Coated glass or glass-ceramic substrate and method for coating a substrate
Patent Information
- Application Number
- DE502018016817
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-11-22
- Filing Date
- 2018-11-22
- Publication Date
- 2026-11-05
- Estimated Expiration
- 2038-11-22
AI Technical Summary
Existing coatings for glass or glass-ceramic substrates with low thermal expansion coefficients face challenges in maintaining strength and temperature resistance, particularly when exposed to high thermal stresses, and are prone to fluid penetration, leading to reduced mechanical strength and aesthetic issues.
A coating with closed pores is applied to the substrate, acting as a barrier against fluid penetration and providing self-sealing properties, maintaining strength and temperature stability even at high temperatures.
The coating effectively prevents fluid ingress, maintains mechanical strength, and ensures thermal stability, allowing for use in applications where high temperatures are encountered without visible fluid penetration or strength reduction.
Description
Field of invention
[0001] The disclosure relates generally to coated glass or glass-ceramic substrates, preferably those with high temperature resistance, high strength, and a low coefficient of thermal expansion. Further aspects of the disclosure relate to a coating comprising pores and being fluid-tight and suitable for coating a glass or glass-ceramic substrate, preferably a glass or glass-ceramic substrate with a low coefficient of thermal expansion, as well as a method for coating such a substrate. Background of the invention
[0002] Coatings for glass or glass-ceramic substrates, especially glass or glass-ceramic substrates with a low coefficient of thermal expansion, for example for low-expansion glasses from the family of silicate glasses or for glass-ceramics, have been known for many years.
[0003] Special challenges arise for such coatings, particularly when the excellent strength properties of these substrates need to be maintained after coating, while simultaneously requiring high temperature resistance. In the case of decorative coatings used, for example, on glass or glass-ceramics exposed to high thermal stresses during operation, not only must the thermal stability of the coating's optical appearance and its adhesion to the substrate be ensured, but other properties are also important. These include scratch resistance, compatibility with adhesives used for mounting such glass or glass-ceramics, for example, in fixtures or for attaching components, and the coating's interaction with fluids.
[0004] For example, it is known that underside coatings of transparent, non-volume-colored, disc-shaped glasses or glass-ceramics used in cooktops must either be dense or require a second layer that is impermeable to fluids such as gases and liquids. Otherwise, if there is continuous porosity, fluids that form during the use of a cooktop, such as condensation, can penetrate the coating. This leads at least to optical changes in the coating; depending on the type of fluid, it can also cause damage to the glass or glass-ceramic.
[0005] These requirements apply not only to underside coatings for cooktops, for example, but also to other applications, such as viewing windows used in ovens or fireplaces. Here, too, the goal is to prevent fluids from passing through the coating. For instance, adhesive seams and similar features should not be visible, and it should be ensured that fluids generated during the operation of a device, such as an oven or fireplace, do not become visible as soiling through the coating. This is not only an aesthetic consideration but also serves to protect the substrate material, which can potentially be attacked by such fluids. Such corrosive attack can, for example, reduce the strength of a coated substrate and thus lead to decreased user safety.
[0006] Coatings for glasses or glass ceramics, in particular glasses or glass ceramics with a low coefficient of thermal expansion, are known in the prior art.
[0007] For example, international patent application WO 2012 / 167932 A1 describes a purely inorganic layer that can be applied without cracking and has a temperature resistance of up to 1000°C. However, the layer is porous.
[0008] International patent application WO 2013 / 156617 A1 describes a dense, non-porous layered composite, wherein a first layer is applied, which is porous, and the resulting pores are filled with a second, polymeric material. Due to this organic filling of the pores, the coating has limited temperature stability and is particularly unsuitable for use at high temperatures above 400°C.
[0009] The international patent application WO 2010 / 081531 A1 relates to a porous sol-gel coating.
[0010] Similarly, the German patent application DE 10 2008 031 426 A1, the German patent application DE 10 2008 040 636 A1 and the US patent application US 2010 / 0047556 A1 only describe porous layers based on sol-gel coatings.
[0011] The porosity of these layers is deliberately adjusted to compensate for the differences in the coefficients of thermal expansion between the layer and the substrate. This ensures that the heating and cooling of the layered composite during normal use does not induce such high thermomechanical stresses that the coated glass or glass-ceramic substrate loses sufficient mechanical strength. This is particularly relevant when the coating is applied to the underside or back of the glass or glass-ceramic substrate, i.e., the side facing away from the user during operation. In such cases, the mechanical load is applied from above or from the front, so any potential stresses on the underside or back are mitigated.Cracks located on the reverse side can severely impair the impact and flexural strength of the glass or glass ceramic, for example to such an extent that minimum strength requirements are no longer met.
[0012] European patent application EP 1 401 781 A2 describes a coating with inorganic foams for the thermal insulation of devices. Carbonate is used as one of the foaming agents. A decorative covering is not addressed.
[0013] Porous coatings for glasses or glass ceramics are also known from German patent DE 100 14 373 C2 and European patent EP 1 267 593 B1.
[0014] However, difficulties arise with these porous coatings when, as explained above, fluids come into contact with them, for example, in addition to water and oil, also food or adhesives. To seal the pores, it is also known to apply, for example, a silicone-based sealant, as described in US patent application US 2013 / 0266781 A1.
[0015] However, such sealants always present two problems: Firstly, they are generally not sufficiently temperature-stable for use at very high temperatures, for example > 400°C.
[0016] Sealing the pores negates the positive effect of mitigating thermal stresses, which result from the different coefficients of thermal expansion between the layer and the substrate. Therefore, under very high temperatures, not only does the seal fail in terms of its sealing effect, but it also suffers a significant reduction in strength, for example, through cracking.
[0017] Therefore, the known coatings can only address applications where the maximum operating temperature is in the range of up to 400°C.
[0018] There is therefore a need for the provision of liquid-tight coatings for glass or glass-ceramic substrates, especially those with a low coefficient of thermal expansion. Object of the invention
[0019] The object of the invention is generally to mitigate the known weaknesses of coated glass or glass-ceramic substrates, in particular with regard to the density and temperature stability of the coating.
[0020] For glass-ceramics and glasses with low coefficients of thermal expansion, there are currently no economically viable decorative coatings with adapted coefficients of thermal expansion. A significant disadvantage, particularly with full-surface coatings or dense decorations, is the reduction in flexural strength. While it is possible to circumvent this problem of reduced flexural strength with a very light, i.e., very thin, coating, this precludes full-surface layers for protection or optically denser decorations as a design option.
[0021] The object of the invention relates in particular to the provision of glass or glass-ceramic substrates, preferably with a low coefficient of thermal expansion, wherein the substrate comprises a coating.
[0022] Another aspect of the disclosure concerns the provision of coatings which include pores and are self-sealing.
[0023] A further aspect of the disclosure includes a method for coating a glass or glass-ceramic substrate with such a layer. Summary of the invention
[0024] The object of the invention is achieved by the subject matter of the independent claims. Preferred embodiments are found in the dependent claims.
[0025] The glass or glass-ceramic substrate of the present disclosure is provided with a coating comprising closed pores, wherein the coating is designed as a barrier against the passage of fluids, e.g. water or water vapor.
[0026] The present disclosure therefore provides a glass or glass-ceramic substrate with a coating comprising closed pores, wherein the coating is designed as a barrier against the ingress and passage of fluids and exerts a barrier effect.
[0027] In this way, fluids that come into contact with the coated substrate during its intended use are not visible and disruptive within the coating itself. In particular, this prevents the fluid from penetrating the coating, making it virtually "water-resistant." A coating is therefore described as "water-resistant" or H₂O-resistant, as defined in the disclosure, if no water vapor penetrates the layer.
[0028] This is particularly advantageous for full-surface coatings, since, according to the present disclosure, coatings can be arranged in the form of an underside or backside coating, for example, facing the inside of an oven, and thus, in intended use, on the side of the glass or glass-ceramic substrate facing away from the user. In such cases, it is particularly advantageous that no condensation or shadows of condensation are visible when viewed from the outside, i.e., from the side of the glass or glass-ceramic substrate opposite the coating.
[0029] In general, however, it is also possible and may even be preferred that the coating according to the present disclosure is not applied over the entire surface, but, for example, only with a coverage of 40% or more, e.g. for frame printing on fireplace viewing windows or for oven windows.
[0030] Provided the substrate is designed as a transparent, non-volume-colored substrate, the barrier effect of the coating can be determined, for example, in a test in which a drop of a fluid medium, e.g., water, is applied to the coating and then left to act for at least 10 seconds and is wiped off after the exposure, whereby the point of contact of the drop is not recognizable as such when viewing the coating through the substrate if this test is passed.
[0031] Such inspection methods are generally known as visual inspection and are carried out in accordance with the relevant standards, such as DIN EN 1330-10, DIN 25435-2, and DIN EN 13018. In this case, a direct or indirect visual inspection by an inspector is preferred. In direct visual inspection, the inspection is performed with an uninterrupted beam path between the inspector's eye and the surface being inspected, whereas in indirect visual inspection, the beam path is interrupted due to the image being captured by suitable photographic or video technology passing through the surface being inspected. Furthermore, a local visual inspection according to DIN EN 13018 is preferred, which defines a minimum illuminance, a distance to the surface being inspected, and a viewing angle for the inspector.
[0032] The minimum illuminance used during testing is at least 500 × on the test surface from a distance of less than 600 mm. The tester's viewing angle is at least 30°. The tester preferably meets the requirements specified in the relevant standards, such as DIN EN 13018 and EN 473.
[0033] Such a test method is particularly preferred because it can be easily adapted to the specific applications of the coated glass or glass-ceramic substrates. For example, the exposure time is usually selected depending on the fluid medium under consideration and can also exceed 10 seconds.
[0034] Fluids within the meaning of the present disclosure preferably comprise liquids, in particular water, aqueous liquids, alcohols, liquids based on or comprising these liquids, such as window cleaners, and / or oils, as well as water vapor.
[0035] A preferred procedure for carrying out a visual inspection by an inspector as explained above, with the aim of determining the water tightness or moisture tightness of a coating in accordance with the present disclosure, comprises the following steps: Applying a liquid to an area on the surface of the substrate's coating, allowing the liquid to act for 15 seconds, wiping off any residual moisture with a dry cloth, turning the substrate over so that the coating is on the side facing away from the inspector, and visually checking whether a color change is visible in the area or an area adjacent to it, wherein a) the visual inspection is carried out under daylight according to standard illuminant D65 or under illumination such as an incandescent lamp, energy-saving lamp, fluorescent lamp, or light-emitting diode, b) the illuminance is at least 500 × at a distance of less than 600 mm from the coating, i.e., the test surface, and c) the inspector's viewing angle is between 5° and 90°, preferably at least 30°.wherein, in the glass or glass-ceramic substrate according to the invention, when viewing the coating through the substrate, the point of contact of the droplet is not disturbingly visible and, in particular, not recognizable as such.
[0036] The aforementioned visual inspection includes, in particular, checking whether a water stain and / or a water mark is visible from the side of the substrate opposite the coated side.
[0037] Preferably, the aforementioned steps of visual inspection are carried out with different liquids, i.e. fluids, including water, alcohol and / or window cleaner (e.g. "Sidolin" or "Ajax"). Preferably, the glass or glass-ceramic substrate has a low coefficient of thermal expansion, preferably a coefficient of thermal expansion of less than 5*10 -6< / K in the temperature range of 20°C to 700°C.
[0038] In the context of this disclosure, the term thermal expansion coefficient is the nominal mean coefficient of linear thermal expansion according to ISO 7991, which is determined by static measurement.
[0039] According to a further embodiment of the disclosure, the coating is designed as a high-temperature-stable, self-sealing coating.
[0040] A coating is described as self-sealing if no further coating is necessary to ensure sufficient impermeability against the ingress or penetration of fluids. The layer thus exhibits a barrier effect against fluids. The pore-encompassing coating according to embodiments of this disclosure is therefore self-sealing, for example, acting as a barrier against the penetration of fluids.
[0041] Furthermore, a high-temperature stable coating is characterized by the fact that, when used on a hotplate during normal, intended heating by IR radiation or induction heating, it shows no change in color, adhesion to the substrate or transmission after cooling compared to before heating.
