Paper-containing structure, and method for producing paper-containing structure

HK40137391APending Publication Date: 2026-09-11SHIBAURA INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
HK62026124975
Authority / Receiving Office
HK · HK
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-10-17
Filing Date
2026-06-17
Publication Date
2026-09-11

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

In this paper-containing structure, a paper-containing sheet (2) has a first surface (1a) and a second surface (1b), a first hydroxyl group high-concentration region (11) is formed on the first surface (1a), and a second hydroxyl group high-concentration region (14) is formed on the second surface (1b). A tensile stress is generated in each of the hydroxyl group high-concentration regions (11, 14), and the tensile stress is balanced with the deformation resistance of the paper-containing sheet (2) to form a first stable state and maintain the first shape. When the paper-containing structure (1) is in the second shape, the force is balanced to form a second stable state, and the second shape is maintained. The paper-containing structure (1) switches the first shape and the second shape in at least one direction by applying a trigger force.
Need to check novelty before this filing date? Find Prior Art

Description

(19) State Intellectual Property Office (12) Invention Patent Application (10) Application Publication Number (43) Application Publication Date (21) Application Number 202380073120.1 (22) Application Date 2023.09.20 (30) Priority Data 2022-166403 2022.10.17 JP (85) PCT International Application Entering National Phase Date 2025.04.15 (86) PCT International Application Application Data PCT / JP2023 / 034082 2023.09.20 (87) PCT International Application Publication Data WO2024 / 084882 JA 2024.04.25 (71) Applicant's School / Legal Entity: Shibaura Institute of Technology Address: Japan (72) Inventors: Hiroki Shigemune, Daiki Kawagishi, Shuta Okamoto (74) Patent Agency: Beijing Luhao Intellectual Property Agency Co., Ltd. 11002 Patent Attorney Liu Yan Zhang Jing (51) Int.Cl. B65D 75 / 00 (2006.01) B65D 81 / 02 (2006.01) (54) Invention Title Paper-containing Structure and Method for Manufacturing Paper-containing Structure (57) Abstract In this paper-containing structure, the paper-containing sheet (2) has a first surface (1a) and a second surface (1b). A first high-hydroxyl concentration region (11) is formed on the first surface (1a), and a second high-hydroxyl concentration region (14) is formed on the second surface (1b). Tensile stress is generated in each high-hydroxyl concentration region (11, 14), which balances with the deformation resistance of the paper-containing sheet (2) to form a first stable state and maintain a first shape. When the paper-containing structure (1) is in a second shape, the forces are also balanced to form a second stable state and maintain a second shape. The paper-containing structure (1) switches the first shape and the second shape in at least one direction by applying a triggering force. Claims 2 pages, Description 23 pages, Drawings 42 pages, CN 121646554 A 2026.03.10 CN 1 21 64 65 54 A 1. A paper-containing structure, characterized in that it is formed from a paper-containing sheet in a dry state containing paper, the paper-containing sheet having a first surface and a second surface forming opposite sides to each other, a first high-hydroxyl concentration region being formed on the first surface with a higher hydroxyl density than other parts of the first surface, a second high-hydroxyl concentration region being formed on the second surface with a higher hydroxyl density than other parts of the second surface, tensile stress being generated in the first high-hydroxyl concentration region and the second high-hydroxyl concentration region respectively, the tensile stress in the first high-hydroxyl concentration region of the first surface and the tensile stress in the second high-hydroxyl concentration region of the second surface being balanced with the deformation resistance of the paper-containing sheet when the paper-containing structure is in a first shape to form a first stable state, capable of maintaining the first shape, and also when the paper-containing structure is in a second shape.A second stable state is formed by balancing the deformation resistance of the paper-containing sheet, which can maintain the second shape. The paper-containing structure can switch the first shape and the second shape in at least one direction by applying a triggering force to a portion thereof. 2. The paper-containing structure according to claim 1, characterized in that, in the first high hydroxyl concentration region and the second high hydroxyl concentration region, when the infrared absorption spectrum of the surface portion is measured by reflecting infrared light using a total internal reflection method with a wavenumber of 3331 cm⁻¹, the infrared transmittance is lower than that of the other portions. 3. The paper-containing structure according to claim 1 or 2, characterized in that one or more notches are formed on the paper-containing sheet, through which the first stable state and the second stable state can be formed. 4. The paper-containing structure as claimed in claim 1 or 2, characterized in that the triggering force is generated by water penetration into the paper-containing structure, humidity change of the environment in which the paper-containing structure is placed, local compression of the paper-containing structure, heating of the paper-containing structure, cooling of the paper-containing structure, cutting of a portion of the paper-containing structure, or applying an external force to the paper-containing structure. 5. The paper-containing structure as claimed in claim 1 or 2, characterized in that the paper-containing structure switches between the first shape and the second shape bidirectionally by applying the triggering force to a portion thereof. 6. A gripping member, characterized in that it comprises the paper-containing structure as claimed in claim 1 or 2, for gripping an article, wherein the first shape is an article-releasing shape with an open end, the second shape is an article-holding shape with the narrowed end, and the triggering force is generated by the gripping member colliding with the article or by the gripping member contacting a support surface supporting the article, thereby causing the paper-containing structure to change from the article-releasing shape to the article-holding shape to grip the article. 7. A gripper for a drone, characterized in that it comprises the gripper of claim 6, wherein the gripper has a fixing portion fixed to a support portion of the drone at its central portion. 8. A cushioning material, characterized in that it comprises a paper-containing structure of claim 1 or 2 for arranging one or more items therein, the paper-containing structure having an origami structure, the first shape being a reduced shape of the paper-containing structure folded without a bag or a flat shape of the paper-containing structure unfolded, the second shape being an unfolded shape of the paper-containing structure unfolded to form one or more bags, and changing from the reduced shape or flat shape to the unfolded shape by applying a triggering force to a portion of the paper-containing structure. Claims 1 / 2 page 2 CN 121646554 A 9. An origami device, characterized in that it comprises: a paper-containing structure of claim 1 or 2; and a fixing portion disposed in the...At least one of the first and second surfaces of the paper-containing structure, at least one of electronic components and wiring. 10. A cushioning material, characterized in that it comprises the paper-containing structure of claim 1 or 2, for arranging one or more articles therein, the paper-containing structure having a folding structure, the first shape being a reduced shape of the paper-containing structure folded without having a bag or a flat shape of the paper-containing structure unfolded, the second shape being an unfolded shape of the paper-containing structure unfolded to form one or more bags, changing from the reduced shape or flat shape to the unfolded shape by applying a triggering force to a portion of the paper-containing structure. 11. A cushioning material, characterized in that it comprises a paper-containing structure as described in claim 1 or 2, the paper-containing structure having one or more openings and a first high-hydroxyl concentration region and a second high-hydroxyl concentration region disposed around the openings, the first shape being a flat plate shape unfolded from the paper-containing structure, the second shape being a three-dimensional shape of the paper-containing structure having a cylindrical wall portion and a support portion, wherein the cylindrical wall portion stands upright at the periphery of the openings, the support portion extends from the cylindrical wall portion, and changes from the flat plate shape to the three-dimensional shape by applying a triggering force to a portion of the paper-containing structure. 12. A method of manufacturing a paper-containing structure, comprising the steps of: applying a liquid containing water to portions of the first and second surfaces of the paper-containing sheet where the first and second high-hydroxyl concentration regions are to be formed; and drying the liquid. 13. The paper-containing structure as described in claim 1 or 2, characterized in that at least a portion of at least one of the first and second surfaces of the paper-containing sheet is adhered with a flexible protective film. 14. The paper-containing structure as claimed in claim 1 or 2, characterized in that a flexible protective film is respectively pasted on the first and second surfaces of the paper-containing sheet. Claims 2 / 2 Page 3 CN 121646554 A Paper-containing structure and method for manufacturing paper-containing structure Technical Field

[0001] The present invention relates to a paper-containing structure whose three-dimensional shape changes when a triggering force is applied and a method for manufacturing paper-containing structures.

[0002] This application claims priority based on Japanese Patent Application No. 2022-166403 filed on October 17, 2022, the contents of which are incorporated herein by reference. Background Art

[0003] Origami technology has the advantage of being able to form a variety of three-dimensional structures by folding a sheet of paper. By studying the folding pattern, the unfolding and folding functions can be repeatedly utilized, or structures with high mechanical strength can be formed. Therefore, applications in various fields are expected. For example, in the manufacture of three-dimensional electronic devices, the manufacture of lightweight and inexpensive impact cushioning materials,In the area of ​​space saving resulting from the folding of sheet materials, origami techniques are envisioned for application.

[0004] In such a process, autonomous paper bending techniques, in which paper is bent by itself through some external action, have attracted much attention. Such techniques are sometimes described using the term "self-folding." With the development of such autonomous paper bending techniques, it is expected that the utilization of the characteristics of such origami will make great progress.

[0005] As such bending techniques, techniques have been reported to date in which a material that responds to external stimuli is pre-positioned on the paper, and the paper is bent autonomously by utilizing the response of the material when the stimulus is applied. Here, electric current, heat, etc., can be listed as stimuli.

[0006] However, in such bending techniques, since the supply of certain energy such as electric current or heat is required, there is a problem that the utilization environment may be limited, and since the paper also needs to be modified with special materials, there is a problem of high cost.

[0007] As a method to solve such problems, a method is disclosed that uses an inkjet printer to spray an aqueous solution containing 2-propanol onto paper and then dries it (see Non-Patent Document 1). In this method, it is not necessary to supply the paper with energy such as current or heat, and it has the advantage that the paper does not need to be modified with special materials.

[0008] Prior Art Documents

[0009] Non-Patent Documents

[0010] Non-Patent Document 1: Hiroki Shigemune, Shingo Maeda, Yusuke Hara, and Shuji Hashimoto. "Design of paper mechatronics: Towards a fully printed robot" Proceedings of 2014 IEEE / RSJ International Conference on Intelligent Robots and Systems (IROS 2014) Summary of the Invention

[0011] (a) Technical Problem to be Solved

[0012] The method disclosed in Non-Patent Document 1 is useful in terms of being able to solve the problems of other methods to date, but further improvements are desired for application in the manufacturing method of practical three-dimensional structures.

[0013] The objective of this invention is to provide a novel paper-containing structure with high practicality utilizing origami technology, and a method thereof. (Page 1 / 23, CN 121646554 A)

[0014] (II) Technical Solution

[0015] This invention provides the following method.

