HOT REPAIR PROCEDURE

DE602023026062T2Active Publication Date: 2026-11-18SAINT GOBAIN CENT DE RES & DEVS & DETUD EUROEN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
DE602023026062
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-11-30
Filing Date
2023-11-30
Publication Date
2026-11-18
Estimated Expiration
2043-11-30

AI Technical Summary

Technical Problem

Existing repair methods for industrial installations at high temperatures face challenges such as complex geometry reconstruction, difficulty in handling heavy metal formworks, and slow repair processes, leading to prolonged downtime and potential leaks due to protruding or penetrating repair areas.

Method used

A hot repair method using Ceramic Matrix Composite (CMC) formworks that can be installed at elevated temperatures, allowing for precise adaptation to complex geometries and remaining in place after repair, facilitating rapid production resumption.

Benefits of technology

Enables rapid and efficient repair of industrial installations by maintaining formwork integrity during high-temperature operations, reducing downtime, and ensuring precise reconstruction of original shapes without the need for post-repair removal.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader
Need to check novelty before this filing date? Find Prior Art

Description

technical field

[0001] The present invention relates to a hot repair method for an industrial installation, in particular for an industrial installation other than a glass furnace. Previous art

[0002] An industrial installation subjected to high temperatures typically includes components made of a refractory material, chosen according to their location to withstand local stresses, particularly chemical and / or thermal stresses related to the operation of the industrial installation, and ensure a satisfactory service life. The choice may also be guided by the need to avoid defects during the operation of the industrial installation, especially when it is a steel melting furnace. For example, in an induction steel melting furnace, the introduction of phosphorus, which weakens the steel, must be avoided.

[0003] To extend the lifespan of an industrial installation, particularly an industrial furnace, the operator may need to carry out repairs. A repair involves filling a void resulting from wear and tear on the industrial installation with a repair material; that is, fixing a repair material in an area initially occupied by a refractory material that has disappeared due to wear. This area is called the "area to be repaired."

[0004] There figure 1This represents a region of an industrial installation 10 as it appears before wear (left) and after wear (right). As illustrated in this figure, a repair area 30 can be "recessed," i.e., in the form of a cavity 301, for example, in a bottom wall 24. It can also be "protruding," i.e., a region 302 extending from a block that was initially protruding. The repair area can also penetrate the wall of an enclosure, for example, the side wall of a tank 31, creating a fluid connection between the inside and outside of the enclosure. Such a penetrating repair area can lead to leaks, particularly of gas or product, especially molten product. These leaks are dangerous and can cause a shutdown of operations. The repair area 303 is an example of a penetrating repair area created in a side wall 22.

[0005] A repair area is an empty space, that is to say, devoid of refractory material, partially delimited by one or more refractory parts of the industrial installation.

[0006] To repair an industrial installation, particularly an industrial furnace, a formwork is typically constructed to define the area to be repaired and, possibly using refractory material, to create a mold capable of holding the repair compound before it hardens. The formwork components, for example in the form of flat or curved plates, are typically held in a working position by accessories, thus defining the mold.

[0007] The formwork includes, or is made up of, a section positioned on the side where the initial wear occurred. This section of the formwork is called the "inner formwork." For example, to repair the wall of a furnace chamber made of refractory blocks, an inner formwork is installed to delimit, within the chamber, the area to be repaired.

[0008] When wear has led to a penetration through the wall, the formwork may also include a portion outside the enclosure, or "external formwork," to prevent the repair material from escaping outside the enclosure. The external portion of the formwork is typically a veneer.

[0009] A "hot" repair is a repair that is carried out at a temperature typically above 250°C. Hot repair therefore requires only a limited reduction in temperature, or even no reduction in temperature, which considerably limits the duration of interruption of the operation of the industrial installation, or even eliminates it.

[0010] Furthermore, the area to be repaired, particularly within an enclosed space, is often difficult to access, making the construction of internal formwork challenging in certain areas. Specifically, inserting the internal formwork elements may require creating openings through the enclosure wall. Additionally, during hot repairs, it is sometimes impossible for any operator to enter the enclosure. The internal formwork installation must then be carried out remotely from the area to be repaired. The size and weight of the internal formwork elements can therefore significantly slow down the formwork construction process.

[0011] These constraints also make it very difficult to create an internal formwork of complex shape, especially when the area to be repaired protrudes towards the inside of the enclosure.

[0012] The mold is then filled with repair material, typically using a pump. The repair material experiences a sudden temperature increase upon entering the mold, which reduces its flowability. This makes it difficult to fill the mold evenly.

[0013] Typically, the inner formwork is made of metal and is cooled by circulating water. After the repair product has hardened, the inner formwork is removed.

[0014] After the repair product has hardened, the formwork is removed, revealing the reconstituted refractory pieces. Generally, however, metal formwork does not allow for the reconstruction of the original shapes if they are complex.

[0015] Furnace repair procedures are described in particular in DE3601621, DE2143241A1, DE1927816A1 or EP0739861A2.

[0016] There is also a hot repair solution that involves spraying ("guniting") a repair product into the area to be repaired. However, this repair technique is not suitable for repairs of significant thickness.

[0017] There is therefore a permanent need for a repair process that solves the aforementioned problems, in particular allowing for a rapid return to production of the industrial installation.

[0018] The present invention aims to satisfy, at least partially, this need. Summary of the invention

[0019] The invention proposes a hot repair method for a region of an industrial installation at a temperature above 250°C, in particular inside an enclosure of the industrial installation, in particular inside an enclosure of an industrial furnace, referred to as the "region to be repaired", the industrial installation preferably being different from a glass furnace, said method comprising the following steps: a) installation of a formwork in a service position, so as to create a mold around the area to be repaired; b) filling, preferably by pouring, of the mold with a repair product, at least part of the formwork being made of a Ceramic Matrix Composite (CMC).

[0020] As will be seen in more detail later in the description, the inventors discovered in particular that a CMC does not substantially alter the quality of the product manufactured in said installation when it is put in contact with said product, and / or does not substantially alter the operation of said industrial installation, and therefore does not require removal of the formwork at the end of the repair.

[0021] Furthermore, a CMC It is lightweight, which facilitates its handling, and is easy to conform to complex geometries, allowing for precise adaptation to the configuration of the area to be repaired.

[0022] In addition, a CMC is highly resistant to thermal shock, which in particular allows for hot repair without damage to the formwork elements when they are introduced into an industrial installation enclosure.

[0023] The invention thus allows for a particularly rapid return to production of the industrial installation.

