TOOL AND METHOD FOR MANUFACTURING A COMPOSITE SHOVEL FOR A TURBOMACHINE
Patent Information
- Application Number
- DE602023026046
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-09-26
- Filing Date
- 2023-09-18
- Publication Date
- 2026-11-18
- Estimated Expiration
- 2043-09-18
AI Technical Summary
The challenge in manufacturing composite material blades for turbomachines lies in the complex and demanding process of attaching metal shields to the edges, which requires precise geometric matching and involves complex processes to ensure optimal bonding and mechanical performance, while avoiding adhesive degradation and resin polymerization issues.
The use of tooling with independent temperature management elements for different parts of the mold cavity allows for controlled heating and cooling, optimizing resin diffusion and adhesive bonding by adjusting temperatures to specific requirements during the manufacturing process.
This approach ensures precise positioning and robust attachment of metal shields, optimizing resin impregnation and polymerization, thereby enhancing the mechanical performance and reliability of composite blades.
Description
Technical field of the invention
[0001] The present invention relates to tooling and a method for manufacturing a blade made of composite material for an aircraft turbomachine. Technical background
[0002] The prior art includes in particular documents FR-A1-2 956 057, FR-A1-3 029 134, FR-A1-3 051 386 and EP-A2-2 353 830, which discloses the preamble of claim 1.
[0003] The use of composite materials is advantageous in the aeronautical industry in particular because these materials have interesting mechanical performance for relatively low masses.
[0004] A manufacturing process for composite parts in the aerospace industry, well known to those skilled in the art, is the RTM molding process, whose initials refer to the Anglo-Saxon acronym for Resin Transfer Molding .
[0005] This is a process for manufacturing a part from a composite material based on resin-impregnated fibers. Such a process is used, for example, to manufacture a blower blade and involves several successive steps.
[0006] The process begins by weaving fibers to create a three-dimensional rough preform. This preform is then cut to obtain a final shape that closely resembles the desired blade shape. This preform is then placed in a tooling consisting of a mold and a counter-mold. The tooling is closed, and liquid resin is injected while maintaining pressure on the injected resin as the part is polymerized by heating the tooling.
[0007] The resins used are very fluid and capable of penetrating the preform fibers well, even when injected under low pressure. During polymerization, under the influence of heat, the injected resin successively transitions from a liquid to a gelled state and finally to a solid state.
[0008] For the manufacture of a turbine blade, for example for a turbomachine fan, a preform is created by three-dimensional weaving and then impregnated with resin to form a blade. This blade has an intrados and an extrados that extend from a leading edge to a trailing edge of the blade.
[0009] The composite material of the blade is relatively fragile, and particularly sensitive to impacts, and it is known to protect it by means of a metal shield which is attached and fixed to the leading edge of the blade.
[0010] The shield can be attached to the blade in several ways. One method involves gluing the shield to the blade after the resin has polymerized. The adhesive is then in the form of a paste or a film.
[0011] In current technology, the matching of shields to the edges of the blades is a key and demanding step in the manufacturing process. Indeed, the shields are very complex parts and can vary from one to another depending on the manufacturer and manufacturing tolerances, and can therefore have different geometric characteristics.
[0012] Therefore, before pairing and gluing a shield onto the edge of a blade, it is necessary to ensure that the dimensions and shapes of the shield are in accordance with those of the blade in order to optimize the gluing surface and therefore the material health of the part once glued (glue thickness, porosity rate, etc.).
[0013] By eliminating the bonding step and integrating it directly into the injection molding step, the geometry of the bonding interface is directly conformed to the geometry of the blade edge at every point, thus removing the step of finding the optimum shield / blade edge fit. This also eliminates any surface preparation of the blade before bonding. Finally, it eliminates the need for additional heat treatment equipment (furnace, autoclave, etc.).
[0014] Another method for attaching a shield to a blade has already been proposed, which involves co-molding the shield with the fibrous preform. Adhesive is applied between the shield and the preform, and the assembly is then placed in the tooling. Injected resin impregnates the preform, and a curing and pressure-curing process ensures the polymerization and hardening of both the adhesive and the resin.
[0015] The curing cycle must be adapted to account for the physical properties and application conditions of both the adhesive and the resin. This constraint necessitates the development of a complex process that is difficult to industrialize. A thermal compromise must be found to guarantee the robustness of the process in terms of physicochemical properties and the mechanical performance of the final assembly.
