降解主链骨架的生物降解性,稠化剂28天生物降解率达60.2%以上。(2)高效广谱阻垢性能:将多羧基氨基化合物引入聚环氧琥珀酸或聚琥珀酰亚胺的可降主链骨架,形成“本色阻垢+强化阻垢”的双重阻垢机制。聚环氧琥珀酸或聚琥珀酰亚胺主链本身含有大量羧基,可实现本色阻垢;多羧基氨基化合物在侧链的接枝引入,增加了密集的羧基、亚氨基和酰胺基螯合位点,可实现强化阻垢;同时抗盐功能单体中的磺酸基也可起到一定螯合阻垢功能,进一步促进阻垢性能,从而使得0.6wt%稠化剂的破胶液对CaCO3的阻垢率在98.2%以上、对CaSO4的阻垢率在96.1%以上、对BaSO4的阻垢率在92.2%以上。(3)突出的高抗盐性能:通过在可降解主链骨架的接枝侧链中引入高含量的含磺酸基团的抗盐功能单体,利用磺酸基团的强水化能力和抗盐屏蔽效应,结合长链烷基不饱和硅烷的自缔合盐增稠特性,使0.6wt%稠化剂在150000mg/L高矿化度(钙镁离子总含量3000mg/L)条件下的表观粘度在82mPa·s以上,120℃剪切120min后稳定粘度在57.1mPa·s以上。(4)高增稠和强减阻携砂能力:通过增稠单体的引入,结合含磺酸基团的抗盐功能单体和长链烷基不饱和硅烷形成的疏水缔合网络,赋予稠化剂优异的增稠和减阻携砂性能,0.08wt%稠化剂溶液的减阻率在75.2%以上,静态悬砂测试中30%(v/v)砂比下0.6wt%稠化剂溶液中30~50目陶粒支撑剂的支撑剂沉降速率在0.55cm/min以下。(5)简化施工流程和降低综合成本:稠化剂集可降解、阻垢、增稠、抗盐四大功能于一体,可直接采用高矿化度返排液等复杂水质配液,无需额外添加阻垢剂和专用降解助剂,减少化工料品种和数量,降低施工流程和综合成本。
Smart Images

Figure CN122832213A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of oil and gas production enhancement technology, specifically relating to a polycarboxylated amino-modified biodegradable scale inhibitor and anti-salt thickener and its preparation method. Background Technology
[0002] With the continuous upgrading of oil and gas exploration and development technologies, unconventional oil and gas such as tight oil and gas, shale oil and gas, and coalbed methane have become core replacement resources for increasing oil and gas production. Hydraulic fracturing is the core technology for the efficient utilization and large-scale production of these unconventional oil and gas reserves. However, water resources are generally scarce in the field. Conventional fracturing fluid preparation with clean water consumes a large amount of water and post-fracturing flowback fluid, has high treatment costs, and is subject to strict environmental regulations. Directly preparing fracturing fluid using high-mineralized flowback fluid from the formation is an inevitable requirement for cost reduction and green development in the industry. At the same time, the formation water salinity of unconventional reservoirs such as coalbed methane and deep shale is generally as high as 150,000 mg / L or more, and the calcium, magnesium, and barium ion content can reach 3,000 mg / L or more. Under complex water conditions such as high salinity, not only will the performance of fracturing fluid be significantly affected, but it will also be prone to form insoluble scale such as calcium carbonate (CaCO3), calcium sulfate (CaSO4), and barium sulfate (BaSO4) during and after fracturing. These scales will deposit on the fractures and wellbore walls, blocking seepage channels, significantly reducing the conductivity of fractures, and causing serious corrosion problems to the production tubing and wellhead equipment. This will significantly affect oil and gas migration, ultimate recovery rate, and the entire life cycle of the wellbore.
[0003] To address the aforementioned issues, existing technologies typically employ a physical composite system of anti-salt thickeners and added scale inhibitors to achieve both thickening and scale inhibition functions. However, this physical composite system suffers from significant drawbacks, including limited synergistic effects or even mutual interference, and high application difficulty.
[0004] To overcome the inherent defects of physical composite systems, some studies have attempted to directly introduce scale-inhibiting functional groups into the molecular structure of thickeners to achieve the integration of thickening and scale inhibition functions. For example, Chinese patent CN115322283B discloses an integrated fracturing emulsion that prevents scale, reduces drag, and thickens. This integrated fracturing emulsion is prepared by reverse emulsion polymerization of acrylamide, acrylic acid, and vinylphosphonic acid or isopropenylic acid, followed by the addition of diethylenetriaminepentamethylenephosphonic acid. Chinese patent application CN120965932A discloses a low-molecular-weight scale-inhibiting thickener for fracturing deep coal-gas reservoirs. It is prepared via free radical copolymerization using acrylic acid and acrylamide as hydrophilic monomers, itaconic acid and epoxysuccinic acid as scale-inhibiting monomers, sodium 2-acrylamido-2-methylpropanesulfonate and sodium p-styrenesulfonate as functional monomers, hexadecyl dimethyl allyl ammonium chloride and octadecyl dimethyl allyl ammonium chloride as hydrophobic monomers, and Tween 80 and OP-10 as water-soluble emulsifiers. However, these technical solutions all involve functional modification of mainstream thickeners such as polyacrylamide. Polyacrylamide thickeners have poor biodegradability (28-day degradation rate is typically less than 10%), leading to cumulative ecological risks from long-term residues in the formation. Furthermore, their salt resistance and scale inhibition properties under high salinity are unclear.
[0005] Given the inherent limitation of poor biodegradability in traditional polyacrylamide thickeners, some researchers have begun to focus on biodegradable polymeric frameworks. Polyaspartic acid (PASP), as a biodegradable green polymer material, has been widely studied and applied in the field of scale inhibition in water treatment. However, existing polyaspartic acid scale inhibitors are mostly water-soluble small molecules or oligomers with extremely low aqueous solution viscosity, completely lacking the thickening and sand-carrying capacity required for fracturing fluids, and cannot be used directly as thickeners. To address this issue, Chinese patent CN115449074B discloses a polyaspartamide derivative thickener with a side chain containing straight-chain alkyl chains and lysine. However, this thickener requires a high addition amount of more than 1 wt% to exhibit a thickening effect, far exceeding the conventional upper limit for fracturing thickeners (≤0.6 wt%), and it completely lacks salt resistance and scale inhibition function under high salinity conditions.
[0006] In summary, no biodegradable scale-inhibiting and salt-resistant thickener has been reported that simultaneously possesses good biodegradability (28-day degradation rate ≥60%), good thickening effect, high scale inhibition function (scale inhibition rate ≥92% for various scale types), and high salt resistance (mineralization ≥150000 mg / L) under low dosage conditions of ≤0.6 wt%. Therefore, there is an urgent need to develop a green and environmentally friendly thickener with a biodegradable polymer as the main chain backbone, integrating multiple functions such as biodegradability, scale inhibition, thickening, and salt resistance. Summary of the Invention
[0007] To address the issues of excessive dosage of biodegradable thickeners in existing technologies, their lack of salt resistance, and their inability to inhibit scale under high salinity conditions, this invention provides a polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener and its preparation method.
[0008] This invention is achieved through the following technical solution: In a first aspect, the present invention provides a polycarboxylated amino-modified degradable scale inhibitor and anti-salt thickener, the raw materials for which are prepared by weight percentage include: 8%~15% of a degradable main chain backbone, 2%~6% of a polycarboxylated amino compound, 3%~5% of a long-chain alkyl unsaturated silane, 10%~18% of a thickening monomer, 8%~15% of an anti-salt functional monomer containing sulfonic acid groups, 0.1%~0.4% of an initiator, and the balance being water; the degradable main chain backbone is polyepoxysuccinic acid or polysuccinimide; the polycarboxylated amino compound is N,N'-ethylenediaminedisuccinic acid, N-(2-aminoethyl)-N-(carboxymethyl)-glycine or iminodiacetic acid.