[0024] A method according to the invention may further include one or more of the following optional and preferred features: The industrial installation is chosen from: an iron or steel smelting furnace, and part of such a furnace; a non-ferrous metal smelting furnace; an element configured to transfer molten metal, in particular from a smelting furnace of said metal, said element being able to be physically separated from said furnace; a cement kiln; an ore reduction kiln; an incinerator; a hazardous waste treatment furnace; a gasifier; a reformer; a ceramic firing kiln; a carbon black reactor; a containment tank intended to retain a molten product at a temperature above 250°C, particularly in the event of an accidental spill of said product; an aluminum electrolysis cell; a turbine combustion chamber; a boiler;the process comprises, after step b), a step 5) of sintering the repair product introduced into the mold in step b), the sintered repair product obtained being composed of a plurality of constituents, the mass content of any constituent of the sintered repair product present in a mass content greater than 5%, differing by less than 20% from the mass content of said constituent in said ceramic matrix composite, and / or differing by less than 20% from the mass content of said constituent in a region of the industrial installation delimiting the area to be repaired; at least one element of said formwork has the shape of a part of the industrial installation that was protruding before said part disappeared by wear; the manufacture of the formwork comprises taking an impression on a replica, at least partial, of said industrial installation as it was before the wear that led to the area to be repaired;the formwork is left in the area to be repaired after said repair; the formwork is entirely made of a ceramic matrix composite; at least one element of the formwork made of a ceramic matrix composite has through holes and / or indentations arranged so as to be filled by the repair product during step b); preferably the mass of one formwork element, preferably the mass of more than 50% by number of the formwork elements, preferably the mass of each of the formwork elements is greater than 3 kg, preferably greater than 4 kg and / or preferably less than 50 kg, preferably less than 40 kg, preferably less than 30 kg, preferably less than 20 kg;preferably, the largest dimension of a formwork element, preferably more than 30% by number of formwork elements, preferably more than 50% by number of formwork elements, is greater than 400 mm, preferably greater than 600 mm and preferably less than 1600 mm, preferably less than 1400 mm; the formwork includes formwork elements partially delimiting the area to be repaired, and accessories for holding said formwork elements in a service position; said accessories being made of a ceramic matrix composite, identical or different from the ceramic matrix composite of the formwork elements; the ceramic matrix composite of at least part of the formwork, or even of the entire formwork, and / or the ceramic matrix composite of at least one accessory is / are sintered, and / or has / have an open porosity greater than 15% and less than 50%, and / or contains / contains more than 20% and less than 80% by volume of fibers, and / or contains / contains fibers of which at least a part are fibers comprising more than 95% by mass of oxides, and / or contains / contains fibers of which at least a part are fibers comprising more than 95% by mass of a material other than an oxide, and / or comprises / contains a matrix composed of more than 90% oxides and / or carbides and / or nitrides and / or at least one oxynitride compound of at least the elements Si, Al and N, in particular of a sialon, by mass percentage,and / or have an apparent density greater than 1.0 g / cm³ and less than 2 g / cm³; said process comprises the following steps: 2) optionally, rinsing said area to be repaired, 3) optionally, reducing the temperature in said industrial installation to a temperature above 250°C; 4) carrying out steps a) and b); 5) preferably, in particular when the process includes step 3), raising and maintaining the temperature of the industrial installation between 400°C and 1400°C in order to sinter the repair product; 6) if said process includes step 3), raising the temperature of said industrial installation to its operating temperature; the industrial installation comprises a container holding a fluid product, preferably a powdered or molten product, in particular a molten metal, and said process comprises, before step a), the following step: if the area to be repaired is,at least partially, delimited by a surface of the industrial installation in contact with said fluid product, draining, at least partially, of said enclosure so as to expose said area to be repaired; and, after step b), the following step: resumption of normal operation, the temperature of the industrial installation being maintained in said area to be repaired during all steps of the process; the industrial installation comprises an enclosure containing a fluid product, preferably a powdered or molten product, in particular a molten metal, and said process comprises, before step a), the following steps: 1) if the area to be repaired is, at least partially, delimited by a surface of the industrial installation in contact with said fluid product, draining, at least partially, of said enclosure,so as to expose said area to be repaired; 3) reducing the temperature in the area to be repaired to a temperature above 250°C; and, after step b), the following steps: 5) increasing and maintaining the temperature of the area to be repaired between 1000°C and 1400°C in order to sinter the repair product; 6) resuming normal operation of the industrial installation, i.e., setting the temperature of said industrial installation to its operating temperature; in step 3) the temperature in the area to be repaired is reduced to a temperature above 900°C and below 1500°C; said process includes a step of rinsing the area to be repaired after exposure of the area to be repaired; at least one element of the formwork has the shape of a part of the industrial installation that protruded before said part disappeared through wear and, preferably,the manufacture of the formwork involves taking an impression on a replica of said part of said industrial installation before wear; the inner formwork comprises a ceramic plate, preferably in the form of a ceramic matrix composite, having two large faces substantially parallel to each other, the ratio of the surface area of ​​one large face (in cm²) to the thickness (in cm, measured between the two large faces) being greater than 30 cm, preferably greater than 50 cm, preferably greater than 100 cm, preferably greater than 200 cm, preferably greater than 500 cm, preferably greater than 1000 cm, preferably greater than 2000 cm, and / or less than 250,000, preferably less than 200,000, preferably less than 150,000, preferably less than 100,000, preferably less than 50,000, preferably less than 10,000, preferably less than 8,000, preferably less than 5,000.each large face of the plate preferably having a surface area greater than 1000 cm², preferably greater than 1500 cm², preferably greater than 2000 cm², preferably greater than 2500 cm², and / or less than 10000 cm², preferably less than 8000 cm², preferably less than 5000 cm²; the area to be repaired is at least partially delimited by a side wall and / or a bottom wall of an enclosure, for example, of a tank intended to contain a molten product, said formwork comprising or being constituted by an internal formwork installed inside said enclosure in step a); the enclosure is closed and inaccessible to an operator; the area to be repaired is at least partially delimited by a pouring channel.

[0025] The characteristics described for formwork in general are applicable, in the specific case of container repair, particularly for a tank, to internal formwork, regardless of whether the formwork used to repair the container includes external formwork, and regardless of whether any external formwork is made of CMC (carbon composite material). Specifically, at least one element of the internal formwork may be shaped like a portion of the container that protruded inwards before that portion was lost through wear. The manufacture of the internal formwork may involve taking an impression from a replica of the unworn portion of the container.

[0026] The internal formwork can be left in the area to be repaired after said repair.

[0027] The invention also relates to an industrial installation, in particular an industrial furnace, comprising at least one region repaired according to a process according to the invention. Brief description of the figures

[0028] Other features and advantages of the invention will become apparent upon examination of the following description and with regard to the attached drawing in which: there Figure 1 [Fig 1 ] schematically represents part of an enclosure before (left diagram) and after wear (right diagram); the Figure 2 [Fig 2] ] schematically represents a process according to the invention; the figure 3 [Fig 3 ] represents an example of formwork according to the invention; the figure 4 [Fig 4 ] represents an example of an internal formwork element with through holes; the figure 5 [Fig 5 ] schematically represents a pouring channel for molten iron (or « runner » (in English), before wear, after wear and at the end of step b). Definitions

[0029] The term "enclosure" refers to a portion of an industrial installation that defines a chamber. An enclosure is delimited laterally by a side wall (the shape of which is not limited), a back wall, and optionally, a vault wall. The side wall, back wall, and vault wall may have one or more access openings to the chamber.

[0030] The term “tank” refers to an enclosure which, in use, contains a molten product, in particular a molten metal.

[0031] By "closed" tank or enclosure, we mean a tank or enclosure which an individual cannot enter while on duty.

[0032] The invention is particularly well suited to the repair of an enclosure, especially a tank, but is not limited to this embodiment.

[0033] A "formwork" is a part of the "mold" into which the repair product is introduced.

[0034] It generally results from the assembly of one or more "formwork elements" and the positioning of the assembled formwork element(s) in the "service position." The portion of the mold defined by the formwork is completed with a part of the industrial installation to constitute the mold. For example, the worn portion of the inner surface of an enclosure can be used to complete the formwork to delimit the area to be repaired.

[0035] In addition to the formwork elements, formwork includes "accessories" used to assemble and secure the formwork elements in their service position, and which do not come into contact with the repair material during the repair process. Unlike accessories, the formwork elements are components that do come into contact with the repair material during the repair.

[0036] The area to be repaired can be compartmentalized using partitions. A partition is considered a formwork element.