[0016] Regarding glue, for example, it is important to: do not degrade the rheology in order to ensure wetting on the surfaces to be bonded, ensure that the viscosity is relatively high before applying pressure in the tooling, and do not prematurely age the glue at temperature to guarantee the final mechanical properties of the glue joint.
[0017] Regarding the resin, it is important to: ensure a low viscosity to fill the mold cavity and impregnate the preform, and therefore ensure a sufficient mold temperature, and ensure that the polymerization advancement rate is as low as possible before applying pressure to the mold.
[0018] The present invention proposes an improvement to the current technique which makes it possible to provide a solution to at least some of the problems mentioned above. Summary of the invention
[0019] The invention provides tooling for manufacturing a composite material blade for a turbomachine, particularly for aircraft, this blade comprising a blade having an intrados and an extrados extending from a leading edge to a trailing edge of the blade, the blade also comprising a root and an upper edge opposite its root, the blade further comprising at least one metal shield extending along at least one of said edges of the blade, the tooling comprising: a mold and a counter-mold which define between them a cavity configured to receive a woven preform of the blade, the cavity comprising a first part configured to receive the shield and the edge(s) of the preform intended to receive this shield, and a second part configured to receive at least a part of the rest of the preform, at least one resin injection port in the cavity in order to impregnate said preform, and temperature management elements for the cavity, characterized in that the temperature management elements comprise first temperature management elements for the first part of the footprint, and second temperature management elements for the second part of the footprint which are independent of the first temperature management elements so that the first and second management elements can heat the first and second parts of the footprint to different temperatures during at least one step of a blade manufacturing process.
[0020] The tooling according to the invention thus comprises temperature control elements that are independent and configured to temperature the first and second parts of the impression respectively. It is therefore understood that the temperature of the part of the impression containing the edge(s) and the adhesive can be adjusted to facilitate resin diffusion within the preform while preventing accelerated aging of the adhesive, and the temperature of the other part of the impression can be adjusted to facilitate resin diffusion while optimizing the conditions for resin polymerization.
[0021] In this application, "temperature control" refers to heating and / or cooling. The components are therefore capable of heating and / or cooling the tooling and the mold cavity. For example, the first control components are heating and / or cooling components, and the second control components are heating components.
[0022] The tooling according to the invention may comprise one or more of the following features, taken individually or in combination with each other: The second temperature control elements are heating elements that are configured to heat the tooling to a predetermined temperature, denoted T1; the first temperature control elements are heating elements that are configured to heat the tooling to a predetermined temperature, denoted T1, during one step of a manufacturing process, and to another predetermined temperature, denoted T2 and lower than T1, during another step of the manufacturing process; the first temperature control elements are cooling and heating elements that are configured to heat the tooling to a predetermined temperature, denoted T1, during one step of a manufacturing process, and to cool the tooling to a predetermined temperature, denoted T2 and lower than T1, during another step of the manufacturing process;The cavity includes an intermediate section, located between the first and second sections, with the temperature control elements configured to create a gradual temperature transition zone in this intermediate section; the temperature control elements are of the heating element, induction, or heat transfer fluid type; the temperature control elements are distributed throughout the mold and counter-mold; and the temperature control elements are integrated into the mold and counter-mold; the first temperature control elements can be arranged in the first section of the cavity, and the second temperature control elements can be arranged in the second section of the cavity.
[0023] The invention also proposes a method for manufacturing a composite material blade for a turbomachine, particularly for aircraft, this blade comprising a blade having an intrados and an extrados extending from a leading edge to a trailing edge of the blade, the blade also comprising a root and an upper edge opposite its root, the blade further comprising at least one metal shield extending along at least one of said edges of the blade, the method using tooling as described above and comprising the steps of: a) place a shield and a preform made by weaving fibers in the mold cavity, with a polymerizable adhesive interposed between the shield and the edge(s) of the preform intended to receive the shield, the shield and the edge(s) of the preform being positioned in the first part of the cavity, and the remainder of the preform being positioned in the second part of the cavity, b) close the mold, and c) control the mold temperature and inject polymerizable resin into the mold cavity so that it impregnates the preform to form the blade after solidification, characterized in that step c) comprises: c1) a first sub-step of resin injection during which the second part of the impression is heated to a predetermined temperature, denoted T1, and the first part of the impression is managed so as not to exceed a predetermined temperature, denoted T2, which is lower than T1, and c2) a second sub-step of curing during which the first and second parts are heated to temperature T1.