[0042] Within the scope of this disclosure, a coating is therefore described as high-temperature stable if, after a thermal stress, for example a stress to verify its suitability for IR radiant heating or induction heating as described above, it does not exhibit any deviations within the measurement accuracy that are significant, for example, in transmission, in particular in τ vis (in-line transmission) in the wavelength range of visible light (from approximately 380 nm wavelength to less than or equal to 700 nm), in strength, in particular determined by the value of the ball drop test, and / or in barrier effect against the passage of fluids between the state before the thermal stress and the state after the thermal stress.
[0043] Within the scope of this disclosure, the terms layer and coating are used synonymously in the sense that, unless expressly stated otherwise, a layer, like a coating, is considered to be a layer of material obtained by applying a coating material, for example a printing ink, to a substrate; thus, both a layer and a coating are layers of material obtained by a coating process.
[0044] For the purposes of this disclosure, a substrate is understood to be a product whose surface is refined or is to be refined. In particular, a substrate is understood to be a product whose surface is to be coated or is coated.
[0045] In the context of this disclosure, the substrate is generally thicker than the layer or coating applied to it. It can generally be assumed that the layer has a thickness of no more than 500 µm. A substrate, on the other hand, will have a thickness of 1 mm or more.
[0046] A substrate is considered disc-shaped if its spatial extent in one direction of a Cartesian coordinate system is at least one order of magnitude smaller than in the other two directions perpendicular to that direction. The smallest lateral dimension of a product, such as a substrate, is generally referred to as its thickness, while the other two lateral dimensions are typically called length and width. The lateral dimensions of a product, such as a substrate, are determined by its bounding surfaces. If a product, such as a substrate, is disc-shaped, it generally has two principal surfaces arranged perpendicular to its thickness.Depending on the precise spatial arrangement, these main surfaces are referred to as the top (facing the viewer) and the bottom (the side of the product, such as the substrate, facing away from the viewer) in the case of horizontal storage of the product, such as a substrate; in the case of vertical storage of the product, such as a substrate, they are generally referred to as the front (facing a viewer or user) and the back (facing away from a viewer or user).
[0047] For the purposes of this disclosure, a substrate can, for example, be a flat or a curved disc.
[0048] A pigment is generally understood to be a colorant, that is, a substance that imparts color. Unlike dyes, they consist of particles and are therefore practically insoluble in the application medium. Pigments can be distinguished according to their chemical structure (inorganic or organic), their optical properties (white, colored, black, special effects), and their technical properties (corrosion protection, magnetism). The color perception arises from the absorption and remission (scattering or reflection) of specific frequency components of visible light. Solid-state properties such as crystal structure, crystal modification, particle size, and particle size distribution, the latter determined by the specific surface area, are also crucial for the properties of pigments.
[0049] Furthermore, pigments are known that are used to create a specific optical effect, particularly a metallic appearance. Such pigments are also called effect pigments. Effect pigments include, for example, platelets or flakes of metal, mica, glass, or another inorganic, usually transparent material, such as SiO₂ or Al₂O₃. Through a specific coating design of such transparent platelets, not only can a particular reflection occur, but also color effects resulting from interference. Coating materials for creating specific effects can include SiO₂ and TiO₂. Materials that themselves absorb light, such as iron oxides, may also be used as coatings.
[0050] An example of such effect pigments are the mica-based effect pigments known under the brand name "Iriodin".
[0051] For the purposes of this disclosure, a suspension is understood to be a slurry of a solid component in a liquid. By way of example, the term suspension includes slurries, where a slurry consists of a slurry of essentially, i.e., at least 95% by weight (based on the solids content), inorganic material in a liquid. The liquid itself can be aqueous or organic, for example, containing an organic solvent. Such slurries typically have a solids content between 40% and 80% by weight, based on the total weight of the slurry.
[0052] For the purposes of this disclosure, the term "suspension" also includes, by way of example, printing inks or printing pastes which have a powder-to-medium ratio of 10:12 to 10:2.5 and viscosities (determined by plate viscometer) which are between 2000 and 10000 mPas at a rotational speed of 200 / s.
[0053] Tg denotes the glass transition temperature or transformation temperature of a glass. The transformation temperature Tg is determined by the intersection point of the tangents to the two branches of the expansion curve when measured at a heating rate of 5 K / min. This corresponds to a measurement according to ISO 7884-8 or DIN 52324.
[0054] For example, the coating described in this disclosure may comprise a glaze or an enamel. Glazes are generally defined as coating materials consisting of clear or colored glass, also known as glass flux. Enamels are coating materials that, in addition to glass flux, also include materials such as color and / or effect pigments.
[0055] Glazes and enamels have also been known for a long time. They are fired at temperatures that are generally below the softening temperature of the substrate to be coated, in order to prevent warping during firing. During this process, the specific composition of the glass flux melts and bonds stably to the surface of the substrate. Firing also serves to volatilize any organic additives used, such as those that act as suspension agents for applying the coating.
[0056] When coating glass or glass-ceramic substrates with a coefficient of thermal expansion of 5 x 10⁻⁶ K / K or more, it is possible to find glazes or enamels with adapted coefficients of thermal expansion. However, this is not possible for substrates with a low coefficient of thermal expansion. To avoid a critical reduction in the strength of the substrate, the coating of this disclosure is therefore designed to include pores. For this purpose, the suspension of this disclosure comprises, in addition to the glass powder, an agent that decomposes upon temperature increase to form a volatile substance.
[0057] By way of example, the closed-pore coating of the present disclosure can therefore also be designed as a foam enamel according to one embodiment.
[0058] According to a further embodiment of the disclosure, the substrate is disk-shaped, wherein the thickness of the substrate is between at least 1 mm and at most 10 mm, preferably between at least 2 mm and at most 5 mm and particularly preferably between at least 2 mm and at most 4 mm.
[0059] According to a further embodiment, the closed-pore coating is arranged on the side of the substrate that faces away from the user during intended use. In particular, such a coating can be arranged on the back of a viewing window, such as a viewing window of an oven door, or a fireplace or oven viewing window.
[0060] Preferably, the coating is applied in a laterally structured manner such that at least one area of the glass or glass-ceramic substrate is free of the coating. This is advantageous, for example, when electro-optical display elements, such as displays, are arranged on the substrate.
[0061] The inventors assume that the coating comprising the closed pores according to the present disclosure exhibits a certain IR reflection in such a way that there is a reduction in the temperature of one side, in particular the uncoated front of a viewing window (the side facing away from the oven interior in the case of an oven door, or the side facing away from the chimney in the case of a chimney), for example an oven viewing window, such as the viewing window of an oven door, or the viewing window in a chimney or an oven, compared to a coating which comprises no pores or very few pores, in particular no or very few closed pores.
[0062] According to a further embodiment of the disclosure, the coating comprises color and / or effect agents, in particular a color pigment and / or an effect pigment, preferably an IR-reflecting color pigment.
[0063] Coloring pigments in the form of metal oxides can be used as pigments, especially metal oxides with a spinel structure, for example cobalt-containing spinels, in particular cobalt-aluminum oxide / spinel, cobalt-aluminum-zinc oxide / spinel, cobalt-aluminum-silicon oxide / spinel, cobalt-titanium oxide / spinel, cobalt-chromium oxide / spinel, cobalt-aluminum-chromium oxide / spinel, cobalt-nickel-manganese-iron-chromium oxide / spinel, cobalt-nickel-zinc-titanium-aluminum oxide / spinel, chromium-iron-nickel-manganese oxide / spinel, cobalt-iron-chromium oxide / spinel, Nickel-iron-chromium oxide / spinel, iron-manganese oxide / spinel, copper-chromium spinel, zirconium-silicon-iron oxide / spinel, as well as other oxides, for example iron oxides, iron-chromium oxides, iron-chromium-tin-titanium oxides, nickel-chromium-antimony-titanium oxide, or titanium oxide. Of course, mixtures of these pigments are also possible, especially to achieve special color effects.Graphite can also be used as a pigment.
[0064] According to one embodiment of the disclosure, the coating can comprise an IR-reflective color pigment. An IR-reflective color pigment is understood to be, in particular, a color pigment that exhibits a reflectance of at least 50% at a wavelength of 1500 nm. Due to the high reflectance of infrared (IR) radiation, a large portion of the thermal radiation is thus reflected. The reflectance was determined according to the measurement standard ISO 13468.
[0065] Furthermore, the pigment in this training course exhibits a TSR value of at least 20%. The TSR value ( total solar reflectance ) provides information about the percentage of reflected electromagnetic radiation in the wavelength range from 200 nm to 2500 nm and is determined according to the measurement standards ASTM G 173.
[0066] It has been shown that a high TSR value of the pigments also influences the remission behavior of a coating produced from the paste, even towards longer-wavelength thermal radiation. A high TSR value is advantageous for achieving high remission of thermal radiation, i.e., electromagnetic radiation in the 1 to 4 µm range. This is surprising because the wavelength ranges of thermal radiation and the wavelength range relevant for determining the TSR value only partially overlap. In particular, the TSR value, as a transmittance value for solar radiation, also refers to the wavelength range from 200 nm to 1000 nm, and thus to significantly shorter wavelengths.
[0067] According to one embodiment, the paste has at least one IR-reflective pigment with a TSR value of at least 25%. Alternatively or additionally, the pigment has a reflectance measured according to ISO 13468 of at least 60% or even at least 70% at a wavelength of 1500 nm.
[0068] One embodiment provides that the particles of the IR-reflective pigment have a particle size distribution with a d50 value in the range of 0.5 µm to 2 µm. This small particle size allows the paste to be applied even with fine-mesh screens, for example, screens with a thread count of 77 threads / cm or even 100 threads / cm, so that coatings or decorations with high graphic resolution can be produced using screen printing. Furthermore, the mesh size of the screen used, together with the oil content and powder densities, determines the coating thickness after firing. According to a preferred embodiment, the IR-reflective pigments have a particle size distribution with a d50 value in the range of 0.8 µm to 1.8 µm. According to one embodiment, the IR-reflecting pigments have particles with a specific surface area in the range of 1.1 to 8 m² / g, preferably in the range of 1.8 to 4.5 m² / g.
[0069] The table below lists some examples of screens used in screen printing. Sieve designation in the text Thread count (cm -1< ) Nominal yarn diameter (µm) Mesh size (µm) 77T 77 55 67 90T 90 48 55 100T 100 40 37
[0070] The pigment-containing coating is intended to reflect or remit radiation as effectively as possible, thereby ensuring that the glass or glass-ceramic of the respective coated substrate is heated as little as possible. In particular, within the scope of this disclosure, reflection and remission are to be as high as possible in a wavelength range corresponding to a temperature of approximately 150°C to a maximum of 500°C.
[0071] For the radiated power at different wavelengths, it is assumed that it is in the form of blackbody radiation, where the radiated spectrum is defined by the temperature. Consequently, the temperatures disclosed herein can be assigned to corresponding spectra of blackbody radiators with high accuracy.
[0072] Such a design of a glass or glass-ceramic substrate with a coating allows for the controllable reflection of thermal radiation. This is particularly advantageous when the glass or glass-ceramic substrate is designed, for example, as a viewing window for an oven, fireplace, or other combustion chamber. By designing the coating as an IR-reflective pigment, it is possible to increase the reflection of thermal radiation, i.e., IR radiation, into the combustion chamber, such as an oven, fireplace, or other combustion chamber. In this way, combustion processes can be made more efficient, or the energy consumption of an oven, for example, can be reduced because less thermal radiation is dissipated through the window.Such a design can result in a further reduction of the temperature at the front of a coated glass or glass-ceramic substrate.
[0073] It has been shown that chromium-containing color pigments, such as chromium-containing iron oxide, chromium-containing hematite, chromium-iron-nickel spinel, cobalt chromite spinel, indium manganese yttrium oxide, niobium tin sulfide oxide, tin zinc titanate, and / or cobalt titanate spinel, exhibit such IR-reflective properties. Preferably, IR-reflective color pigments with a black or black-brown color are used.
[0074] The corresponding pigments exhibit, in particular, high thermal stability and high chemical inertness towards the glass components of the glass powder in the paste, which is especially advantageous with regard to the firing of the paste to produce the corresponding enamel coating. According to one embodiment, the maximum possible firing temperature is not limited by the stability of the pigments. In a further development of the invention, this allows the paste to be fired onto a glass or glass-ceramic substrate at high temperatures in the range of 500 to 1000°C, so that the glass substrate can be thermally prestressed during the firing process.
