Cross-linked solid electrolyte for lithium-ion battery

DE602023026027T2Active Publication Date: 2026-11-18IFP ENERGIES NOUVELLES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE602023026027
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-09-12
Filing Date
2023-09-06
Publication Date
2026-11-18
Estimated Expiration
2043-09-06

AI Technical Summary

Technical Problem

Existing solid electrolytes for lithium-ion batteries face challenges in achieving high conductivity and mechanical stability, often requiring solvents that hinder industrial development and result in suboptimal mechanical properties.

Method used

A crosslinkable electrolyte formulation using a hydrocarbon molecule with 3 to 6 thiol groups, a bifunctional chain extender with C=C double bonds, a monofunctional single-ion chain terminator, and a nucleophilic base catalyst, allowing for a stoichiometric molar ratio of [alkenes]/[thiols] to form a self-supporting chemical network without solvents, enhancing mechanical properties and conductivity.

Benefits of technology

The formulation achieves conductivities several orders of magnitude higher than prior art, with a transport number of 1, and is synthesized in a single step, providing improved mechanical stability and reduced solvent dependency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

technical field

[0001] The invention relates to the preparation of crosslinked solid electrolytes for lithium-ion batteries based on thiol-ene reactions. Previous technique

[0002] The thiol-ene reaction has applications in many fields, including batteries.

[0003] The thiol-ene reaction (also alkene hydrothiolation) is a reaction between a thiol and an alkene to form a thioether. This reaction was first reported in 1905, but it gained importance in the late 1990s and early 2000s due to its feasibility and wide range of applications, particularly in electrolytes.

[0004] Thiols are excellent nucleophiles through the formation of thiolate anions (RS-) and are also electrophiles via thiyl radicals (RS*). One of the most studied reactions involving thiols is the hydrothiolation of double bonds (C=C). Depending on the nature of the double bond substituents, electron donors or acceptors, and the type of catalyst used, the thiol-C=C reaction can proceed via a radical or nucleophilic mechanism.

[0005] In the case of a nucleophilic mechanism, the reaction used is a Michael polyaddition also called "nucleophilic thiol-ene" on a double bond substituted by an electron-withdrawing group, such as (meth)acrylates (monomers containing an active double bond), and a nucleophilic base is used as a catalyst.

[0006] The Michael polyaddition reaction has applications in many fields.

[0007] Li et al. ACS Energy Letters 2018, vol. 3, p. 20-27. DOI: 10.1021 / acsenergylett.7b00999 propose a single-ion polymer solid electrolyte synthesized via a photo-induced click reaction of an azide with an alkyne. It features a PEG (poly(ethylene oxide)) repeating unit and a TFSI (bis(trifluoromethyl)sulfonyl) imide counteranion attached to the polymer chain. No crosslinking agent is used; viscous liquid polymers are obtained, not networks (the mechanical and physicochemical properties are therefore completely different). Although the transport number is close to 1, the conductivity values ​​described at 90 °C are on the order of 2 × 10⁻⁵ S·cm⁻¹.

[0008] Shen et al. (ChemElectroChem 2019, vol. 6, 4483-4490. DOI: 10.1002 / celc.201901045) propose a quasi-solid electrolyte in the form of a semi-interpenetrating network formed by a polyacrylate-based single-ion crosslinked polymer and a PEO matrix, thus unrelated to the thiol-ene reaction. The counteranion is a sulfonate. A conductivity of 1.34 × 10⁻⁵ S·cm⁻¹ at 60 °C is observed following the addition of 5 µL of plasticizer (EC:PC 1:1 vol) at the cathode-electrolyte interface during button cell assembly. The transport number is 0.77.

[0009] Du et al. ACS Appl. Energy Mater. 2020, vol. 3, 1128-1138. DOI: 10.1021 / acsaem.9b02180 propose a quasi-solid single-ion electrolyte obtained by solvent-phase coating of a mixture of PVDF and a single-ion polyimide. The counter-anion is a TFSI, but the resulting electrolyte is a physical, not a chemical, network; moreover, the synthesis does not involve a thiol-ene reaction. It exhibits very good conductivity of 1.6 × 10⁻⁴ S·cm⁻¹ at 25 °C thanks to its prior immersion in carbonate solvents during its electrochemical characterization. However, the presence of solvents hinders the industrial development of this type of material, since the goal is to use a solid electrolyte precisely to avoid the thermal problems associated with solvents in batteries (evaporation, pressure buildup, risk of ignition). The transport number is 0.93.