[0016] [1]A paper-containing structure is formed from a paper-containing sheet in a dry state, the paper-containing sheet having a first side and a second side forming opposite sides. A first high-hydroxyl concentration region is formed on the first side, where the density of hydroxyl groups is higher than in other parts of the first side. A second high-hydroxyl concentration region is formed on the second side, where the density of hydroxyl groups is higher than in other parts of the second side. Tensile stress is generated in both the first and second high-hydroxyl concentration regions. The tensile stress in the first and second high-hydroxyl concentration regions of the first and second sides balances with the deformation resistance of the paper-containing sheet when the paper-containing structure is in a first shape, forming a first stable state that maintains the first shape. Furthermore, when the paper-containing structure is in a second shape, it also balances with the deformation resistance of the paper-containing sheet, forming a second stable state that maintains the second shape. The paper-containing structure can switch between the first and second shapes in at least one direction by applying a triggering force to a portion of it.

[0017] According to method [1], by applying a triggering force to a portion of a paper-containing structure having a first high-hydroxyl concentration region and a second high-hydroxyl concentration region, the antagonistic balance between tensile stress and deformation resistance within the paper-containing structure changes, switching between the first shape and the second shape in at least one direction. Through this switching action, various functions such as holding, storing, opening and closing, moving, and valve opening and closing of the item can be realized.

[0018] [2] In the paper-containing structure of method 1, in the first high-hydroxyl concentration region and the second high-hydroxyl concentration region, when the infrared absorption spectrum of the surface portion is measured by reflecting infrared light at the surface portion of the paper-containing structure using a total internal reflection measurement method with a wavenumber of 3331 cm⁻¹, the transmittance of the infrared light can be lower than that of the other portions. At a wavenumber of 3331 cm⁻¹, the change in hydroxyl concentration is most sensitively reflected. The infrared transmittance of the high hydroxyl concentration region is not limited, and can be more than 0.01%, more than 0.1%, more than 0.5%, more than 1%, more than 2%, more than 3%, more than 4%, more than 5%, or more than 10% lower than the other parts.

[0019] [3] In the paper-containing structure described in method 1 or 2, one or more notches may be formed on the paper-containing sheet, through which the first stable state and the second stable state can be formed. A triggering force may also be applied to the notch.

[0020] [4] In any of the paper-containing structures in methods 1-3, the triggering force may be through water penetration into the paper-containing structure, changes in humidity of the environment in which the paper-containing structure is placed, or local pressure on the paper-containing structure.The triggering force is generated by shrinking, heating the paper-containing structure, cooling the paper-containing structure, cutting a part of the paper-containing structure, or applying an external force to the paper-containing structure. The triggering force is a stimulus to the paper-containing sheet, which may be a force applied to the paper-containing sheet or a force generated inside the paper-containing sheet. For example, it may be a local temperature change of the paper-containing sheet caused by strong light irradiation, a bullet impact, a part of the paper-containing sheet being burned off by a laser beam, a vibration of the paper-containing sheet caused by sound waves, or pressure on the paper-containing sheet by air or wind blowing.

[0021] [5] In any of the paper-containing structures in methods 1-4, the paper-containing structure may switch between the first shape and the second shape in both directions by applying the triggering force to a part of it. The method and type of application of the triggering force may also be different in the case of changing from the first shape to the second shape and in the case of changing from the second shape to the first shape. A third shape or a fourth shape may also be present.

[0022] [6] A gripping member having a paper-containing structure of any one of the embodiments 1-5, for gripping an item. The first shape is an item release shape with an open end, and the second shape is an item gripping shape with a narrowed end. The triggering force is generated by the gripping member colliding with the item or by the gripping member contacting a support surface supporting the item. Thus, the paper-containing structure changes from the item release shape to the item gripping shape to grip the item. The end can be set to match the position of the item to be gripped, and can be the lower end of the paper-containing sheet, the side end, or the upper end.

[0023] [7] A gripping member for a drone, having the gripping member described in embodiment 6, with a fixing part fixed to the support part of the drone at the center of the gripping member. In the case of a drone, the gripping member is lightweight and does not have an additional opening and closing mechanism, which are significant advantages. It can also handle ultra-small drones. In addition, the gripper for drones of the present invention can also change from a second shape to a first shape, gripping an item until the destination, and releasing or dropping the item from the drone at the destination.

[0024] [8] A cushioning material having a paper-containing structure described in any one of embodiments 1-5 for arranging one or more items therein may be that the paper-containing structure has a folding structure, the first shape is a reduced shape of the paper-containing structure folded without a bag or the paper-containing structure is a flat shape without a bag, the second shape is an unfolded shape of the paper-containing structure unfolded to form one or more bags, and the shape changes from the reduced shape or flat shape to the unfolded shape by applying a triggering force to a part of the paper-containing structure. In this caseThe paper sheet can be folded into a Miura fold shape or an egg carton shape after the first high-hydroxyl concentration area and the second high-hydroxyl concentration area are printed into the desired pattern, or with creases. The bag can have a honeycomb structure.

[0025] [9] An origami device includes: a paper-containing structure described in any one of the methods 1-5, and at least one of an electronic component and wiring provided on at least one of the first surface and the second surface of the paper-containing structure. As an electronic component, it can be an active component or a component composed of active components (transistor, IC, diode, operational amplifier, etc.), or a passive component such as a resistor, coil, or capacitor, or a printed antenna, relay, switch, connector, printed circuit board, terminal, etc. As wiring, it can be wiring formed by thinly printing copper or aluminum on the paper sheet. The paper sheet can also be deformed between the first shape and the second shape by applying a triggering force to the paper sheet by a heating element or a solenoid.

[0026]

[10] A cushioning material having a paper-containing structure described in any one of the methods 1-5 for arranging one or more articles therein may have a paper-containing structure having a folding structure, a first shape being a flat shape in which the paper-containing structure is unfolded without having a bag, and a second shape being an unfolded shape in which the paper-containing structure is folded to form one or more bags, and changing from the flat shape to the unfolded shape by applying a triggering force to a portion of the paper-containing structure.

[0027]

[11] A cushioning material comprising a paper-containing structure as described in any one of embodiments 1-5 may be wherein the paper-containing structure has one or more openings and a first high-hydroxyl concentration region and a second high-hydroxyl concentration region disposed around the openings, the first shape being a reduced shape of the paper-containing structure folded without a bag or a flat shape of the paper-containing structure unfolded, and the second shape being a three-dimensional shape of the paper-containing structure having a cylindrical wall portion and a support portion, wherein the cylindrical wall portion stands upright at the periphery of the openings, and the support portion extends from the cylindrical wall portion, changing from the reduced shape or flat shape to the three-dimensional shape by applying a triggering force to a portion of the paper-containing structure. The cylindrical wall portion and the support portion may integrally have a honeycomb structure.

[0028]

[12] A method for manufacturing a paper-containing structure, wherein the paper-containing structure is manufactured in any one of methods 1-5, comprises the following steps: coating a liquid containing water onto the first and second surfaces of the paper-containing sheet at portions where a first high-concentration hydroxyl region and a second high-concentration hydroxyl region are to be formed; and drying the liquid.

[0029]

[13] In any of the paper-containing structures described in methods 1-5, at least a portion of at least one of the first and second surfaces of the paper-containing sheet may be adhered with a flexible protective film. By covering at least a portion of the paper-containing sheet with the protective film in this way, especially forming a protective film at the part in contact with water, unwanted water will not penetrate into the paper-containing sheet, and the deformation function of the paper-containing sheet caused by the first and second high hydroxyl concentration regions can be maintained. In addition, when holding items with high water content such as fruits by means of the paper-containing structure, by forming a protective film at the part in contact with the item, it is also possible to prevent the paper-containing structure from absorbing the water of the item, and the water content of the fruit, etc. can be maintained. Furthermore, in the part whose surface is covered by the protective film, the coefficient of friction of the surface in contact with the fruit, etc. increases, so the positional stability of the item in the stored state can be improved.

[0030]

[14] In any of the paper-containing structures described in methods 1-5, a flexible protective film may be adhered to the first and second surfaces of the paper-containing sheet respectively. In this way, by sandwiching the paper-containing sheet with the protective film, even if the paper-containing structure 1 is placed in a humid or high-humidity environment, unwanted moisture will not penetrate into the paper-containing sheet, thus maintaining the deformation function of the paper-containing sheet caused by the high concentration regions of the first and second hydroxyl groups. Furthermore, when holding items with high moisture content, such as fruits, with the paper-containing structure, it is also possible to prevent the paper-containing structure from absorbing moisture from the items. Therefore, the water content of fruits, etc., can be maintained. Moreover, by covering the surface with the protective film, the coefficient of friction of the surface in contact with fruits, etc., increases, thereby improving the positional stability of the items in the contained state. Alternatively, the end face of the paper-containing sheet can be covered with the material of the protective film to form an end face protective film. In this case, moisture resistance can be further improved, and the protective film can be prevented from peeling off from the end face.

[0031] (III) Beneficial Effects

[0032] According to the present invention, by applying a triggering force to a portion of a paper-containing structure having a first high-hydroxyl concentration region and a second high-hydroxyl concentration region, the antagonistic balance between tensile stress and deformation resistance within the paper-containing structure changes, switching between a first shape and a second shape in at least one direction. Various functions can be achieved through this switching action. Brief Description of the Drawings

[0033] FIG1A is an enlarged cross-sectional view illustrating the principle of the paper-containing structure of the present invention.

[0034] FIG1B is an enlarged cross-sectional view illustrating the principle of the paper-containing structure of the present invention.

[0035] FIG1C is an enlarged cross-sectional view illustrating the principle of the paper-containing structure of the present invention.

[0036] FIG2 is an enlarged cross-sectional view illustrating the principle of the paper-containing structure of the present invention.

[0037] FIG3 is an enlarged cross-sectional view showing an example of a high-hydroxyl concentration region in the present invention.

[0038] Figure 4A is an enlarged cross-sectional view showing the effect of the high hydroxyl concentration region in the present invention.

[0039] Figure 4B is an enlarged cross-sectional view showing the effect of the high hydroxyl concentration region in the present invention.

[0040] Figure 5 is a cross-sectional view showing the method for measuring the concentration of hydroxyl groups.

[0041] Figure 6 is a graph illustrating the high hydroxyl concentration region in the present invention.