[0075] The use of chromium-containing color pigments as IR-reflective pigments has proven particularly advantageous. Preferably, the coating comprises a chromium-containing iron oxide, a chromium-containing hematite, and / or a chromium-iron-nickel spinel as the IR-reflective color pigment. These color pigments have proven advantageous with regard to their spectral properties, especially their IR reflectance, as well as their temperature stability. The temperature stability of these color pigments is relevant not only for the use of the coated substrate, for example, in an oven door or a fireplace viewing window, but also for the manufacturing process of the corresponding coating, which includes curing at temperatures in the range of 500°C to 1000°C.
[0076] Preferably, the IR-reflective color pigment has a black or black-brown color. In particular, the IR-reflective color pigment is selected from the group containing elements of the pigments CI Brown 29, CI Green 17, and CI Black 7.
[0077] According to one embodiment of the invention, the glass powder contained in the paste has a particle size distribution with a d50 value in the range of 0.1 µm to 3 µm, and particularly in the range between 0.1 µm and 2 µm. Corresponding particle sizes ensure a homogeneous distribution of the pigments and the formation of a largely homogeneous glass layer during the firing process.
[0078] The glass in the paste preferably contains zinc oxide and / or bismuth oxide. Glass powders with a zinc oxide content in the range of 0.1 to 70 wt.%, and especially a zinc oxide content in the range of 0.1 to 30 wt.%, have proven particularly advantageous. Alternatively or additionally, the glass powder contains 0.1 to 70 wt.%, and especially 8 to 70 wt.%, bismuth oxide. The zinc oxide or bismuth oxide content in the embodiments described above has a particularly advantageous effect on the softening temperature of the glass. According to a further development of these embodiments, the glass powders have softening temperatures in the range of 500 to 950 °C. Preferably, the softening temperature is less than 800 °C, or even less than 750 °C, and particularly preferably less than 680 °C, but more than 450 °C. Due to the low softening temperatures, a homogeneous glass matrix is formed even at low firing temperatures.a glass flux from the glass powder. This allows glass substrates with different glass compositions (and therefore different softening temperatures) to be coated with the paste without reducing the viscosity of the glass substrate being coated during firing.
[0079] Furthermore, the bismuth oxide content in the glass increases the chemical resistance of the corresponding coating, i.e., the coating produced with the paste.
[0080] Since the glass matrix or glass flux in the coating of the coated substrate has the same composition as the glass powder in the paste, the information regarding the composition of the glass powder also applies accordingly to the composition of the glass matrix in the coating in some embodiments or further developments.
[0081] According to one embodiment of this further development, the glass powder in the paste or the glass matrix of the corresponding coating has the following composition in wt.%: SiO2 30-75 preferably 44-75 Al2O3 0-25 preferably 0.2-25, particularly preferably 2-25 B2O3 0-30 preferably 1-30, particularly preferably 5-30 Li 2 O 0-12 Na₂O 0-25 preferably 0-15 CaO 0-12 MgO 0-9 BaO 0-27 SrO 0-4 ZnO 0-35 preferably 0-20 Bi 2 O 3 0-5 TiO2 0-10 preferably 0-5 ZrO 2 0-7 As 2 O 3 0-1 Sb 2 O 3 0-1,5 F 0-3 Cl 0-1 preferably 0 H₂O 0-3.
[0082] Preferably, the glass has a minimum Al₂O₃ content of 0.2 wt.%, preferably at least 2 wt.%. Alternatively or additionally, the glass has a B₂O₃ content of at least 1 wt.%, preferably at least 5 wt.%.
[0083] It has also proven advantageous if the glass contains at least 1 wt% of an alkali oxide selected from the group consisting of Na2O, Li2O and K2O or mixtures of these oxides.
[0084] Alternatively or additionally, the glass comprises at least 1 wt% of another oxide or a mixture of oxides selected from the group consisting of CaO, MgO, BaO, SrO, ZnO, ZrO 2 , and TiO 2 .
[0085] According to another training, the glass has the following composition in wt.%: SiO2 6-65, preferably 10-65, particularly preferably 15-65 Al2O3 0-20 B2O3 0-40, preferably 1-30, particularly preferably 3-30 Li 2 O 0-12 Na₂O 0-18 K2O 0-17 CaO 0-17 MgO 0-12 BaO 0-38 SrO 0-16 ZnO 0-70 TiO2 0-5 ZrO 2 0-5 Bi 2 O 3 0-75 preferably 0-60, particularly preferably 5-60, most particularly preferably 10-60 CoO 0-5 Fe2O3 0-5 MnO 0-10 CeO 2 0-3 F 0-3 Cl 0-1 H₂O 0-3.
[0086] In a preferred embodiment of the further development, the glass has a minimum SiO₂ content of 10 wt.%, preferably at least 15 wt.%. Alternatively or additionally, the glass has a minimum Bi₂O₃ content of 5 wt.%, preferably at least 10 wt.%. Alternatively or additionally, the glass contains at least 1 wt.%, preferably at least 3 wt.%, of B₂O₃. Preferably, the total content of the alkali oxides Na₂O, Li₂O, and K₂O is at least 1 wt.%.
[0087] The glass contained in the paste or the glass flux in the corresponding coating can be, in particular, an alkali-free glass, an alkali-containing glass, a silicate glass, a borosilicate glass, a zinc silicate glass, a zinc borate glass, a zinc borosilicate glass, a bismuth borosilicate glass, a bismuth borate glass, a bismuth silicate glass, a phosphate glass, a zinc phosphate glass, an aluminosilicate glass, or a lithium aluminosilicate glass. According to one embodiment of the invention, the paste comprises glass powders with different glass compositions.
[0088] According to one embodiment of this further development, the coating exhibits a remission of at least 35% at a wavelength of 1500 nm, measured according to the measurement standard ISO 134 68.
[0089] It has been shown that a high TSR value of the pigments in the coating also influences the remission behavior of the manufactured coating with respect to thermal radiation. A high TSR value has proven advantageous for the remission of thermal radiation in a temperature range of 200 to 475 °C. This is surprising because the corresponding wavelength for the aforementioned temperature range has its maximum in the range of 1 µm to 4 µm, while the TSR value refers to the solar spectrum with significantly shorter wavelengths in the range of 200 nm to 1000 nm. According to a preferred embodiment, the pigment has a TSR value of at least 25%.
[0090] The pigments are homogeneously distributed within the glass matrix, hereinafter also referred to as the glass flux. According to one embodiment, the pigments have a particle size distribution with a d50 value in the range of 0.5 µm to 2 µm, preferably in the range of 0.8 µm to 1.8 µm. According to this embodiment, the pigments thus have a particle size that is below the wavelength of the thermal radiation to be reflected. Surprisingly, the layer nevertheless exhibits high reflectance for radiation in the IR range. For example, the layers according to the invention exhibit a reflectance of at least 35% at a wavelength of 1500 nm. According to a preferred embodiment, the reflectance at 1500 nm is at least 40% or even at least 45%.
[0091] In a further embodiment, the coating comprises at least a first and an IR-reflecting color pigment. The color of the coating can be adjusted, in particular, by means of the second IR-reflecting color pigment. Preferably, the coating comprises a cobalt chromite spinel, an indium manganese yttrium oxide, a niobium tin sulfide oxide, a tin zinc titanate, and / or a cobalt titanate spinel as the second IR-reflecting color pigment. The use of one of the color pigments from the group containing the elements CI Pigment Blue 36, CI Pigment Blue 86, CI Pigment Yellow 227, CI Pigment Yellow 216, CI Pigment Green 26, and CI Pigment Green 50 has proven to be particularly advantageous.
[0092] Preferably, the proportion of the second IR-reflecting pigment in the coating is 0.75 to 18.5 wt.%, particularly preferably 4.5 to 14 wt.%. According to one embodiment, the volume ratio between the volume of the second pigment and the volume of the first pigment is 0.03 to 0.6, preferably 0.05 to 0.56, and particularly preferably 0.14 to 0.47.
[0093] Such a design allows not only for a further reduction of the temperature on the front side of a coated glass or glass-ceramic substrate by means of the second IR-reflecting pigment, but also for the adjustment of the color point of the coating.
[0094] Platelet- or rod-shaped pigments, for example based on mica or iriodine, are preferred as effect pigments.
[0095] Advantageously, the substrate comprises an oxide glass or an oxide glass ceramic, preferably a silicate glass or a silicate glass ceramic, particularly preferably a lithium aluminum silicate glass ceramic.
[0096] According to another embodiment, the substrate comprises a soda-lime glass or a borosilicate glass. Preferably, the glass is thermally prestressed to increase its strength.
[0097] The coating can also include organic substances. These are generally incompletely decomposed residues of organic compounds that were added to the suspension, for example, in the form of solvents. They can also include residues of incompletely decomposed, organically based blowing agents. According to one embodiment, the coating is essentially inorganic. Essentially inorganic here means that the coating comprises at least 95% by weight of inorganic components, preferably at least 98% by weight of inorganic components, and particularly preferably at least 99% by weight of inorganic components. Most preferably, the proportion of inorganic components in the coating is 99.9% by weight or more.
[0098] According to a further embodiment of the disclosure, the thermal expansion coefficients of the substrate and the coating are matched such that the resulting thermal expansion coefficient of the coating and the thermal expansion coefficient of the substrate differ from each other by no more than 4*10 -6< / K in the temperature range from 20°C to 700°C.
[0099] In this context, the focus is on the resulting coefficient of thermal expansion of the coating, since the coating is generally an inhomogeneous material comprising materials with different coefficients of expansion, in particular glass flux, pores, and optionally a pigment and / or other components. Therefore, the relevant factor is not the resulting coefficient of thermal expansion that arises from the porous structure and the coefficients of thermal expansion of the individual components of the coating.
[0100] According to one embodiment of the disclosure, the resulting coefficient of thermal expansion of the coating has a value between at most 9*10 -6< / K and at least 3*10 -6< / K.
[0101] For example, the glass ceramic can be transparent and not colored by volume. By way of example, the glass ceramic can have a composition from one of the following composition ranges in wt.%: Element oxide Glass ceramic composition Area 1 Area 2 SiO2 66-70 50-80 Al2O3 >19,8-23 12-30 Li 2 O 3-4 1-6 MgO 0-1,5 0-5 ZnO 1-2,2 0-5 BaO 0-2,5 0-8 Na₂O 0-1 0-5 K2O 0-0,6 0-5 TiO2 2-3 0-8 ZrO 2 0,5-2 0-7 P2O5 0-1 0-7 Sb 2 O 3 Typical quantities 0-4 As 2 O 3 Typical quantities 0-2 CaO 0-0,5 0 SrO 0-1 0 For example, glass ceramics such as those sold under the name CERAN can still be used. ® , for example CERAN ® Cleartrans or Zerodur are distributed.
[0102] For example, the glass substrate can have a composition from one of the following composition ranges in wt.%: Element oxide Glass substrate composition (wt%) Area 1 Area 2 Area 3 Area 4 SiO2 60-80 60-85 40-55 65-80 Al2O3 <2 5-15 15-30 0-5 Li 2 O 0-5 0-5 0-5 0-20 MgO 0-5 0-5 2-10 0-15 ZnO 0-10 0-5 0-5 0-5 BaO 0-5 0-5 0-5 0-5 Na₂O 10-20 2,5-12,5 2,5-12,5 0-20 K2O 5-15 0-5 0-5 0-20 B2O3 0-3 12-25 12-25 0-5 P2O5 0-1 0-2,5 0-2,5 0-1 CaO 5-15 0-1 5-15 0-15 SrO 0-1 0-1 0-1 0-1 Sb 2 O 3 Typical quantities Typical quantities Typical quantities Typical quantities As 2 O 3 Typical quantities Typical quantities Typical quantities Typical quantities
[0103] Substrates based on soda-lime glass, aluminosilicate glass, or borosilicate glass can also be used, for example. Preferably, the glass is thermally or chemically tempered to increase its strength.
[0104] According to one embodiment of the disclosure, the coating has a thickness of at least 0.1 µm and at most 500 µm, preferably between at least 1 µm and at most 100 µm, and particularly preferably between at least 1.5 µm and at most 20 µm.
[0105] According to a further embodiment of the disclosure, the substrate is designed such that the coating is essentially opaque to electromagnetic radiation in the wavelength range of 380 nm to 780 nm, in particular such that components arranged below the substrate are not visible in the intended use.
[0106] The coating is essentially opaque, also referred to as "opaque", when τ vis (in-line transmission) in the wavelength range of visible light (from approximately 380 nm wavelength to less than or equal to 700 nm) assumes a value of less than 10%.