[0010] Zhang et al., Energy Storage Materials 2020, vol. 24, pp. 579-587. DOI: 10.1016 / j.ensm.2019.06.029, propose a quasi-solid single-ion electrolyte produced by a photo-induced thiol-ene reaction from a mixture of four monomers dissolved in acetonitrile, deposited on a polypropylene nonwoven. The counter-anion is a TFSI, and the thiol crosslinker is pentaerythritol tetrakis(3-mercaptopropionate). The authors use a solvent in the starting mixture and a support. Furthermore, the resulting membrane is immersed in a mixture of ethylene carbonate and dimethylene carbonate before being characterized. The excellent conductivity is 8.4. The 10⁻⁴ < S.cm⁻¹ < at 25 °C is therefore not intrinsic to the material. Furthermore, the network presented does not contain PEO segments, which facilitate ionic conduction in the absence of a significant amount of solvent.

[0011] Patents CN 106935904 B and CN 110172 115 B disclose processes for preparing crosslinked solid electrolytes for secondary lithium batteries, these processes being based on a thiol-ene reaction involving a hydrocarbon molecule which has at least three thiol functions and a compound which contains at least one alkene function.

[0012] US patent application 2020 / 099089 A1 describes a solid electrolyte composition comprising an ionic conductor made of a polymer (A) having a mass average molecular weight of 5,000 or more and an electrolytic salt (B) containing an ion of a metal belonging to Group I or II of the periodic table. It also includes a compound (C) having two or more carbon-carbon double bond groups, and a compound (D) having two or more sulfanyl groups. Furthermore, US 2020 / 099089 A1 specifies a sheet containing a solid electrolyte, a solid-state secondary battery, and associated manufacturing processes, including for the sheet containing the solid electrolyte and for the solid-state secondary battery.

[0013] The publication by Weber et al. (Soft Matter vol. 13 no. 41, 2017, 7633-7643) describes research aimed at developing advanced polymer electrolytes for next-generation lithium-ion batteries. In this study, the researchers synthesized a new monomer, lithium bis(non-8-enyl-malonato)borate (LiBNMB), via a three-step process. This α,ω-diene monomer undergoes thermally initiated thiol-ene cross-polymerization in propylene carbonate to produce gel-like polymer electrolytes with a high lithium ion concentration (approximately 0.9 M). US patent applications 2016 / 0315348 A1 JR Long, J. Van Humbeck, RP Ameloot Polymer networks single ion conductors and US 2018 / 0166744 A1 R. Long, J. Van Humbeck, JC Axelson Polymer networks single ion conductors with flexible linkersThey describe single-ion polymer networks based on the borate anion (C6F4)4B. Tetrafluorophenyl borate anions form the nodes, and the neutral crosslinker provides varying degrees of mechanical flexibility depending on its chemical structure. The crosslinker, which also acts as a spacer, is presented as the most interesting, cis-2-butene-1,4-diol, because it allows for good structural flexibility. The network formation reaction occurs in two steps: the deprotonation of cis-2-butene-1,4-diol by the n -butyl lithium, then nucleophilic substitution between methyl chloride (from the precursor lithium chloromethyl tetrafluorophenyl borate) and deprotonated cis-2-butene-1,4-diol. The final membrane is obtained by coating using solvents N,N-dimethylformamide and 2,2'-Azobis(2-methylpropionitrile). Note that the Young's modulus (E = 0.27 GPa) and the ionic conductivity (σ = 8.5 × 10⁻⁵ S·cm⁻¹ at 40 °C) are given for a membrane containing 30 wt% plasticizer. Thus, the examples in these patents only concern gels containing a very high quantity of propylene carbonate. Summary of the invention

[0014] Surprisingly, the Applicant observed that, in non-aqueous formulations of solid electrolytes, crosslinking improved the mechanical properties of the network compared to the use of homopolymers, and that the use of a hydrocarbon molecule bearing between 3 and 6 thiol groups in association with a hydrocarbon molecule containing two C=C double bonds in the presence of a nucleophilic base catalyst, in which the [alkenes] / [thiols] molar ratio in the formulation is substantially stoichiometric, increased the network's resistance to chemical degradation. The [alkenes] / [thiols] molar ratio is defined as the ratio of all C=C double bonds to all thiol bonds in the formulation.

[0015] The electrolyte formulation according to the invention makes it possible to obtain conductivities several orders of magnitude higher than those obtained in the prior art (10⁻⁵ to 10⁻⁷ S / cm). The crosslinkable electrolyte formulation according to the invention makes it possible to obtain a self-supporting chemical network with a transport number of 1 that can be synthesized in a single step by a thiol-ene reaction and without necessarily requiring the use of a solvent.

[0016] The invention relates to a crosslinkable electrolyte formulation comprising at least: A hydrocarbon molecule comprising three to six thiol groups, preferably four; A bifunctional chain extender in the form of a hydrocarbon chain bearing two C=C double bonds; A monofunctional single-ion chain terminator comprising a C=C double bond and mobile lithium; A monofunctional polyethylene glycol-type chain terminator; A nucleophilic base-type catalyst, in which the molar ratio [C=C double bonds] / [thiols] is 1.