[0037] A "passage" is an opening that goes through a wall, for example, connecting the inside and outside of an enclosure, such as a tank, a carbon black reactor, or a combustion chamber. It may result from wear and tear on the wall or be intentionally created, for example, to allow the insertion of formwork elements through the wall.

[0038] The "equivalent diameter" of a surface is the diameter of a disk with the same area as that surface.

[0039] A dry particulate mixture is called an "unprocessed product".

[0040] By product "in a material" or "of a material" is meant a product consisting of more than 95%, more than 98%, preferably substantially 100% of its mass of said material.

[0041] The term "refractory material" refers to a material with a melting point above 1500°C. This definition is commonly used by those in the trade and is cited in "Refractory Materials and Technical Ceramics (Elements of Ceramics and Technology)," by G. Aliprandi, Septima Paris, 1979. This work also provides examples of refractory materials on pages 297 to 301, including oxides, carbides, and nitrides.

[0042] The "glass transition temperature" of a glass is the temperature at which the glass transitions from a solid to a viscous state. The glass transition temperature can be determined by differential thermal analysis (DTA). The glass transition temperature is the temperature at which the glass has a viscosity approximately equal to 1012 Pa·s. A glass is conventionally considered to be "in the solid state" at a temperature below its glass transition temperature.

[0043] By "hot binder" we mean a constituent having a melting point above 600°C, and capable of binding together, after hardening under the effect of a drop in temperature, particles with which it has been mixed.

[0044] The "maximum size" is defined as the 99.5th percentile (D 99.5) of a powder. This percentile corresponds to the mass percentage of 99.5% on the cumulative particle size distribution curve of the powder, with the particle sizes arranged in ascending order. Particle size distributions and the maximum size can be determined using a laser particle size analyzer. A suitable laser particle size analyzer is the Partica LA-950 from HORIBA.

[0045] "Hot self-casting" refers to a repair product capable of spreading under its own weight and filling the mold without segregation, within a temperature range of 250°C to 1550°C. Segregation is considered to have occurred when the casting face of the product obtained after placement of the repair product and sintering exhibits a surface layer of laitance extending from said casting face to a depth of 3 mm or more. This surface layer of laitance can be easily exposed after drying or sintering the product, with sawing carried out in a plane perpendicular to the casting face.

[0046] When referring to ZrO₂ or zirconia, this should be understood to mean ZrO₂ and traces of HfO₂. Indeed, a small amount of HfO₂, chemically inseparable from ZrO₂ in a melting process and exhibiting similar properties, is always naturally present in zirconia sources at mass concentrations generally below 2%. Hafnium oxide is therefore not considered an impurity.

[0047] By "Ceramic Matrix Composite", or "CMC", we classically mean a ceramic composed of a ceramic textile stiffened by a ceramic matrix.

[0048] A "textile" is an assembly of fibers, possibly a yarn, particularly an assembly of yarns. The textile typically represents between 20% and 80% of the volume of a CMC, with the matrix making up the remaining 100%.

[0049] In general, when referring to a volume percentage relative to an object, for example a CMC (e.g., a percentage of fibers) or the matrix of a CMC (as in the previous sentence), the volume to be considered is that of the object defined by its outer surface, i.e., it includes the empty spaces inside the object.

[0050] A "fiber" is a filament whose length is greater than 5 times its equivalent diameter.

[0051] The "equivalent diameter" of a fiber is the diameter of a disk with the same surface area as its cross-section at mid-length.

[0052] In a textile, the fibers can be assembled in a disordered way, as in felt or paper, or along one or more preferred directions, preferably in the form of yarns, themselves preferably in the form of one or more fabrics. A yarn in a textile can be a "single yarn", which is an assembly of fibers which, in cross-section, comprises more than 10 and preferably less than 500,000 fibers, and whose length is more than 5 times the diameter, or an "assembled yarn", which is an assembly of single yarns which, in cross-section, preferably comprises more than 2 and preferably less than 500 single yarns.

[0053] A textile can be, in particular: an organized structure of fibers, and / or yarns, simple or assembled, in particular a knit or a fabric, or a random structure of fibers, and / or yarns, simple or assembled, for example a veil, and / or of fibers not incorporated in the form of yarns, said random structure being for example a paper or a felt, a random structure not being preferred.

[0054] A "fabric" consists of a network of parallel warp threads and weft threads passing transversely through said network.

[0055] A "knit" consists of a network of threads arranged in the form of loops.

[0056] A "sheet" is made up of a set of parallel threads.

[0057] The term "ceramic" refers to a product that is neither metallic nor organic. For the purposes of this invention, carbon is considered a ceramic product.

[0058] A "sialon", SiAlON, is an oxynitride compound of at least the elements Si, Al and N, in particular a compound conforming to one of the following formulas: Si x Al y O u N v , in which: x is greater than or equal to 0, greater than 0.05, greater than 0.1 or greater than 0.2, and less than or equal to 1, less than or equal to 0.8 or less than or equal to 0.4, y is greater than or equal to 0, or greater than 0.1, greater than 0.3 or greater than 0.5, and less than or equal to 1, uis greater than 0, greater than 0.1 or greater than 0.2, and less than or equal to 1 or less than or equal to 0.7, v is greater than 0, greater than 0.1, greater than 0.2 or greater than 0.5, or greater than 0.7, and less than or equal to 1, x + y > 0 , x, y, u And v being stoichiometric indices normalized with respect to the highest one, made equal to 1; Me x Si 12-(m+n) Al (m+n) O n N 16-n , with 0 ≤ x ≤ 2, Me a cation chosen from the lanthanide cations, Fe, Y, Ca, Li and their mixtures, 0 ≤ m ≤ 12, 0 ≤ n ≤ 12 and 0 < n+m ≤ 12, the SiAlONs following this formula are generally called "α' - SiAlON" or "SiAlON-α'".

[0059] “Contain” or “understand” or “present” should be interpreted in a non-limiting manner. Detailed description Hot repair

[0060] A method according to the invention is used for the hot repair of a region of an industrial installation.

[0061] Preferably, the industrial facility is chosen from: an iron or steel smelting furnace, and part of such a furnace, in particular an electric arc furnace (or "electric arc furnace" in English"), a submerged arc furnace (or "submerged arc furnace" (in English), an electric immersion electrode furnace (or "open slag bath furnace" (in English), a blast furnace (or "blast furnace" (in English), an oxygen converter (or "Basic oxygen furnace" (in English), a direct iron ore reduction furnace (or “direct reduction iron shaftfurnace” (in English), a flow channel (or " runner » (in English), a steel reheating furnace (or “metal and iron reheat furnace” (in English), a holding oven (or "holder and melterfurnace" (in English), a casting basket (or " "Tundish"(in English); a non-ferrous metal melting furnace, in particular an aluminum melting furnace, a magnesium melting furnace, a copper melting furnace; a physically independent component of a metal melting furnace, or one that can be physically separated from a metal melting furnace, in contact with said molten metal and enabling the transfer of said molten metal from said melting furnace to another installation, in particular a transfer ladle (or "Ladle transfer"(in English); a cement kiln, in particular a rotary kiln; an ore reduction kiln, in particular an iron ore reduction kiln; an incinerator, in particular a municipal waste incinerator, a municipal waste incineration boiler; a hazardous waste treatment kiln; a gasifier, in particular a coal gasifier, a petroleum coke gasifier, a biomass gasifier; a reformer, in particular a methane reformer or a secondary reformer; a ceramic firing kiln; a carbon black reactor; a containment tank intended to contain a product at a temperature above 250°C in the event of an accidental spill of said product; an aluminum electrolysis cell; a turbine combustion chamber, in particular a gas turbine; a boiler, in particular a thermal power plant boiler.