[0107] The invention relates to a method for coating a glass or glass-ceramic substrate, preferably a substrate with a low coefficient of thermal expansion, preferably with a coefficient of thermal expansion of less than 5 x 10⁻⁶ K / K in the temperature range of 20°C to 700°C. The applied coating is porous, thus forming a barrier against the passage of fluids.
[0108] The process includes the following steps: a. Preparation of a suspension. The suspension comprises a glass powder and an agent which decomposes upon heating to form a volatile substance.
[0109] Examples include agents that release gas. Preferably, these agents are designed such that their anions form gas within the temperature range of the viscous melt of the glass flux, and the cations of the agent are incorporated into the glass matrix without impairing the desired properties. Such agents are also referred to as blowing agents or foaming agents.
[0110] Phosphates are a possible anti-gas remedy.
[0111] In addition to the aforementioned inorganic substances, organic substances can also be used as antigas. These include, for example, substances that decompose at the temperatures considered here, producing gas, especially tartrates such as potassium bicarbonate, but also sugar, wood dust, wheat flour, or starch.
[0112] Certain oxides also decompose by releasing a gas, for example cerium(IV) oxide or manganese(IV) oxide.
[0113] Generally, an expanding or foaming agent is understood to be one that decomposes upon temperature increase, forming at least one substance that is volatile at the decomposition temperature of the expanding agent. The volatile substance in this context is understood to be, in particular, a gas. However, it should be noted that the volatile substance formed at the decomposition temperature may exist in a different state of matter after the coated substrate has cooled to room temperature. For example, if water vapor is formed as the volatile substance from an expanding agent at its decomposition temperature, it is possible that liquid water, rather than water vapor, will be present in the pores after the coated substrate has cooled.
[0114] Since the pores formed by the decomposition of an expanding agent are closed according to the present disclosure, it is assumed that the substance, which is volatile at decomposition temperature, can be present at least partially in the pores of the coating. However, this need not necessarily be in volatile form. For example, it is also possible that the substance, which is volatile at decomposition temperature, exists as a condensate at room temperature.
[0115] An exemplary list of suitable anti-flatulence remedies, which can be used alone or in combination, can be found in the following table. Substance group Examples Common name formula Sulfates plaster CaSO₄ * 2H₂O Anhydrite, cerium (IV) sulfate hydrate CaSO 4 Ce(SO4)2 * 2H2O Carbonates Potash K 2 CO 3 limestone CaCO3 Magnesite MgCO3 Phosphates Na 4 P 2 O 7 *10H 2 O Na₂H₂P₂O₇ *2H₂O NaHPO₄ * 2H₂O Borates borax Na 2 [B 4 O 5 (OH) 4 ]*8H 2 O Manganite Potassium permanganate KMnO 4 Silicates clay minerals, e.g. Kaolinite Al 4 [(OH) 8 Si 4 O 10 ] Carbide silicon carbide SiC Calcium carbide CaC 2 Organic substances Potassium hydrogen tartrate KC 4 H 5 O 6 wheat flour Carbohydrate, e.g. sugar Wood dust elements carbon C Oxide Cerium(IV) oxide CeO 2 Manganese(IV) oxide MnO 2 Silica gel SiO₂ * x H₂O Inorganic-organic mixtures Contains baking powder, disodium phosphate, sodium bicarbonate, starch
[0116] It has been shown that particularly advantageous results are achieved according to the invention with blowing agents comprising phosphates, especially with coating layer thicknesses between 0.1 µm and 500 µm.
[0117] Furthermore, advantageous results according to the invention were achieved with gas-blowing agents comprising starch. In particular, it has been shown that rice starch, corn starch, and potato starch are especially suitable as gas-blowing agents.
[0118] The spatial arrangement and shape of the pores can be influenced by the specific expanding agent used. This allows for the production of both porous enamels with largely symmetrical pores and porous enamels with anisotropic pores. The following table shows various expanding agents and the resulting pore shapes.
[0119] The glass powder is selected as an example from the following composition range in wt.%: SiO2 30-75 preferably 44-75 Al2O3 0-25 preferably 0.2-25, particularly preferably 2-25 B2O3 0-30 preferably 1-30, particularly preferably 5-30 Li 2 O 0-12 Na₂O 0-25 preferably 0-15 CaO 0-12 MgO 0-9 BaO 0-27 SrO 0-4 ZnO 0-35 preferably 0-20 Bi 2 O 3 0-5 TiO2 0-10 preferably 0-5 ZrO 2 0-7 As 2 O 3 0-1 Sb 2 O 3 0-1,5 F 0-3 Cl 0-1 preferably 0 H₂O 0-3.
[0120] The glass advantageously comprises a minimum Al 2 O 3 content of 1 wt.%, preferably of at least 2 wt.%.
[0121] According to a further advantageous embodiment, the glass comprises at least 1 wt.% B 2 O 3 , preferably at least 5 wt.%.
[0122] According to a further advantageous embodiment, the glass comprises at least 1 wt.% of an alkali oxide selected from the group consisting of Na 2 O, Li 2 O and K 2 O or mixtures of these oxides.
[0123] According to a further advantageous embodiment, the glass comprises at least 1 wt.% of a further oxide or a mixture of oxides selected from the group consisting of CaO, MgO, BaO, SrO, ZnO, ZrO 2 , and TiO 2 .
[0124] According to another embodiment, the glass is selected from the following composition range in wt.%: SiO2 6-65, preferably 10-65, particularly preferably 15-65 Al2O3 0-20 B2O3 0-40, preferably 1-30, particularly preferably 3-30 Li 2 O 0-12 Na₂O 0-18 K2O 0-17 CaO 0-17 MgO 0-12 BaO 0-38 SrO 0-16 ZnO 0-70 TiO2 0-5 ZrO 2 0-5 Bi 2 O 3 0-75 preferably 0-60, preferably 5-60, particularly preferably 10-60 CoO 0-5 Fe2O3 0-5 MnO 0-10 CeO 2 0-3 F 0-3 Cl 0-1 H₂O 0-3. The glass flux can be further selected from the following types of glass: alkali-free glasses, alkali-containing glasses, silicate glasses, borosilicate glasses, zinc silicate glasses, zinc borate glasses, zinc borosilicate glasses, bismuth borosilicate glasses, bismuth borate glasses, bismuth silicate glasses, phosphate glasses, zinc phosphate glasses, aluminosilicate glasses or lithium aluminosilicate glasses.
[0125] Of course, it is also possible that the glass powder comprises mixtures of different types of glass.
[0126] When preparing the suspension, it is possible to initially introduce only the glass powder into a suspending agent. The suspending agent is a liquid and can, for example, comprise water. Preferably, the suspending agent comprises solvents, such as organic solvents. The solvents preferably have a vapor pressure of less than 10 bar, more preferably less than 5 bar, and most preferably less than 1 bar. Examples include water, n-butanol, diethylene glycol monoethyl ether, tripropylene glycol monomethyl ether, terpineol, n-butyl acetate, n-(n-butoxyethoxy)ethanol, n-methoxymethylethoxypropanol, and n-methoxymethylethoxypropanol, which can be present alone or in mixtures. The use of commercially available screen printing oils is also possible.
[0127] To achieve the desired viscosity, appropriate additives, which can be inorganic or organic, are used. Organic additives include, for example, hydroxyethyl cellulose and / or hydroxypropyl cellulose and / or xanthan gum and / or polyvinyl alcohol and / or polyethylene alcohol and / or polyethylene glycol, block copolymers and / or triblock copolymers and / or tree resins and / or polyacrylates and / or polymethacrylates.
[0128] After the powder is introduced into the suspending agent, the next step is to homogenize the mixture, for example in a three-roller chair.
[0129] It is also possible to introduce another powder, for example containing the antiflatulent agent, into another suspension medium and homogenize it. The two suspensions can then be mixed together.
[0130] It is also possible to first prepare a mixture of the different powders, for example, comprising a glass powder, a blowing agent, and a pigment, and to homogenize this mixture, for example, in a rotary mixer. This powder can then be applied as described above.
[0131] The suspension preferably has a viscosity at a shear rate of 200 / s, measured with a cone plate viscometer, between 2,000 mPas and 20,000 mPas, preferably between 2,500 mPas and 15,000 mPas, and particularly preferably between 3,000 mPas and 10,000 mPas.
[0132] b. Applying the suspension to a substrate so that at least part of the substrate is covered with the suspension.
[0133] The suspension can be applied to the substrate, such as a glass or glass-ceramic substrate, particularly one with a low coefficient of thermal expansion, over the entire surface. However, it is also possible to apply the suspension in the form of specific patterns. For example, patterns, lettering, or other grids can be applied to the substrate in this way.
[0134] In principle, all common liquid coating processes are suitable for application. For example, the suspension can be applied using a printing process, particularly screen printing, pad printing, or inkjet printing. Application using a decal process is also possible. Application by spraying, spin coating, or roll coating is also feasible. To ensure optimal processability of the suspension, it can be adapted to the respective application process by adding various additives, such as solvents or thixotropic agents. The necessary additives, which are usually organic, evaporate during curing.
[0135] Particularly preferred application methods include inkjet printing, offset printing, pad printing, wet decals, screen printing, dip coating, roll coating, spray coating, doctor blade application, flooding and spin coating.
[0136] c. preferably fixing the suspension applied in step b onto the substrate, preferably at a temperature between 0°C and 300°C.
[0137] After the suspension has been at least partially applied to the substrate in step b, such as a glass or glass-ceramic substrate, particularly one with a low coefficient of thermal expansion, the suspension is preferably fixed to the substrate. This can be achieved, for example, by a drying step at elevated temperatures, such as between 0°C and 300°C. Fixing the suspension to the substrate is particularly advantageous if, after application, the substrate needs to be transferred to another processing unit, for example, for further processing steps. Depending on the exact composition of the suspension, temperature ranges between 0°C and 100°C and between 100°C and 300°C have proven to be preferred for fixing.
[0138] In addition to purely thermal fixation of the suspension to the substrate, it is also possible to assist the fixation process with IR radiation and / or UV radiation. With suitable adjustment of the suspension, fixation can also be achieved solely through IR radiation and / or UV radiation.
[0139] d. Tempering the at least partially coated substrate at a temperature between 500°C and 900°C, preferably 550°C and 900°C, so that the blowing agent decomposes to form at least one volatile substance and closed pores are formed in the coating.
[0140] Tempering is preferably carried out at a temperature between 500°C and 900°C, preferably between 550°C and 900°C.
[0141] During tempering, the blowing agent decomposes, and simultaneously the coating bonds to the substrate. This results in a closed-pore coating that exhibits good adhesion to the substrate.
[0142] e. Cooling the substrate to room temperature.
[0143] According to an advantageous embodiment, the coating is applied laterally structured in the form of a predetermined pattern to the substrate, such as a glass or glass-ceramic substrate, in particular a glass or glass-ceramic substrate with a low coefficient of thermal expansion. This makes it very easy, for example, to mark cooking zones or to exclude areas where electro-optical display devices, such as displays, are installed from the coating. Frame and pattern printing for fireplace viewing windows and ovens can also be easily achieved in this way.
[0144] It can also be advantageous to apply a non-adherent coating to the layer after the suspension has been applied, and for this coating to remain on the layer during the tempering process. This ensures that the layer remains uniformly thick and prevents the formation of disruptive layer irregularities or ripples. A coating is considered "non-adherent" in particular if, after tempering, it can be removed from the coating essentially without leaving any residue.
[0145] The suspension is advantageously applied using a printing process, for example inkjet printing, offset printing, pad printing or screen printing, or by rolling, flooding, dipping, spraying, squeegeeing or spin coating. Examples
[0146] The invention will be explained in more detail below using examples.