[0042] Figure 7 is a graph illustrating the high hydroxyl concentration region in the present invention.

[0043] Figure 8 is a graph illustrating the high hydroxyl concentration region in the present invention.

[0044] Figure 9 is a graph illustrating the high hydroxyl concentration region in the present invention.

[0045] Figure 10 is a perspective view showing an embodiment of the paper-containing structure of the present invention.

[0046] Figure 11 is a top view showing an embodiment of the paper-containing structure of the present invention.

[0047] Figure 12 is a perspective view showing an embodiment of the paper-containing structure of the present invention. Specification 4 / 23 Page 7 CN 121646554 A

[0048] FIG13 is a perspective view showing another embodiment of the paper-containing structure of the present invention.

[0049] FIG14 is a top view showing another embodiment of the paper-containing structure of the present invention.

[0050] FIG15 is a perspective view showing another embodiment of the paper-containing structure of the present invention.

[0051] FIG16 is a top view showing another embodiment of the paper-containing structure of the present invention.

[0052] FIG17A is a cross-sectional view showing the operation of another embodiment of the present invention.

[0053] FIG17B is a cross-sectional view showing the operation of another embodiment of the present invention.

[0054] FIG18 is a top view showing a test piece of an embodiment of the present invention.

[0055] FIG19 is a graph showing the test results of the amount of movement and load using the test piece of FIG18.

[0056] FIG20 is a graph showing the thickness and angle changes of the paper using the test piece of FIG18.

[0057] FIG21 is a graph showing the changes in horizontal printing width and angle of the test piece using FIG18.

[0058] FIG22 is a perspective view showing another embodiment of the paper-containing structure of the present invention.

[0059] FIG23 is a top view showing another embodiment of the paper-containing structure of the present invention.

[0060] FIG24 is a top view showing another embodiment of the paper-containing structure of the present invention.

[0061] FIG25 is a top view showing another embodiment of the paper-containing structure of the present invention.

[0062] FIG26 is a front view showing another embodiment of the paper-containing structure of the present invention.

[0063] FIG27 is a perspective view showing another embodiment of the paper-containing structure of the present invention.

[0064] FIG28 is a front view showing the article release state of a drone-mounted clamp as another embodiment of the paper-containing structure of the present invention.

[0065] Figure 29 is a front view showing the article-holding state of a drone-mounted clamp as another embodiment of the paper-containing structure of the present invention.

[0066] Figure 30 is a top view showing another embodiment of the paper-containing structure of the present invention.

[0067] Figure 31 is a top view showing another embodiment of the paper-containing structure of the present invention.

[0068] Figure 32 is a perspective view showing another embodiment of the paper-containing structure of the present invention.

[0069] Figure 33 is a top view showing another embodiment of the paper-containing structure of the present invention.

[0070] Figure 34 is a top view showing another embodiment of the paper-containing structure of the present invention.

[0071] Figure 35 is a front view showing another embodiment of the paper-containing structure of the present invention.

[0072] Figure 36 is a top view showing another embodiment of the paper-containing structure of the present invention.

[0073] Figure 37 is a top view showing another embodiment of the paper-containing structure of the present invention.

[0074] Figure 38 is a top view showing another embodiment of the paper-containing structure of the present invention.

[0075] Figure 39 is a perspective view showing another embodiment of the paper-containing structure of the present invention.

[0076] FIG40 is a perspective view showing another embodiment of the paper-containing structure of the present invention.

[0077] FIG41 is a perspective view showing another embodiment of the paper-containing structure of the present invention.

[0078] FIG42 is an enlarged cross-sectional view showing another embodiment of the paper-containing structure of the present invention.

[0079] FIG43 is an enlarged cross-sectional view showing another embodiment of the paper-containing structure of the present invention.

[0080] FIG44 is an enlarged cross-sectional view showing another embodiment of the paper-containing structure of the present invention.

[0081] FIG45 is an enlarged cross-sectional view showing another embodiment of the paper-containing structure of the present invention.

[0082] FIG46 is a top view showing a sensing pad as another embodiment of the paper-containing structure of the present invention.

[0083] FIG47 is a perspective view showing the state in which the sensing pad is fixed to the human head.

[0084] FIG48 is a top view showing a partial cross-section of the absorbent pad as another embodiment of the paper-containing structure of the present invention. (Page 5 / 23, CN 121646554 A, Specification)

[0085] FIG49 is a cross-sectional view of the absorbent pad.

[0086] FIG50 is a top view showing a conical structure as another embodiment of the paper-containing structure of the present invention.

[0087] FIG51 is a front photograph showing the state before a triggering force is applied to the conical structure.

[0088] FIG52 is a front photograph showing the state after a triggering force is applied to the conical structure.

[0089] FIG53 is a cross-sectional view showing a catalyst unit as another embodiment of the paper-containing structure of the present invention.

[0090] FIG54 is a deformation of a buffer material without a protective film as another embodiment of the paper-containing structure of the present invention.

[0091] FIG55 is a photograph of the cushioning material without the protective film after deformation.

[0092] FIG56 is a photograph of the cushioning material with the protective film before deformation, as another embodiment of the paper-containing structure of the present invention.

[0093] FIG57 is a photograph of the cushioning material with the protective film after deformation.

[0094] FIG58 is a photograph showing the use of the cushioning material with the protective film.

[0095] FIG59 is an explanatory diagram showing the moisture absorption test method for investigating the difference in moisture absorption when the paper-containing sheet has no protective film and when it has a protective film.

[0096] FIG60 is a graph showing the results of the moisture absorption test. Detailed Embodiments

[0097] Hereinafter, embodiments of the paper-containing structure and the method for manufacturing the paper-containing structure of the present invention will be described with reference to the accompanying drawings.

[0098] FIG1A to FIG1C are enlarged cross-sectional views for explaining the operating principle of the present invention. As shown in Figures 1A to 1C, the paper-containing structure of the present invention is formed from a paper-containing sheet 2 in a dry state containing paper. The paper-containing sheet 2 has a first surface 1a and a second surface 1b that form opposite sides to each other. On the first surface 1a, a first hydroxyl high concentration region 11 is formed by allowing a liquid 9 composed of water or an aqueous solution to penetrate a portion of the paper-containing sheet 2, thereby forming a first hydroxyl high concentration region 11 where the density of hydroxyl groups is higher than that of other parts of the first surface 1a. A second hydroxyl high concentration region (not shown) is also formed on the second surface 1b where the density of hydroxyl groups is higher than that of other parts of the second surface 1b.

[0099] Tensile stress is generated in the first hydroxyl high concentration region 11 and the second hydroxyl high concentration region in a direction parallel to the paper-containing sheet 2, respectively. The tensile stress in the first hydroxyl high concentration region 11 of the first surface 1a, the tensile stress in the second hydroxyl high concentration region of the second surface 1b, and the deformation resistance of the paper sheet 2 itself antagonize each other when the paper structure 1 is in the first shape, forming a first stable state that can maintain the first shape. Furthermore, when the paper structure is in the second shape, it antagonizes each other to form a second stable state that can maintain the second shape. Moreover, the invention is characterized in that the paper structure 1 can switch between the first shape and the second shape in at least one direction by applying a triggering force to a portion thereof.

[0100] As shown in FIG1A, water 9 is attached to the first surface 1a of the paper sheet 2 and permeates to form the first hydroxyl high concentration region 11. Considering the thickness T1 of the paper sheet 2, an appropriate amount of water 9, which will not be excessive, is attached to the first surface 1a. Thus, as shown in FIG1B and FIG1C, water 9 permeates from the first surface 1a into the paper sheet 2. Figure 1B shows the state where the paper sheet 2 is slightly swollen due to the penetration of water 9, causing the first surface 1a to become convex and the paper sheet 2 to warp. Typically, after this state, when the water 9 evaporates, as shown in Figure 1C, the warping is eliminated, and tensile stress remains in the first high hydroxyl concentration region 11.

[0101] As shown in Figure 2, water 9 can penetrate from the first surface 1a to the second surface 1b. In this case, the first surface 1a forms a first high-hydroxyl concentration region with a wide width or a high concentration of hydroxyl groups, and the second surface 1b forms a second high-hydroxyl concentration region with a narrow width or a low concentration of hydroxyl groups.

[0102] As shown in Figure 3, a first high-hydroxyl concentration region 12 in which water 9 does not penetrate from the first surface 1a to the second surface 1b and a first high-hydroxyl concentration region 13 in which water 9 penetrates from the first surface 1a to the second surface 1b can also be formed. In this case, a difference in tensile stress between the first surface 1a side and the second surface 1b side is also generated, which can achieve the effect of the present invention.

[0103] The paper sheet 2 is a sheet material composed of paper itself (i.e., a paper sheet material), or a sheet material with paper as the main component, containing cellulose as the main component. As a paper sheet material, for example, a relatively thick paper such as tracing paper is preferred, and paper in which the cellulose bundles are compressed by strong pressure during the manufacturing process is preferred.

[0104] The sheet material with paper as the main component may contain paper and other components. These other components can be selected arbitrarily according to the purpose, without impairing the effects of the present invention. Specifically, examples of other components include cosmetics such as resins, silicone, calcium carbonate, and clay; brighteners; starch; and adhesives such as PVA.

[0105] When water 9 is applied to the paper sheet 2, not only pure water can be used, but also aqueous solutions containing various water-soluble compounds, or aqueous solutions containing small amounts of organic solvents such as alcohols, can be used. In this case, the solute in the aqueous solution can penetrate and remain in the paper sheet 2. Examples of solutes in the aqueous solution include organic solvents (2-propanol, ethylene glycol, etc.) used to adjust the viscosity and surface tension of inkjet inks, electrolytes such as various salts, and dyes. The aqueous solution may contain only one type of solute or two or more types. For example, by adding dye, it is possible to obtain the advantage that the first high-hydroxyl concentration region 11 and the second high-hydroxyl concentration region 14 are easily visually identifiable.

[0106] The lower the concentration of components other than water in the aqueous solution, the better. For example, it is preferably 5% by mass or less of the total liquid, more preferably 3% by mass or less, and even more preferably 1% by mass or less.