[0017] The formulation may include a lithium salt or a mixture of lithium salts soluble in the formulation; the amount of lithium salt(s) may represent between 2 and 30% by mass relative to the total formulation mass, preferably between 5 and 15% by mass relative to the total formulation mass.

[0018] The catalyst may be chosen from 1,8-diazobicyclo[5.4.0]undec-7-ene, dimethylphenylphosphine, triphenylphosphine or triethylamine, pyridine and dimethylaminopyridine and preferably chosen from 1,8-diazobicyclo[5.4.0]undec-7-ene, dimethylphenylphosphine, triphenylphosphine or triethylamine, most preferably the catalyst is triethylamine.

[0019] The hydrocarbon molecule containing 3 to 6 thiol groups may be selected from pentaerythritol tetrakis(3-mercaptopropionate), trimethylolpropane tris(3-mercaptopropionate), a poly(mercaptopropyl)methylsiloxane, or a copolymer (mercaptopropyl)methylsiloxane)-co-dimethylsiloxane with an average functionality greater than or equal to 3; preferably, pentaerythritol tetrakis(3-mercaptopropionate). The bifunctional chain extender may be selected from any oligoethylene glycol unit bearing two C=C double bonds or any norbornene, vinyl ether, allyl ether, acrylate, methacrylate, or alkene unit.

[0020] The bifunctional chain extender can be chosen from poly(ethylene glycol)dimethacrylate, PEG diacrylate, PEG diallyl, PEG divinyl.

[0021] The monofunctional single-ion chain terminator is preferably lithium-3-((trifluoromethane)sulfonamidosulfonyl)propyl methacrylate.

[0022] The polyethylene glycol chain terminator can be chosen from poly(ethylene glycol) methyl ether acrylate, poly(ethylene glycol) allyl methyl ether, poly(ethylene glycol) vinyl methyl ether or poly(ethylene glycol) maleimide methyl ether.

[0023] The catalyst can be present in such quantity that the molar ratio of thiol functions to catalyst is between 200 and 600.

[0024] The formulation may include a second chain extender from the dithiol family, preferably selected from polydimethylsiloxane (PDMS) or polyethylene glycol (PEG) polymers terminated by mercaptoethyl or mercaptopropyl functions at both ends.

[0025] The formulation may include a plasticizer selected from the following compounds: oligoethylene glycol, carbonate ester, succinonitrile, aprotic polar solvent or aprotic ionic liquid, said plasticizer representing from 2 to 30%, preferably from 5 to 15% by mass relative to the total mass of formulation.

[0026] The invention also relates to a method for preparing a cross-linked solid electrolyte in which: a) the crosslinkable electrolyte formulation is crosslinked according to any of the preceding variants, possibly in the presence of a non-aqueous solvent, using the catalyst present in the formulation and by thermal activation to form a lithium ion-conducting polymer, b) the possible solvent present in said polymer is evaporated to obtain a crosslinked solid electrolyte.

[0027] Thermal activation can be achieved by heating the formulation to a temperature between 50 and 80°C for a period of between 1 and 24 hours and preferably between 6 and 12 hours.

[0028] The invention also relates to the preparation of a crosslinked solid electrolyte in the form of an electrode in which, in step a), a porous electrode is impregnated with the crosslinkable electrolyte formulation by coating or spraying, then the coated or sprayed formulation is crosslinked, or an active material and an electronic percolant are added to the crosslinkable electrolyte formulation in step a) to formulate an electrode ink which is coated, then crosslinked to obtain a solid electrode.

[0029] The invention finally relates to the use of the crosslinked electrolyte obtained by crosslinking the formulation according to any of its variants or obtained by the process according to any of its variants as a solid electrolyte for a solid Li-ion battery or as a component of the positive (posolyte or catholyte) or negative (negolyte or anolyte) electrode of an electrochemical system. List of figures

[0030] There figure 1 represents the conductivity (S / cm) as a function of the inverse of the temperature (1000 / T with T in K) for a cycle (down-up-down) in temperature between 20 and 80°C of the ABC preparations (according to the invention) in the example. Description of the implementation methods Detailed description of the invention

[0031] The invention relates to a crosslinkable electrolyte formulation using thiol-ene reactions, in which at least one of the monomers comprises a covalently bonded anion with a delocalized charge, such as the TFSI ion, and may include a lithium salt to ensure efficient transport of lithium ions within the electrolyte and catholyte. The formulation yields crosslinked electrolytes used as solid-state electrolytes in all-solid-state lithium batteries or as components of the positive electrode (positive or positive electrode).

[0032] The originality of the invention lies in the development of a single-ion electrolyte that is polymerized and crosslinked in situ. This electrolyte has the advantage of being initially liquid, forming a chemical network in a single step via a thiol-ene reaction, and exhibiting lithium ion transport properties that are beneficial for the application, even without the need for a solvent. The crosslinkable formulation according to the invention is particularly advantageous for the preparation of all-solid-state battery electrodes. Electrodes prepared using conventional methods can be immersed with the precursors of the formulation according to the invention to form an in situ ionic percolation network with good interfaces with the active materials.