[0009] Preferably, the long-chain alkyl unsaturated silane is 10-undecenyltrimethoxysilane or 10-undecenyltrichlorosilane.
[0010] Preferably, the thickening monomer is acrylamide or acrylic acid.
[0011] Preferably, the salt-resistant functional monomer containing sulfonic acid groups is 2-acrylamido-2-methylpropanesulfonic acid, vinylbenzenesulfonic acid, allylbenzenesulfonic acid, or acrylamidobenzenesulfonic acid.
[0012] Preferably, the initiator is a composite system of persulfate and sodium bisulfite, with a mass ratio of persulfate to sodium bisulfite of (1.18~1.20):1.
[0013] Preferably, the polyepoxysuccinic acid has a molecular weight of 2,000 to 10,000 Daltons, and the polysuccinimide has a molecular weight of 1,800 to 9,500 Daltons.
[0014] Preferably, the viscosity-average molecular weight of the polycarboxylated amino-modified degradable scale inhibitor and salt thickener is 720-1120 million Daltons.
[0015] Secondly, the present invention provides a method for preparing the aforementioned polycarboxylated amino-modified biodegradable scale inhibitor and anti-salt thickener, comprising the following steps: Step S1: The biodegradable main chain backbone is reacted with a polycarboxylated amino compound in water to obtain a reaction solution containing product A. Step S2: Add an aqueous solution of long-chain alkyl unsaturated silane in ethanol to the reaction solution containing product A, and react to obtain a reaction solution containing product B. Step S3: Add thickening monomer and salt-resistant functional monomer containing sulfonic acid group to the reaction solution containing product B, heat to 65~70℃, add initiator aqueous solution, carry out polymerization reaction, and obtain graft copolymer colloid. Step S4: The graft copolymer colloid is washed, dried, pulverized and sieved in sequence to obtain a dry powder of polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener.
[0016] Preferably, the preparation method of the polycarboxylated amino-modified biodegradable scale inhibitor and salt thickener includes step S1 as follows: under stirring, the biodegradable main chain skeleton is added to water, the pH value is adjusted to 9.5~10, a polycarboxylated amino compound is added, and the reaction is carried out at 50~60℃ for 20~24h to obtain a reaction solution containing product A.
[0017] Preferably, in the preparation method of the polycarboxylated amino-modified biodegradable scale inhibitor and salt thickener, step S2 specifically involves: adding and dissolving a long-chain alkyl unsaturated silane in an ethanol aqueous solution with a mass concentration of 99%, and then adding it dropwise at a rate of 0.01~0.02 mL / s to a reaction solution containing product A that has been pre-cooled to room temperature. The reaction is then continued to be stirred at room temperature for 2~4 h to obtain a reaction solution containing product B.
[0018] Preferably, in the preparation method of the polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener, step S3 specifically involves: adding a thickening monomer and a salt-resistant functional monomer containing sulfonic acid groups to the reaction solution containing product B; adjusting the pH value to 6.5-7.5 with a pH adjuster; and purging with an inert gas to remove oxygen for 25-30 minutes; heating to 65-70°C; adding an initiator aqueous solution; and carrying out a polymerization reaction for 5-6 hours to obtain a graft copolymer colloid.
[0019] Furthermore, the pH adjuster is one or more of sodium hydroxide, ethylenediamine, sodium carbonate, sodium bicarbonate, and diethanolamine; the inert gas is one or two of high-purity nitrogen and high-purity argon.
[0020] Furthermore, the initiator in the aqueous initiator solution has a mass concentration of 2% to 5%.
[0021] Preferably, in the preparation method of the polycarboxylated amino-modified biodegradable scale inhibitor and salt thickener, step S4 specifically involves: cooling the graft copolymer colloid to room temperature and then cutting it into small pieces, washing it with anhydrous ethanol and precipitating it 2-3 times, placing it in a vacuum dryer at 60-65°C for 15-18 hours, and then pulverizing and sieving it to obtain a 70-120 mesh polycarboxylated amino-modified biodegradable scale inhibitor and salt thickener dry powder.
[0022] Compared with the prior art, the present invention has the following beneficial effects: This invention employs a molecular-level graft copolymerization design of a salt-resistant thickening functional polymer formed by a green biodegradable polymer material (polyepoxysuccinic acid or polysuccinimide) with a thickening monomer and a salt-resistant functional monomer containing sulfonic acid groups. This constructs a novel thickener molecular structure that features a "multi-carboxylated amino-modified biodegradable main chain, salt-resistant thickening side chains, and overall scale inhibition properties," thereby preparing a multi-carboxylated amino-modified biodegradable scale-inhibiting and salt-resistant thickener. The modified polycarboxylated amino degradable scale inhibitor and anti-salt thickener has the following advantages: (1) Excellent biodegradability: Polyepoxysuccinic acid or polysuccinimide is used as the degradable main chain skeleton of the thickener. Polyepoxysuccinic acid or polysuccinimide are both green degradable polymer materials with excellent biodegradability. When the degradable main chain skeleton is covalently combined with the anti-salt thickening polymer chain segment through graft copolymerization, the resulting graft copolymer still retains the biodegradability of the degradable main chain skeleton. The biodegradation rate of the thickener reaches more than 60.2% after 28 days. (2) High efficiency and broad-spectrum scale inhibition performance: Polycarboxylated amino compounds are introduced into the degradable main chain skeleton of polyepoxysuccinic acid or polysuccinimide to form a dual scale inhibition mechanism of "natural scale inhibition + enhanced scale inhibition". The main chain of polyepoxysuccinic acid or polysuccinimide contains a large number of carboxyl groups, which can achieve natural scale inhibition. The grafting of polycarboxylated amino compounds into the side chains increases the number of dense carboxyl, imino, and amide chelating sites, which can enhance scale inhibition. At the same time, the sulfonic acid groups in the salt-resistant functional monomers can also play a certain role in chelating scale inhibition, further promoting scale inhibition performance. As a result, the scale inhibition rate of the 0.6wt% thickener in the gelling solution is above 98.2% for CaCO3, above 96.1% for CaSO4, and above 92.2% for BaSO4. (3) Outstanding high salt resistance performance: By introducing a high content of salt-resistant functional monomers containing sulfonic acid groups into the grafted side chains of the biodegradable main chain backbone, the strong hydration ability and salt resistance shielding effect of sulfonic acid groups are utilized, combined with the self-associative salt thickening properties of long-chain alkyl unsaturated silanes, so that the apparent viscosity of 0.6wt% thickener under high mineralization conditions of 150000mg / L (total calcium and magnesium ion content of 3000mg / L) is above 82mPa·s, and the stable viscosity after shearing at 120℃ for 120min is above 57.1mPa·s. (4) High thickening and strong drag reduction and sand carrying capacity: By introducing thickening monomers, combined with salt-resistant functional monomers containing sulfonic acid groups and hydrophobic association network formed by long-chain alkyl unsaturated silanes, the thickener is endowed with excellent thickening and drag reduction and sand carrying performance. The drag reduction rate of 0.08wt% thickener solution is above 75.2%. In the static sand suspension test, the proppant settling rate of 30~50 mesh ceramsite proppant in 0.6wt% thickener solution at a sand ratio of 30% (v / v) is below 0.55cm / min.(5) Simplify the construction process and reduce the overall cost: The thickener integrates four functions: degradability, scale inhibition, thickening and salt resistance. It can be used directly to prepare complex water quality solutions such as high mineralization backflow solution without the need to add scale inhibitors and special degradation aids, thereby reducing the types and quantities of chemical materials and reducing the construction process and overall cost.