[0107] Non-Patent Document 1 discloses a technique for voluntarily bending a sheet of paper by using an aqueous solution containing water and 2-propanol in a mass ratio of "water: 2-propanol = 90:10". However, although lower alcohols such as 2-propanol are fully miscible with water, they do not have the effect of voluntarily bending paper sheets, or even if they do, it is significantly worse than that of water. Therefore, when comparing the same amount, the use of an aqueous solution containing 2-propanol is preferable.In contrast, compared to the use of pure water or aqueous solutions where the liquid component is mostly water, the self-deformation speed of the paper sheet is slow, remaining at a small bending angle.

[0108] In contrast, the paper-containing structure and its manufacturing method of the present invention can achieve self-deformation of the paper sheet at a faster speed and a larger bending angle compared to the use of aqueous solutions containing a high concentration of 2-propanol, which has a significant effect in this respect. However, the liquid used in the manufacturing method of the paper-containing structure according to the embodiments of the present invention can be any liquid as long as it is at a low concentration. In the manufacturing method of the paper-containing structure according to the embodiments of the present invention, an aqueous solution containing 2-propanol can also be used as long as it is at a low concentration as described above.

[0109] In the above process, when water or an aqueous solution is attached to and permeates the paper sheet 2, two aqueous solutions with different concentrations of the additive can be attached to different areas of the paper sheet 2 respectively. The solute is not particularly limited as long as it is water-soluble and can be arbitrarily selected. The aqueous solution is preferably neutral.

[0110] In the solute, the salt can be any one of organic salt and inorganic salt, preferably inorganic salt. Examples of such inorganic salts include alkali metal chlorides such as lithium chloride (LiCl, hydration parameter: 7.1), sodium chloride (NaCl, hydration parameter: 3.5), potassium chloride (KCl, hydration parameter: 1.9), and rubidium chloride (RbCl, hydration parameter: 1.2); alkali metal bromides such as lithium bromide (LiBr, hydration parameter: 7.6), sodium bromide (NaBr, hydration parameter: 4.2), potassium bromide (KBr, hydration parameter: 2.1), and rubidium bromide (RbBr, hydration parameter: 0.9); alkali metal bromides such as lithium iodide (LiI, hydration parameter: 9.0), sodium iodide (NaI, hydration parameter: 5.5), potassium iodide (KI, hydration parameter: 2.5), and rubidium iodide (RbI, hydration parameter: 0.6); and magnesium chloride. (See page 7 / 23 of the specification, CN 121646554 A). Chlorides of Group II metals such as MgCl2 (hydration parameter: 13.7), calcium chloride (CaCl2, hydration parameter: 12.0), and strontium chloride (SrCl2, hydration parameter: 10.7); bromides of Group II metals such as magnesium bromide (MgBr2, hydration parameter: 17.0), calcium bromide (CaBr2, hydration parameter: 14.6), and strontium bromide (SrBr2, hydration parameter: 12.7); iodides of Group II metals such as magnesium iodide (MgI2, hydration parameter: 19.0), calcium iodide (CaI2, hydration parameter: 17.0), and strontium iodide (SrI2, hydration parameter: 15.5); manganese chloride (MnCl2, hydration parameter: 11.0), ferrous chloride (FeCl2, hydration parameter: 12.0), and cobalt chloride (CoCl2, hydration parameter: 10.7).13.0), nickel chloride (NiCl2, hydration parameter: 13.0), and other transition metal chlorides, etc.

[0111] By adding the solute as described above to the paper sheet 2, the penetration and drying of water 9 in the aqueous solution can be suppressed. When the suppression effect can be small, a substance with a hydration parameter of 0.5 to 9 can be selected. In order to increase the suppression effect, a substance with a hydration parameter of 15 to 20 can be selected, but it is not limited in this invention.

[0112] The temperature at which water 9 adheres to and penetrates the paper sheet 2 is not limited, for example, it can be 10 to 35°C. Under such temperature conditions, water 9 can penetrate into the paper sheet 2 more well.

[0113] The relative humidity at which water 9 adheres to and penetrates the paper sheet 2 is preferably 10 to 80%, for example, it can be any one of 20 to 65% and 20 to 40%. Under such relative humidity conditions, water 9 can penetrate into the paper sheet 2 more well.

[0114] After the infiltration process, the paper sheet 2 containing water 9 is dried. When the paper sheet 2 containing water 9 is dried, for example as shown in FIG4A, the cellulose in the portion 11 containing water 9 in the paper sheet 2 shrinks, generating tensile stress. As a result, the first surface 1a is bent in a concave manner. If drying is carried out, the bending angle becomes larger. As shown in FIG4B, a three-dimensional structure 10 is formed in the state after drying. If the paper sheet 2 is dried while suppressing this deformation, tensile stress can be generated in the region of high hydroxyl concentration in the paper sheet 2.

[0115] In the paper sheet 2, cellulose molecules are bonded to each other by hydrogen bonds. It is speculated that if water 9 is infiltrated into the paper sheet 2, the first surface 1a side expands, but in the paper sheet 2, water molecules break the hydrogen bonds between cellulose molecules, and water molecules are in a state between cellulose molecules, forming intermolecular bonds of cellulose molecule-water molecule-cellulose molecule.

[0116] The paper sheet 2 is manufactured by clamping the pulp with a pressure roller to allow water to fall off, and then applying pressure and heating while using the pressure roller. Due to this manufacturing method, the paper sheet 2 is initially in a state where it is under compressive strain due to external force. If such a paper sheet 2 is permeated with water 9 and dried, as the water 9 in the paper sheet 2 decreases due to drying, the cellulose molecules in the paper sheet 2 are bonded to each other again by hydrogen bonds. At this time, the paper sheet 2 becomes stable with reduced or eliminated strain compared to the initial state, and it is presumed to shrink compared to before the permeation of water 9. It is presumed that due to the shrinkage force generated at this time, as shown in FIG4B, the paper sheet 2 flexes autonomously in the high hydroxyl concentration region.

[0117] The first and second water concentration gradient regions formed on the paper sheet 2 are not limited in this invention, but printing using an inkjet printer is preferred in order to coat it into complex shapes. In the case of using an inkjet printer, ink is sprayed from the inkjet printer.The printer sprays a liquid consisting of water or an aqueous solution onto the paper sheet 2, allowing it to adhere to and penetrate the paper sheet.

[0118] [Method for measuring the density of hydroxyl groups]

[0119] Figure 5 illustrates the measurement principle of the total internal reflection (ATR) method for measuring the density of hydroxyl groups. A transparent crystal 15, serving as an optical waveguide, is disposed on the paper sheet 2, which is the sample. Infrared light is incident through the crystal 15 while continuously changing the wavelength, and is irradiated from the lower surface of the crystal 15 into a region at a depth dp of the surface layer of the paper sheet 2. The reflected light that penetrates into the interior of the paper sheet 2 and is reflected is again incident on a light sensor through the crystal 15. The transmittance of the incident light at each wavenumber is determined by the light sensor. In the figure, θ is the incident angle, which is set to a value of 45° in this specification. The penetration depth dp that produces the reflected light also varies depending on the sample, and is approximately in the range of 0.5 to 5 μm. The actual measurement was performed using a Fourier transform infrared spectrophotometer manufactured by Shimadzu Corporation, trade name "IRAffinity-S". The measurement conditions were set as follows: resolution: 4 cm⁻¹, apodization function (the function used in Fourier transform): Happ-Genzel, and number of measurements: 30.

[0120] Figures 6 and 7 show an example of data obtained using the ATR method in Figure 5. Figures 6 to 9 show the transmittance (%) spectra obtained by continuously changing the wavenumber of the infrared radiation on the surface of the paper sheet 2 before water penetration, the surface of the paper sheet 2 after printing water and drying, and the back side of the paper sheet 2. As these graphs show, around wavenumber 3331 (cm⁻¹), a significant decrease in transmittance occurs due to the high density of hydroxyl groups, resulting in a downward peak. Therefore, it was demonstrated that by measuring and comparing the transmittance at a wavenumber of 3331 (cm⁻¹), the density of hydroxyl groups in the surface portion of the paper sheet 2 could be compared.

[0121] Next, Figures 8 and 9 show the results of comparative experiments conducted to confirm whether the reduction in infrared transmittance of the paper sheet 2 was caused by other reasons. In these comparative experiments, the infrared spectra of the surface and back of the paper sheet after four different treatments were measured while the wavenumber of the infrared light was continuously changed. “Water surface” refers to the measurement results of the surface when water was printed on the surface of the paper sheet 2 and then dried; “Water back” refers to the measurement results of the back when water was printed on the surface of the paper sheet 2 and then dried; “Mold back” refers to the measurement results of the back of the paper sheet 2 after being stamped with a load of 1 ton / (40mm × 40mm); “Mold surface” refers to the measurement results of the surface of the same paper sheet 2 after stamping; and “Compression back” refers to the measurement results of the back of the paper sheet 2 after being stamped with a load of 3 tons / (40mm × 40mm).The measurement results of the back side of the paper sheet 2 after it is stamped with an aluminum block are shown. "Compressed surface" refers to the measurement results of the surface of the same paper sheet 2 after it is stamped with an aluminum block. "Hand-folded back side" refers to the measurement results of the surface when the crease is inserted into the paper sheet 2 by hand. "Hand-woven surface" refers to the measurement results of the back side when the crease is inserted into the paper sheet 2 by hand. As shown in these graphs, around wavenumber 3331 (cm-1), the significant decrease in transmittance due to the high density of hydroxyl groups only occurs in the graph of the "water surface". Therefore, it is proved that the decrease in transmittance caused by the concentration of hydroxyl groups is a result of water permeation.

[0122] [First Embodiment]

[0123] Figures 10 to 12 show the paper structure 20 as a specific first embodiment of the paper structure of the present invention. In this paper-containing structure 20, a first high-hydroxyl concentration region 11 extending in the short side direction is formed at the center of the width direction of the first surface 1a of the rectangular paper-containing sheet 2 by printing with water or an aqueous solution. Additionally, a second high-hydroxyl concentration region 14 is formed at a certain distance from both ends of the long side of the second surface 1b by printing with water or an aqueous solution. Furthermore, the paper-containing sheet 2 is thoroughly dried. As shown in FIG11, at the center of both ends of the first high-hydroxyl concentration region 11 in the length direction, the paper-containing sheet 2 can be intermittently cut in a dotted line shape, or a shallowly cut weakening line 22 can be pre-formed into the paper-containing sheet 2. The length of the weakening line 22 can reach or not reach the second high-hydroxyl concentration region 14.