[0033] In the following description, a self-doped block polymer or unipolar conductive polymer is called a "single-ion" polymer.

[0034] The starting components, all liquids, are: A molecule comprising 3 to 6 thiol functions, preferably four, which acts as a crosslinking agent: a tetrafunctional molecule ( A 4 ) may notably be pentaerythritol tetrakis(3-mercaptopropionate) (preferably), but a trivalent thiol ( A 3 ) such as trimethylolpropane tris(3-mercaptopropionate) can be used, or a poly(mercaptopropyl)methylsiloxane) or a (mercaptopropyl)methylsiloxane) dimethylsiloxane copolymer with an average functionality greater than or equal to 3. A bifunctional chain extender can be chosen from any oligo- or poly(ethylene glycol) chain bearing 2 C=C double bonds ( B 2 ): The bifunctional chain extender can thus be a methacrylate, often more stable than acrylates, particularly poly(ethylene glycol)dimethacrylate (preferably). More generally, the bifunctional chain extender can be an oligo- or poly(ethylene glycol) chain bearing two C=C double bonds chosen from the following compounds: PEG diacrylate, PEG dimethacrylate, PEG diallyl, PEG divinyl) or any norbornene, vinyl ether, allyl ether, acrylate, methacrylate, maleimide, or alkene unit. A monofunctional single-ion chain terminator ( B' 1), comprising a C=C double bond providing the mobile lithium and the counter-anion anchored to the chain, which may notably be lithium-3-((trifluoromethane)sulfonamidosulfonyl)propyl methacrylate. A monofunctional polyethylene glycol chain terminator ( B"1), which can be chosen from poly(ethylene glycol) methyl ether methacrylate, poly(ethylene glycol) methyl ether acrylate, poly(ethylene glycol) allyl methyl ether, poly(ethylene glycol) vinyl methyl ether, poly(ethylene glycol) maleimide methyl ether etc.

[0035] It is not necessary to have the same chemical function on the bifunctional chain extender ( B 2 ) and on the PEG- single-function chain terminator (B 1").

[0036] In the crosslinkable electrolyte formulation according to the invention, it is preferable to maintain a molar equivalence between the thiol and alkene functionalities (stoichiometry equal to 1). The originality of the formulation according to the invention lies in the fact that the crosslinking density of the network and its mechanical and physicochemical properties are independent of the amount of single-ion chain terminator (B'1) thanks to the presence of the PEG chain terminator (B"1). It is therefore easy to adjust the ionic conductivity of the network by changing the molar ratio B1' / B1" without altering the mechanical properties of the electrolyte.

[0037] In one embodiment, a second chain extender from the dithiol family can be added (for example, a PDMS or PEG polymer terminated by mercaptoethyl or mercaptopropyl functions at both ends).

[0038] The crosslinking reaction is initiated by a catalyst commonly used in the Michael polyaddition reaction, also called an initiator, of the nucleophilic base type. The catalyst can be chosen from 1,8-diazobicyclo[5.4.0]undec-7-ene, dimethylphenyl phosphine, triphenyl phosphine, triethylamine, pyridine, or dimethylaminopyridine, and preferably 1,8-diazobicyclo[5.4.0]undec-7-ene, dimethylphenyl phosphine, triphenyl phosphine, or triethylamine; even more preferably, the catalyst is triethylamine. Advantageously, a thiol-to-catalyst molar ratio of between 200 and 600 is used, which corresponds in particular to a tetrafunctional crosslinking agent-to-catalyst molar ratio of approximately 50 to 150, when the molecule containing the thiols is tetrafunctional (4 thiol groups).

[0039] The crosslinkable electrolyte formulation according to the invention therefore comprises at least the following constituents: A molecule bearing three to six thiol groups, for example, four thiol groups (pentaerythritol tetrakis(3-mercaptopropionate) in the examples), or three or six if the flexibility of the final material is to be varied; a chain extender bearing two C=C double bonds (poly(ethylene glycol) dimethacrylate in the examples): the chain extender is advantageously chosen from any oligoethylene glycol unit bearing two C=C double bonds or any norbornene, vinyl ether, allyl ether, acrylate, methacrylate, maleimide, or alkene unit; a monofunctional single-ion chain terminator bearing one C=C double bond that provides the mobile lithium and the anchored counter-anion, i.e., covalently bound, to the chain and allows the generation of dangling chains, thus providing mechanical flexibility (lithium-3-((trifluoromethane)sulfonamidosulfonyl)propyl (methacrylate in the examples), A single-function polyethylene glycol chain terminator,A nucleophilic base-type catalyst (triethylamine in the examples): The amount of catalyst to be used is advantageously on the order of 0.04 molar equivalents, the choice of the exact amount being adjustable by a person skilled in the art.