[0024] The process according to the invention may comprise one or more of the following steps or features, taken individually or in combination with each other: In substep c1), the first part of the impression is heated to the predetermined temperature T2; it is therefore understood that this first part goes from a temperature below T2 to the temperature T2, by heating; in substep c1), the first part of the impression is cooled so as not to exceed the predetermined temperature T2; it is therefore understood that this first part tends to heat up beyond T2 and is cooled so as not to exceed this temperature; the temperature T1 is greater than or equal to 160°C, and preferably greater than or equal to 180°C, and the temperature T2 is between 80 and 140°C, and preferably between 100 and 130°C; the weaving of the preform is carried out in two dimensions or in three dimensions. Brief description of the figures
[0025] Other features and advantages of the invention will become apparent upon reading the detailed description that follows, for an understanding of which reference should be made to the attached drawings in which: [ Fig.1 ] there figure 1 is a schematic perspective view of a composite turbine blade for an aircraft turbomachine, [ Fig. 2 ] there figure 2 is a block diagram showing steps in a process according to the invention for manufacturing a blade such as that shown in the figure 1 , [ Fig.3 ] there figure 3 is a schematic perspective view of a mold in which a preform and a shield are intended to be placed, and into which a resin is intended to be injected, [ Fig. 4 ] there figure 4 is a graph representing the temperature evolution of a blade manufacturing tool according to the figure 1 over time, and illustrates two heating cycles, [ Fig. 5 ] there figure 5is a schematic cross-sectional view of a tool according to an embodiment of the invention; [ Fig. 6 ] there figure 6 is a schematic cross-sectional view of a tool according to an alternative embodiment of the invention; and [ Fig. 7 ] there figure 7 is a graph representing the temperature evolution of a blade manufacturing tool according to the figure 1 over time, and illustrates a manufacturing process according to the invention. Detailed description of the invention
[0026] We first refer to the figure 1 which illustrates a blade 10 made of composite material for a turbomachine, this blade 10 being for example a fan blade or a rectifier blade of a secondary flow in the case of a turbofan engine.
[0027] The blade 10 includes a blade 12 connected by a strut 14 to a foot 16 which has for example a dovetail shape and is shaped to be engaged in a cavity of complementary shape of a rotor disk, in order to retain the blade on this disk.
[0028] The blade 12 comprises a leading edge 12a and a trailing edge 12b of the gases flowing into the turbomachine. The blade 12 has a curved or even twisted aerodynamic profile and comprises an intrados 18 and an extrados 20 extending between the leading edge 12a and trailing edge 12b. The blade 12 further comprises a top edge 12c opposite the root 16.
[0029] The blade 12 is made from a fibrous preform obtained by weaving fibers, for example carbon fiber. The weaving can be done in two dimensions and preferably in three dimensions.
[0030] The leading edge 12a of the blade is reinforced and protected by a metal shield 22 which is fixed to this leading edge 12a. The shield 22 is for example made of nickel and cobalt alloy, titanium, stainless steel, etc.
[0031] The following description concerns the attachment of a shield 22 to a leading edge 12a. By analogy, it can be understood that the shield 22, or another shield, could be attached to the trailing edge 12b. It can also be understood that the shield 22, or another shield, could be attached to the upper edge 12c. Furthermore, the shield provided, for example, on the trailing edge 12b could extend to the upper edge 12c, or the shields of the trailing edges 12b and upper edges 12c could be formed from a single piece. Several variations are therefore conceivable with regard to the number and position of a shield as defined by the invention, even though the following description is made in relation to a shield located on the leading edge 12a of the blade 12.
[0032] In the present invention, the attachment of the shield 22 is achieved on the one hand by co-molding the preform with the shield 22, and on the other hand by gluing the shield 22 using an adhesive 26.
[0033] There figure 2 is a flowchart that illustrates the steps in a manufacturing process for a composite blade 10 such as the one shown in the figure 1 .
[0034] The process includes steps a), b) and c).
[0035] The first step a) of the process involves creating a fibrous preform by weaving fibers, preferably in three dimensions, using a Jacquard-type weaving machine, for example. The resulting preform is in its raw state and can undergo operations such as cutting, shaping, or compression.