[0124] Furthermore, the first high-hydroxyl concentration region 11 and the second high-hydroxyl concentration region 14 also include cases where the hydroxyl concentration is not constant in the horizontal direction and / or thickness direction of the paper-containing sheet 2 (i.e., a gradient exists). A concentration gradient can be formed along the thickness direction as diffusion occurs, so a gradient can be formed if coating is usually performed from one side. For ease of explanation, the long side and short side are described as above, but the long side and short side can also be reversed. In addition, the paper sheet 2 can be square, or it can be any shape such as round, elliptical, triangular, pentagonal, or irregular. The shape of the first high hydroxyl concentration region 11 and the second high hydroxyl concentration region 14 can also be a non-straight strip, a curve, a discontinuous dashed line, or they can intersect at acute or obtuse angles instead of being orthogonal, or they can be a shape in which the width varies along the length direction of the first high hydroxyl concentration region 11 and the second high hydroxyl concentration region 14. The above points are common to other embodiments unless otherwise specifically mentioned.

[0125] The paper sheet 2 that has undergone the drying process is reduced in the width direction by the tensile stress generated inside the second high hydroxyl concentration region 14, so that both ends are recessed along the second high hydroxyl concentration region 14 and the second surface 1b side. (See page 9 / 23 of the specification, 12 CN)121646554 A is bent along the upper crease line (Japanese: yama ore sen) 5. On the other hand, although a tensile stress that shrinks in the width direction of the first hydroxyl high-concentration region 11 is also generated inside the first hydroxyl high-concentration region 11, since the second hydroxyl high-concentration region 14 is bent first, the deformation resistance of the paper-containing sheet 2 becomes higher relative to the force bending the paper-containing sheet 2 in the longitudinal direction, and deformation caused by the tensile stress of the second hydroxyl high-concentration region 14 is hardly generated. Accordingly, in the first shape in which the long sides shown in FIG. 10 are bent respectively, the tensile stress of the first hydroxyl high-concentration region 11, the tensile stress of the second hydroxyl high-concentration region 14, and the deformation resistance of the paper-containing sheet 2 antagonize each other to maintain a stable shape.

[0126] Subsequently, applying a pressing force to the central portion of the first surface 1a to the paper-containing structure 20 stabilized in the first shape of FIG. 10, or cutting notches 21 at both ends of the first hydroxyl high-concentration region 11, or doing both, or cutting the weakened line 22 if it exists, thereby forming the notch 21 orthogonal to the second hydroxyl high-concentration region 14, or the width of the second hydroxyl high-concentration region 14 becomes smaller due to the notch 21, so that the deformation resistance of the paper-containing sheet 2 is reduced. Then, due to the tensile stress generated by the first hydroxyl high-concentration region 11, the paper-containing sheet 2 is bent along the width direction of the first hydroxyl high-concentration region 11, deformed into a V-shaped cross section recessed toward the first surface 1a side, and stops while maintaining this second shape. In the second shape, the tensile stress generated by the first hydroxyl high-concentration region 11, the tensile stress of the second hydroxyl high-concentration region 14, and the deformation resistance of the paper-containing sheet 2 are balanced, and no further deformation occurs.

[0127] Therefore, according to the paper-containing structure 20, in the first shape shown in FIG. 10, applying a pressing force to the central portion of the first surface 1a, or cutting notches 21 at both ends of the first hydroxyl high-concentration region 11, or doing both, or cutting the weakened line 22 if it exists, thereby changing to the second shape shown in FIG. 12, so that various functions can be exerted in this process. For example, the paper-containing structure 20 is V-shaped in the second shape, so that it can clamp other articles, perform certain switching operations at the moving end, or press other articles by using the increased overall thickness of the paper-containing structure 20.

[0128] In addition, the paper-containing structure 20 can be simply formed at low cost by coating water or an aqueous solution on the paper-containing sheet 2 and drying it, various changes can be made to the dimension, and the weight is also light, so it can be used for extremely various applications.

[0129] In addition, as the triggering force, the pressing force is used in the above description, but in the present invention, as the triggering force, it may also be achieved by water penetrating into the paper-containing structure, the humidity change of the environment where the paper-containing structure is placed, local compression of the paper-containing structure, heating of the paper-containing structure, cooling of the paper-containing structure, cutting of a part of the paper-containing structure, or applying to the paper-containing structureis generated by applying an external force from another direction. This also applies to the following embodiments.

[0130] [Second Embodiment]

[0131] Figures 13 to 15 show a paper-containing structure 30 which is a second embodiment of the paper-containing structure of the present invention. In this paper-containing structure 30, a band-shaped first hydroxyl high-concentration region 11 extending along the short-side direction is formed by printing with water or an aqueous solution or the like at the width-direction central portion of the first surface 1a of the rectangular paper-containing sheet 2. As shown in Figure 14, on the second surface 1b of the paper-containing sheet 2, V-shaped band-shaped second hydroxyl high-concentration regions 14 in a top view are formed by printing with water or an aqueous solution or the like from two corners of one short side toward the center of the other short side. Then, the paper-containing sheet 2 is sufficiently dried.

[0132] In this paper-containing structure 30, an upper folding line 5 is pre-formed along the width-direction center of the second hydroxyl high-concentration region 14. In addition, after a lower folding line (Japanese: taniorisen) 6 is once formed along the width-direction center of the first hydroxyl high-concentration region 11, the paper-containing sheet 2 is spread flat. In this state, the lower folding line 6 is hardly visible.

[0133] The paper-containing sheet 2 that has undergone the drying step, by virtue of the tensile stress generated inside the second hydroxyl high-concentration region 14 that tends to shrink in the width direction, is bent into a V shape bounded by the upper folding line 5 such that both end portions follow the second hydroxyl high-concentration region 14 and the second surface 1b side becomes recessed. On the other hand, tensile stress that tends to shrink in the width direction of the first hydroxyl high-concentration region 11 is also generated inside the first hydroxyl high-concentration region 11. However, since the paper-containing sheet 2 is first bent into a V shape bounded by the upper folding line 5, the deformation resistance against the force that bends the paper-containing sheet 2 along the longitudinal direction becomes higher, and deformation caused by the tensile stress of the second hydroxyl high-concentration region 14 hardly occurs. As a result, as shown in Figure 13, the upper folding lines 5 arranged in a V shape in a top view are each stabilized in the first shape of being bent into a V shape in cross section.

[0134] Next, by applying a force pressing down the central portion of the first surface 1a to the paper-containing structure 20 stabilized in the first shape shown in Figure 13, as shown in Figure 15, the paper-containing sheet 2 is bent bounded by the hidden lower folding line 6, and the upper folding line 5 bends at the center. Then, the deformation resistance caused by the upper folding line 5 weakens, and the tensile stress caused by the first hydroxyl high-concentration region 11 becomes larger, so the paper-containing sheet 2 deforms into a V shape in cross section recessed toward the first surface 1a side. Then, it stops while maintaining the second shape shown in Figure 15. In the second shape shown in Figure 15, the tensile stress generated by the first hydroxyl high-concentration region 11, the tensile stress of the second hydroxyl high-concentration region 14, and the deformation resistance of the paper-containing sheet 2 are balanced, and no further deformation occurs.

[0135] Therefore, according to this paper-containing structure 30, in the first shape shown in Figure 13, by applying a force to the central portion of the first surface 1aApplying a pressing force can easily change it into the second shape shown in FIG15, and various functions can be realized in the process. For example, by forming a V-shape with the paper-containing structure 30 in the second shape, it is possible to clamp other items, perform opening and closing operations, or press other items by increasing the thickness of the paper-containing structure 30. The cross-sections of the upper fold line 5 and the lower fold line 6 do not have to be V-shaped as shown in FIG15, but can be gently bent into a U-shape.

[0136] In addition, for ease of explanation, the long side and the short side of the paper-containing sheet 2 in the paper-containing structure 30 are described as described above, but the long side and the short side can be opposite, or can be square. The paper-containing sheet 2 can be any shape such as circular, elliptical, triangular, pentagonal, or irregular. The shape of the first high-hydroxyl concentration region 11 and the second high-hydroxyl concentration region 14 does not have to be a straight strip, but can be a curve, or can be a shape in which the width varies in the length direction of the first high-hydroxyl concentration region 11 and the second high-hydroxyl concentration region 14.

[0137] [Third Embodiment]

[0138] Figures 16, 17A, and 17B show a paper-containing structure 40 as a third embodiment of the paper-containing structure of the present invention. In this paper-containing structure 40, a first hydroxyl high concentration region 11 extending in the short side direction is formed on the first surface 1a of the rectangular paper-containing sheet 2 by printing with water or an aqueous solution. In addition, a second hydroxyl high concentration region 14 is formed on the second surface 1b of the paper-containing sheet 2 by printing with water or an aqueous solution. The second hydroxyl high concentration region 14 connects the two ends of each long side, forming a semi-circular or semi-elliptical shape passing through the center of the paper-containing sheet 2. Moreover, the paper-containing sheet 2 is thoroughly dried.

[0139] In this paper-containing structure 40, an upper bend line 5 with a small radius of curvature is formed in advance along the second hydroxyl high concentration region 14 by stamping with a die. However, in this invention, the stamping process is not necessary, and the operation can be performed even in the coated and dried state. In addition, a downward fold line 6 is formed along the center of the width direction of the first hydroxyl high concentration region 11 and extends flat. In this state, the downward fold line 6 is almost invisible. In addition, creases are generated depending on the type of printing press or the printing sequence, but due to the high resistance to deformation, bending can be prevented, so a flat state can be formed even if it is not re-flattened after printing. In this case, the flattening process is not required. Regarding whether it becomes flat or forms creases after printing, it should be set separately because it is affected by the design (thickness, curvature, etc.) of the printing lines on the first surface 1a and the second surface 1b of the paper sheet 2. This is also the case in the following embodiments.

[0140] The paper sheet 2 after the drying process is formed in the width direction of the second hydroxyl high concentration region 14 by the process of forming a crease line in the second hydroxyl high concentration region 11.The tensile stress, which decreases in the direction of curvature, applies force to the upper bend line 5 in the direction of further decreasing the radius of curvature, and bends with a smaller curvature with the upper bend line 5 as the boundary. On the other hand, although tensile stress that decreases in the width direction of the first high hydroxyl concentration region 11 is also generated inside the first high hydroxyl concentration region 11, since the paper sheet 2 bends first along the semi-circular or semi-arc-shaped upper bend line 5, the deformation resistance of the paper sheet 2 relative to the force of bending the paper sheet 2 along the long side direction becomes higher, and deformation caused by the tensile stress of the second high hydroxyl concentration region 14 does not occur. As a result, as shown in FIG17A, the upper bend line 5 shown in FIG13 protrudes towards the first surface 1a side, and is stabilized by the first dome-shaped first shape of the paper sheet 2 bulging in the center.