[0023] Furthermore, the viscosity-average molecular weight of polycarboxylated amino-modified biodegradable scale inhibitors and salt-resistant thickeners can reach 7.2 million to 11.2 million Daltons. The higher molecular weight can endow the thickeners with excellent thickening, drag reduction and sand-carrying properties.
[0024] The present invention discloses a method for preparing a polycarboxylated amino-modified biodegradable scale inhibitor and anti-salt thickener. First, a polycarboxylated amino compound is reacted with the carboxyl groups on polyepoxysuccinic acid or polysuccinimide, causing it to be grafted onto the biodegradable main chain backbone. The dense carboxyl and imino structures in the polycarboxylated amino compound increase its resistance to calcium chloride. 2+ Ba 2+ The chelating sites of scale-forming ions significantly enhance the scale inhibition function of the thickener. Then, long-chain alkyl unsaturated silanes react with the carboxyl and amino groups in the polycarboxylated amino compounds via siloxane or chlorosilane bonds, grafting the long-chain alkyl groups and unsaturated double bonds onto the biodegradable backbone. This introduces a hydrophobic association network with thickening properties and provides polymerization anchors for the next graft polymerization step. Furthermore, unsaturated double bond graft copolymerization introduces salt-resistant monomers containing sulfonic acid groups and thickening monomers, thus preparing a polycarboxylated amino-modified biodegradable scale-inhibiting and salt-resistant thickener. This preparation method uses water as a solvent, is environmentally friendly, and produces a dry powder product with low transportation costs.
[0025] Furthermore, in the preparation method of the present invention, the pH value in S1 is adjusted to 9.5~10, which is conducive to the ring opening of the degradable main chain skeleton and its full reaction with the polycarboxylated amino compound.
[0026] Furthermore, in the preparation method of the present invention, the pH value is adjusted to 6.5~7.5 in S3 and an inert gas is introduced to provide an oxygen-free and suitable pH environment for free radical graft polymerization, thereby ensuring that the thickener has a high molecular weight and high thickening ability. Attached Figure Description
[0027] Figure 1 The graph shows a comparison of the biodegradability of the thickeners prepared in Examples 1-13 and Comparative Examples 1-6.
[0028] Figure 2 The chart shows a comparison of the tackification time of the thickeners prepared in Examples 1-13, Comparative Examples 1-4, and Comparative Examples 9-10.
[0029] Figure 3 The viscosity comparison chart shows the thickeners prepared in Examples 1-13 and Comparative Examples 1-10.
[0030] Figure 4 The graph shows a comparison of the drag reduction rates of the thickeners prepared in Examples 1-13 and Comparative Examples 1-10.
[0031] Figure 5 The graph shows a comparison of the stable viscosity of the thickeners prepared in Examples 1-13 and Comparative Examples 1-10 in the temperature resistance and shear resistance test.
[0032] Figure 6 The graph shows a comparison of the proppant settling rates of the thickeners prepared in Examples 1-13 and Comparative Examples 1-10 in static suspended sediment tests.
[0033] Figure 7 The graph shows a comparison of the scale inhibition rates of the thickeners prepared in Examples 1-13, Comparative Examples 1-4, and Comparative Examples 9-10. Detailed Implementation
[0034] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.
[0035] This invention is not limited to the following embodiments, and specific implementation methods can be determined according to the technical solutions and actual conditions of this invention. Unless otherwise specified, all chemical reagents and chemicals mentioned in this invention are chemical reagents and chemicals known and commonly used in the prior art; unless otherwise specified, all solutions in this invention are aqueous solutions with water as the solvent, for example, hydrochloric acid solution is an aqueous solution of hydrochloric acid; room temperature in this invention generally refers to a temperature between 15°C and 25°C, generally defined as 25°C.
[0036] The present invention will be further described below with reference to embodiments: (I) Preparation of polycarboxylated amino-modified biodegradable scale inhibitors and salt-resistant thickeners Example 1 The biodegradable backbone, polycarboxylated amino compounds, long-chain alkyl unsaturated silanes, thickening monomers, salt-resistant monomers containing sulfonic acid groups, and initiators were fixed at 8%, 2%, 3%, 10%, 8%, and 0.1% by mass, respectively, with the remainder being deionized water. Under stirring, 80g of polyepoxysuccinic acid (molecular weight 10000 Daltons) was dissolved in 668.4g of deionized water. The pH of the solution was adjusted to 9.8 with sodium hydroxide. 20g of N,N'-ethylenediaminedisuccinic acid was added, and the mixture was stirred until homogeneous. The reaction was continued at 55°C for 22 hours. Then, 50g of an ethanol-water solution containing 30g of 10-undecenyltrimethoxysilane (ethanol concentration 99%) was added dropwise at a rate of 0.015mL / s, and the reaction was continued at room temperature for 3 hours. After the reaction was complete, 100g of acrylamide and 80g of 2-acrylamido-2-methylpropane were added sequentially. After thoroughly dissolving sulfonic acid, the pH was adjusted to 7.0 with sodium bicarbonate, and high-purity nitrogen was purged for 28 minutes to remove oxygen. The temperature was raised to 68°C, and a 5% initiator (a mixture of ammonium persulfate and sodium bisulfite in a mass ratio of 1.2:1) pre-prepared with 20g of deionized water was added. The polymerization reaction was carried out at a constant temperature for 5.5 hours to obtain a graft copolymer colloid. After cooling the graft copolymer colloid to room temperature, it was shredded, washed with anhydrous ethanol, precipitated three times, and vacuum dried at 62°C for 17 hours. After pulverization and sieving, a white, dry powder of polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener JSIKYP-1 was obtained. The viscosity-average molecular weight of the thickener JSIKYP-1 obtained in Example 1 was determined to be 7.43 million Daltons using an Ubbelohde viscometer (0.55mm capillary inner diameter) according to the standard GB / T 12005.10-1992 Determination of Molecular Weight of Polyacrylamide.
[0037] Example 2 The biodegradable backbone, polycarboxylated amino compounds, long-chain alkyl unsaturated silanes, thickening monomers, salt-resistant monomers containing sulfonic acid groups, and initiators were fixed at 12%, 4%, 4%, 14%, 12%, and 0.25% by mass, respectively, with the balance being deionized water. Under stirring, 120g of polyepoxysuccinic acid (molecular weight 5000 Daltons) was dissolved in 489.4g of deionized water. The pH of the solution was adjusted to 10 with sodium hydroxide. 40g of N,N'-ethylenediaminedisuccinic acid was added, and the mixture was stirred until homogeneous. The reaction was continued at 60℃ for 20h with stirring. Then, 60g of an ethanol-water solution containing 40g of 10-undecenyltrimethoxysilane (ethanol concentration 99%) was added dropwise at a rate of 0.01mL / s, and the reaction was continued at room temperature with stirring for 4h. After the reaction was complete, 140g of acrylamide and 120g of 2-acrylamide-2- Methylpropanesulfonic acid was thoroughly dissolved by stirring, and the pH was adjusted to 7.5 with sodium bicarbonate. High-purity nitrogen was then introduced for deoxygenation for 30 minutes. The temperature was raised to 70°C, and a 5% initiator (a mixture of ammonium persulfate and sodium bisulfite in a mass ratio of 1.2:1) pre-prepared with 50g of deionized water was added. The mixture was subjected to a constant-temperature polymerization reaction for 6 hours to obtain a graft copolymer colloid. After cooling the graft copolymer colloid to room temperature, it was shredded, washed with anhydrous ethanol, precipitated three times, and vacuum dried at 65°C for 15 hours. After pulverization and sieving, a polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener, JSIKYP-2, was obtained. The viscosity-average molecular weight of the thickener JSIKYP-2 obtained in Example 2 was determined to be 9.58 million Daltons using an Ubbelohde viscometer (0.55mm capillary inner diameter) according to the standard GB / T 12005.10-1992 "Determination of Molecular Weight of Polyacrylamide".