[0036] The first step a) also includes the application of glue 26 between the shield 22 and the edge 12a of the preform 24, and then the placement of the assembly thus obtained in a mold 30 for manufacturing the blade, which is shown in the figure 3 The adhesive 26 can be applied using a brush or a spray, for example. Alternatively, it can be supplied in the form of a paste. Preferably, the adhesive is in the form of an adhesive film (such as a pre-impregnated fabric, for example) which is cut to the desired shape and then placed on the leading edge by the operator before the shield is attached to the leading edge.
[0037] Glue 26 is preferably a film adhesive consisting of a braided backing impregnated with a thermosetting epoxy-based resin, for example marketed by 3M ®< , Hexcel ®< , or Solvay ®< .
[0038] The shield 22 generally has a dihedral shape and defines a V-shaped groove into which an edge of the preform 24 is inserted. The adhesive 26 can be deposited in the groove of the shield 22 and / or on the edge of the preform 24.
[0039] The preform 24, equipped with the glue 26 and the shield 22, is then placed in the mold 30 ( figure 3 ). This mold 30 is part of a tooling that also includes a counter-mold (not shown). The mold 30 and the counter-mold have complementary shapes and together define a cavity 32 for receiving the preform 24 and the shield 22. Part or half of the cavity 32, intended for example to form the intrados 18 of the blade 12, is formed in the mold 30, and the other part or half of the cavity 32, intended for example to form the extrados 20 of the blade 12, is formed in the counter-mold.
[0040] During step b), the tooling is closed by bringing the counter-mold onto the mold 30 and keeping them tightly pressed together in particular to ensure a seal of the cavity 32.
[0041] The process then includes a step c) of managing the temperature of the tooling and injecting the polymerizable resin into the mold cavity so that it impregnates the preform 24 in order to form the blade after solidification.
[0042] The management, and in particular the heating, of the tooling is achieved through temperature control elements. These control elements may be part of an oven or autoclave and / or may be directly integrated into the mold and / or counter-mold of the tooling.
[0043] The resin injected into the tooling is intended to impregnate the preform 24 and to come into contact with the glue 26 of the shield 22. After polymerization and hardening of the resin, the shield 22 is joined to the blade 12 by means of the glue 26 and the resin.
[0044] The blade 10 thus obtained, after polymerization of the resin, is advantageous insofar as its shield 22 is perfectly positioned and held on the blade 12.
[0045] The resin is, for example, a thermosetting resin based on epoxy, polyimide, or bismaleimide. These resins are commercially available. Adhesive 26 and the resin are therefore two distinct materials with different physicochemical and, in particular, rheological properties that depend on the temperature.
[0046] There figure 4This is a graph representing two different heating cycles of the tooling. Heating cycle C2 shows the "ideal" cycle for good adhesion of the adhesive 26 and optimized bonding of the shield 22 to the leading edge 12a. Heating cycle C1 shows the "ideal" cycle for optimal injection and diffusion of the resin into the mold cavity 32. It can be seen that cycles C1 and C2 each include a similar initial heating phase A (left-hand slope of cycles C1 and C2), as well as a similar final cooling phase F (right-hand slope of cycles C1 and C2). However, cycles C1 and C2 also have different holding phases B, C, and E.Cycle C1 includes a first stage B at 160°C followed by a second stage C at 180°C, while cycle C2 includes a stage D at 150°C which is reached after a preliminary part D (just after the first part A) of temperature rise with a lower heating rate.
[0047] It is therefore clear that it would be preferable to optimize the heating of the tooling to take into account the different physicochemical behaviors of the adhesive 26 and the resin. This is what the present invention proposes with tooling that allows this objective to be achieved.
[0048] There figure 5 This illustrates, in a very schematic way, a first embodiment of a tool 40 according to the invention. This tool 40 comprises: a mold 30 and a counter-mold 34 which define between them a cavity 32 configured to receive a preform 24 woven from the blade, such as that described above, the cavity 32 having a first part Z1 configured to receive the shield 22 and the leading edge 12a of the preform, and a second part Z2 configured to receive at least a part of the rest of the preform 24, at least one resin injection port 36 in the cavity 32 of the tooling 40 in order to impregnate said preform 24, and temperature management elements 42, 44 which are preferably integrated into the mold 30 and the counter-mold 34.
[0049] According to the invention, the temperature management elements 42, 44 comprise first management elements 42 which are arranged at the level of the first part Z1 of the footprint 32, and second management elements 44 which are arranged at the level of the second part Z2 of the footprint 32 and which are independent of the first management elements 42.