[0147] The following tables list some composition ranges of exemplary glass families from which glass powders for coating according to embodiments are advantageously selected. Glass families 1 % by weight Glass A Glass B Glass C Glass D Glass E Glass F Glass G Glass H Glass I Glass J SiO2 44-57 53-63 57-62 47-52 40-50 63-73 50-66 45-60 45-75 25-70 Al2O3 5-25 15-25 5-8 2-6 9-15 0-7 0-20 6-17 1-10 0-20 B2O3 0-27 15-22 18-23 17-21 10-15 12-29 0-8 0-10 10-30 10-30 Li 2 O 0-10 2-7 2-6 3-5 0-4 0-6 0-12 0-7 0-5 0-7 Na₂O 0-10 0-1 0-1 1-5 1-4 0-8 7-15 0-7 0-10 0-20 K2O 0-10 0-1 0-4 5-10 0-3 0-8 0-3 0-7 0-5 0-5 CaO 0-4 1-4 1-2 0-2 0-3 0-5 0-10 0-12 0-4 0-5 MgO 0-3 1-4 0-2 0-1 0-3 0,1-5 3-8 0-9 0-4 0-3 BaO 0-4 0-1 0-2 0-2 16-24 0-5 0-15 13-27 1-10 0-2,5 SrO 0-4 1-4 0,5-2 0-1 0-2 0-4 0-4 0-4 0-4 0-1 ZnO 0-15 1-4 0-2 0-3 8-15 0-15 0-5 3-17 0-20 1-35 TiO2 0-3 0-1 0-2 0-2 0-3 0-5 0-5 0-2 0-2 0-10 ZrO 2 0-7 1-4 2-5 0-2 0-4 0-5 0-5 0-7 0-7 0-2,5 As 2 O 3 0-1 0-1 0-1 0-1 0-1 0-1 0-1 0-1 0-1 0-1 Sb 2 O 3 0-1,5 0-1 0-1 0-1 0-1,5 0-1 0-1 0-1 0-1 0-1 F 0-3 0-1 0-1 0-1 0-1 0-1 0-1 0-1 0-2 0-3 Cl 0 - 1 0-1 0-1 0-1 0-1 0-1 0-1 0-1 0-1 0-1 Glass families 2 % by weight Glass K Glass L Glass M Glass N Glass O Glass P Glass Q SiO2 25-55 35-65 30-54 6-20 6-15 45-65 20-60 Al2O3 3-18 - 0-17,5 0-5 - 0-15 0-10 B2O3 5-25 - 13-28 20-38 20-28 5-30 2-25 Li 2 O 0-12 0-6 3-6 - - 0-10 0-7 Na₂O 3-18 0-6 4-10 - - 0-10 0-5 K2O 3-18 0-6 0-2 - - 0-10 0-2,5 CaO 3-17 0-12 0-6 - - 0-5 0-1 MgO 0-10 0-12 0-4 - - 0-5 0-1 BaO 0-12 0-38 - - - 0-20 - SrO - 0-16 0-4 - - 0-16 - ZnO - 17,5-38 3-13 35-70 58-70 0-35 0-15 TiO2 0-5 - 0-2 0-5 - 0-5 0-5 ZrO 2 0-3 - 0-2 0-5 - 0-5 0-2,5 Bi 2 O 3 - - - 0-20 - 0-20 10-75 CoO - - - 0-5 - - - Fe2O3 - - - 0-5 - - - MnO - - - 0-10 0,5-1 - - CeO 2 - - - - 0-3 - F - - 0-3,3 0-6 - -
[0148] The following table lists characteristic temperatures for four test glasses. For glasses 1 and 2, the coating can advantageously be applied in a so-called primary firing, i.e., a firing that occurs during the thermal treatment of a so-called green glass, which is ceramicized by the thermal treatment, i.e., transformed into a glass-ceramic. For glasses 3 and 4, the coating is advantageously applied in a so-called secondary firing, i.e., in a separate tempering step that takes place independently of any temperature treatment of a substrate. Tab: Test tubes Primary burn-in Secondary burn-in Glass ID Glass 1 Glass 2 Glass 3 Glass 4 Glass family A B P P Tg (upper cooling point) (log ) 13 578 675 477 468 EW (log ) 7,6 755 939 697 604 VA (log ) 4 1064 863 840
[0149] The glass powders listed in the table above have proven to be particularly advantageous with regard to their processability during the coating of a KNG or borosilicate glass or an aluminosilicate glass substrate, as well as with regard to the optical, mechanical and chemical properties of the corresponding coating.
[0150] "EW" refers to the softening temperature, and "VA" to the processing temperature. The second column shows the values of the decadic logarithm of the viscosity (in dPa·s). All temperatures are given in °C.
[0151] The following table characterizes various coatings on a glass-ceramic substrate with regard to their properties. Nr. Glass ID Antigas remedies (Vol%) Pigment (Vol%) Sieve Burn-in temperature (°C) Ball drop value Remarks Tesa test 0 Glass 3 none 15% IRON COBALT CHROMITE BLACK SPINEL (D50 ~ 0.5-2µM) 77 720 failed Slightly transparent; porous chipt 1 Glass 3 15% CaCO3 15% IRON COBALT CHROMITE BLACK SPINEL (D50 ~ 0.5-2µM) 77 700 passed Opaque, porous 10% 2 Glass 3 15% CaCO3 15% IRON COBALT CHROMITE BLACK SPINEL (D50 ~ 0.5-2µM) 77 720 passed Opaque, porous 95% 3 Glass 3 30% CaCO3 15% IRON COBALT CHROMITE BLACK SPINEL (D50 ~ 0.5-2µM) 77 740 passed Opaque, porous OK 4 Glass 3 30% CaCO3 15% Chromium-Iron-Nickel Black Spinel d50~1-2.5µm 77 740 passed Slightly transparent, porous OK 5 Glass 3 15% Na₂HPO₄·2H₂O 15% CoFe 2 O 4 (nano) 77 720 passed Slightly transparent, H2O-resistant OK 6 Glass 3 15% Na₂HPO₄·2H₂O 15% Chromium-Iron-Nickel Black Spinel d50~1-2.5µm 100 750 passed Almost opaque, H₂O-resistant OK 7 Glass 4 15% Na₂HPO₄·2H₂O 15% Chromium-Iron-Nickel Black Spinel d50~1-2.5µm 77 720 failed Opaque, H₂O-resistant OK Chromium-iron-nickel black spinel d50-1-2.5µm (fine) 8 Glass 4 15% Na₂HPO₄·2H₂O 15% IRON COBALT CHROMITE BLACK SPINEL (D50 ~ 0.5-2µM) 77 660 failed Opaque, H₂O-resistant OK 9 Glass 4 20% Na₂HPO₄·2H₂O 15% IRON COBALT CHROMITE BLACK SPINEL (D50 ~ 0.5-2µM) 77 680 passed Almost opaque, H₂O-resistant OK 10 Glass 4 20% Na₂HPO₄·2H₂O 15% Chromium-Iron-Nickel Black Spinel d50~1-2.5µm 77 680 passed Opaque, H₂O-resistant OK Chromium-iron-nickel black spinel d50-1-2.5µm (fine) 11 Glass 4 20% Na₂HPO₄ 15% IRON COBALT CHROMITE BLACK SPINEL (D50 ~ 0.5-2µM) 77 720 failed Opaque, H₂O-resistant OK 12 Glass 4 20% NaPO3 15% Chromium-Iron-Nickel Black Spinel d50~1-2.5µm 77 740 failed Almost opaque, H₂O-resistant OK Chromium-iron-nickel black spinel d50-1-2.5µm 13 Glass 4 15% rice starch 15% IRON COBALT CHROMITE BLACK SPINEL (D50 ~ 0.5-2µM) 77 740 failed Opaque, H₂O-resistant OK 14 Glass 4 15% monosaccharide 15% IRON COBALT CHROMITE BLACK SPINEL (D50 ~ 0.5-2µM) 77 740 failed Opaque, H₂O-resistant OK 15 Glass 4 15% KNO3 15% IRON COBALT CHROMITE BLACK SPINEL (D50 ~ 0.5-2µM) 77 740 failed Opaque, H₂O-resistant OK 16 Glass 4 25% Mowital 15% IRON COBALT CHROMITE BLACK SPINEL (D50 ~ 0.5-2µM) 77 740 failed Opaque, H₂O-resistant OK
[0152] The stated percentage values for the blowing agent and the pigment refer to volume percent of the total solids content. The firing temperature is also given. The layers were obtained using screen printing with a 77 mesh screen (77 threads per 1 cm).
[0153] A coating is described as "water-resistant" or H₂O-resistant if no water vapor penetrates the layer. This is particularly important for full-surface coatings, as these coatings are often applied as undercoats or backcoats facing the inside of the oven, meaning they are located on the side of the glass or glass-ceramic substrate facing away from the user during normal use. In this case, no condensation or shadows of condensation should be visible from above.
[0154] In the case of a coating applied as a bottom or backside coating—that is, a coating located on the side of the glass or glass-ceramic substrate that faces away from the user during normal use, such as the backside coating of a fireplace or oven viewing window, for example, on an oven door—it can be important that the areas behind the substrate are not visible from the user's perspective. Such a backside coating should therefore be as opaque as possible, or at least it should be possible to apply such a backside coating in an opaque manner. This is verified through a visual inspection in which objects positioned under the glass or glass-ceramic substrate are approximately 12 cm away from the substrate. This visual inspection checks whether the objects are visible from above.The technical rules mentioned above for carrying out a visual inspection are taken into account, with preference given to the rules for direct, local visual inspection.
[0155] Slightly transparent means that objects underneath are faintly visible with some light. A coating is considered opaque if nothing is visible in these tests. A coating is considered opaque or essentially impermeable, in particular, if τvis (in-line transmission) in the wavelength range of visible light (~380 to <= 700 nm) is less than 10%.
[0156] Furthermore, the opacity or optical density can be determined using a transmitted light densiometer (X-Rite 361 TX). A value of at least 2.5 indicates that the disc is considered opaque, meaning that, according to the nomenclature mentioned above, no objects are visible upon visual inspection.
[0157] Furthermore, the results of the ball drop test are listed. This test determines the mechanical strength. For this purpose, at least five samples, each with lateral dimensions of 10 x 10 cm² and a thickness of approximately 4 mm, were coated according to the exemplary embodiments. The samples were then placed on a rubber-lined support frame, ensuring that the rubber surface was free of glass fragments or similar particles that could potentially damage the glass or glass-ceramic, and that the sample was not clamped to the frame. A steel ball with a diameter of 36 mm and a mass of 200 g was then dropped from a height of 5 cm onto the surface of the sample in a drop test rig. The drop height is readable on the rig and is measured between the underside of the steel ball and the top of the sample.The drop height is then increased by 5 cm at a time until the sample breaks. The last successfully completed drop height is recorded. The strength is considered sufficient if the average of the last successfully completed drop heights is greater than 12.5 cm.
[0158] The adhesion of the coating was determined using a tape test. For this test, a strip of tape is applied to the coating and pressed firmly. The tape is then removed. The test is considered passed if no peeling occurs.