[0038] Example 3 The biodegradable backbone, polycarboxylated amino compounds, long-chain alkyl unsaturated silanes, thickening monomers, salt-resistant monomers containing sulfonic acid groups, and initiators were fixed at mass percentages of 15%, 6%, 5%, 18%, 15%, and 0.4%, respectively, with the remainder being deionized water. Under stirring, 150 g of polyepoxysuccinic acid (molecular weight 2000 Daltons) was dissolved in 329.2 g of deionized water. The pH of the solution was adjusted to 9.5 with sodium hydroxide. 60 g of N,N'-ethylenediaminedisuccinic acid was added, and the mixture was stirred until homogeneous. The reaction was continued at 50°C for 24 h with stirring. Then, 80 g of an ethanol-water solution containing 50 g of 10-undecenyltrimethoxysilane (ethanol mass concentration 99%) was added dropwise at a rate of 0.02 mL / s, and the reaction was continued at room temperature with stirring for 2 h. After the reaction was complete, 180 g of acrylamide and 150 g of 2-acrylamide-2- Methylpropanesulfonic acid was thoroughly dissolved by stirring, and the pH was adjusted to 6.5 with sodium bicarbonate. High-purity nitrogen was then introduced for deoxygenation for 25 minutes. The temperature was raised to 65°C, and a 5% initiator (a mixture of ammonium persulfate and sodium bisulfite in a mass ratio of 1.2:1) pre-prepared with 80g of deionized water was added. The mixture was subjected to a constant-temperature polymerization reaction for 5 hours to obtain a graft copolymer colloid. After cooling the graft copolymer colloid to room temperature, it was shredded, washed with anhydrous ethanol, precipitated three times, and vacuum dried at 60°C for 18 hours. After pulverization and sieving, a polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener, JSIKYP-3, was obtained. The viscosity-average molecular weight of the thickener JSIKYP-3 obtained in Example 3 was determined to be 10.98 million Daltons using an Ubbelohde viscometer (0.55mm capillary inner diameter) according to the standard GB / T 12005.10-1992 "Determination of Molecular Weight of Polyacrylamide".
[0039] Example 4 The only difference from Example 1 is that polyepoxysuccinic acid was replaced with polysuccinimide (molecular weight 9500 Daltons), resulting in the polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener JSIKYP-4. The viscosity-average molecular weight of the thickener JSIKYP-4 obtained in Example 4 was determined to be 7.95 million Daltons using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard GB / T 12005.10-1992 "Determination of Molecular Weight of Polyacrylamide".
[0040] Example 5 The only difference from Example 3 is that polyepoxysuccinic acid was replaced with polysuccinimide (molecular weight 1800 Daltons), resulting in the polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener JSIKYP-5. The viscosity-average molecular weight of the thickener JSIKYP-5 obtained in Example 5 was determined to be 11.2 million Daltons using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard GB / T 12005.10-1992 "Determination of Molecular Weight of Polyacrylamide".
[0041] Example 6 The only difference from Example 1 is that N,N'-ethylenediaminedisuccinic acid is replaced with N-(2-aminoethyl)-N-(carboxymethyl)-glycine, resulting in the polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener JSIKYP-6. The viscosity-average molecular weight of the thickener JSIKYP-6 obtained in Example 6 was determined to be 7.65 million Daltons using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard GB / T 12005.10-1992 "Determination of Molecular Weight of Polyacrylamide".
[0042] Example 7 The only difference from Example 3 is that N,N'-ethylenediaminedisuccinic acid is replaced with N-(2-aminoethyl)-N-(carboxymethyl)-glycine, resulting in the polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener JSIKYP-7. The viscosity-average molecular weight of the thickener JSIKYP-7 obtained in Example 7 was determined to be 10.87 million Daltons using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard GB / T 12005.10-1992 "Determination of Molecular Weight of Polyacrylamide".
[0043] Example 8 The only difference from Example 1 is that N,N'-ethylenediamine disuccinic acid is replaced with iminodiacetic acid, resulting in the polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener JSIKYP-8. The viscosity-average molecular weight of the thickener JSIKYP-8 obtained in Example 8 was determined to be 7.75 million Daltons using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard GB / T 12005.10-1992 "Determination of Molecular Weight of Polyacrylamide".
[0044] Example 9 The only difference from Example 3 is that N,N'-ethylenediamine disuccinic acid is replaced with iminodiacetic acid, resulting in a polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener, JSIKYP-9. The viscosity-average molecular weight of the thickener JSIKYP-9 obtained in Example 9 was determined to be 10.54 million Daltons using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard GB / T 12005.10-1992 "Determination of Molecular Weight of Polyacrylamide".
[0045] Example 10 The only difference from Example 1 is that 10-undecenyltrimethoxysilane was replaced with 10-undecenyltrichlorosilane, resulting in the polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener JSIKYP-10. The viscosity-average molecular weight of the thickener JSIKYP-10 obtained in Example 10 was determined to be 7.56 million Daltons using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard GB / T 12005.10-1992 "Determination of Molecular Weight of Polyacrylamide".
[0046] Example 11 The only difference from Example 3 is that 10-undecenyltrimethoxysilane was replaced with 10-undecenyltrichlorosilane, resulting in the polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener JSIKYP-11. The viscosity-average molecular weight of the thickener JSIKYP-11 obtained in Example 11 was determined to be 10.23 million Daltons using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard GB / T 12005.10-1992 "Determination of Molecular Weight of Polyacrylamide".
[0047] Example 12 The only difference from Example 1 is that 2-acrylamido-2-methylpropanesulfonic acid was replaced with vinylbenzenesulfonic acid, resulting in a polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener, JSIKYP-12. The viscosity-average molecular weight of the thickener JSIKYP-12 obtained in Example 12 was determined to be 7.2 million Daltons using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard GB / T 12005.10-1992 "Determination of Molecular Weight of Polyacrylamide".
[0048] Example 13 The only difference from Example 3 is that 2-acrylamido-2-methylpropanesulfonic acid was replaced with vinylbenzenesulfonic acid, resulting in a polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener, JSIKYP-13. The viscosity-average molecular weight of the thickener JSIKYP-13 obtained in Example 13 was determined to be 9.95 million Daltons using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard GB / T 12005.10-1992 "Determination of Molecular Weight of Polyacrylamide".
[0049] (II) Preparation of Comparative Thickeners Comparative Example 1 The only difference from Example 1 is that polyepoxysuccinic acid was not introduced, and the original mass percentage of polyepoxysuccinic acid was made up by deionized water to obtain thickener DBP-1. The viscosity-average molecular weight of the thickener DBP-1 obtained in Comparative Example 1 was determined to be 8.56 million Daltons using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard GB / T12005.10-1992 "Determination of Molecular Weight of Polyacrylamide".
[0050] Comparative Example 2 The only difference from Example 3 is that polyepoxysuccinic acid was not introduced, and the original mass percentage of polyepoxysuccinic acid was made up by deionized water to obtain thickener DBP-2. The viscosity-average molecular weight of the thickener DBP-2 obtained in Comparative Example 2 was determined to be 13.41 million Daltons using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard GB / T12005.10-1992 "Determination of Molecular Weight of Polyacrylamide".