[0062] The area to be repaired may in particular be located in a wall of the industrial installation, for example in the side wall of an enclosure, for example of a tank, of said industrial installation, in particular a wall of a closed enclosure, in particular of a closed tank.

[0063] The invention is particularly useful for repairing a side wall 22 of an enclosure. In such cases, it is necessary to contain the repair material to prevent it from flowing out due to gravity. This problem generally does not arise when repairing the back wall of the enclosure. The use of ceramic formwork elements, particularly in the form of plates, and especially ceramics such as CMC, advantageously allows for the creation of formwork that does not require cooling. This formwork can therefore be lighter (especially if made of thin plates). Furthermore, because it does not require cooling and can be left in place after repair, this formwork is very quick to install and does not need to be dismantled. The downtime of the industrial installation for repair is thus advantageously reduced. Finally, the formwork can be of complex shapes.

[0064] The area to be repaired may have the form of a cavity, through or not, for example a region in depression, in particular due to wear, for example opening into the interior of an enclosure of the industrial installation.

[0065] There figure 2 illustrates an example of a method according to the invention.

[0066] In one embodiment, particularly for the repair of an enclosure having a wall in contact with a fluid product, especially a molten or powdered product, in the area to be repaired, For example, for repairing a furnace vessel in an iron or steel smelting furnace, or a furnace for smelting a non-ferrous metal, in particular an aluminum smelting furnace, a magnesium smelting furnace, a copper smelting furnace, or for repairing a pouring channel, especially for such furnaces, or for repairing an incinerator vessel, the process includes a step 1) of emptying, at least partially, of said enclosure so as to expose said area to repair.

[0067] The fluid product can be in liquid form or in powder form, for example in the form of ashes.

[0068] The oil change can be carried out using any technique known to the person in the trade.

[0069] For example, it is possible to evacuate the fluid product, including the molten product or the ashes, through passages, for example drilled in the bottom wall of the enclosure or created by dismantling one or more electrodes or one or more burners.

[0070] Step 1) is optional for the repair of an enclosure where the part to be repaired is exposed, for example a part to be repaired which is not in contact with a fluid product, in particular with a molten product or with ashes, such as for the repair of a vault wall, or a turbine chamber wall, or a ceramic firing kiln.

[0071] At the stage2) Optionally, the area to be repaired is rinsed, that is, cleared of a large quantity of product residue with which it came into contact during the use of the industrial installation, using any conventional technique. Preferably, a suitable product is sprayed, at least on the area to be repaired, particularly to liquefy the product residue with which it came into contact during use, so that the removal of said residue is easier. For example, spraying sodium carbonate is well suited to liquefying a metallurgical slag residue.

[0072] At the stage3), optionally, the temperature in the area to be repaired can be reduced to a temperature above 250°C, preferably above 400°C, preferably above 500°C, preferably above 600°C, preferably above 700°C, preferably above 800°C, preferably above 900°C, and preferably below 1550°C, preferably below 1500°C, or even below 1450°C or 1400°C.

[0073] In one embodiment, the repair product used in step b) contains a hot binder, and in step 3), the temperature in the area to be repaired is reduced to a temperature at which the hot binder is not in a solid state. In particular, when the hot binder is a glass, the temperature is reduced to a temperature that remains above the glass transition temperature of said glass. Said glass is preferably chosen so that its glass transition temperature is between 600°C and 1350°C, preferably between 900°C and 1350°C, preferably between 1000°C and 1300°C, preferably between 1150°C and 1250°C.

[0074] In step 4), the repair product is installed following steps a) and b).

[0075] At the stage a) the area to be repaired is delimited using formwork 32, so as to constitute, with the industrial installation, in particular an industrial oven, a mold for the repair product.

[0076] Formwork 32 includes, or is made up of ( figure 3 ) of an internal formwork 32i, which delimits the mold inside the industrial installation. The internal formwork specifically follows the opening of the areas to be repaired 30 1 in the shape of a cavity.

[0077] When the area to be repaired penetrates a wall of the industrial installation, particularly the wall of an enclosure, for example, the wall of a tank containing molten product in operation, it opens through internal and external openings onto the internal and external faces of the wall, respectively. The formwork 32 then preferably includes an external formwork, not shown, which delimits the external opening of the area to be repaired. The internal and external formworks retain the repair material before it hardens, preferably by sintering, to prevent it from escaping through the internal and external openings, respectively.

[0078] According to the invention at least part of the inner formwork, preferably all of the inner formwork, is made of a CMC.

[0079] In one embodiment, at least part of the external formwork, or even all of the external formwork, is made of a CMC.

[0080] In one embodiment, the outer formwork is made of a CMC, preferably identical to that of the inner formwork.

[0081] The manufacture of a CMC can be carried out by any conventional method.

[0082] The person in the trade knows how to adjust the parameters of the process chosen for the manufacture of the CMC, and in particular determine the particle size of the raw materials, the water content during shaping, and the sintering temperature if the CMC is sintered.

[0083] The manufacturing of a CMC may include the following steps: i) disposition, on or in a textile, of a slip suitable for forming a ceramic matrix after consolidation; ii) before or after step i), shaping of the textile; iii) consolidation of the preform obtained after the preceding steps, preferably by drying and / or sintering, so as to form said matrix and obtain the CMC.

[0084] At step i), A textile is a collection of fibers, preferably assembled into yarns, with a yarn typically comprising several hundred to several thousand fibers. The fibers, preferably yarns, are preferably longer than 50 mm, or even longer than 100 mm. In one embodiment, the fibers, preferably yarns, are arranged to form at least one fabric.

[0085] Textiles can take the form of a felt of unordered yarns and / or fibers, a sheet, for example a sheet made up of yarns extending substantially parallel to each other (these yarns being called "unidirectional yarns"), a knit, a fabric (i.e. a woven textile) or a stack of one or more felts and / or sheets, and / or knits and / or fabrics.

[0086] The textile preferably takes the form of felt, fabric, a layer, or a stack of felt(s) and / or layers and / or fabric(s). The stacking of fabrics and / or layers can be arranged so that the threads of the different fabrics or layers all extend substantially in the same direction, or in 2, 3, 4, 5, or 6 different directions, depending in particular on the desired mechanical properties.

[0087] Preferably, at least some, preferably all, of the said ceramic fibers of the textile, possibly assembled in the form of single yarns and / or assembled, are: fibre comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of oxides, and / or fibre comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a material other than an oxide.

[0088] Preferably, said ceramic textile fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of oxides are: fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of oxides and exhibiting a chemical analysis such as SiO₂ + Al₂O₃ + ZrO₂ > 50%, preferably SiO₂ + Al₂O₃ + ZrO₂ > 60%, or even SiO₂ + Al₂O₃ + ZrO₂ > 70%, or even SiO₂ + Al₂O₃ + ZrO₂ > 80%, or even SiO₂ + Al₂O₃ + ZrO₂ > 90%, by mass percentage, and / or fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of oxides and exhibiting a chemical analysis such as SiO2 > 70%, preferably SiO2 > 80%, preferably SiO2 > 90%, or even SiO2 > 99%, by mass percentage, and / or fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of oxides and exhibiting a chemical analysis such as Al2O3 > 65%,Preferably Al₂O₃ > 70%, or even Al₂O₃ > 80%, or even Al₂O₃ > 90%, or even Al₂O₃ > 95%, as a percentage by mass.