[0141] Next, by applying a pressing force to the center of the first surface 1a of the paper-containing structure 40, which is stable in the first shape of FIG. 16, as shown in FIG. 17A and FIG. 17B, the paper-containing sheet 2 is bent with the hidden lower fold line 6 as the boundary, the upper fold line 5 bends in the center, the anti-deformation force caused by the upper fold line 5 is weakened, and the tensile stress caused by the first high hydroxyl concentration region 11 is greater, and the paper-containing sheet 2 is deformed by concave (warping upward) towards the first surface 1a side. Then, the process stops while maintaining the second shape shown in FIG. 17B. In the second shape, the tensile stress generated by the first high hydroxyl concentration region 11, the tensile stress of the second high hydroxyl concentration region 14, and the anti-deformation force of the paper-containing sheet 2 are balanced, and no further deformation occurs.

[0142] Therefore, according to this paper-containing structure 40, in the first shape shown in FIG. 16, by applying a pressing force to the center of the first surface 1a, it changes to the second shape shown in FIG. 17B, and various functions can be achieved in the process. For example, by using the paper-containing structure 40 in a second V-shape, it is possible to clamp other items, perform opening and closing operations, or allow other items to descend due to the reduced height of the dome of the paper-containing structure 30.

[0143] In addition, for ease of explanation, the long side and short side of the paper-containing sheet 2 are described as described above in the paper-containing structure 40, but the long side and short side can be opposite, or they can be square. The paper-containing sheet 2 can be any shape such as circular, elliptical, triangular, pentagonal, or irregular. It can also be a shape in which the width changes in the length direction of the first high hydroxyl concentration region 11 and the second high hydroxyl concentration region 14.

[0144] FIG18 shows a test piece used to confirm the effect of the first high hydroxyl concentration region 11 and the second high hydroxyl concentration region 14 of the third embodiment described above. On the first surface 1a of the rectangular paper-containing sheet 2, a strip-shaped first high hydroxyl concentration region 11 extending in the short side direction is formed by printing with water or an aqueous solution. On the second surface 1b of the paper-containing sheet 2, throughA strip-shaped first high-hydroxyl concentration region 14 is formed by printing with water or aqueous solution, which connects the two ends of each long side to form a semi-circular or semi-elliptical shape passing through the center of the paper sheet 2. An upper fold line 5 with a small radius of curvature is formed in advance along the center of the width direction of the second high-hydroxyl concentration region 14 by stamping with a die. Moreover, the paper sheet 2 is thoroughly dried. In addition, a lower fold line 6 is formed once along the center of the width direction of the first high-hydroxyl concentration region 11 and extends flat. In this state, the lower fold line 6 is almost invisible. In this embodiment, if the paper sheet is flat after printing, it is not necessary to re-stamp.

[0145] The length r1 of the vertical line from the center of the second high-hydroxyl concentration region 14 to the long side of the paper sheet 2 is set to 24 mm, and the length r2 of half the long side of the paper sheet 2 is set to 15 mm. The paper sheet 2 is a commercially available tracing paper with a thickness of 39.5 kg, 56.0 kg, and 88.0 kg per full sheet (1000 sheets). The width of the second high-hydroxyl concentration region 14 is set to 2 mm.

[0146] First, using a commercially available tracing paper with a full sheet weight (1000 sheets) of 56.0 kg, the narrowest width W of the two second high-hydroxyl concentration regions 14 is changed to 10 mm, 20 mm, 30 mm, and 40 mm respectively to manufacture paper-containing structures 50. These paper-containing structures 50 are in a dome-shaped first shape. The pressure change is recorded while pressing the center P of these dome-shaped paper-containing sheets 2 with a measuring device. The results are shown in the curve of Figure 19.

[0147] As shown in Figure 19, when the distance between the curves is 30 mm, a peak value larger than that in the cases of 10 mm, 20 mm, and 40 mm appears, and a peak value of load is generated when the movement amount (press amount) is 12.5 mm. If the amount of movement exceeds the peak value, the load decreases suddenly, and the dome shape is flattened and displaced towards the second shape. In this way, by adjusting the geometry of the second hydroxyl high concentration region 14, various adjustments can be made to the action point reaching the paper-containing structure 50 and the triggering force for shape change.

[0148] Next, FIG20 shows the results in the test piece of FIG18, where the thickness of the tracing paper 2, which is the paper-containing sheet 2, was changed to 39.5 kg, 56.0 kg, and 88.0 kg, and the narrowest width W of the two second hydroxyl high concentration regions 14 was set to 10 mm, the length r1 to 24 mm, and the length r2 to 15 mm. Then, while gradually applying the load, the cross-sectional angle of the clamping first hydroxyl high concentration region 11 before and after the shape change was measured.

[0149] As shown in Figure 20, a large angle change is obtained when the weight is 39.5 kg and 56.0 kg, but when the weight is...At 88.0 kg, the paper sheet 2 is too thick, resulting in insufficient angle variation.

[0150] Next, FIG21 shows the results of measuring the cross-sectional angle of the clamped first hydroxyl high concentration region 11 when the printing width of the first hydroxyl high concentration region 11 is changed to 6 mm, 8 mm, and 10 mm in the test piece of FIG18. The narrowest width W of the two second hydroxyl high concentration regions 14 is set to 10 mm, the length r1 is set to 24 mm, and the length r2 is set to 15 mm. Then, the cross-sectional angle of the clamped first hydroxyl high concentration region 11 is measured while gradually applying the load.

[0151] As shown in FIG21, the angle variation increases as the printing width of the first hydroxyl high concentration region 11 becomes thicker to 6 mm, 8 mm, and 10 mm. This proves that the tensile stress generated by the first hydroxyl high concentration region 11 increases with the increase of the width of the first hydroxyl high concentration region 11.

[0152] [Fourth Embodiment]

[0153] Figures 22 and 23 show a paper-containing structure 60 as a fourth embodiment of the present invention. In this paper-containing structure 60, a circular opening 61 is formed in the center of a square paper-containing sheet 2. On the first surface 1a of the paper-containing sheet 2, a strip-shaped first hydroxyl high concentration region 11 is formed radially from the opening 61 along the diagonal of the paper-containing sheet 2 by printing with water or an aqueous solution. In addition, on the second surface 1b of the paper-containing sheet 2, a strip-shaped second hydroxyl high concentration region 14 is formed radially from the opening 61 by printing with water or an aqueous solution, reaching the center of each side of the paper-containing sheet 2. Moreover, the paper-containing sheet 2 as a whole is bent into a spherical shape and is sufficiently dried while being stamped or otherwise required. The width of the first hydroxyl high concentration region 11 and the second hydroxyl high concentration region 14 becomes thicker as they approach the outer edge. Furthermore, the opening 61 is formed to properly bend the fold lines at the points where the fold lines are concentrated on the paper sheet 2.

[0154] After the drying process, the paper sheet 2 generates tensile stress that needs to be reduced in the width direction inside the second high hydroxyl concentration region 14. In addition, tensile stress that needs to be reduced in the width direction of the first high hydroxyl concentration region 11 is also generated inside the first high hydroxyl concentration region 11. However, since the paper sheet 2 is stamped in a manner that the entire paper sheet 2 is bent, the resistance to deformation relative to the force of bending the paper sheet 2 along the first high hydroxyl concentration region 11 and the second high hydroxyl concentration region 14 is high, and almost no deformation is generated due to the tensile stress of the first high hydroxyl concentration region 11 and the second high hydroxyl concentration region 14. Thus, as shown in FIG23, the paper sheet 2 is stabilized in a first shape that is bent as a whole.

[0155] Next, by applying a force pressing down on the central part of the first surface 1a to the paper structure 60 that is stabilized in the first shape of FIG23, the bending shape of the paper sheet 2 is close to flat, the resistance to deformation of the paper sheet 2 is weakened, and the first high hydroxyl concentration regionThe tensile stress caused by 11 and the tensile stress caused by the second high-hydroxyl concentration region 14 are even greater. The paper sheet 2 is concave towards the first surface 1a along the first high-hydroxyl concentration region 11 and towards the first surface 1a along the second high-hydroxyl concentration region 14, thus deforming. As a result, it stops maintaining the second shape shown in FIG22, which is cross-shaped when viewed from above and triangular in front view. In the second shape, the tensile stress generated by the first high-hydroxyl concentration region 11, the tensile stress of the second high-hydroxyl concentration region 14, and the deformation resistance of the paper sheet 2 are balanced, and no further deformation occurs.

[0156] Therefore, according to this paper-containing structure 60, in the convex curved first shape shown in FIG23, by applying a pressing force to the central part of the first surface 1a, it changes to the second shape shown in FIG22, and various functions can be realized in the process. For example, by the paper-containing structure 60 taking the second shape into a mountain shape, it is possible to clamp other items, perform opening and closing operations, or raise other items by increasing the height of the dome of the paper-containing structure 60.

[0157] Alternatively, instead of bending the paper sheet 2, an annular protrusion 62 can be formed coaxially with the opening 61 at the center of the paper sheet 2 (see page 13 / 23, CN 121646554 A). The cross-section of the annular protrusion 62 is convexly curved. Using the annular protrusion 62, the resistance to deformation relative to the force applied when bending the paper sheet 2 along the first high-hydroxyl concentration region 11 and the second high-hydroxyl concentration region 14 is improved, and deformation caused by tensile stress in the first high-hydroxyl concentration region 11 and the second high-hydroxyl concentration region 14 is almost non-existent. Thus, as shown in FIG23, the paper sheet 2 as a whole is stable in a flat first shape. On the other hand, by pressing down the center of the paper sheet 2, the annular protrusion 62 becomes nearly flat, the deformation resistance of the paper sheet 2 weakens, and the tensile stress caused by the first high hydroxyl concentration region 11 and the tensile stress caused by the second high hydroxyl concentration region 14 are greater. The paper sheet 2 is concave towards the first surface 1a along the first high hydroxyl concentration region 11 and towards the first surface 1a along the second high hydroxyl concentration region 14, and deforms. Thus, the second shape shown in FIG22, which is cross-shaped when viewed from above and triangular in front view, is maintained. In this case, in the second shape, the tensile stress generated by the first high hydroxyl concentration region 11, the tensile stress of the second high hydroxyl concentration region 14, and the deformation resistance of the paper sheet 2 are balanced and no further deformation occurs.