[0051] Comparative Example 3 The only difference from Example 1 is that N,N'-ethylenediaminedisuccinic acid was not introduced, and the original mass percentage of N,N'-ethylenediaminedisuccinic acid was made up by deionized water to obtain thickener DBP-3. The viscosity-average molecular weight of the thickener DBP-3 obtained in Comparative Example 3 was determined to be 8.72 million Daltons using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard GB / T 12005.10-1992 "Determination of Molecular Weight of Polyacrylamide".
[0052] Comparative Example 4 The only difference from Example 3 is that N,N'-ethylenediaminedisuccinic acid was not introduced, and the original mass percentage of N,N'-ethylenediaminedisuccinic acid was made up with deionized water to obtain thickener DBP-4. The viscosity-average molecular weight of the thickener DBP-4 obtained in Comparative Example 4 was determined to be 14.15 million Daltons using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard GB / T 12005.10-1992 "Determination of Molecular Weight of Polyacrylamide".
[0053] Comparative Example 5 The only difference from Example 1 is that 10-undecenyltrimethoxysilane was not introduced, and the original mass percentage of 10-undecenyltrimethoxysilane was made up with deionized water to obtain thickener DBP-5. The viscosity-average molecular weight of the thickener DBP-5 obtained in Comparative Example 5 was determined to be 10.75 million Daltons using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard GB / T 12005.10-1992 "Determination of Molecular Weight of Polyacrylamide".
[0054] Comparative Example 6 The only difference from Example 3 is that 10-undecenyltrimethoxysilane was not introduced, and the original mass percentage of 10-undecenyltrimethoxysilane was made up with deionized water to obtain thickener DBP-6. The viscosity-average molecular weight of the thickener DBP-6 obtained in Comparative Example 6 was determined to be 17.36 million Daltons using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard GB / T 12005.10-1992 "Determination of Molecular Weight of Polyacrylamide".
[0055] Comparative Example 7 The only difference from Example 1 is that acrylamide was not introduced, and the original mass percentage of acrylamide was made up by deionized water to obtain thickener DBP-7. The viscosity-average molecular weight of the thickener DBP-7 obtained in Comparative Example 7 was determined to be 6.42 million Daltons using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard GB / T 12005.10-1992 "Determination of Molecular Weight of Polyacrylamide".
[0056] Comparative Example 8 The only difference from Example 3 is that acrylamide was not introduced, and the original mass percentage of acrylamide was made up by deionized water to obtain thickener DBP-8. The viscosity-average molecular weight of the thickener DBP-8 obtained in Comparative Example 8 was determined to be 8.26 million Daltons using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard GB / T 12005.10-1992 Determination of Molecular Weight of Polyacrylamide.
[0057] Comparative Example 9 The only difference from Example 1 is that 2-acrylamide-2-methylpropanesulfonic acid was not introduced, and the original mass percentage of 2-acrylamide-2-methylpropanesulfonic acid was made up with deionized water to obtain thickener DBP-9. The viscosity-average molecular weight of the thickener DBP-9 obtained in Comparative Example 9 was determined to be 9.63 million Daltons using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard GB / T 12005.10-1992 "Determination of Molecular Weight of Polyacrylamide".
[0058] Comparative Example 10 The only difference from Example 3 is that 2-acrylamide-2-methylpropanesulfonic acid was not introduced, and the original mass percentage of 2-acrylamide-2-methylpropanesulfonic acid was made up with deionized water to obtain thickener DBP-10. The viscosity-average molecular weight of the thickener DBP-10 obtained in Comparative Example 10 was determined to be 16.21 million Daltons using an Ubbelohde viscometer (0.55 mm capillary inner diameter) according to the standard GB / T 12005.10-1992 "Determination of Molecular Weight of Polyacrylamide".
[0059] (III) Performance Testing (1) Biodegradability The biodegradation rate of the thickener shall be determined in accordance with the provisions of the national standard GB / T 21856-2008 "Test for Rapid Biodegradability of Chemicals and Carbon Dioxide Generation".
[0060] (2) Adhesion time Accurately weigh the calculated amount of thickener powder into a 500mL beaker pre-filled with an appropriate amount of high-mineralization brine (total mineralization 150000mg / L, of which the total calcium and magnesium ion content is 3000mg / L). Dissolve the powder by stirring with a high-powered stirrer at a speed of 600±50rad / min at room temperature. The time corresponding to when the powder forms a string when lifted with a glass rod is the viscous time.
[0061] (3) Viscosity release rate Prepare a thickener solution of the target mass concentration using high-mineralized brine according to the method in (2). At room temperature, use a six-speed rotational viscometer at 100 r / min (170 s⁻¹). -1 The viscosity values of the thickener solution were tested at different dissolution times, and the viscosity release rate was calculated according to the following formula. When the viscosity was below 10 mPa·s, a capillary viscometer was used to test the kinematic viscosity of the thickener solution.
[0062]
[0063] In the formula, V R The viscosity before stabilization is expressed in mPa·s (or mm). 2 / s); V F For the final stable viscosity, mPa·s (or mm) 2 / s); R V The viscosity release rate is expressed as %.
[0064] (4) Drag reduction rate The drag reduction rate was determined in accordance with the industry standard SY / T 7627-2021 "Technical Requirements for Water-based Fracturing Fluids". A flow loop friction test device (10mm diameter) was used to test the drag reduction rate data of the thickener solution. The drag reduction rate change curve over time was recorded, and the drag reduction rate of 10 minutes was taken as the final drag reduction rate.
[0065] (5) Temperature resistance and shear resistance Using the RS6000 advanced rheometer PZ38 coaxial cylindrical rotor system at 120℃ for 170s -1 The thickener solution prepared with the obtained high-mineralization brine was subjected to a temperature resistance and shear resistance test. The viscosity change curve over time and the final stable viscosity were recorded. The duration from heating to the end of the test was 2 hours.
[0066] (6) Static suspended sediment performance With a fixed sand ratio (volume ratio) of 30%, mix 30-50 mesh ceramsite proppant with a thickener solution prepared from high-mineralization brine until homogeneous. Then, transfer the mixture into a graduated stoppered cylinder, start a stopwatch to record the settling time of the ceramsite proppant, and calculate the proppant settling rate according to the following formula.
[0067]
[0068] In the formula, H 沉 The settling height of the ceramsite proppant is in cm; t 沉 The time (in minutes) for the ceramsite proppant to settle completely. ν 沉 denoted as proppant settling rate, in cm / min.
[0069] (7) Debonding performance Weigh 100g of the thickener solution prepared with high-mineralization brine and place it in a sealed metal container. Add 0.025% ammonium persulfate and bring the solution to 90°C. o After being sealed and aged for different times under C, the fluid was removed and tested for viscosity at room temperature in accordance with the industry standard SY / T 5107-2016 "Evaluation Method for Performance of Water-based Fracturing Fluid".
[0070] (8) Scale inhibition performance Take the degelatinized liquid from (7) and test its scale inhibition performance according to the provisions of SY / T 5673-2020 "General Technical Conditions for Scale Inhibitors for Oilfield Use".
[0071] The biodegradability of the polycarboxylated amino-modified degradable scale inhibitors and salt-resistant thickeners obtained in Examples 1-13 and Comparative Examples 1-10 was tested using the above methods, and the results are listed in Table 1.