[0089] Preferably, at least some, and preferably all, of the said ceramic fibers are: fibers composed of more than 95%, preferably more than 98%, preferably more than 99%, preferably substantially 100% by mass of alumina, and / or fibers composed of more than 95%, preferably more than 98%, preferably more than 99%, preferably substantially 100% by mass of silica, preferably composed of more than 95%, preferably more than 98%, of amorphous silica, and / or fibers composed of more than 95%, preferably more than 98%, preferably more than 99%, preferably substantially 100% by mass of mullite and corundum, and / or fibers composed of more than 95%, preferably more than 98%, preferably more than 99%, preferably substantially 100% by mass of glass, preferably washed, and / or a mixture of said fibers.

[0090] Preferably, said ceramic textile fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a material other than an oxide are: fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a carbide, preferably selected from silicon carbide, boron carbide and mixtures thereof, and / or fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a boride, preferably titanium boride, and / or fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99%, preferably more than 99.5% carbon by mass.

[0091] Preferably, said ceramic textile fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a material other than an oxide are: fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of silicon carbide, and / or fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of carbon.

[0092] In one embodiment, at least some, preferably all, of said ceramic fibers are fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of oxides.

[0093] In one embodiment, at least some, preferably all, of said ceramic fibers are fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a material other than an oxide.

[0094] In one embodiment, substantially all the fibers have the same composition.

[0095] The slip can be applied to or within the textile, for example, by impregnation. This layering can be achieved by pressing or vacuum application, preferably after impregnation.

[0096] The manufacture of slip is well known to those in the trade. Slip is classically a suspension, for example of an aqueous base or an organic solvent, containing ceramic particles and / or ceramic particle precursors, i.e. compounds which are transformed into ceramic particles during the manufacture of CMC, and in particular during hardening, in particular during sintering, and optionally dispersants, plasticizers, lubricants, and / or temporary binders.

[0097] The composition of the slip, the size distribution of the ceramic particles or ceramic precursors, and the mineral content of the slip are adapted to the type of fiber and the shaping technique. For example, the slip can be deposited on or within the textile, notably by direct lamination, infusion, injection, infiltration, or deposition, under atmospheric pressure, higher pressure, or vacuum, at ambient temperature or higher temperatures.

[0098] In step ii),The resulting textile, preferably impregnated with slip, is shaped. The desired shape is preferably the final shape of the CMC. In one embodiment, however, the shape can be modified after the matrix has hardened, for example by machining or deformation.

[0099] Preferably, to create the inner formwork, the textile is shaped so that the shape of the CMC is adapted so that, after installation of the formwork, the repair material only replaces material that has been extracted by wear, preferably replaces all the material that has been extracted by wear.

[0100] The shape can be created by making an impression with the textile (before or preferably after the introduction of the slip) on a reproduction of the part of the industrial installation to be repaired before wear. The mold is then a "negative" of the area to be repaired. For example, if the area to be repaired is a pouring channel, the CMC (Closed Molding Machine) can be made by depositing the textile, preferably in the form of a single fabric or a layering of several fabrics, onto a replica of the pouring channel, either before or after impregnation with the slip but before consolidation, so that the textile conforms to the surface of the pouring channel, at least in the area corresponding to the region to be repaired. The use of a CMC advantageously allows for the easy creation of complex shapes, even those that cannot be developed.The repair thus makes it possible to reconstruct with precision the initial profile of the surface of the industrial installation, in particular the internal surface of an enclosure, for example a tank, of the industrial installation.

[0101] CMC can be manufactured by layering pre-impregnated materials, each consisting of a fabric impregnated with a slip of ceramic particles. The pre-impregnated materials are flexible, allowing them to take the desired shape.

[0102] In step iii), Consolidation, preferably by sintering, is preferably carried out before installation of the formwork, which facilitates this installation.

[0103] In general, the characteristics of CMC result from its manufacturing process.

[0104] Preferably, the CMC should have one or more of the following optional features: The CMC is preferably sintered; the CMC preferably has an open porosity, measured by imbibition, according to the principle of Archimedes' buoyancy, greater than 10%, preferably greater than 15%, preferably greater than 20%, preferably greater than 25%, preferably greater than 30%, and preferably less than 50%, preferably less than 45%, preferably less than 40%; preferably, the CMC comprises more than 20%, preferably more than 25%, preferably more than 30%, preferably more than 40%, preferably more than 50%, preferably more than 60% and / or less than 80%, preferably less than 70% by volume of fibers; at least part, preferably all of the ceramic fibers of the CMC, are fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of oxides;at least part, preferably all of the ceramic fibers of the CMC, are fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a material other than an oxide; the matrix of the CMC is composed of more than 90%, preferably more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of oxides, and / or carbides and / or nitrides and / or sialons, in particular of the type described above; CMC has an apparent density greater than 1.0 g / cm³, preferably greater than 1.20 g / cm³, preferably greater than 1.40 g / cm³ and / or less than 2.50 g / cm³, preferably less than 2.00 g / cm³, preferably less than 1.90 g / cm³.

[0105] In a first embodiment, the CMC consists of oxides for more than 90% of its mass, preferably for more than 95% of its mass, preferably for more than 98% of its mass, preferably for more than 99% of its mass, preferably for more than 99.5% of its mass.

[0106] In said first embodiment, the CMC has one or more of the following optional and preferred features: CMC comprises fibers, said fibers being composed of oxides for more than 90%, preferably for more than 95%, preferably for more than 97%, preferably for more than 98%, preferably for more than 99%, preferably for more than 99.5% by mass; at least some, preferably all, of said ceramic fibers are: fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of oxides and having a chemical analysis such as SiO₂ + Al₂O₃ + ZrO₂ > 50%, preferably SiO₂ + Al₂O₃ + ZrO₂ > 60%, or even SiO₂ + Al₂O₃ + ZrO₂ > 70%, or even SiO₂ + Al₂O₃ + ZrO₂ > 80%, or even SiO₂ + Al₂O₃ + ZrO₂ > 90%, by mass percentage, and / or fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of oxides and exhibiting a chemical analysis such as SiO2 > 70%,preferably SiO2 > 80%, preferably SiO2 > 90%, or even SiO2 > 99%, by mass percentage, and / or fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of oxides and exhibiting a chemical analysis such as Al2O3 > 65%, preferably Al2O3 > 70%, or even Al2O3 > 80%, or even Al2O3 > 90%, or even Al2O3 > 95%, or even Al2O3 > 97%, or even Al2O3 > 98%, by mass percentage; the matrix of said CMC is composed of oxides for more than 90%, preferably more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass; preferably, the matrix of the CMC is substantially composed of oxides; the matrix of the CMC comprises Al₂O₃ and / or SiO₂ and / or ZrO₂ and / or Cr₂O₃; preferably, the matrix of the CMC comprises Al₂O₃ and SiO₂; in one embodiment, the Al₂O₃ content in the matrix of the CMC,in mass percentage based on the mass of the matrix, is greater than 65%, preferably greater than 70%; in one embodiment, the SiO2 content in the CMC matrix, in mass percentage based on the mass of the matrix, is greater than 15%, preferably greater than 20% and / or less than 35%, preferably less than 30%; in one embodiment, the SiO2 content in the CMC matrix, in mass percentage based on the mass of the matrix, is greater than 60%, preferably greater than 70%, preferably greater than 80%; in one embodiment, the content of oxides other than Al2O3 and SiO2 in the CMC matrix, in mass percentage based on the mass of the matrix, is less than 3%, preferably less than 2%, preferably less than 1%; In one embodiment, the total content of Al2O3 and SiO2 in the CMC matrix is ​​greater than 80%, preferably greater than 85%.preferably greater than 90%, preferably greater than 95%, as a mass percentage based on the mass of the matrix; in one embodiment, the silica of the CMC matrix is ​​amorphous; preferably, the CMC has a total mass content of SiO₂ + Al₂O₃ + ZrO₂ + Cr₂O₃ greater than 80%, preferably greater than 85%, preferably greater than 90%, preferably greater than 95%, preferably greater than 97%, preferably greater than 97%. Preferably, the CMC has a total mass content of SiO₂ + Al₂O₃ greater than 80%, preferably greater than 85%, preferably greater than 90%, preferably greater than 95%, preferably greater than 97%, preferably greater than 97%. In a preferred embodiment, the CMC presents the following chemical analysis, in mass percentages and for a total of 100%: SiO2: 47% - 67%, Al2O3: 32% - 52%, species other than Al2O3 and SiO2: < 5%, preferably < 4%, preferably < 3%,preferably < 2%; in one embodiment, the CMC is preferably amorphous, and has the following chemical analysis, as a percentage by mass and for a total of 100%: SiO2: > 95%, preferably > 96%, preferably > 97%, preferably > 98%, preferably > 99%.