[0159] Examples for glasses 1 and 2 can be found in the table below. Nr. Glass ID Antigas remedies (Vol%) Pigment (Vol%) Sieve Burn-in temperature (°C) ball fall value Remarks Tesa test 17 Glass 1 none 15% Chromium-Iron-Nickel Black Spinel d50~1-2.5µm 77 750 failed Slightly transparent; porous OK Chromium-iron-nickel black spinel d50-1-2.5µm 18 Glass 1 5% CaCO3 15% Chromium-Iron-Nickel Black Spinel d50~1-2.5µm 77 735 failed Opaque, H₂O-resistant OK Chromium-iron-nickel black spinel d50-1-2.5µm 19 Glass 1 5% CaCO3 15% Chromium-Iron-Nickel Black Spinel d50~1-2.5µm 140 735 failed Opaque, H₂O-resistant OK Chromium-iron-nickel black spinel d50-1-2.5µm 20 Glass 1 10% CaCO3 15% Chromium-Iron-Nickel Black Spinel d50~1-2.5µm 77 735 failed Opaque, slightly porous OK Chromium-iron-nickel black spinel d50-1-2.5µm 21 Glass 1 10% CaCO3 15% Chromium-Iron-Nickel Black Spinel d50~1-2.5µm 140 735 failed Opaque, slightly porous OK Chromium-iron-nickel black spinel d50-1-2.5µm 22 Glass 1 5% CaCO3 15% Chromium-Iron-Nickel Black Spinel d50~1-2.5µm 54 920 passed Opaque, slightly porous OK Chromium-iron-nickel black spinel d50-1-2.5µm 23 Glass 2 10% CaCO3 15% Chromium-Iron-Nickel Black Spinel d50~1-2.5µm 54 920 passed Opaque, slightly porous OK 24 Glass 2 15% Na₂HPO₄·2H₂O 15% CoFe 2 O4 (nano) 77 800 passed Almost opaque, H₂O-resistant OK 25 Glass 2 15% Na₂HPO₄·2H₂O 15% Chromium-Iron-Nickel Black Spinel d50~1-2.5µm 100 820 passed Almost opaque, slightly porous OK 26 Glass 2 15% Na₂HPO₄·2H₂O 15% IRON COBALT CHROMITE BLACK SPINEL (D50 ~ 0.5-2µM) 77 800 Failed Almost opaque, H₂O resistant OK 27 Glass 2 20% Na₂HPO₄·2H₂O 15% IRON COBALT CHROMITE BLACK SPINEL (D50 ~ 0.5-2µM) 77 800 passed Opaque, slightly porous OK 28 Glass 2 20% Na₂HPO₄·2H₂O 15% Chromium-Iron-Nickel Black Spinel d50~1-2.5µm (fine) 77 800 passed Opaque, slightly porous OK 29 Glass 2 20% Na₂HPO₄ 15% IRON COBALT CHROMITE BLACK SPINEL (D50 ~ 0.5-2µM) 77 820 passed Opaque, H₂O-resistant OK 30 Glass 2 20% NaPO3 15% Chromium-Iron-Nickel Black Spinel d50~1-2.5µm 77 850 passed Almost opaque, H₂O-resistant OK 31 Glass 2 15% rice starch 15% IRON COBALT CHROMITE BLACK SPINEL (D50 ~ 0.5-2µM) 54 900 passed Opaque, H₂O-resistant OK 32 Glass 2 15% monosaccharide 15% IRON COBALT CHROMITE BLACK SPINEL (D50 ~ 0.5-2µM) 77 875 passed Opaque, H₂O-resistant OK 33 Glass 2 15% KNO3 15% IRON COBALT CHROMITE BLACK SPINEL (D50 ~ 0.5-2µM) 54 800 passed Opaque, H₂O-resistant OK 34 Glass 2 25% Mowital 15% IRON COBALT CHROMITE BLACK SPINEL (D50 ~ 0.5-2µM) 77 850 passed Opaque, H₂O-resistant OK
[0160] The layer thickness is significantly determined by the application method. For example, in screen printing, the resulting layer thickness depends on the thread count and the screen-to-wall ratio (GFR). The influence of the thread count for coatings according to the embodiments is shown in the following table. The influence of the blowing agent content was also investigated for a specific coating system. The layer thicknesses are given in µm. With a lower GFR (e.g., 10:3), the layer thicknesses increase by up to three times for the same screen size. Sieve strength (APV 10:12) Layer thickness after foaming at 5 vol% blowing agent (µm) Layer thickness after foaming with 10 vol% blowing agent (µm) 77 sieve: 5-6,2 4,8-6,9 100 sieve ~4 ~4,5 140 sieve 1,7-2,3 ~3,4
[0161] The resulting layer thickness can also be varied when applying the coating using a squeegee. Values can be found in the following table. Squeegee gap setting After foaming (µm) 30 µm ~ 15 - 30 100 µm ~ 40 - 55 250 µm ~ 100-150 500 µm ~ 130 - 250
[0162] The composition of a first attempt at a suspension can be found in the following table. S-0001 solid solvent Dispersing agent binder Plasticizers Density (g / cm³< ) 2,58 1,2 1,1 1,073 Vol% 30,0 57,4 0,4 7,0 6,0 Weight % 56,1 33,9 0,3 5,5 4,2
[0163] The row labeled "Density" lists the densities of the respective components. The percentages refer to the entire suspension.
[0164] A second example suspension is listed in the following table. S-0002 solid solvent Dispersing agent binder Plasticizers Density (g / cm³< ) 2,58 1,2 1,1 1,073 Vol% 45 31 5 10 9 Weight % 70 15,2 3,0 6,5 5,2
[0165] The two suspensions listed above are particularly well suited for application using a doctor blade.
[0166] Doctor blade coating is a stripping technique. First, excess coating material is applied to the substrate surface. Then, a doctor blade with a defined gap is used to spread the coating material and remove the excess. The thickness of the wet film is controlled by the size of the doctor blade gap. This allows large, flat surfaces to be coated using the doctor blade method. The coating thickness is limited only by the critical film thickness of the coating system. The doctor blade method is characterized by: Layer thicknesses from 4 µm up to the critical film thickness are possible. Suitable only for flat surfaces. Easily automated (large production volumes possible). Only complete surface wetting is possible.
[0167] The doctor blade method comprises the following steps.
[0168] Preparation of a suspension of glass, blowing agent and solvent (for example, comprising distilled H₂O), including: 1) Grind glass to a grain size d 50 ~ 1-10µm. 2) Mix glass powder with blowing agent (proportion of blowing agent 0.5 vol-% to 40 vol-%, preferably 5 vol-% to 30 vol-%, particularly preferably 15-25 vol-%) and solvent as well as surfactants, dispersants, binders, plasticizing agents and flocculants to obtain a suspension with a viscosity between 2000 mPas to 8000 mPas, preferably 2500 mPas to 7000 mPas, particularly preferably 3000 mPas to 6000 mPas and a solids content of 15 vol-% to 50 vol-%, preferably 20 vol-% to 40 vol-%, particularly preferably approximately 35 vol-%. The addition of dispersants, binders, plasticizers, etc., can vary between 0.25 and 25 wt% based on the solids content, depending on the manufacturer and chemical composition. a) SOLVENTS include water, organic solvents (mostly methyl acetone, trichloroethylene, acetones, alcohols, liquid waxes, refined petroleum, polymers (e.g.,PVB, PVA) and mixtures thereof) and serve to dissolve or slurry particles. b) Surfactants (these include polar and non-polar surfactants, ionic surfactants and non-ionic surfactants, such as ethoxylated nonylphenol or ethoxylated tridecyl alcohol, sodium stearate or sodium diisopropylnaphthalene sulfate, and dodecyltrimethylammonium chloride) can improve the wetting of the particles with the solvent. c) Thinners / dispersants prevent agglomeration by electrostatic repulsion (water-based [aqueous] environment) or by steric repulsion. Inorganic dispersants in water-based environments are based, for example, on sodium carbonate, sodium silicate, sodium borate, and tetrasodium pyrophosphate. Organic dispersants are preferably sodium polyacrylate, ammonium polyacrylate, sodium citrate, sodium succinate, sodium tartrate, sodium polysulfonate or ammonium citrate.
[0169] Other liquefying and dispersing agents, preferably used in the field of technical ceramics, are based, for example, on alkali-free polyelectrolytes, carboxylic acid esters, and alkanolamines. Examples of strong polyelectrolytes are sodium polystyrenesulfonate (anionic) or polydiallyldimethylammonium chloride (cationic), while weak polyelectrolytes include polyacrylic acid (acidic) or polyethyleneimine (basic). The properties of a polyelectrolyte solution are largely determined by the repulsive interactions of the like-charged groups on the polymer chain.
[0170] Other examples of dispersants are H2O, ROH, C7H8 (toluene), C2HCl3 (trichloroethylene), which prevent the agglomeration or flocculation of the powder particles by interacting with the powder surface.
[0171] Other suitable substances include, for example, Darvan®, Dolapix®, polyarylic acids, ammonium oxalate (as monohydrate), oxalic acid, sorbitol ammonium citrate or others.
[0172] d) Binders / flocculators are used to increase viscosity or delay particle settling. Binders can also increase the mechanical strength of the green body (advantageous for injection molding and die-casting techniques). There are colloidal binders (primarily used in traditional ceramics) and molecular binders (polymers: ionic, cationic, and anionic). Examples of synthetic binders include polyvinyl alcohol (PVA), polyvinyl butyral (PVB), polyvinyl methacrylate (PMA), and polyacetals. Examples of plant-based binders include cellulose, waxes, oils, and paraffin.
[0173] e) Plasticizing agents are used to adjust the transformation temperature of a polymer binder to temperatures below ambient temperature. Examples include residual water, PVB, PMMA, light glycols (polyethylene glycol (PEG), glycerol), phthalates (dibutyl phthalate, DBP, benzyl phthalate, BBP) and others.
[0174] 3) Application to glass ceramic via squeegee technique onto the substrate, for example a glass ceramic plate.
[0175] 4) Drying the applied layer at 100-300°C
[0176] 5) Foaming and firing at 550-900°C, preferably 600-900°C
[0177] Another example of coating using a doctor blade process is shown below: Preparation of a suspension of glass, blowing agent and solvent (distilled H₂O), to which: 1) Grind glass to a particle size d50 ∼ 1-10 µm. 2) Mix glass powder with blowing agent (proportion of blowing agent 0.5 vol% to 40 vol%, preferably 5 vol% to 30 vol%, particularly preferably 15 vol% to 25 vol%). 3) Prepare the suspension; for this purpose, deagglomerate the powders with solvent and dispersant; add binder and further homogenize; degas the casting suspension. The addition of dispersing agents, binders, etc. can vary between 0.25 and 25 wt% based on the solids content, depending on the manufacturer and chemical composition.
[0178] The casting suspension was prepared in PE containers (100 ml and 250 ml filling volumes) by adding aluminum oxide grinding balls (grinding ball diameter approx. 3 & 5 mm) in a gyratory mixer (Turbula, WAB AG, Basel, Switzerland). The PE containers were filled to approximately 50% with suspension, with the grinding ball content at about 30% of the container volume. The finished casting suspension was then sieved using a steel mesh (0.224 mm mesh size) to remove any remaining agglomerates or undissolved organic components, as well as the grinding balls. The suspension has a solids content of 15 vol% to 50 vol%, preferably 20 vol% to 40 vol%, and particularly preferably approximately 35 vol%. The viscosity, at a shear rate of 20 s⁻¹ and a solids content of 35 vol%, was 2000 mPas to 8000 mPas, preferably 2500 mPas to 7000 mPas, and particularly preferably 3000 mPas to 6000 mPas. The suspension exhibits thixotropy.
[0179] In one formulation, Mowiol (polyvinyl alcohols, Kuraray) is used as a temporary binder. It is used in different molecular weights: Mowiol 28-99 = 145,000 g / mol and Mowiol 4-88 = 131,000 g / mol. The viscosity of the suspension can be varied by adjusting the chain length of the Mowiol.
[0180] Water is placed in a beaker and heated to 90°C. Mowiol, dispersant, and plasticizer / binder are added to the water while stirring continuously in a dissolver. After stirring the solution for 20 minutes, the evaporated water is replenished to maintain a constant mixing ratio. Then, LAS glass-ceramic powder with a d50 of -1.8 µm and a d99 of -14 µm is gradually added. The dispersion is stirred in a dissolver for 30 minutes.
[0181] Overnight, the suspension is further homogenized by rotating it on a roller bench in a container additionally filled with ZrO₂ spheres (Ø = 5 mm, 10% volume fraction based on the suspension volume). The ZrO₂ spheres are then removed with a sieve. The suspension, now heavily permeated with bubbles, is degassed on a rotary evaporator by applying a pressure of <50 mbar. % by weight solvent 1% Rheological additive 1% Binders for liquids 0,07% Temporary binder 70% Glass frit + foaming agent
[0182] The resulting suspension is then applied to a glass-ceramic surface using screen printing. The layer is dried at a temperature between 100°C and 300°C. Foaming and firing take place at temperatures between at least 550°C, preferably at least 600°C and at most 900°C, particularly preferably at least 650°C and at most 900°C.
[0183] Another embodiment of the manufacturing process provides that the suspension provided in step a) comprises at least one IR-reflecting pigment. According to this variant, the suspension or paste further contains a glass powder with a softening temperature TEW,GlassPowder and a screen-printing medium.
[0184] After the suspension is applied to the glass or glass-ceramic substrate by screen printing, the applied layer is fired at temperatures in the range of Tfiring ≥ TEW,glass powder. It has been found that further process steps can be combined with the firing of the layer. One variant involves applying the layer to a glass substrate, preferably soda-lime glass or borosilicate glass, and thermally prestressing the glass substrate together with the firing of the coating. Preferably, the firing and thermal prestressing take place at a temperature in the range of 500 to 1000°C.
[0185] In another preferred variant of the process, a crystallizable green glass is used as the substrate. Here, ceramicization of the substrate can occur simultaneously with the firing of the layer. Both variants described above are advantageous in terms of energy and time savings.
[0186] A suitable test for checking the tightness of the pores, including coatings, is explained below as an example.
[0187] The impermeability of the closed-pore coating to aqueous and oily media as well as cleaning agents is determined by a drop test. A drop of the liquid to be tested is applied to the coating and allowed to act for varying durations depending on the medium, but at least 10 seconds.