[0040] In one embodiment of the invention, the crosslinkable electrolyte formulation comprises: pentaerythritol tetrakis(3-mercaptopropionate) ( A 4 ) ; poly(ethylene glycol)dimethacrylate ( B 2 ) ; lithium-3-((trifluoromethane)sulfonamidosulfonyl)propyl methacrylate ( B' 1), poly(ethylene glycol) methyl ether methacrylate ( B" 1), of triethylamine as a catalyst, preferably with a tetrafunctional crosslinking molar ratio ( A4 ) on catalyst between 50 and 150.

[0041] Optionally, a soluble lithium salt or a mixture of several soluble salts may be added to the starting formulation. The soluble lithium salt(s) in the starting formulation are preferably chosen from LiTFSi, LiPF6, LiFSI, LiClO4, and LiTDI. LiTFSi is the preferred soluble lithium salt, or any mixture of several soluble lithium salts may be added to the starting formulation. The exact quantity of soluble lithium salt can be between 2 and 30% by mass of the starting formulation, and preferably between 5 and 15% by mass.

[0042] It is also possible to add a plasticizer, chosen from the following compounds: oligoethylene glycol, alkyl carbonates, succinonitrile, a low-volatility polar aprotic solvent, or an aprotic ionic liquid. The amount of plasticizer can be between 2% and 30% by mass of the starting formulation, and preferably between 5% and 15% by mass.

[0043] The crosslinkable liquid formulation according to the invention can be formed between two plates or by coating or spraying onto a substrate. Crosslinking to form the network is then achieved by heating at a temperature between 50 and 80 °C for a period of 1 to 24 hours, and preferably between 6 and 12 hours. The catholytes or anolytes can be formed by impregnating a porous electrode with the liquid formulation (coating or spraying) or by mixing the liquid formulation with an active ingredient to form an ink, optionally with the addition of a solvent that will evaporate after crosslinking.

[0044] In cases where the solid electrolyte is in contact with the positive electrode, the crosslinkable formulation according to the invention, in its liquid state, can be coated or sprayed onto a positive electrode already prepared according to protocols known to those skilled in the art, so that the liquid formulation wets the electrode's porosity. Crosslinking is then achieved after thermal initiation. Preferably, the formulation is coated or sprayed and then crosslinked before calendering the electrode.

[0045] For example, the formulations according to the invention can be used to formulate a positive electrode (cathode) ink, notably by adding to the formulation the active material (for example, a lithium nickel manganese cobalt mixed oxide or a lithium iron phosphate) and an electron percolant. This ink, once coated and dried, can constitute a solid positive electrode. Characterization techniques

[0046] The ionic conductivity of an electrolyte is measured in S / cm and characterizes the electrolyte's ability to transport ions.

[0047] The ionic conductivity of the electrolyte is measured by electrochemical impedance spectroscopy in a Biologic®< CESH cell. The measurement is performed at various temperatures using a Biologic®< ITS temperature-controlled chamber. The impedance spectrum is acquired using a Biologic®< MTZ 35 potentiostat operating between 30 MHz and 0.1 Hz around 0 V with an amplitude of ±10 mV. The conductivity value can be determined by fitting the curve to an equivalent circuit of the type (R1 + R2 / / CPE1 + CPE2) or visually by taking the value of the real impedance Re(Z) at the minimum point reached by the curve between the semicircle and the half-line corresponding to the capacitive part on the Nyquist diagram.

[0048] The cation transport number (t+) corresponds to the fraction of the total conductivity related to charge transport by cations and is characterized by impedance spectroscopy on a sample mounted between two non-blocking (lithium metal) electrodes at 60°C with a Biologic VMP3 potentiostat operating between 1 MHz and 0.1 MHz around 0 V with an amplitude of 10 mV. The transport number is obtained by fitting an equivalent circuit (R1 + R2 / / CPE2 + R3 / / CPE3 + Wd1) and then applying the formula: t+ = R2 / (RWd1 + R2). This measurement method corresponds to the so-called "Watanabe" method (Solid State Ionics 28-30 (1988) 911-917).

[0049] The solvent swelling test and calculation of the soluble fraction are classic methods for characterizing polymer networks to obtain an indirect estimate of their crosslinking density and chemical stability. After immersing approximately 300 mg of polymer network sample for 72 hours at room temperature in a large excess of chloroform (CHCl3), the swollen samples are weighed and then dried under vacuum.

[0050] The soluble fraction (ws) is calculated using the following equation: ws = 1 − m d / m 0 with m 0 the initial mass of the sample swollen with solvent (estimated by linear regression on the curve of masses measured at regular intervals of 0.5 to 5 minutes after removing the sample from the solvent) and md the mass of the latter after extraction of the soluble fraction and drying.