[0107] In a second embodiment, the CMC is made up of a material other than an oxide, for more than 90% of its mass, preferably for more than 95% of its mass, preferably for more than 98% of its mass, preferably for more than 99% of its mass, preferably for more than 99.5% of its mass.

[0108] In said second embodiment, the CMC has one or more of the following optional and preferred features: CMC comprises fibers, said fibers being composed of a non-oxide material for more than 90%, preferably for more than 95%, preferably for more than 97%, preferably for more than 98%, preferably for more than 99%, preferably for more than 99.5% by mass; at least a part, preferably all of said ceramic fibers, are: fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of carbon, and / or fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a carbide, preferably selected from silicon carbide, boron carbide and mixtures thereof, and / or fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a boride, preferably titanium boride,and / or fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a nitride, preferably silicon nitride, and / or fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of carbon.

[0109] In said second embodiment, the CMC has one or more of the following optional and preferred features: preferably, said ceramic textile fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a material other than an oxide are fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of silicon carbide, and / or fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of carbon; the matrix of said CMC is composed of more than 90%, preferably more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of a material other than an oxide, preferably selected from carbides, borides, nitrides, SiAlON and mixtures thereof; preferably, the matrix of the CMC comprises,or even consists of silicon carbide, silicon nitride, metallic silicon, or a mixture of the latter; in a particular embodiment of the second embodiment, the CMC comprises fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of silicon carbide, and / or fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of carbon, and a matrix composed of more than 90%, preferably more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of silicon carbide, silicon nitride, metallic silicon, and mixtures thereof. In said embodiment, the matrix is ​​preferably composed of, for more than 90%, preferably for more than 95%, preferably more than 97%,preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass, of silicon carbide or a mixture of silicon carbide and metallic silicon or a mixture of silicon carbide and silicon nitride; in one embodiment, the silicon carbide of the matrix is ​​recrystallized silicon carbide.

[0110] In a third embodiment, the CMC includes fibre composed of a non-oxide material for more than 90%, preferably for more than 95%, preferably for more than 97%, preferably for more than 98%, preferably for more than 99%, preferably for more than 99.5% by mass and a matrix composed of oxides for more than 90%, preferably for more than 95%, preferably for more than 97%, preferably for more than 98%, preferably for more than 99%, preferably for more than 99.5% by mass.

[0111] In said third embodiment, the CMC has one or more of the following optional and preferred features: at least part, preferably all of the fibers composed of a non-oxide material for more than 90%, preferably more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass, are fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of carbon and / or fibers comprising more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass of carbide, preferably silicon carbide, and / or the CMC matrix comprises, or is even made up of, Al 2 O 3 and / or SiO 2 and / or ZrO 2 and / or Cr 2 O 3; preferably, the CMC matrix includes, or is made up of, Al 2 O 3 and SiO 2;In one embodiment, the Al2O3 content in the CMC matrix, as a percentage by mass on the basis of the matrix, is greater than 65%, preferably greater than 70%; in one embodiment, the SiO2 content in the CMC matrix, as a percentage by mass on the basis of the matrix, is greater than 15%, preferably greater than 20% and / or less than 35%, preferably less than 30%; in one embodiment, the SiO2 content in the CMC matrix, as a percentage by mass on the basis of the matrix, is greater than 60%, preferably greater than 70%, preferably greater than 80%; in one embodiment, the content of species other than Al2O3 and SiO2 in the CMC matrix, as a percentage by mass on the basis of the matrix, is less than 3%, preferably less than 2%, preferably less than 1%;In one embodiment, the total content of Al2O3 and SiO2 in the CMC matrix is ​​greater than 80%, preferably greater than 85%, preferably greater than 90%, preferably greater than 95%, as a percentage by mass on the basis of the matrix; in one embodiment, the silica in the CMC matrix is ​​amorphous.

[0112] In a fourth embodiment, the CMC includes fibre composed of oxides for more than 90%, preferably for more than 95%, preferably for more than 97%, preferably for more than 98%, preferably for more than 99%, preferably for more than 99.5% by mass, and a matrix composed for more than 90%, preferably for more than 95%, preferably for more than 97%, preferably for more than 98%, preferably for more than 99%, preferably for more than 99.5% by mass of a material other than an oxide, preferably selected from carbon, carbides, borides, nitrides, and SiAlON.

[0113] In said fourth embodiment, the CMC preferably has one or more of the following optional characteristics: CMC comprises fibers with a chemical analysis such as SiO2 + Al2O3 + ZrO2 > 50%, preferably SiO2 + Al2O3 + ZrO2 > 60%, or even SiO2 + Al2O3 + ZrO2 > 70%, or even SiO2 + Al2O3 + ZrO2 > 80%, or even SiO2 + Al2O3 + ZrO2 > 90%, as a percentage by mass; CMC comprises fibers with a chemical analysis such as SiO2 > 70%, preferably SiO2 > 80%, preferably SiO2 > 90%, or even SiO2 > 99%, as a percentage by mass; CMC comprises fibers exhibiting a chemical analysis such as Al 2 O 3 > 65%, preferably Al 2 O 3 > 70%, or even Al 2 O 3 > 80%, or even Al 2 O 3 > 90%, or even Al 2 O 3 > 95%, or even Al 2 O 3 > 97%, or even Al 2 O 3 > 98%, as a percentage by mass;the CMC matrix is ​​preferably composed, for more than 90%, preferably for more than 95%, preferably more than 97%, preferably more than 98%, preferably more than 99%, preferably more than 99.5% by mass, of silicon carbide or a mixture of silicon carbide and metallic silicon or a mixture of silicon carbide and silicon nitride;

[0114] In one embodiment, the CMC is chosen so as to have a chemical analysis close to that of the material of the industrial installation which delimits the area to be repaired, preferably so that the content of any constituent of the sintered repair product present in a mass content greater than 5% differs by less than 20%, preferably by less than 10%, from the content of said constituent in said material.

[0115] The formwork is then installed by assembling its elements.

[0116] Installing the internal formwork within an enclosure can be tricky due to access difficulties.

[0117] The internal formwork elements can be introduced through a passage that opens inside the enclosure, in the area to be repaired or not.

[0118] During their installation, internal formwork elements which have two large opposite faces can be held by the large face which, in the service position, is exposed inside the industrial installation, or by the opposite large face.

[0119] In one embodiment, as illustrated in the figure 4At least one element of the formwork, particularly the inner formwork, in a CMC (Construction Material Construction) system has through holes and / or recesses. Filling these holes and recesses with the repair product in step b) advantageously improves the immobilization of the inner formwork and reduces the thermal gradient in the repair product in step 5). Preferably, the average equivalent diameter of the holes is greater than 8 mm and preferably less than 20 mm, preferably less than 15 mm.