[0158] [Fifth Embodiment]

[0159] FIG24 to FIG29 show a gripper (paper-containing structure) 70 for a drone as a fifth embodiment of the present invention. Furthermore, the gripping component of this invention is not limited to drones; it can be applied to any object as long as it is installed on a moving object and used to grip it. For example, it can also be installed on the front end of a robot, a robotic arm, or a small autonomous vehicle.Insects and other organisms, and human bodies. Furthermore, the gripping direction can be set according to the position of the object to be gripped; it can be the lower end, side end, or upper end of the paper sheet.

[0160] As shown in Figures 28 and 29, the drone grip 70 is mounted on the support 75 at the lower end of the flying drone 74 and covers the target object 77, thereby automatically closing the drone grip 70 to grip and lift the object 77. Furthermore, the installation method of the drone grip 70 is not limited to the downward state shown in the figures. For example, it can be mounted sideways to the side of the drone 74 to grip an object located on the side, or it can be mounted upwards to the upper end of the drone 74 to grip an object located above the drone 74. Additionally, the drone grip of the present invention can also change from a second shape to a first shape, gripping the object until the destination point, releasing and dropping the object from the drone at the destination point, or placing the object.

[0161] As shown in Figures 24 and 25, the paper sheet 2 of the drone gripper 70 has rectangular roll-forming portions 71 formed on both sides of the two long sides of the rectangular main body, forming an overall approximately H-shape. Gaps 72 are formed between the roll-forming portions 71.

[0162] As shown in Figure 24, four first hydroxyl high-concentration regions 11 are formed radially from the opening 73 toward each roll-forming portion 71 on the first surface 1a of the paper sheet 2. Furthermore, as shown in Figure 25, multiple second hydroxyl high-concentration regions 14 are formed on the second surface 1b of the paper sheet 2 at the illustrated position through printing with water or an aqueous solution. Specifically, there are strip-shaped high-concentration second hydroxyl regions 14 extending from the opening 73 to each gap 72, strip-shaped high-concentration second hydroxyl regions 14 extending from the opening 73 along both sides of the upper bend line 5 formed in the center of the paper sheet 2, high-concentration second hydroxyl regions 14 formed on the entire surface of the roll-formed portion 71, and high-concentration second hydroxyl regions 14 close to the roll-formed portion 71. Moreover, as shown in FIG28, the paper sheet 2 is bent and fully dried in a recessed manner on the first surface 1a. The roll-formed portion 71 is wound into a cylindrical shape in the initial state by the tensile stress of the high-concentration second hydroxyl regions 14. This roll-formed portion 71 is formed to sufficiently increase the strength of the contact area with the article 77 when holding the article 77.

[0163] The drone grip 70 is fixed to the support 75 of the drone 74 through the opening 73, and is suspended from the drone 74. In this state, the opening 73 is warped upwards and the roll-formed portion 71 is open. This state is the first shape.

[0164] Next, the drone 74 is lowered so that the drone grip 70, which is stabilized in the first shape of FIG. 28, comes into contact with the article 77. Upon collision with the article 77, the central portion of the drone grip 70 is lifted and protrudes upwards, as shown on pages 14 / 23 of the specification in FIG. 29.17 CN 121646554 A It flips over like that. Thus, the drone covers the item 77 with the gripper 70, and the roll-up deformation portion 71 abuts against the lower end of the item 77 for support. Therefore, by raising the drone 74, the item 77 can be lifted.

[0165] That is, by applying the force to lift the second surface 1b to the paper sheet 2, the paper sheet 2 flips downwards, the deformation resistance of the paper sheet 2 weakens, and the tensile stress caused by the first high-hydroxyl concentration region 11 and the tensile stress caused by the second high-hydroxyl concentration region 14 are greater. The paper sheet 2 is deformed by being recessed along the first high-hydroxyl concentration region 11 towards the first surface 1a and along the second high-hydroxyl concentration region 14 towards the second surface 1b. Thus, as shown in Figures 26 and 27, the three-dimensional shape with the narrowed lower end, i.e., the second shape, is maintained and stopped. In the second shape, the tensile stress generated by the first high-hydroxyl concentration region 11, the tensile stress of the second high-hydroxyl concentration region 14, and the deformation resistance of the paper sheet 2 are balanced without further deformation. With the item 77 supported, the item 77 is clamped and compressed because of the anti-deformation force applied by the item 77.

[0166] Therefore, according to this drone gripper 70, in the first upward-curving shape shown in FIG28, by applying an upward pushing force to the central part of the second surface 1b, it changes to the second downward-narrowing shape shown in FIG29, thus achieving the function of gripping the item 77 in this process. In this way, the drone gripper 70 automatically closes and grabs the item 77 simply by the lifting and lowering action of the drone 74, so the structure of the drone 74 is not complicated, and the automatic gripping device can be realized at low cost. If the curling deformation part 71 is lifted from the state of gripping the item 77, it will curl back to the state of FIG28, so the release of the item 77 is also easy. As the item 77, various uses such as agricultural products such as fruits, medicine, mail, food in food chemical processes, etc. can be considered.

[0167] [Sixth Embodiment]

[0168] Figures 30-32 show a buffer material 80 with a honeycomb structure as a sixth embodiment of the present invention. The honeycomb structure has the advantageous structural characteristics of high porosity and light weight. The air layer in the hexagonal pores of the honeycomb structure prevents convection and also provides excellent heat buffering performance, i.e., heat insulation effect. Furthermore, in the event of an impact, energy is also dispersed to adjacent surfaces, resulting in excellent impact absorption characteristics. The buffer material of the present invention can be widely used as the core material of a sandwich structure sandwiched between two panels. Small holes can also be opened on the flat plate on one side of the sandwich structure to allow sound to resonate inside the honeycomb, thereby achieving a sound-absorbing effect. Therefore, the buffer material of the present invention can be used in various applications as a buffer material with advanced functions. In addition, in the present invention, instead of a honeycomb structure, a triangular cylindrical or quadrilateral shape can also be realized.Cylindrical, pentagonal, etc. The cushioning material of the present invention can also be used as a support for temporary landing of drones, a support for laying sensors at heights, a container for the recovery of items and abandoned items at disaster or accident sites, and a support.

[0169] Regarding the cushioning material with a honeycomb structure, the cushioning material 80, in its second shape as a mode of use, as shown in FIG32, has a three-dimensional shape having one or more openings 81, a cylindrical wall portion 82 standing around the openings 81, and a support portion 83 extending from the cylindrical wall portion 82. In the non-use state, as shown in FIGS. 30 and 31, it adopts a first shape that is flat. In the flat first shape, there is an advantage that multiple cushioning materials 80 can be stacked and stored. If expanded, items can be stored into the openings 81 of the cylindrical wall portion 82, becoming a cushioning material 80 that protects items from forces from the vertical and horizontal directions by the cylindrical wall portion 82 and the support portion 83.

[0170] As shown in Figures 30 and 31, the paper sheet 2 of the cushioning material 80 is elongated rectangular in shape, with rectangular openings 81 spaced apart from each other in the center of its width direction.

[0171] As shown in Figure 30, nine first hydroxyl high-concentration regions 11 are formed on the first surface 1a of the paper sheet 2, extending from each opening 81, by printing with water or an aqueous solution. Furthermore, as shown in Figure 31, multiple second hydroxyl high-concentration regions 14 are formed on the second surface 1b of the paper sheet 2 at the illustrated position by printing with water or an aqueous solution. Instruction manual 15 / 23 pages 18 CN 121646554 A

[0172] Specifically, as shown in FIG30, the first high hydroxyl concentration region 11 is formed as follows: a thin first high hydroxyl concentration region 11 extending from the foot of the perpendicular line along the trisection position of the long side of the opening 81 toward the long side of the paper sheet 2; a relatively thick first high hydroxyl concentration region 11 connecting the short sides of the opening 81; and a relatively thick first high hydroxyl concentration region 11 extending from the short side of the opening 81 toward the center of the short side of the paper sheet 2.

[0173] Furthermore, as shown in FIG31, the second hydroxyl high concentration region 14 includes: a thin second hydroxyl high concentration region 14 extending from both ends of the long side of the opening 81 along the foot of the perpendicular line towards the long side of the paper sheet 2; a semi-circular thin second hydroxyl high concentration region 14 arranged to surround both ends of the long side of the opening 81; and a semi-circular thin second hydroxyl high concentration region 14 arranged to surround the center of each short side of the paper sheet 2.

[0174] After the first hydroxyl high concentration region 11 and the second hydroxyl high concentration region 14 are formed by printing or the like, the cushioning material 80 is pressed into a flat shape as needed, and the cushioning material 80 is stacked and stored. If the printing is dryIf the material can remain flat after drying, stamping is not required. In this state, due to the overlap of the cushioning material 80, the tensile stress of the first high-hydroxyl concentration region 11 and the second high-hydroxyl concentration region 14 antagonizes the deformation resistance of the paper sheet 2, thus maintaining the first flat shape.

[0175] If the cushioning material 80 is removed and a mechanical stimulus, i.e., a triggering force, is applied to the cushioning material 80, the deformation resistance of the paper sheet 2 weakens, and the tensile stress caused by the first high-hydroxyl concentration region 11 and the second high-hydroxyl concentration region 14 becomes greater. The paper sheet 2 is deformed by being recessed along the first high-hydroxyl concentration region 11 toward the first surface 1a and along the second high-hydroxyl concentration region 14 toward the first surface 1a. Thus, the cushioning material 80 changes to the second shape as shown in FIG32 and stops. In the second shape, the tensile stress generated by the first high-hydroxyl concentration region 11, the tensile stress of the second high-hydroxyl concentration region 14, and the deformation resistance of the paper sheet 2 are balanced, and no further deformation occurs.