[0051] The swelling rate, which corresponds to the gain in volume of the network after immersion in the solvent, (1 / q 2 ) is calculated with the following equation: 1 / q 2 = ρ p q 1 − 1 / ρ s where q1 is the ratio of the swollen sample mass to the dry sample mass, ρs is the density of the solvent (ρs = 1.492 g.cm-3 for CHCl3) and ρp is the density of the polymer network.

[0052] Various techniques allow the thermo-mechanical properties of single-ion polymer networks to be characterized.

[0053] Differential scanning calorimetry (DSC for Differential Scanning Colorimetry ) is a technique that allows the characterization of thermochemical processes, particularly phase transitions and changes of state. It is used here to determine glass transition temperatures ( T g ) of the polymer networks obtained.

[0054] Differential scanning calorimetry (DSC) experiments were performed using a DSC Q200 instrument (TA Instruments) calibrated with an indium standard. Samples (5 to 10 mg) were prepared using airtight capsules and measured under a helium flow of 25 mL / min. The samples were first heated to 120 °C at a rate of 10 °C / min and held at this temperature for 2 min. The temperature was then lowered to -80 °C at a rate of 10 °C / min before being reheated, after a 2-min isotherm, to 200 °C at a rate of 10 °C / min. The glass transition temperatures ( T g ) were measured at mid-height of the transitions appearing during the second heating using TA Thermal Analysis software.

[0055] Thermogravimetric analysis is a technique used to characterize the mass loss profile of a sample subjected to temperature variations. It characterizes the chemical changes in materials as a function of temperature, such as evaporation or chemical degradation.

[0056] Thermogravimetric analysis (TGA) experiments were performed using a TGA Q500 instrument (TA Instruments). A temperature ramp to 20 °C / min followed by an isotherm at 110 °C for 8 min was carried out to eliminate mass loss due to the presence of water. Then, approximately 8 mg samples were heated from 20 to 600 °C at a rate of 10 °C / min under a continuous flow of helium at 60 mL / min. Advantages of the invention

[0057] The crosslinkable electrolyte formulation according to the invention has the advantage, particularly compared to pre-polymerized polymers, of being initially liquid. This allows for good cohesion at the interfaces with the electrodes, notably due to the facilitated filling of the material's porosity. The single-ion characteristic (t+=1) leads to a homogeneous distribution of Li+ ions within the material, thus eliminating the ion concentration gradient under an electric field (battery charging and discharging). Consequently, overvoltages related to the diffusion of Li+ ions through this material are significantly reduced.

[0058] The use of controlled crosslinking on a mixture of specific monomers and the particular morphology of the three-dimensional network also impart increased chain mobility and consequently improved ionic conduction. The performance of the solid electrolyte according to the invention relies in particular on the specific selection of certain highly flexible monomers that are good solvents for lithium ions, and on controlled crosslinking.

[0059] The rheological behavior obtained for the crosslinked electrolyte samples according to the invention advantageously corresponds to that of a crosslinked polymer. Examples : Materials and methods:

[0060] For the sake of simplicity in notation, the products comprising the network will be named as follows: pentaerythritol tetrakis(3-mercaptopropionate): A 4 poly(ethylene glycol) dimethacrylate: B 2 lithium-3-((trifluoromethane)sulfonamidosulfonyl)propyl methacrylate B' 1 poly(ethylene glycol) methyl ether methacrylate: B" 1 triethylamine: And 3 N

[0061] The molar equivalence of the functionalities is such that 2 A 4 = 2 B 2 + 2 (B' 1 + B" 1 ).

[0062] The initial liquid mixture is placed between two glass plates coated with Teflon tape and separated by a 200 µm thick PTFE film for ionic conductivity and transport number measurements, and a 2 mm thick film for thermo-mechanical characterizations. The apparatus is placed in an oven at 60 °C for 12 hours. The resulting solid samples are dried on a Buchi drying rack before being characterized.

[0063] The solvent swelling test and calculation of the soluble fraction are classic methods for characterizing polymer networks to obtain an indirect estimate of their crosslinking density and chemical stability. These measurements are performed after immersing approximately 300 mg of network for 72 hours at room temperature in a large excess of chloroform (CHCl3). The swollen networks are weighed and then dried under vacuum. The insoluble fraction is calculated using the following equation: Ti = m d / m 0 × 100 with m0 the initial mass of the sample and md the mass of the sample after extraction of the soluble fraction and drying.

[0064] The swelling ratio (1 / q2) is calculated using the following equation: 1 / q 2 = ρ p q 1 − 1 / ρ s where q1 is the ratio of the swollen sample mass to the dry sample mass, ρs is the density of the solvent (ρs = 1.492 g.cm-3 for CHCl3) and ρp is the density of the polymer network (ρp ≈ 1).