[0120] In one embodiment, said formwork element in a CMC is in the form of a grid, the holes being preferably distributed homogeneously, the total surface of the holes representing more than 10%, preferably more than 15% and preferably less than 50%, preferably less than 40% of the internal surface of said formwork element, i.e. the surface participating in the definition of the mold around the region to be repaired (surface of the holes and of the material of the grid).

[0121] In one embodiment, said holes are located on the lower two-thirds of said formwork element, and preferably distributed homogeneously. Preferably, in said embodiment, the total surface area of ​​the holes represents more than 1% and less than 5% of the internal surface area of ​​said formwork element (surface area of ​​the holes and of the material of said formwork element).

[0122] The creation of through holes and / or indentations can be achieved using any technique known to a person skilled in the art. In particular, through holes can be made by drilling or cutting the CMC obtained after sintering using a water jet. Through holes and / or indentations can also be made in the textile, preferably a woven fabric, before coating with slip.

[0123] Accessories are then typically used to hold the formwork elements in the service position.

[0124] In one embodiment, the sealing between the formwork, in particular the inner formwork, and the surface of the industrial installation defining the area to be repaired is increased by placing a layer of ceramic fibers between said formwork and said surface.

[0125] There figure 3illustrates an example of an internal formwork according to the invention. In particular, the internal formwork 32i is distinguished, and in particular three adjacent panels 351, 352 and 353 held in position by means of metal clamps 39, shoring bricks 43 and cooled tubes 45. Repair product 47 fills the area to be repaired 301 delimited by the surface of the worn area and the internal formwork.

[0126] After the formwork has been installed, the repair product can be introduced into the area to be repaired, for example via a water-cooled nozzle.

[0127] In step b), The mold that delimits the area to be repaired is filled with a repair product, preferably by pouring. Repair product

[0128] The repair product can be a conventional repair product and can be prepared by any known technique.

[0129] Preferably, the repair product is the result of moistening an unformed product. This moistening can be carried out using any known technique, for example, in a mixer. A person skilled in the art knows how to determine the quantity of solvent, preferably water, to use to moisten the unformed product and obtain the repair product.

[0130] The unfinished product may include, in particular: Pural T concrete and / or Pural M concrete, in particular where the industrial installation is an iron or steel smelting furnace, and part of such a furnace, a non-ferrous metal smelting furnace, or an element configured to transfer molten metal, in particular from a smelting furnace of said metal, said element being able to be physically separated from said furnace, Sialfrax 18 Cast, Sialfrax 30 Shot, Alfrax 60 Shot or Castfrax 902, in particular where the industrial installation is a casting channel.

[0131] These unshaped products are marketed by the company Saint-Gobain Performance Ceramics & Refractories.

[0132] Preferably, the maximum particle size of the repair product or, equivalently, of the unshaped product, is less than 10 mm, preferably less than 8 mm, preferably less than 6 mm.

[0133] The particle size distribution of the repair product or, equivalently, of the unshaped product is preferably determined so that the repair product is self-casting when hot.

[0134] Preferably, the repair product is chosen so as to have, after sintering, a chemical analysis close to that of the material of the industrial installation which delimits the area to be repaired, preferably so that the mass content of any constituent of the sintered repair product present in a mass content greater than 5%, differs by less than 20%, preferably by less than 10% of the content of said constituent in said material.

[0135] In one embodiment, the repair product is chosen so as to exhibit, after sintering, a chemical analysis close to that of the CMC of the formwork elements, preferably so that the mass content of any constituent of the sintered repair product present in a mass content greater than 5% differs by less than 20%, preferably by less than 10%, from the content of said constituent in said CMC.

[0136] For example, if the area to be repaired is delimited by one or more refractory blocks in a product with a high alumina content, the unshaped product used to manufacture the repair product is preferably Pural T concrete.

[0137] The repair product can be brought to the area to be repaired using any technique known to the person in the trade.

[0138] If access to the area to be repaired is difficult, one or more openings, for example by drilling, can be created to facilitate access. These openings advantageously allow the introduction of a conveying device for the repair product, for example a cooled rod, to the area to be repaired.

[0139] In one embodiment, the repair product is pumped by means of a pump producing a suction pressure preferably less than or equal to 180 bar and preferably conveyed to the area to be repaired by means of a water-cooled lance or nozzle.

[0140] Throughout step b), the area to be repaired is preferably maintained at a temperature above 300°C, preferably above 400°C, preferably above 500°C, preferably above 600°C, preferably above 700°C, preferably above 800°C, preferably above 900°C, and / or preferably below 1550°C, preferably below 1500°C.

[0141] At step 5), optional, and in particular if the process includes a step 3), the industrial installation is maintained at a temperature between 400°C and 1400°C, preferably between 600°C and 1400°C, preferably between 1000°C and 1400°C, in order to allow the sintering of the repair product, preferably for a period of more than 8 hours, preferably more than 10 hours and preferably less than 15 hours.

[0142] In step 6),normal operation of the installation is resumed, and if the process includes a step 3), the temperature of the industrial installation is increased for a restart. Examples

[0143] The following non-limiting examples are given to illustrate the invention.

[0144] In a particular embodiment, especially when the area to be repaired is part of a wall separating an "interior" and an "exterior" space, the interior formwork is made of a CMC (cement-resistant composite material), preferably one or more CMC panels, preferably held against the sound part of the wall by means of one or more metal rods, preferably cooled by circulating water. If the area to be repaired opens onto the exterior side of the wall, an exterior formwork, preferably made of ceramic, preferably in the form of a CMC, is fixed so as to externally seal the area to be repaired.

[0145] The area to be repaired is then filled with the repair product. The repair product is preferably brought in from the outside through a pipe passing through one or more openings made in the wall, and then poured into the area to be repaired using a pipe cooled by a water circulation.

[0146] Preferably, at least the inner formwork, preferably the formwork, is not removed after the repair product has been put in place.

[0147] In a second specific embodiment, particularly when the area to be repaired results from wear on a tank in the industrial installation, at least a partial draining of said tank is carried out. The internal casing is made of a CMC material, preferably one or more CMC plates, preferably held against the tank by means of one or more ceramic tubes, preferably in the form of a CMC material, and / or one or more metal rods, preferably cooled by circulating water. If the area to be repaired opens to the outside of the tank, a facing, constituting the external casing, preferably made of a ceramic material, preferably in the form of a CMC material, is fixed so as to externally seal the area to be repaired.

[0148] The area to be repaired is then filled with the repair product. The repair product is preferably conveyed from outside the tank through a pipe passing through one or more openings made in the tank wall, and then poured into the area to be repaired using a nozzle cooled by a water circulation.

[0149] Preferably, the CMC formwork is not removed after the repair product has been installed.

[0150] THE figure 5 This illustrates the repair of a casting channel initially composed, from the outside in, of a metal casing 50, a thermal insulation layer 52, an outer coating 54, and an inner coating 56 (left diagram). The central diagram illustrates the casting channel after wear of the inner coating 56, and the figure on the right illustrates the casting channel after repair.

[0151] The following example was created.

[0152] To manufacture the repair product, the unshaped Castfrax 902 SRAW product, marketed by Saint-Gobain Performance Ceramics & Refractories, was mixed for 1 minute in a rotary paddle mixer with a fixed bowl, with 0.15% of a modified polycarboxylate ether, by mass percentage based on the unshaped product. Then, 8% water, by mass percentage based on the unshaped product, was added, and mixing continued until a homogeneous repair product was obtained.