[0072] Table 1. Results of the biodegradability test of the thickener
[0073] As shown in Table 1 and Figure 1As shown in Examples 1-13, polycarboxylated amino compounds were first grafted onto the biodegradable backbone of polyepoxysuccinic acid or polysuccinimide. Then, salt-resistant functional monomers and thickening monomers containing sulfonic acid groups were introduced through long-chain alkyl unsaturated silane graft copolymerization to construct a multifunctional integrated molecular structure with "polycarboxylated amino modified biodegradable backbone, side chain salt-resistant thickening, and overall scale inhibition properties". The resulting polycarboxylated amino modified biodegradable scale inhibitor and salt-resistant thickeners (JSIKYP-1~JSIKYP-13) showed a 28-day biodegradation. The biodegradability rate reached 60.2%~66.2%, which was at least 51.1% higher than that of the thickeners (DBP-1~DBP-2) obtained without the introduction of a degradable main chain backbone in Comparative Examples 1~2, at least 49.3% higher than that of the thickeners (DBP-3~DBP-4) obtained without the introduction of polycarboxylated amino compounds in Comparative Examples 3~4, and at least 46.6% higher than that of the thickeners (DBP-5~DBP-6) obtained without the introduction of long-chain alkyl unsaturated silanes in Comparative Examples 5~6. This indicates that without the introduction of a degradable backbone, the resulting thickener exhibits very low degradability. Without the introduction of polycarboxylated amino compounds or long-chain alkyl unsaturated silanes, the lack of key groups to bond the salt-resistant functional monomers and thickening monomers containing sulfonic acid groups to the degradable backbone results in a thickener that is essentially a mixture of polyepoxysuccinic acid or polysuccinimide and a thickening monomer-salt-resistant functional monomer copolymer (or a long-chain alkyl unsaturated silane-thickening monomer-salt-resistant functional monomer copolymer). Only polyepoxysuccinic acid or polysuccinimide itself has good degradability, while the copolymer exhibits poor degradability. However, by simultaneously introducing polycarboxylated amino compounds or long-chain alkyl unsaturated silanes, and covalently introducing an appropriate amount of green degradable polymers as a degradable backbone into the salt-resistant thickener molecule, the biodegradability of the thickener can be significantly improved.
[0074] The tack time, viscosity at 2 minutes, and viscosity release rate of the polycarboxylated amino-modified biodegradable scale inhibitors and salt-resistant thickeners obtained in Examples 1-13 and Comparative Examples 1-10 were tested using the above methods at different dosages (0.08 wt% and 0.6 wt%). The results are listed in Table 2. Figure 2 and Figure 3 .
[0075] Table 2. Test results of thickener tack time, viscosity at 2 min, and viscosity release rate.
[0076] As shown in Table 2 and Figure 2As shown in Examples 1-13, polycarboxylated amino compounds were first grafted onto the biodegradable backbone of polyepoxysuccinic acid or polysuccinimide. Then, salt-resistant functional monomers and thickening monomers containing sulfonic acid groups were introduced through long-chain alkyl unsaturated silane graft copolymerization to construct a multifunctional integrated molecular structure with "polycarboxylated amino modified biodegradable backbone, side chain salt-resistant thickening, and overall scale inhibition properties". The resulting polycarboxylated amino modified biodegradable scale inhibitor and salt-resistant thickeners (JSIKYP-1~JSIKYP-13) had a tack time of no more than 13 seconds and a viscosity release rate of more than 2 minutes at additions of 0.08 wt% and 0.6 wt%. The viscosity of the thickeners obtained in Comparative Examples 1 and 2 without the introduction of a degradable main chain backbone (DBP-1 to DBP-2) was 90%, while the tack time of the thickeners obtained in Comparative Examples 1 and 2 without the introduction of a degradable main chain backbone (DBP-1 to DBP-2) was all above 18 seconds and the viscosity release rate in 2 minutes was all below 86.6%. The tack time of the thickeners obtained in Comparative Examples 3 and 4 without the introduction of polycarboxylated amino compounds (DBP-3 to DBP-4) was all above 18 seconds and the viscosity release rate in 2 minutes was all below 86.3%. The tack time of the thickeners obtained in Comparative Examples 9 and 10 without the introduction of salt-resistant functional monomers (DBP-9 to DBP-10) was all above 16 seconds and the viscosity release rate in 2 minutes was all below 79.6%. This indicates that the introduction of appropriate amounts of polyepoxysuccinic acid or polysuccinimide and polycarboxylated amino compounds can ensure the excellent solubility of the thickener through the strong hydration ability of polycarboxylated amino compounds.
[0077] Meanwhile, as shown in Table 2 and Figure 3 As shown, the viscosities of the obtained polycarboxylated amino-modified biodegradable scale inhibitors and salt-resistant thickeners (JSIKYP-1~JSIKYP-13) at dosages of 0.08 wt% and 0.6 wt% were 8.15 mm. 2The viscosity of the thickeners (DBP-1 to DBP-2) obtained without the introduction of a degradable main chain backbone in Comparative Examples 1 and 2 is at least 8.37% and 10.81% higher, respectively; the viscosity of the thickeners (DBP-3 to DBP-4) obtained without the introduction of polycarboxylated amino compounds in Comparative Examples 3 and 4 is at least 9.84% and 12.33% higher, respectively; and the viscosity of the thickeners (DBP-3 to DBP-4) obtained without the introduction of long-chain alkyl unsaturated silanes in Comparative Examples 5 and 6 is at least 82 mPa·s higher, respectively. The viscosities of the thickeners (DBP-5~DBP-6) were at least 5.17% and 6.49% higher, respectively, compared to the thickeners (DBP-7~DBP-8) obtained in Comparative Examples 7~8 without the introduction of thickening monomers, respectively, which were at least 30.82% and 30.16% higher, respectively. Furthermore, the viscosities of the thickeners (DBP-9~DBP-10) obtained in Comparative Examples 9~10 without the introduction of salt-resistant functional monomers, respectively, were at least 78.73% and 86.36% higher, respectively. This indicates that the simultaneous introduction of a degradable main chain backbone, polycarboxylated amino compounds, long-chain alkyl unsaturated silanes, thickening monomers, and salt-resistant functional monomers not only maintains excellent solubility in high-saltification brine but also significantly enhances the salt-resistant thickening ability of the thickener, achieving a balance between excellent solubility and high salt resistance.
[0078] At room temperature, the drag reduction rates of the polycarboxylated amino-modified biodegradable scale inhibitors and salt-resistant thickeners obtained in Examples 1-13 and Comparative Examples 1-10 were tested at a dosage of 0.08 wt% using the above method. The results are listed in Table 3 and Figure 4 .
[0079] Table 3. Drag Reduction Rate Test Results of Thickener
[0080] As shown in Table 3 and Figure 4As shown, in Examples 1-13, polycarboxylated amino compounds were first grafted onto the biodegradable backbone of polyepoxysuccinic acid or polysuccinimide. Then, salt-resistant functional monomers and thickening monomers containing sulfonic acid groups were introduced through long-chain alkyl unsaturated silane graft copolymerization to construct a multifunctional integrated molecular structure with "polycarboxylated amino modified biodegradable backbone, side chain salt-resistant thickening, and overall scale inhibition properties". The drag reduction rate of the obtained polycarboxylated amino modified biodegradable scale inhibitor and salt-resistant thickener (JSIKYP-1~JSIKYP-13) at an addition of 0.08wt% was significantly higher than that of the thickeners (DBP-1~DBP) obtained in Comparative Examples 1-2 without the introduction of a biodegradable backbone. The drag reduction rate of DBP-2) is at least 3.1% higher than that of the thickeners (DBP-3 to DBP-4) obtained without the introduction of polycarboxylated amino compounds in Comparative Examples 3 to 4, at least 1.7% higher than that of the thickeners (DBP-5 to DBP-6) obtained without the introduction of long-chain alkyl unsaturated silanes in Comparative Examples 5 to 6, at least 2.4% higher than that of the thickeners (DBP-7 to DBP-8) obtained without the introduction of thickening monomers in Comparative Examples 7 to 8, and at least 8.4% higher than that of the thickeners (DBP-9 to DBP-10) obtained without the introduction of salt-resistant functional monomers in Comparative Examples 9 to 10, and 11.7% higher than that of the thickeners (DBP-9 to DBP-10) obtained without the introduction of salt-resistant functional monomers in Comparative Examples 9 to 10. This indicates that the simultaneous introduction of a biodegradable main chain backbone, polycarboxylated amino compounds, long-chain alkyl unsaturated silanes, thickening monomers, and salt-resistant functional monomers can significantly improve the salt resistance of the thickener in high-salinity brine, making the thickener molecular chain more extended and viscoelastic, thereby achieving a significant viscoelastic drag reduction effect.