[0065] The thermo-mechanical properties of single-ion polymer networks are characterized by DSC, ATG and DMA in order to determine the glass transition value respectively T g, the value of the degradation temperature for 10% loss T d10 and the values ​​of the conservation modulus E' at the rubbery plateau and the alpha transition temperature T α .

[0066] Differential scanning calorimetry (DSC) experiments were performed using a DSC Q200 instrument (TA Instruments) calibrated with an indium standard. Samples (5 to 10 mg) were prepared using airtight capsules and measured under a helium flow of 25 mL / min. The samples were first heated to 120 °C at a rate of 10 °C / min and held at this temperature for 2 min. The temperature was then lowered to -80 °C at a rate of 10 °C / min before being reheated, after a 2-min isotherm, to 200 °C at a rate of 10 °C / min. The glass transition temperatures ( T g ) were measured at mid-height of the transitions appearing during the second heating using TA Thermal Analysis software.

[0067] Thermogravimetric analysis (TGA) experiments were performed using a TGA Q500 instrument (TA Instruments). A temperature ramp to 20 °C / min followed by an isotherm at 110 °C for 8 min was carried out to eliminate mass loss due to the presence of water. Then, approximately 8 mg samples were heated from 20 to 600 °C at a rate of 10 °C / min under a continuous flow of helium at 60 mL / min.

[0068] The ionic conductivity of the electrolyte is measured by impedance spectroscopy in a Biologic®< CESH cell. The measurement is performed at several temperatures using a Biologic®< ITS temperature-controlled chamber. The impedance spectrum is acquired using a Biologic®< MTZ 35 potentiostat between 30 MHz and 0.1 Hz around 0 V and with an amplitude of 10 mV.

[0069] The transport number of the samples is measured by impedance spectroscopy. The electrolytes are placed between two metallic lithium electrodes and characterized at 60 °C. The impedance spectrum is acquired using a Biologic® VMP3 potentiostat at 0 V with an amplitude of 10 mV between 1 MHz and 0.1 MHz. The impedance spectrum is fitted by an equivalent circuit, and the electrolyte and diffusion resistances can then be extracted. The transport number is calculated from these resistances.

[0070] Three formulations were tested to vary the molar ratios of the four starting components, particularly the amount of lithium in the resulting single-ion network (proportional to the mass percentage of B'1), and to test the impact of adding a lithium salt (LiTFSI) and a plasticizer (succinonitrile). The catalyst (a nucleophilic base initiator) was added last, and its molar equivalent remained constant (0.04). Table 1 presents the molar equivalent compositions of samples A to C and the mass percentages of the lithium chain terminator and the plasticizer in the starting formulation. Table 1 A 4 B 2 B' 1 B" 1 LiTFSI Molar equation Succinonitrile % mass A 4 5 5 (or 26%m) 1 0 0 B 4 5 6 (or 32%m) 0 0 0 C 4 5 6 (or 32%m) 0 1 10

[0071] Table 2 presents the results obtained after immersing the networks in chloroform at room temperature (insoluble content Ti and swelling G of networks A to C). It can be seen that the three formulations lead to materials with good chemical stability, as the insoluble content is all greater than 85%. The low swelling values ​​(all less than 5) indicate very good crosslinking of the networks. Table 2 G Ti (%) A 4,5 91 B 4,3 87 C 3,1 90

[0072] Table 3 (Glass transition temperature Tg and decomposition temperature of 10% of the initial mass Td10 of networks A to C) presents the results from DSC and TGA analyses. The glass transition temperature is low (not exceeding -15 °C), indicating adequate segmental mobility for lithium transport within the operating temperature range of a battery. All three tested formulations exhibit a decomposition temperature of 10% of the initial mass above 280 °C, which is perfectly satisfactory for the intended application. Table 3 T g (°C) T d10 (°C) A -20 314 B -17 316 C -21 283

[0073] There Figure 1represents the conductivity measurements of the networks resulting from the three tested formulations A, B, C. It is observed that when the mass fraction of single-ion chain terminator increases from 26 to 32% by mass, the conductivity of the final network also increases due to the addition of mobile lithium ions to the system (6.7 x 10⁻⁶ < vs 9.5 x 10⁻⁶ < S.cm⁻¹ < at 60 °C). Furthermore, if a small amount of lithium salt and plasticizer is added to the initial formulation, the conductivity is further improved (1.4 x 10⁻⁵ < S.cm⁻¹ < at 60 °C).

[0074] The transport numbers obtained for formulations A and B are equal to one, which is characteristic of a single-ion system. Network C has a transport number less than 1, due to the presence of the lithium salt.