[0153] 160 kg of repair product were prepared. This repair product was hot-pourable.

[0154] A one-piece mold in a CMC was created.

[0155] This mold had a general rectangular parallelepiped shape, with a length of 600 mm, a width of 150 mm, and a height of 450 mm, the thickness of the walls of said mold being substantially constant and equal to 10 mm.

[0156] The CMC constituting the mold exhibited a thermal conductivity between 20°C and 500°C of less than 0.6 Wm-1.K-1.

[0157] The CMC was composed of: of a layering of fabrics (or "woven fabrics" in English) made of washed glass fibers (or "leached glass" in English) with a silica content greater than 90% by mass, representing 44% of the mass of the CMC, and of an alumina and silica matrix, representing 56% of the mass of the CMC.

[0158] The said CMC had an open porosity of 38%, an apparent density of 1.65 g / cm³, an Al₂O₃ content of 42%, a SiO₂ content of 57% and a content of other constituents, for example oxides, of 1%, the contents of Al₂O₃, SiO₂ and other constituents being expressed as mass percentages on the basis of the said CMC.

[0159] The mold was placed in an oven equipped with a gas burner.

[0160] The furnace was then started up to reach a temperature of 1200°C in 2 hours and 40 minutes, simulating a hot introduction of the CMC mold into an industrial installation, in particular a cast iron pouring channel of a blast furnace.

[0161] The pouring of the repair product into the mold, maintained at 1200°C, was carried out using a metal chute positioned above an opening made in the vault of the oven.

[0162] The repair product was poured continuously, with a flow rate approximately equal to 100 kg / min.

[0163] During filling, it was observed that the CMC mold resisted the pressure of the repair product, without breaking or opening.

[0164] After filling the mold, the temperature was maintained at 1200°C for 4 hours. The temperature was then gradually reduced to 800°C at a rate of approximately 25°C / h. The burner was then switched off, and the temperature decreased naturally without opening the oven.

[0165] The sintered repair product found in the mold was then recovered.

[0166] After sawing, it had a homogeneous texture, without cracks or internal cavities that could correspond to a break in the power supply.

[0167] As is now clear, the invention thus provides a hot repair method that uses CMC elements, particularly for creating the internal formwork, which: allows for rapid manufacturing and is perfectly adapted to the area to be repaired, in particular because a CMC can be formed into complex shapes, and especially to fit the profile of the area to be repaired; facilitates the introduction of these elements to the area to be repaired; facilitates their arrangement, these elements being lightweight; allows for a sacrifice of the formwork element, i.e. its retention in position after the repair, in particular because the composition of a CMC can be chosen to be similar to that of the repair product.

[0168] Of course, the present invention is not limited to the embodiments described or represented, provided by way of illustrative and non-limiting examples.

[0169] In particular, the CMC compositions of the different parts of the formwork and / or accessories may be identical or different.

Claims

1. Process for the hot repair a region of an industrial facility different from a glassmaking furnace, said region being at a temperature above 250°C, referred to as the "region to be repaired"(301, 302, 303), said process comprising the following steps: a) installation of formwork (32) in a working position, so as to make a mould around the region to be repaired; b) filling, preferably by casting, the mould with a repair product (47), the process being characterized in that at least a portion of the formwork is made of a Ceramic Matrix Composite.

2. Process according to the preceding claim, in which the industrial facility is chosen from: - an iron or steel smelting furnace, and a part of such a furnace; - a furnace for melting a non-ferrous metal; - an element configured to transfer molten metal; - a cement plant furnace; - an ore reduction furnace; - an incinerator; - a hazardous waste treatment furnace; - a gasifier; - a reformer; - a ceramic firing furnace; - a carbon black reactor; - a holding tank intended to contain a molten product at a temperature in excess of 250°C; - an aluminium electrolysis cell; - an impeller combustion chamber; - a boiler.

3. Process according to either one of the preceding claims, including, after step b), a step 5) of sintering the repair product introduced into the mould in step b), the sintered repair product obtained consisting of a plurality of constituents, the mass content of any constituent of the sintered repair product present in a mass content greater than 5%, - differing by less than 20% from the mass content of said constituent in said ceramic matrix composite, and / or - differing by less than 20% from the mass content of said constituent in a region of the industrial facility delimiting the region to be repaired.

4. Process according to any one of the preceding claims, in which at least one element of said formwork has the shape of a part of the industrial facility which was protruding before said part disappeared as a result of wear.

5. Process according to any one of the immediately preceding claims, in which manufacture of the formwork includes taking an impression on an at least partial replica of said industrial facility as it was before the wear which led to the generation of the region to be repaired.

6. Process according to one of the preceding claims, in which the formwork is abandoned in the region to be repaired after said repair.

7. Process according to any one of the preceding claims, in which the inner formwork is made entirely of a ceramic matrix composite.

8. Process according to any one of the preceding claims, in which at least one element of the formwork made of a ceramic matrix composite includes through holes and / or recesses arranged so as to be filled with the repair product during step b).

9. Process according to any one of the preceding claims, in which the formwork includes - formwork elements partially delimiting the region to be repaired, and - optionally, accessories for holding said formwork elements in a working position, said accessories being made of a ceramic matrix composite, identical to or different from the ceramic matrix composite of the formwork elements.

10. Process according to the immediately preceding claim, in which at least one formwork element has the shape of a flat or non-planar plate, the thickness of the plate being greater than 3 mm and less than 50 mm.

11. Process according to one of the preceding claims, in which: - the ceramic matrix composite of at least a part of the formwork and / or, - when the formwork includes accessories for holding said formwork elements in a working position of a ceramic matrix composite, the ceramic matrix composite of at least one accessory - is (are) sintered, and - has (have) an open porosity greater than 15% and less than 50%, and - include(s) more than 20% and less than 80% by volume of fibres, and and - include(s) a matrix made up of more than 90% oxides and / or carbides and / or nitrides and / or oxynitride compound(s) of at least the elements Si, Al and N, in percentage by mass, and - has (have) a bulk density greater than 1.0 g / cm3 and less than 2 g / cm3.

12. Process according to any one of the preceding claims, said process including the following steps: 3) reducing the temperature in said industrial facility to a temperature above 250°C; 4) performing steps a) and b); 5) increasing and maintaining the temperature of the industrial facility between 400°C and 1400°C so as to sinter the repair product; 6) raising the temperature of said industrial facility to its operating temperature.

13. Process according to any one of Claims 1 to 11, the industrial facility including a chamber containing a fluid product, said process including, prior to step a), the following step: - if the region to be repaired is, at least partially, delimited by a surface of the industrial facility in contact with said fluid product, at least partial emptying of said chamber so as to expose said region to be repaired; and, after step b), the following step: - resumption of normal operation, the temperature of the industrial facility being maintained in said region to be repaired throughout all the steps of the process, or including, prior to step a), the following steps: 1) if the region to be repaired is, at least partially, delimited by a surface of the industrial facility in contact with said fluid product, at least partial emptying of said chamber, so as to expose said region to be repaired; 3) reducing the temperature in the region to be repaired to a temperature above 250°C; and, after step b), the following steps: 5) increasing and maintaining the temperature of the region to be repaired between 1000°C and 1400°C so as to sinter the repair product; 6) resumption of normal operation of the industrial facility.

14. Process according to any one of the preceding claims, in which the region to be repaired is at least partly delimited - by a runner or - by a side wall (22) or a bottom wall (24) of a tank (31) intended to contain a molten product, said formwork (32) including or consisting of an inner formwork (32i) installed inside said tank in step a).

15. Process according to the immediately preceding claim, in which the region to be repaired is at least partly delimited by a said side wall (22).