[0050] As can be seen in the figure, the management elements 42, 44 are advantageously distributed in the mold 30 and the counter-mold 34.
[0051] In the example shown, the second control elements 44 are heating elements which are configured to heat the tooling 40 to a predetermined temperature, denoted T1. T1 is for example greater than or equal to 160°C, and preferably greater than or equal to 180°C.
[0052] The first control elements 42 can be heating elements that are configured to heat the tooling 40 to temperature T1 during one step of a manufacturing process, and to another predetermined temperature, denoted T2, which is lower than T1, during another step of the manufacturing process. T2 is, for example, between 80 and 140°C, and preferably between 100 and 130°C.
[0053] Alternatively, these first control elements 44 could be cooling and heating elements configured to heat the tooling to temperature T1 during one step of a manufacturing process, and to cool the tooling to temperature T2 during another step of the manufacturing process. In yet another variant, only the first elements 42 are integrated into the tooling and are cooling elements. The tooling 40 is intended to be placed in a heated press, oven, or autoclave for heating. When the first elements 42 are activated by the circulation of a heat transfer fluid, zone Z1 is cooled to prevent it from exceeding temperature T2, while the zone is heated to temperature T1. When the first elements 42 are not activated, zones Z1 and Z2 are heated to temperature T1.
[0054] These control devices can be electrical or fluidic. For example, they can be electric heating elements, or induction systems (both of which can only heat), or heat transfer fluid pipes (which can heat or cool).
[0055] In the variant implementation of the figure 6 In addition to parts Z1 and Z2, the footprint 32 includes an intermediate part Z3, located between the first and second parts Z1 and Z2. The temperature control elements are configured to create a gradual temperature transition zone at this intermediate part Z3. This intermediate part Z3 can be equipped with its own temperature control elements 46.
[0056] With reference to the figure 2 The present invention also relates to a method for manufacturing a blade in which step c) comprises: c1) a first substep of resin injection during which the second part Z2 of the impression 32 is heated to temperature T1, and the first part Z1 of the impression 32 is managed so as not to exceed temperature T2, and c2) a second substep of baking during which the first and second parts Z1, Z2 are heated to temperature T1.
[0057] During substep c1), the first part Z1 of the cavity 32 can be heated to the predetermined temperature T2. Alternatively, the first part Z1 of the cavity 32 is cooled so as not to exceed the predetermined temperature T2.
[0058] There figure 7 is a graph representing two different heating cycles of the tooling 40 according to the invention.
[0059] The C3 heating cycle is the heating cycle performed by the secondary control units 44, and therefore represents the heating cycle of part Z2 of the footprint 32 not including the shield 22 and the adhesive 26. By comparing this C3 heating cycle to the graph of the figure 4 , we observe that this cycle corresponds to the ideal C1 heating cycle for resin injection.
[0060] The C4 heating cycle is the heating cycle carried out by the first control units 42, and therefore represents the heating cycle of the part Z1 of the impression 32 comprising the shield 22 and the glue 26. These cycles C3, C4 overlap except with regard to the moment or the time interval ΔT of injection and diffusion of the resin.
[0061] During this substep c1) the first part Z1 of the footprint is heated and / or cooled to temperature T2. This temperature can vary and is 100°C in the example shown for cycle C4, and 130°C (temperature T2') for a variant of this cycle C4' shown in dashed lines.
[0062] The process according to the invention makes it possible to keep the adhesive as cold as possible to prevent it from creeping during resin injection, while simultaneously heating the rest of the mold cavity sufficiently so that the resin is fluid enough to optimize its diffusion. Since these two constraints are conflicting, the invention achieves a compromise by creating different temperature control zones within the tooling, thereby adding degrees of freedom in defining the heating cycle and thus facilitating its development.