[0081] The temperature and shear resistance of the polycarboxylated amino-modified biodegradable scale inhibitors and salt-resistant thickeners obtained in Examples 1-13 and Comparative Examples 1-10 at a dosage of 0.6 wt% were tested using the above methods. The results are listed in Table 4 and Figure 5 .
[0082] Table 4. Test results of the temperature resistance and shear strength of the thickener
[0083] As shown in Table 4 and Figure 5As shown, in Examples 1-13, polycarboxylated amino compounds were first grafted onto the biodegradable backbone of polyepoxysuccinic acid or polysuccinimide. Then, salt-resistant functional monomers and thickening monomers containing sulfonic acid groups were introduced through long-chain alkyl unsaturated silane graft copolymerization to construct a multifunctional integrated molecular structure with "polycarboxylated amino modified biodegradable backbone, side chain salt-resistant thickening, and overall scale inhibition properties". The stable viscosity of the obtained polycarboxylated amino modified biodegradable scale inhibitor and salt-resistant thickener (JSIKYP-1~JSIKYP-13) in the temperature resistance shear test at an addition of 0.6wt% was significantly higher than that of the thickeners (DBP-1~DBP-13) obtained in Comparative Examples 1-2 without the introduction of a biodegradable backbone. 2) The stable viscosity is at least 9.4% higher, at least 7.5% higher than the stable viscosity of the thickeners (DBP-3~DBP-4) obtained without the introduction of polycarboxylated amino compounds in Comparative Examples 3~4, especially at least 24.7% higher than the stable viscosity of the thickeners (DBP-5~DBP-6) obtained without the introduction of long-chain alkyl unsaturated silanes in Comparative Examples 5~6, at least 39.6% higher than the stable viscosity of the thickeners (DBP-7~DBP-8) obtained without the introduction of thickening monomers in Comparative Examples 7~8, and particularly 109.9% higher than the stable viscosity of the thickeners (DBP-9~DBP-10) obtained without the introduction of salt-resistant functional monomers in Comparative Examples 9~10. This indicates that the simultaneous introduction of a biodegradable main chain backbone, polycarboxylated amino compounds, long-chain alkyl unsaturated silanes, thickening monomers, and salt-resistant functional monomers can not only significantly improve the salt-resistant thickening performance of the thickener in high-saltification brine, but also significantly improve the temperature resistance and shear resistance of the resulting thickener in high-saltification brine.
[0084] The static sand suspension performance of the polycarboxylated amino-modified biodegradable scale inhibitors and salt-resistant thickeners obtained in Examples 1-13 and Comparative Examples 1-10 at a dosage of 0.6 wt% was tested using the above methods. The results are listed in Table 5 and Figure 6 .
[0085] Table 5. Static suspension performance test results of thickener
[0086] As shown in Table 5 and Figure 6As shown, in Examples 1-13, polycarboxylated amino compounds were first grafted onto the biodegradable backbone of polyepoxysuccinic acid or polysuccinimide. Then, salt-resistant functional monomers and thickening monomers containing sulfonic acid groups were introduced through long-chain alkyl unsaturated silane graft copolymerization to construct a multifunctional integrated molecular structure with "polycarboxylated amino modified biodegradable backbone, side chain salt-resistant thickening, and overall scale inhibition properties". The resulting polycarboxylated amino modified biodegradable scale-inhibiting and salt-resistant thickeners (JSIKYP-1~JSIKYP-13) with a proppant sedimentation rate at 0.6wt% was at least lower than that of the thickeners (DBP-1~DBP-2) obtained in Comparative Examples 1-2 without the introduction of a biodegradable backbone. The sedimentation rate of the proppant was 15.38%, which is at least 5.17% lower than that of the thickeners (DBP-3 to DBP-4) obtained without the introduction of polycarboxylated amino compounds in Comparative Examples 3 and 4. In particular, it is at least 9.84% lower than that of the proppants (DBP-5 to DBP-6) obtained without the introduction of long-chain alkyl unsaturated silanes in Comparative Examples 5 and 6. It is at least 29.49% lower than that of the proppants (DBP-7 to DBP-8) obtained without the introduction of thickening monomers in Comparative Examples 7 and 8. In particular, it is at least 40.22% lower than that of the proppants (DBP-9 to DBP-10) obtained without the introduction of salt-resistant functional monomers in Comparative Examples 9 and 10. This indicates that the simultaneous introduction of a biodegradable main chain backbone, polycarboxylated amino compounds, long-chain alkyl unsaturated silanes, thickening monomers, and salt-resistant functional monomers can not only significantly improve the salt-resistant thickening and temperature-resistant shear resistance of the thickener in high-salt water, but also significantly improve the proppant carrying capacity of the obtained thickener in high-salt water.
[0087] The debonding properties of the polycarboxylated amino-modified biodegradable scale inhibitors and salt-resistant thickeners obtained in Examples 1-13 and Comparative Examples 1-10 were tested using the above methods at an addition of 0.6 wt% and 0.025 wt% ammonium persulfate, and the results are listed in Table 6.
[0088] Table 6. Test results of the thickener's gel breaking performance.
[0089] As shown in Table 6, in Examples 1-13, polycarboxylated amino compounds were first grafted onto the biodegradable backbone of polyepoxysuccinic acid or polysuccinimide. Then, salt-resistant functional monomers and thickening monomers containing sulfonic acid groups were introduced through long-chain alkyl unsaturated silane graft copolymerization to construct a multifunctional integrated molecular structure with "polycarboxylated amino modified biodegradable backbone, side chain salt-resistant thickening, and overall scale inhibition properties". The obtained polycarboxylated amino modified biodegradable scale inhibitor and salt-resistant thickeners (JSIKYP-1~JSIKYP-13) could be completely broken down within 2 hours at 90°C with an addition of 0.6 wt% and at 0.025 wt% ammonium persulfate, and the viscosity of the broken solution was 4.85 mm.2 The debonding performance is comparable to that of the thickeners (DBP-1 to DBP-10) obtained in Comparative Examples 1 to 10, with a speed of less than 1 / s. This indicates that the simultaneous introduction of a degradable main chain backbone, polycarboxylated amino compounds, long-chain alkyl unsaturated silanes, thickening monomers, and salt-resistant functional monomers containing sulfonic acid groups can not only significantly improve the salt-resistant thickening performance, temperature resistance, shear resistance, and proppant carrying capacity of the thickener in high-salinity brine, but also ensure that the thickener still has good debonding performance in high-salinity brine, resulting in a low risk of reservoir damage.
[0090] The scale inhibition performance of the polycarboxylated amino-modified biodegradable scale inhibitors and salt-resistant thickeners obtained in Examples 1-13 and Comparative Examples 1-10 was tested using the above method at an addition of 0.6 wt% and 0.025 wt% ammonium persulfate. The results are listed in Table 7.