[0188] As an example, water is typically wiped away after 30 seconds, oil drops after 24 hours, and cleaning agent drops after a few minutes. The glass or glass-ceramic substrate is then thoroughly inspected to ensure it has a closed-pore coating. If the glass or glass-ceramic substrate is at least partially transparent in the visible range of the optical spectrum, the coating is inspected from above through the substrate. The droplet, or its shadow, must not be visible during this inspection. A droplet shadow is defined here as a change in the optical appearance of the coating, which can occur, for example, if parts of the fluid forming the droplet migrate into the coating, thus altering its refractive index.
[0189] The coating can be inspected visually, for example by viewing it under specific lighting, such as in a light booth where certain standard light types can be set, and which are used, for example, in the nuanced mixing of colors.
[0190] Preferably, the coating is inspected in accordance with the aforementioned standards, rules and steps for visual inspection in order to determine the water tightness or moisture tightness of the coating.
[0191] In this case, the test was performed using Sidolin as the test liquid. A layer that shows no color change on either the front or back after the test is described as "very good." A layer that shows no color change on the front after the test and a wipeable edge on the back is described as "good."
[0192] Such an examination typically reveals certain changes in the perceived color and / or other optical effects, for example, changes in a metallic effect. An evaluation can also be performed by measuring the color coordinates before and after applying the drop, allowing any changes in the color coordinates to be determined by comparing the measurements. When using effect pigments, the color coordinates can also be determined before and after the application of the fluid medium using angle-dependent measurements.
[0193] A further aspect of the present disclosure relates to the use of a glass or glass-ceramic substrate according to the present disclosure with a coating comprising closed pores according to the present disclosure, wherein the coating is designed as a barrier against the ingress and passage of fluids and exerts a barrier effect, wherein the coating preferably comprises an IR-reflecting color pigment, as a viewing window in an oven or a fireplace, in particular as a viewing window for an oven or as a fireplace viewing window. Description of the drawings
[0194] They show Figs. 1 to 3: Schematic and not to scale representation of a glass or glass-ceramic substrate with a coating comprising closed pores; Figs. 4a to 4d, 5, 6a to 6d: Photographic representations of coatings comprising closed pores; Fig. 7: Transmission curves of an uncoated and various coated glass or glass-ceramic substrates; Fig. 8: Results of strength tests on various coated substrates; Fig. 9: A schematic representation of the structure of an oven door; Fig. 10: A schematic representation of the measuring setup for determining the surface temperature of the outer oven pane; Fig. 11: A graphical representation of the measured temperature profile of the maximum temperature of the outer oven pane of various embodiments, which differ with respect to the porosity of the coating at an oven operating temperature of 450°C; and Fig. 12: A representation of the average values of the Fig. 11temperature profiles shown.
[0195] Fig. 1 The figure shows, in a schematic and not-to-scale representation, a glass or glass-ceramic substrate 1 with a coating 2 comprising closed pores. The coating acts as a barrier against the passage of fluids.
[0196] The coating 2 can be applied to the substrate 1 over its entire surface or - as shown in Fig. 1 schematically represented – it can also be applied to only a part of the substrate. In particular, it is possible to apply the coating 2 to the substrate 1 in the form of a predetermined pattern, for example to apply lettering or a logo to the glass or glass-ceramic substrate.
[0197] Fig. 2Figure 1 shows a schematic, not-to-scale, cross-section through a glass or glass-ceramic substrate 1. A surface 10, which preferably faces away from the operator during the intended use of the glass or glass-ceramic substrate 1, is partially covered with a coating 2. This coating 2 comprises closed pores 3. For the sake of clarity, not all of these pores 3 are labeled.
[0198] The pores 3 are shown schematically as circles or spherical sections. It is possible that the pores exist in different sizes and shapes; therefore, generally speaking, without limiting themselves to the example shown schematically here, they may not be perfectly round.
[0199] Fig. 3Figure 1 shows, in schematic form and not to scale, a section through a further embodiment in which the surface 10 of the glass or glass-ceramic substrate 1 is covered with a porous coating 2 comprising pores 30 with an anisotropic cross-sectional shape. The pores 30 have an elliptical cross-section. Pores with a corresponding shape can be obtained, for example, by using rice starch as a blowing agent.
[0200] It is possible that the pores are of different sizes and shapes, i.e., generally speaking, without limiting themselves to the example shown schematically here, they are not necessarily round. Pore former Pore sizes (by) Pore shape Sodium hydrogen phosphate 5-30 roundish Rice starch 0,1-5 elongated potato starch 10-15 Ovoid-potato-shaped wheat starch 2-10 Grain-shaped
[0201] The ones in the Figs. 2 and 3The schematically depicted coatings, in addition to the closed pores 3, include 30 pores which are arranged at the interface of the layer, i.e., in the form of a downward indentation of the coating. However, such pores open on one side do not impede the effectiveness of the coating 2 as a barrier against the passage of fluids. What is important is that there are no through pores extending from the surface of the coating 2 down to the top surface 10 of the substrate 1.
[0202] Figures 3a and 3b schematically illustrate embodiments in which the coating 2 deposited on the glass 1 has pores 32 and 33, respectively. In both cases, these are closed pores. Figure 3a shows an embodiment with largely spherical pores 32. Such pores can be obtained, for example, by using calcium carbonate as a blowing agent. In contrast, the pores 33 shown in Figure 3b have an elliptical cross-section and thus an anisotropic structure. Pores with a corresponding shape can be obtained, for example, by using rice starch as a blowing agent.
[0203] Fig. 4a - 4dFigure 1 shows various photographic representations of light microscopic images of coatings 2 according to embodiments of the disclosure, which were baked on using sieves of different thicknesses and at different temperatures. The two coatings arranged in the left area were each applied using a sieve with 77 mesh. In the leftmost sample in Fig. 4a The firing took place at approximately 750°C, with the sample positioned halfway to the left in Fig. 4b at approximately 720°C. The two samples arranged on the right in Fig. 4c and 4d The coatings shown were printed using a 100-mesh screen. The firing of the sample positioned halfway to the right in Fig. 4c This was again carried out at approximately 750°C, the firing of the samples shown on the far right in Fig. 4d at approximately 720°C.
[0204] The influence of temperature on pore formation is particularly evident: While the samples fired at approximately 750°C tend to have fewer but larger pores, the samples fired at approximately 720°C have more pores, which, however, have smaller dimensions.
[0205] Fig. 5 Figure 1 shows a photographic representation of a section through a substrate 1 onto which a coating 2 comprising closed samples 3 was applied. Sodium hydrogen phosphate was added to the glass 2 at a volume of 10% as a blowing agent.
[0206] Figs. 6a to 6d Further illustrations show a coating 2 comprising closed pores 3. The coating was obtained by mixing glass 1 with calcium carbonate. In the samples in Figs. 6a and 6b 5% by volume of calcium carbonate was added to glass 1 in each case; in the samples in Figs. 6c and 6dEach contained 10% by volume calcium carbonate. The firing process was carried out on the samples of Figs. 6a and 6c each at approximately 750°C, for the samples of the Figs. 6b and 6d at approximately 720°C. The influence of the amount of the anticoagulant is clearly visible, leading to a significant increase in the number of bubbles.
[0207] In Fig. 7 The transmission profiles of various glass-ceramic substrates in the wavelength range of approximately 300 nm to 5000 nm are shown. Curve 4 represents the transmission profile for an uncoated glass-ceramic substrate. High transmission is observed in the visible spectral range, from approximately 380 nm to approximately 780 nm; the substrate can therefore be described as transparent in this range. Consequently, structures located beneath such a substrate are visible to a user.
[0208] This changes when a coating is applied according to embodiments of the disclosure.
[0209] Curve 5 shows the case of a substrate which, in its uncoated state, exhibits a transmission analogous to that of curve 4, and in which a cobalt-iron spinel with nanoscale particle size was used as the pigment. No blowing agents were added. Curve 6 represents a coating which, in addition to the nanoscale cobalt-iron spinel (at 15 vol%), also includes 20 vol% sodium dihydrogen phosphate as a blowing agent.
[0210] Curve 7 shows a coating which, instead of the pigment used for the coating in Curve 6, comprises the Co / Mn / Fe / Cr spinel pigment (d50 - 0.5 µm), with an otherwise unchanged composition. In Curve 8, chromium-iron-nickel black spinel (d50 ∼ 1 - 2.5 µm) was used as the pigment, with an otherwise unchanged composition.
[0211] It is evident that substrates coated according to embodiments of the present disclosure exhibit transmission profiles that achieve very good opacity in the visible area. This is illustrated by curves 6 to 8. The transmission of the coated substrate is thus further reduced by the pores, thereby increasing the opacity. Opacity is the inverse of transmission.
[0212] In optics, extinction or optical density E is the perceptually logarithmic formulation of opacity O and thus a measure of the attenuation of radiation (e.g. light) after passing through a medium (Wikipedia https: / / de.wikipedia.org / wiki / Extinktion_(Optik)).
[0213] This refers to the representation of in-line transmission (as opposed to total transmission). When measuring total transmission, all forward-scattered light is captured by a detector, whereas in in-line transmission only captures the forward-scattered light (with a typical aperture angle of 5° for measuring instruments, this also includes scattered light exiting at this small angle). The difference between total and in-line transmission indicates a measure of scattering. In this particular case, this scattering results from the pigment particles within the layer and its pores.
[0214] In Fig. 8 The figure shows how the strength, determined here in a so-called ball drop test, changes for a coated substrate depending on the composition of the coating.
[0215] If the coating comprises only a glass or a glass together with a pigment, only very low strength values are achieved in the ball drop test. These are layers that do not comprise closed pores and are therefore not according to the invention.
[0216] If a coating is produced by applying a suspension which, in addition to glass or glass and pigment, also comprises a blowing agent, layers are formed according to embodiments of the present disclosure, which comprise closed pores. The strength of a substrate coated in this way is correspondingly significantly higher than when no blowing agent is present.
[0217] A visual inspection of the coating according to embodiments of the present disclosure is carried out by means of the following steps: Applying a liquid to an area on the surface of the substrate's coating, allowing the liquid to act for 15 seconds, wiping off any residual moisture with a dry cloth, turning the substrate over so that the coating is on the side facing away from the inspector, and visually checking whether a color change is visible in the area or an area adjacent to it, wherein a) the visual inspection is carried out under daylight according to standard illuminant D65 or under illumination such as an incandescent lamp, energy-saving lamp, fluorescent lamp, or light-emitting diode, b) the illuminance is at least 500 × at a distance to the coating, i.e., the test surface, of less than 600 mm, and c) the inspector's viewing angle is between 5° and 90°, preferably at least 30°.
[0218] Water, oil, alcohol and / or window cleaner can be used as the liquid.
[0219] The aforementioned visual inspection includes, in particular, checking whether a watermark and / or water stain is visible on the side of the substrate opposite the coated side. In this case, a layer is described as very good if, after the test, it shows no color change on either the front or back. In this case, a layer is described as good if, after the test, it shows no color change on the front and a wipeable edge on the back.
[0220] Fig. 9Figure 1 schematically shows a possible structure of an oven door. The outer pane 100 has a porous coating 3 on one side. The uncoated side of the substrate faces outwards. The middle pane 101 and the inner pane 102 of the oven door are each coated on one side with a coating 9. The coating 9 can, for example, consist of transparent, conductive oxides.
[0221] In Fig. 10A schematic diagram shows a measuring setup for determining the surface temperature of a coated glass pane under laboratory conditions. A laboratory furnace 12 is heated to a temperature of 450°C. The furnace has an opening with a diameter of 3 cm. The glass pane 1 with the coating 2 to be measured is placed 2.5 cm from this opening, with the coating 2 facing the furnace opening. The surface temperature of the coated glass pane 1 is determined using a pyrometer 13 (impac, IE 120 / 82L), with the focal point set on the outer surface of the coated pane. The pyrometer 13 is positioned behind a glass substrate 14 and at a distance of 50 cm from the glass pane 1 to be measured.
[0222] Fig. 11 and 12The graph shows the temperature profile on the outside of various coated substrates as a function of operating time. The oven was heated to a temperature of 450°C and then cooled with the [missing information - likely a specific fluid or process]. Fig. 10 The measuring device shown determines the surface temperature of the coated glass pane as a function of the operating time.
[0223] In Fig. 11 The measured maximum temperatures are shown here as a function of the operating time of the oven. Fig. 12 shows a fit obtained by averaging of the in Fig. 11 temperature profiles shown.