Claims
1. A tooling (40) for manufacturing a vane (10) made of composite material for a turbomachine, in particular of an aircraft, said vane (10) comprising a blade (12) comprising a pressure side (14) and a suction side (16) which extend from a leading edge (12a) to a trailing edge (12b) of the blade, the vane also comprising a root (16) and an upper edge (12c) opposite its root (16), the vane further comprising at least one metal shield (22) extending along at least one of said edges (12a, 12b, 12c) of the blade (12), the tooling (40) comprising: - a mold (30) and a counter-mold (34) which define between them a cavity (32) configured to receive a woven preform of the blade (12), the cavity (32) comprising a first portion (Z1) configured to receive the shield (22) and the edge or edges (12a, 12b, 12c) of the preform intended to receive this shield (22), and a second portion (Z2) configured to receive at least part of the remainder of the preform, - at least one port (36) for injecting resin into the cavity (32) in order to impregnate said preform, and - elements (42, 44, 46) for managing the temperature of the cavity (32), characterized in that the temperature management elements (42, 44, 46) comprise first elements (42) for managing the temperature of the first portion (42) (Z1) of the cavity (32), and second elements (44) for managing the temperature of the second portion (Z2) of the cavity (32) which are independent of the first temperature management elements (42) so that the first and second management elements (42, 44) can heat the first and second portions (Z1, Z2) of the cavity (32) to different temperatures during at least one step of a method for manufacturing the vane (10).
2. The tooling (40) according to claim 1, wherein the second temperature management elements (44) are heating elements which are configured to heat the tooling (40) to a predetermined temperature, noted T1.
3. The tooling (40) according to claim 1 or 2, wherein the first temperature management elements (42) are heating elements which are configured to heat the tooling (40) to a predetermined temperature, noted T1, during a step of a manufacturing method, and to another predetermined temperature, noted T2 and lower than T1, during another step of the manufacturing method.
4. The tooling (40) according to claim 1 or 2, wherein the first temperature management elements (42) are cooling and heating elements which are configured to heat the tooling (40) to a predetermined temperature, noted T1, during a step of a manufacturing method, and to cool the tooling (40) to a predetermined temperature, noted T2 and lower than T1, during another step of the manufacturing method.
5. The tooling (40) according to one of the preceding claims, wherein the cavity (32) comprises an intermediate portion (Z3), located between the first and second portions (Z1, Z2), the temperature management elements (42, 44, 46) being configured to create a zone of gradual temperature transition at this intermediate portion (Z3).
6. The tooling (40) according to one of the preceding claims, wherein the temperature management elements (42, 44, 46) are of the resistance heating, induction or heat transfer fluid circulation type.
7. The tooling (40) according to one of the preceding claims, wherein the temperature management elements (42, 44, 46) are distributed in the mold (30) and the counter-mold (34).
8. The tooling (40) according to one of the preceding claims, wherein the temperature management elements (42, 44, 46) are integrated in the mold (30) and the counter-mold (34).
9. A method of manufacturing a composite material vane (10) for a turbomachine, in particular of an aircraft, said vane comprising a blade (12) comprising a pressure side (14) and a suction side (16) which extend from a leading edge (12a) to a trailing edge (12b) of the blade, the vane also comprising a root (16) and an upper edge (12c) opposite its root (16), the vane further comprising at least one metal shield (22) extending along at least one of said edges (12a, 12b, 12c) of the blade (12), the method using tooling (40) according to one of the preceding claims and comprising the steps of: a) arranging a shield (22) and a preform (24) made by weaving fibers in the cavity of the tooling (40), a polymerizable adhesive (26) being interposed between the shield (22) and the edge or edges (12a, 12b, 12c) of the preform intended to receive the shield (22), the shield (22) and the edge or edges of the preform being positioned in the first portion (Z1) of the cavity (32), and the remainder of the preform being positioned in the second portion (Z2) of the cavity, b) closing the tooling (40), and c) managing the temperature of the tooling (40) and injecting polymerizable resin into the cavity (32) of the tooling so that it impregnates the preform so as to form the blade (12) after solidification, characterized in that step c) comprises: c1) a first resin injection sub-step during which the second portion (Z2) of the cavity (32) is heated to a predetermined temperature, noted T1, and the first portion (Z1) of the cavity (32) is managed so as not to exceed a predetermined temperature, noted T2, which is lower than T1, and c2) a second curing sub-step during which the first and second portions (Z1, Z2) are heated to temperature T1.
10. The method according to claim 9, wherein, in sub-step c1), the first portion (Z1) of the cavity (32) is heated to the predetermined temperature T2.
11. The method according to claim 9, wherein, in sub-step c1), the first portion (Z1) of the cavity (32) is cooled so as not to exceed the predetermined temperature T2.
12. The method according to one of claims 9 to 11, wherein the temperature T1 is greater than or equal to 160°C, and preferably greater than or equal to 180°C, and the temperature T2 is between 80 and 140°C, and preferably between 100 and 130°C.
13. The method according to one of claims 9 to 12, wherein the weaving of the preform is carried out in two dimensions or in three dimensions.