[0091] Table 7. Test results of scale inhibition performance of thickener-breaking solution
[0092] As shown in Table 7 and Figure 7As shown, in Examples 1-13, polycarboxylated amino compounds were first grafted onto the biodegradable backbone of polyepoxysuccinic acid or polysuccinimide. Then, salt-resistant functional monomers and thickening monomers containing sulfonic acid groups were introduced through long-chain alkyl unsaturated silane graft copolymerization to construct a multifunctional integrated molecular structure with "polycarboxylated amino modified biodegradable backbone, side chain salt-resistant thickening, and overall scale inhibition properties". The resulting polycarboxylated amino modified biodegradable scale inhibitor and salt-resistant thickeners (JSIKYP-1~JSIKYP-13) showed scale inhibition rates of 98.2%, 96.1%, and 92.2% for CaCO3, CaSO4, and BaSO4 respectively when added at 0.6wt%, which were higher than those of the thickeners (DBP-1~DBP-10) obtained in Comparative Examples 1-10. Further comparison showed that the scale inhibition rates of the gelled solutions of the obtained thickeners JSIKYP-1 to JSIKYP-13 for CaCO3, CaSO4, and BaSO4 were at least 21.4%, 26.6%, and 39.0% higher, respectively, than those of the thickeners (DBP-1 to DBP-2) obtained in Comparative Examples 1 and 2 without the introduction of a degradable main chain backbone. These rates were also higher than those of the thickeners (DBP-3 to DBP-4) obtained in Comparative Examples 3 and 4 without the introduction of polycarboxylated amino compounds. Furthermore, these rates were higher than those of the thickeners (DBP-9 to DBP-10) obtained in Comparative Examples 9 and 10 without the introduction of salt-resistant functional monomers. This indicates that the introduction of a biodegradable main chain backbone, polycarboxylated amino compounds, and salt-resistant functional monomers containing sulfonic acid groups can achieve excellent scale inhibition performance after the thickener breaks down through the synergistic effect of the bulk scale inhibition function of the biodegradable main chain backbone, the enhanced scale inhibition function of the polycarboxylated amino compounds, and the chelating scale inhibition function of the salt-resistant functional monomers containing sulfonic acid groups.
[0093] In summary, this invention first grafts a polycarboxylated amino compound onto the biodegradable backbone of polyepoxysuccinic acid or polysuccinimide, and then introduces salt-resistant functional monomers and thickening monomers containing sulfonic acid groups through long-chain alkyl unsaturated silane graft copolymerization. This constructs a multifunctional integrated molecular structure with "polycarboxylated amino modified biodegradable backbone, side-chain salt-resistant thickening, and overall scale inhibition properties." The resulting polycarboxylated amino modified biodegradable scale inhibitor and salt-resistant thickener has the characteristics of fast dissolution, high biodegradability, easy gel breaking, high scale inhibition rate, strong salt resistance, high drag reduction rate, and good sand carrying capacity. It can solve the problems of excessive dosage of biodegradable thickeners in the prior art and the lack of salt resistance and scale inhibition function under high salinity conditions. The present invention can achieve the following technical effects: the biodegradation rate of the thickener reaches over 60.2% after 28 days; the apparent viscosity (viscosity at 2 min) of a 0.6wt% thickener solution under high mineralization conditions (total calcium and magnesium ion content 3000mg / L) is over 82mPa·s, and the stable viscosity after shearing at 120℃ for 120 min is over 57.1mPa·s; the scale inhibition rate of the 0.6wt% thickener solution for CaCO3 is over 98.2%, for CaSO4 it is over 96.1%, and for BaSO4 it is over 92.2%; the drag reduction rate of a 0.08wt% thickener solution is over 75.2%, and in the static suspended sand test, the settling rate of the 30-50 mesh ceramsite proppant in the 0.6wt% thickener solution at a sand ratio of 30% (v / v) is below 0.55cm / min.
[0094] Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener, characterized in that, The raw materials for its preparation, by mass percentage, include: 8%~15% of a biodegradable main chain backbone, 2%~6% of a polycarboxylated amino compound, 3%~5% of a long-chain alkyl unsaturated silane, 10%~18% of a thickening monomer, 8%~15% of a salt-resistant functional monomer containing sulfonic acid groups, 0.1%~0.4% of an initiator, and the balance being water; the biodegradable main chain backbone is polyepoxysuccinic acid or polysuccinimide; the polycarboxylated amino compound is N,N'-ethylenediaminedisuccinic acid, N-(2-aminoethyl)-N-(carboxymethyl)-glycine or iminodiacetic acid.
2. The polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener according to claim 1, characterized in that, The long-chain alkyl unsaturated silane is 10-undecenyltrimethoxysilane or 10-undecenyltrichlorosilane.
3. The polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener according to claim 1, characterized in that, The thickening monomer is acrylamide or acrylic acid.
4. The polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener according to claim 1, characterized in that, The salt-resistant functional monomer containing sulfonic acid groups is 2-acrylamido-2-methylpropanesulfonic acid, vinylbenzenesulfonic acid, allylbenzenesulfonic acid, or acrylamidobenzenesulfonic acid.
5. The polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener according to claim 1, characterized in that, The initiator is a composite system of persulfate and sodium bisulfite.
6. The polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener according to claim 1, characterized in that, The viscosity-average molecular weight of the polycarboxylated amino-modified biodegradable scale inhibitor and salt thickener is 720-1120 million Daltons.
7. A method for preparing a polycarboxylated amino-modified biodegradable scale inhibitor and anti-salt thickener, characterized in that, The polycarboxylated amino-modified degradable scale inhibitor and salt-resistant thickener is the polycarboxylated amino-modified degradable scale inhibitor and salt-resistant thickener according to any one of claims 1 to 6, comprising the following steps: Step S1: The biodegradable main chain backbone is reacted with a polycarboxylated amino compound in water to obtain a reaction solution containing product A. Step S2: Add an aqueous solution of long-chain alkyl unsaturated silane in ethanol to the reaction solution containing product A, and react to obtain a reaction solution containing product B. Step S3: Add thickening monomer and salt-resistant functional monomer containing sulfonic acid group to the reaction solution containing product B, heat to 65~70℃, add initiator aqueous solution, carry out polymerization reaction, and obtain graft copolymer colloid. Step S4: The graft copolymer colloid is washed, dried, pulverized and sieved in sequence to obtain a dry powder of polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener.
8. The preparation method of the polycarboxylated amino-modified biodegradable scale inhibitor and anti-salt thickener according to claim 7, characterized in that, Step S1 is as follows: Under stirring, the biodegradable main chain backbone is added to water, the pH value is adjusted to 9.5~10, a polycarboxylated amino compound is added, and the reaction is carried out at 50~60℃ for 20~24h to obtain a reaction solution containing product A.
9. The preparation method of the polycarboxylated amino-modified biodegradable scale inhibitor and salt-resistant thickener according to claim 7, characterized in that, Step S3 specifically involves: adding a thickening monomer and a salt-resistant functional monomer containing sulfonic acid groups to the reaction solution containing product B, adjusting the pH to 6.5-7.5, and purging with an inert gas to remove oxygen for 25-30 minutes; heating to 65-70°C, adding an initiator aqueous solution, and carrying out a polymerization reaction for 5-6 hours to obtain the graft copolymer colloid.
Citation Information
Patent Citations
A method for preparing an integrated fracturing emulsion with anti-scaling, drag-reducing, and thickening properties.
CN115322283B
Polyasparagine derivative thickeners with side chains containing straight-chain alkyl chains and lysine
CN115449074B
Low-molecular scale-inhibiting thickening agent for deep coal and rock gas reservoir fracturing and preparation method of low-molecular scale-inhibiting thickening agent
CN120965932A