[0224] Curves 15, 16, and 17 correspond to temperature profiles of comparative examples where the coating contains IR-reflecting pigments but is not porous. Curves 18 to 21 correspond to temperature profiles of embodiments where the coating contains closed pores and IR-reflecting pigments.
[0225] The following table describes the comparative and exemplary applications in more detail. The examples use soda-lime glass as the substrate, and glass 1 from the table was used as the frit or glass flux. Firing took place in a laboratory furnace at 680°C for 15 minutes, with the samples stored horizontally. curve Pigment (Vol%) Foaming agent (vol%) Type of foaming agent Tmax (°C) after 1h at 450°C Optical density (glass side up) L*a*b* (SCE; color side up) Gloss (60°) Sclerometer (10N) Sidolin test (porosity) 16 20 0 n / a 47,6 2,6 34,63 / 0,45 / - 3,71 18,5 OK Very good 17 17,5 0 n / a 46,9 2,1 36,04 / 0,44 / - 4,09 55,9 OK Very good 21 17,5 20 CaCO3 43,8 2,2 34,63 / 0,45 / -3,71 4,0 OK good 20 17,5 10 CaCO3 43,2 2,6 31,58 / 0,49 / -3,56 17,5 OK good 19 17,5 20 Rice starch 45,7 2,1 21,38 / 0,6 / -1,75 41,0 OK Very good 18 17,5 10 Rice starch 45,4 2,6 18,56 / 0,65 / -1,95 50,5 OK Very good
[0226] Characterization of the in Fig. 11 and 12 samples shown
[0227] The coatings in comparative examples 16 to 18 were produced without the use of expanding agents. Examples 19 to 21, on the other hand, are porous coatings. These coatings were produced using the expanding agents shown in the table above; the resulting coatings therefore have closed pores. All in Fig. 11 and Fig. 12 The temperature profiles shown were obtained using the in Fig. 10 The measurement setup shown was obtained. The respective coating materials were applied to the substrate using screen printing with a 77 T-screen.
[0228] The coatings of all examples 15 to 21 contain IR-reflecting pigments, resulting in good IR reflectivity. This is particularly evident in the fact that, in all examples, after 60 minutes of oven operation at 450°C, the measured temperature of the outer pane was less than 50°C. This demonstrates that the IR reflectivity of the coating can be significantly increased by its porosity. For example, lower maximum temperatures were measured for samples 18 to 21 than for the comparison samples 15 to 17, which had a dense coating. The measured temperature difference after 60 minutes of operation between the dense sample 15 and the porous sample 20 was more than 4°C. It is assumed that the pores within the coating represent structures that can further scatter the IR radiation.
[0229] The extent of this positive effect on the maximum surface temperature of the disk appears to depend on the pore structure. Rice starch was used as the expanding agent in samples 18 and 19, while CaCO₃ was used in samples 20 and 21. When rice starch is used as the expanding agent, anisotropic pores with an ellipsoidal cross-section are preferentially formed, whereas the use of CaCO₃ as the expanding agent leads to largely spherical pores (cf. Figs. 2 and 3 ).
[0230] Fig. 12 This shows that the insulating effect is higher for the coated glasses 20 and 21, whose pores have a spherical or largely spherical structure, than for the coated glasses 18 and 19, whose coating has ellipsoidal or rice-shaped pores.
[0231] Furthermore, it is assumed that Fig. 12It is evident that the proportion of the expanding agent in the paste affects the IR reflection of the corresponding coating. Samples 20 and 21 differ only in their expanding agent content. While the expanding agent content in the paste used to produce coating 21 is 20 vol%, the corresponding paste used to produce coating 20 contains only 10 vol% CaCO3 as an expanding agent. Sample 20 exhibits better insulating properties than sample 21, such that after an operating time of 180 minutes, the maximum temperature of sample 20 is 0.8 °C lower than the maximum temperature of sample 21 under comparable conditions.
[0232] An excessively high proportion of blowing agents in the paste leads to the formation of so many pores that they partially merge, resulting in open pores. This indicates open pores and a consequent uneven surface. It is assumed that closed pores promote IR reflection.
[0233] Another way to increase the IR reflectivity of the coating is to increase the layer thickness, for example, by applying the corresponding paste or suspension to the substrate multiple times. This is illustrated in the following table. Here, the samples were applied to the substrate using a 77T screen via screen printing, dried, and optionally printed a second time with a 77T screen before the coating was baked horizontally in a laboratory oven for 15 minutes at 680°C. The table shows the number of printing cycles (single or double print) and the corresponding values. Fig. 10 The measuring setup shown shows the maximum temperature on the outside of the disc after 60 minutes of oven operation at a temperature of 450°C. Sample ID Number of prints Pigment content [vol.%] Proportion of antiflatulent agent [vol%] Antigas medication used Tmax (°C) after 1h heating at 450°C Optical density (glass side up) L*a*b* (color side up) Gloss (60°) Sclerometer (10N) Sidolin test (porosity) 21 1 17,5 20 CaCO3 43,8 2,2 34,63 / 0,45 / -3,71 4,0 OK good 21a 2 17,5 20 CaCO3 41,3 3,2 36,04 / 0,44 / -4,09 1,4 OK good 19 1 17,5 20 Rice starch 45,7 2,1 21,38 / 0,6 / -1,75 41,0 OK very good 19a 2 17,5 20 Rice starch 45,2 4,2 23,49 / 0,42 / -2,15 35,4 OK very good 18 1 17,5 10 Rice starch 45,4 2,6 18,56 / 0,65 / -1,95 50,5 OK very good 18a 2 17,5 10 Rice starch 44,9 4,7 19,86 / 0,40 / -2,38 48,9 OK very good Reference symbol list
[0234] 1 Glass or glass-ceramic substrate 2 Coating comprising closed pores 3, 30 Closed pores 4 Transmission curve for uncoated substrate 5 Transmission curve for substrate not coated according to the invention 6, 7, 8 Transmission curves of coated substrates according to embodiments of disclosure 9 Coating comprising conductive oxides 10 Surface of substrate 1 12 Laboratory oven 13 Pyrometer 15, 16, 17 Temperature profile curves of comparative examples with dense coatings 18, 19, 20, 21 Temperature profile curves of embodiments with porous coatings 100 Outer oven window 101 Middle oven window 102 Inner oven window
Claims
1. A method for coating a glass or glass ceramic substrate with a coating that includes closed pores, said coating being formed as a barrier against a passage of fluids, comprising the steps of: (a) preparing a suspension comprising a glass powder and an blowing agent; (b) applying the suspension onto a substrate such that at least part of the substrate is covered by the suspension; (c) preferably fixing the suspension applied in step (b) on the substrate, preferably at a temperature between 0 °C and 300 °C; (d) thermally treating the at least partially coated substrate at a temperature between 500 °C and 900 °C, preferably between 550 °C and 900 °C, such that the blowing agent decomposes while forming at least one volatile substance and cause formation of closed pores in the coating; and (e) cooling the substrate to room temperature; wherein the blowing agent is starch or a phosphate.
2. The method according to claim 1, wherein the coating is applied to the substrate in a laterally patterned manner in the form of a predetermined pattern.
3. The method according to any one of claims 1 or 2, wherein after the application of the suspension, a non-adhering cover sheet is applied to the layer, and the cover sheet remains on the layer for the duration of the thermal treatment.
4. The method according to any one of claims 1 to 3, wherein the applying of the suspension is performed using a printing technique, in particular ink-jet printing, offset printing, pad printing, or screen printing, or by rolling, flooding, dipping, spray coating, doctor blading, or spin coating.
5. A glass or glass ceramic substrate, comprising a coating produced or producible by a method according to any one of claims 1 to 4.
6. The glass or glass ceramic substrate according to claim 5, comprising a coating that includes closed pores, wherein the coating is formed as a barrier against ingress and passage of fluids and exhibits a barrier effect, wherein the coating comprises at least 95 wt% of inorganic constituents and has a thickness between 1.5 µm and 50 µm.
7. The glass or glass ceramic substrate according to any one of claims 5 or 6, exhibiting at least one of the following characteristics: the coating is a high temperature resistant coating, in particular for temperatures of more than 400 °C; the substrate is a sheet-like substrate having a thickness between at least 1 mm and at most 10 mm, preferably between at least 2 mm and at most 5 mm, and most preferably between at least 2 mm and at most 4 mm; the coating is applied in a laterally patterned form such that at least one portion of the substrate remains free of the coating; the coating comprises colourants and / or effect agents, in particular a colour pigment and / or an effect pigment.
8. The substrate according to any one of claims 5 to 7, wherein the coating contains IR-reflecting pigments, wherein the IR-reflecting pigments have a TSR value of at least 20 %, preferably at least 25 %, determined according to ASTM G 173, and wherein for a wavelength of 1500 nm the coating exhibits a remission of at least 35 %, measured according to ISO 13468, preferably exhibiting at least one of the following characteristics: in the entire wavelength range from 1500 nm to 2500 nm, the coating exhibits a remission of at least 35 %, preferably at least 40 %, and most preferably at least 45 %; at a wavelength of 1500 nm, the coating exhibits a remission of at least 35 %, preferably at least 40 %, and most preferably at least 45 %; the IR-reflecting pigments comprise particles with a size distribution having a d50 value in a range from 0.5 µm to 2 µm, preferably in a range from 0.8 µm to 1.8 µm; the IR-reflecting pigments include particles having a specific surface area in a range from 1.1 to 8 m2 / g, preferably in a range from 1.8 to 4.5 m2 / g; the coating includes a chromium-containing IR-reflecting pigment, preferably a chromium-containing iron oxide, a chromium-containing hematite, and / or a chromium-containing spinel.
9. The substrate according to any one of claims 5 to 8, wherein the substrate comprises a soda-lime glass or a borosilicate glass, preferably a toughened soda-lime glass or a toughened borosilicate glass.
10. The substrate according to any one of claims 5 to 9, wherein, in a temperature range from 20 °C to 700 °C, the resulting coefficient of thermal expansion of the coating and the coefficient of thermal expansion of the substrate do not differ from one another by more than 4 * 10-6 / K.
11. The glass or glass ceramic substrate according to any one of claims 5 to 10, wherein the glass matrix of the coating contains bismuth oxide, preferably 8 to 70 wt% of bismuth oxide, and / or zinc oxide, preferably 0.1 to 70 wt% of zinc oxide.
12. The glass or glass ceramic substrate according to any one of the preceding claims 5 to 11, wherein the glass matrix of the coating has the following glass composition, in wt%: SiO230 - 75, preferably 44 - 75Al2O30 - 25, preferably 0.2 - 25, most preferably 2 - 25B2O30 - 30, preferably 1 - 30, most preferably 5 - 30Li2O0 - 12Na2O0 - 25, preferably 0 - 15CaO0 - 12MgO0 - 9BaO0 - 27SrO0 - 4ZnO0 - 35, preferably 0 - 20Bi2O30 - 5TiO20 - 10, preferably 0 - 5ZrO20 - 7As2O30 - 1Sb2O30 - 1.5F0 - 3Cl0 - 1, preferably 0H2O0 - 3.
13. The glass or glass ceramic substrate according to any one of the preceding claims 5 to 11, wherein the glass of the glass matrix of the coating has the following composition, in wt %: SiO26 - 65, preferably 10 - 65, most preferably 15 - 65Al2O30 - 20B2O30 - 40, preferably 1 - 30, most preferably 3 - 30Li2O0 - 12Na2O0 - 18K2O0 - 17CaO0 - 17MgO0 - 12BaO0 - 38SrO0 - 16ZnO0 - 70TiO20 - 5ZrO20 - 5Bi2O30 - 75, preferably 0 - 60, more preferably 5 - 60, most preferably 10 - 60CoO0 - 5Fe2O30 - 5MnO0 - 10CeO20 - 3F0 - 3Cl0 - 1H2O0 - 3.
14. The substrate according to any one of claims 5 to 13, wherein the coating is substantially opaque to electromagnetic radiation in a wavelength range from 380 nm to 780 nm, and / or wherein τvis (in-line transmittance) in the wavelength range of visible light has a value of less than 20 %.
15. Use of a glass or glass ceramic substrate according to any one of claims 5 to 14 and / or produced in a method according to any one of claims 1 to 4 as a viewing window in an oven or fireplace, in particular as a viewing window for a cooking oven or as a fireplace viewing window.