Claims

1. Crosslinkable electrolyte formulation comprising at least: - a hydrocarbon molecule containing three to six thiol functions, preferably four; - a bifunctional chain extender in the form of a hydrocarbon chain bearing two C=C double bonds; - a monofunctional single-ion chain terminator containing a C=C double bond and comprising mobile lithium; - a monofunctional polyethylene glycol (PEG) chain terminator; - a nucleophilic base catalyst, wherein the [C=C double bond] / [thiols] molar ratio is 1.

2. Crosslinkable electrolyte formulation according to Claim 1, which comprises a soluble lithium salt or a mixture of soluble lithium salts in the formulation and wherein the amount of lithium salt(s) represents between 2% and 30% by weight, relative to the total formulation weight, preferably between 5% and 15% by weight, relative to the total formulation weight.

3. Crosslinkable electrolyte formulation according to either of the preceding claims, wherein the catalyst is chosen from 1,8-diazabicyclo[5.4.0]undec-7-ene, dimethylphenylphosphine, triphenylphosphine or triethylamine, pyridine and dimethylaminopyridine and preferably chosen from 1,8-diazabicyclo[5.4.0]undec-7-ene, dimethylphenylphosphine, triphenylphosphine or triethylamine, very preferably triethylamine.

4. Crosslinkable electrolyte formulation according to one of the preceding claims, wherein the hydrocarbon molecule containing 3 to 6 thiol functions is chosen from pentaerythritol tetrakis(3-mercaptopropionate), trimethylolpropane tris(3-mercaptopropionate), a poly[(mercaptopropyl)methylsiloxane] or a (mercaptopropyl)methylsiloxane-co-dimethylsiloxane copolymer with an average functionality of greater than or equal to 3, preferably is pentaerythritol tetrakis(3-mercaptopropionate).

5. Crosslinkable electrolyte formulation according to one of the preceding claims, wherein the bifunctional chain extender is chosen from any oligoethylene glycol unit bearing two C=C double bonds or any norbornene, vinyl ether, allyl ether, acrylate, methacrylate or alkene unit.

6. Crosslinkable electrolyte formulation according to Claim 5 wherein the bifunctional chain extender is chosen from poly(ethylene glycol) ( PEG)dimethacrylate, PEG diacrylate, PEG diallyl, PEG divinyl.

7. Crosslinkable electrolyte formulation according to one of the preceding claims, wherein the monofunctional single-ion chain terminator is lithium 3-[(trifluoromethane)sulfonamidosulfonyl]propyl methacrylate.

8. Crosslinkable electrolyte formulation according to one of the preceding claims, wherein the monofunctional polyethylene glycol chain terminator is chosen from poly(ethylene glycol) methyl ether acrylate, poly(ethylene glycol) allyl methyl ether, poly(ethylene glycol) vinyl methyl ether or poly(ethylene glycol) maleimide methyl ether.

9. Crosslinkable electrolyte formulation according to one of the preceding claims, comprising the catalyst in an amount such that the molar ratio of thiol functions to catalyst is between 200 and 600.

10. Crosslinkable electrolyte formulation according to one of the preceding claims, comprising a second chain extender of the dithiol family, preferably chosen from polydimethylsiloxane (PDMS) or polyethylene glycol (PEG) polymers terminated with mercaptoethyl or mercaptopropyl functions at both ends.

11. Crosslinkable electrolyte formulation according to one of the preceding claims, comprising a plasticizer chosen from the following compounds: oligoethylene glycol, carbonate ester, succinonitrile, polar aprotic solvent or aprotic ionic liquid, said plasticizer representing from 2% to 30%, preferably from 5% to 15% by weight, relative to the total formulation weight.

12. Process for preparing a crosslinked solid electrolyte, wherein: a) the crosslinkable electrolyte formulation according to one of the preceding claims is crosslinked, in the optional presence of a nonaqueous solvent, by means of the catalyst present in the formulation and by thermal activation, in order to form a polymer which conducts lithium ions, b) the optional solvent present in said polymer is evaporated in order to obtain a crosslinked solid electrolyte.

13. Process for preparing a crosslinked solid electrolyte according to Claim 12, wherein the thermal activation is carried out by heating the formulation at a temperature of between 50°C and 80°C for a period of between 1 and 24 hours and preferentially between 6 hours and 12 hours.

14. Process for preparing a crosslinked solid electrolyte in electrode form according to Claim 12 or 13, wherein in step a) a porous electrode is impregnated with the crosslinkable electrolyte formulation by coating or spraying, and then the coated or sprayed formulation is crosslinked, or an active material and an electronic percolant are added to the crosslinkable electrolyte formulation in step a) to formulate an electrode ink which is coated and then crosslinked to obtain a solid electrode.

15. Use of the crosslinked electrolyte obtained by crosslinking of the formulation according to one of Claims 1 to 11 or obtained by the process according to one of Claims 12 to 14 as solid electrolyte of an all-solid-state Li-ion battery or as component of the positive electrode (posolyte or catholyte) or of the negative electrode (negolyte or anolyte) of an electrochemical system.