[0176] According to this cushioning material 80, in the first flat shape, it has the advantage of being able to stack and accommodate multiple cushioning materials 80. If a triggering force is applied and it deforms, an article can be accommodated into the opening 81 of the cylindrical wall portion 82, becoming a cushioning material 80 that protects the article from forces from the vertical and horizontal directions by the cylindrical wall portion 82 and the support portion 83. Therefore, a low-cost cushioning material 80 with sufficient cushioning force can be obtained. Since plastic is not used, it is also environmentally friendly.

[0177] [Seventh Embodiment]

[0178] Figures 33 to 36 show the cushioning material 90 of the seventh embodiment of the present invention. The cushioning material 90 has a structure that makes the cushioning material 80 of the sixth embodiment continuous in the width direction. In the second shape as a way of using the cushioning material 90, as shown in Figure 36, it has a three-dimensional shape having four openings 91, cylindrical wall portions 92 standing around the openings 91, and support portions 93 extending from the cylindrical wall portions 92. The cylindrical wall portions 92 are connected to each other by the support portions 93. When the cushioning material 90 is not used, as shown in Figures 33 and 34, a first flat shape is adopted. This flat first shape has the advantage of being able to accommodate multiple cushioning materials 90 stacked together. If expanded, it can accommodate articles into the openings 91 of the cylinder wall portion 92, becoming a cushioning material 90 that protects the articles from forces from the vertical and horizontal directions by the cylinder wall portion 92 and the support portion 93.

[0179] As shown in Figures 33 and 34, the paper-containing sheet 2 of the cushioning material 90 is rectangular, and rectangular openings 91 are formed in three rows spaced apart from each other.

[0180] As shown in Figure 33, on the first surface 1a of the paper-containing sheet 2, a first high-hydroxyl region 11 is formed by printing with water or an aqueous solution, etc., extending from each opening 91. Furthermore, as shown in Figure 34, on the second surface 1b of the paper-containing sheet 2, in…The illustrated position has multiple second hydroxyl high concentration regions 14 formed by printing with water or aqueous solution, etc.

[0181] Specifically, as shown in FIG33, as the first hydroxyl high concentration region 11, there are: a thin first hydroxyl high concentration region 11 extending from the trisection of the long side of the opening 91, a relatively thick first hydroxyl high concentration region 11 connecting the short sides of the opening 91, a relatively thick first hydroxyl high concentration region 11 extending from the short side of the opening 91 toward the center of the short side of the paper sheet 2, and a semi-circular first hydroxyl high concentration region 11 arranged in a manner that surrounds the short side of the opening 91 in the center.

[0182] Furthermore, as shown in FIG34, the second hydroxyl high concentration region 14 includes: a thin second hydroxyl high concentration region 14 extending from both ends of the long side of the opening 91 toward the foot of the vertical line of the long side of the paper sheet 2; a semi-circular thin second hydroxyl high concentration region 14 arranged to surround both ends of the long side of the opening 91 on both sides; and a semi-circular thin second hydroxyl high concentration region 14 having a center on each short side of the paper sheet 2.

[0183] After the first hydroxyl high concentration region 11 and the second hydroxyl high concentration region 14 are formed by printing or the like, the paper sheet 2 is formed into a flat plate shape by stamping or the like as needed, and the cushioning material 90 is stacked and stored. If it can remain flat after printing and drying, stamping is not required. In this state, since the cushioning material 90 is stacked, the tensile stress of the first hydroxyl high concentration region 11 and the second hydroxyl high concentration region 14 antagonizes the deformation resistance of the paper sheet 2 and maintains the first flat shape.

[0184] If the cushioning material 90 is removed and a mechanical stimulus, i.e., a triggering force, is applied to the cushioning material 90, the deformation resistance of the paper sheet 2 weakens, and the tensile stress caused by the first high-hydroxyl concentration region 11 and the second high-hydroxyl concentration region 14 becomes greater. The paper sheet 2 deforms by indenting along the first high-hydroxyl concentration region 11 towards the first surface 1a and along the second high-hydroxyl concentration region 14 towards the first surface 1a. Thus, the cushioning material 90 changes to the second shape as shown in Figures 35 and 36 and stops. In the second shape, the tensile stress generated by the first high-hydroxyl concentration region 11, the tensile stress of the second high-hydroxyl concentration region 14, and the deformation resistance of the paper sheet 2 are balanced, and no further deformation occurs.

[0185] According to this cushioning material 90, in its flat first shape, it has the advantage of being able to stack and accommodate multiple cushioning materials 90. If it deforms when a triggering force is applied, it can accommodate articles into the openings 91 of multiple cylindrical wall portions 92, becoming a cushioning material 90 that protects articles from forces from the vertical and horizontal directions by the cylindrical wall portions 92 and the support portions 93. Therefore, it is possible to obtain low...A cushioning material 90 that is cost-effective and has sufficient cushioning force. Since it does not use plastic, it is also environmentally friendly.

[0186] [Eighth Embodiment]

[0187] Figures 37-39 show the cushioning material 100 according to the eighth embodiment of the present invention. In a second shape as a mode of use of this cushioning material 100, as shown in Figure 39, it has a three-dimensional shape having interleaved square openings 101 and undulations 102 connecting the openings 101 to each other. The undulations 102 have alternating upper and lower fold lines. In the state where the cushioning material 100 is not used, as shown in Figures 38 and 39, it adopts a first shape that is flat. In the flat first shape, there is an advantage that multiple cushioning materials 100 can be stacked and accommodated. If expanded, items can be accommodated in the valleys of the undulations 102, becoming a cushioning material 100 that protects items from forces from the vertical and horizontal directions.

[0188] As shown in FIG. 37, a first high-hydroxyl concentration region 11 is formed on the first surface 1a of the paper sheet 2 by printing with water or an aqueous solution, extending from each opening 101. Additionally, as shown in FIG. 38, a plurality of second high-hydroxyl concentration regions 14 are formed on the second surface 1b of the paper sheet 2 by printing with water or an aqueous solution at the illustrated position. The first high-hydroxyl concentration regions 11 and the second high-hydroxyl concentration regions 14 form a so-called Miura fold pattern.

[0189] After the first high-hydroxyl concentration regions 11 and the second high-hydroxyl concentration regions 14 are formed by printing, the cushioning material 100 is pressed into a flat shape by stamping, and the cushioning material 100 is stacked and stored. In this state, because the cushioning materials 100 are stacked, the tensile stress of the first high-hydroxyl concentration regions 11 and the second high-hydroxyl concentration regions 14 antagonizes the deformation resistance of the paper sheet 2, maintaining the flat first shape.

[0190] If the cushioning material 100 is removed and a mechanical stimulus, i.e., a triggering force, is applied to the cushioning material 100, the deformation resistance of the paper sheet 2 is weakened, while the tensile stress caused by the first high-hydroxyl concentration region 11 and the tensile stress caused by the second high-hydroxyl concentration region 14 are greater. The paper sheet 2 is deformed by being recessed along the first high-hydroxyl concentration region 11 toward the first surface 1a and along the second high-hydroxyl concentration region 14 toward the first surface 1a. Thus, as shown in FIG39, the cushioning material 100 changes to a second shape with a Miura folding structure and stops. In the second shape, the tensile stress generated by the first high-hydroxyl concentration region 11, the tensile stress of the second high-hydroxyl concentration region 14, and the deformation resistance of the paper sheet 2 are balanced, and no further deformation occurs.

[0191] According to this cushioning material 100, in the first flat shape, multiple cushioning materials can be stacked and accommodated.The advantage of 100 is that if a triggering force is applied and it deforms, it can accommodate items in the valley between the undulating portions 102, becoming a cushioning material 100 that protects the items from forces from the vertical and horizontal directions, as well as the cylindrical wall portion 102 and the support portion 103. Therefore, a low-cost cushioning material 100 with sufficient cushioning force can be obtained. Since plastic is not used, it is also environmentally friendly.

[0192] FIG40 shows an embodiment that further extends the Miura folding structure. As another pattern, as shown in FIG41, it can also be a so-called egg carton shape.

[0193] [Ninth Embodiment]

[0194] FIG42 is a cross-sectional enlarged view showing a ninth embodiment of the paper-containing structure 1 of the present invention. In this ninth embodiment, the characteristic is that a protective film 104 is fixed to the first surface 1a and the second surface 1b of the paper-containing sheet 2, which has a first hydroxyl high concentration region 11 and a second hydroxyl high concentration region 14 formed in various patterns, respectively, via an adhesive layer 103. The paper-containing sheet 2 can be any of the paper-containing sheet 2 described in this application specification.

[0195] By sandwiching the paper sheet 2 with the protective film 104 in this way, even if the paper structure 1 is placed in a humid or high-humidity position, unwanted moisture will not penetrate into the paper sheet 2, and the deformability of the paper sheet 2 based on the first high-hydroxyl concentration region 11 and the second high-hydroxyl concentration region 14 can be maintained. In addition, when holding items with high moisture content such as fruits by the paper structure 1, the effect of preventing the paper structure 1 from absorbing moisture from the items can also be obtained. Therefore, the water content of fruits, etc. can be maintained. Furthermore, by covering the surface with the protective film 104, the coefficient of friction of the surface in contact with fruits, etc., increases, thereby improving the stability of the items in the storage state.

[0196] As the protective film 104, various plastics with excellent moisture resistance are preferred, and the material is not limited. Examples include linear short-chain branched polyethylene (LLDPE), low-density polyethylene (LDPE) and other polyethylene, unstretched polypropylene (CPP) and other polyolefin resins, polyvinyl acetate resins, polyvinyl chloride resins, poly(meth)acrylic acid resins, polyurethane resins and other resins. The thickness of the protective film 104 is not limited, but in order to maintain adequate moisture resistance and not hinder the deformation of the paper sheet 2, it is preferably 0.001 μm or more and 10,000 μm or less, more preferably 0.01 μm or more and 100 μm or less. Furthermore, from the viewpoint that the protective film 104 should not hinder the deformation of the paper sheet 2 as much as possible, the thickness of the paper sheet 2 can be 0.01 μm or more and 10,000 μm or less, more preferably 1 μm or more and 1,000 μm or less, and the thickness of the protective film 104 can be approximately 0.001% or more and 1,000% or less of the thickness of the paper sheet 2, more preferably approximately 1% or more and 100% or less.

[0197] As the adhesive layer 103, for example, single-component or two-component cured or non-cured vinyl adhesive layers, (meth)acrylic adhesive layers, polyamide adhesive layers, polyester adhesive layers, polyether adhesive layers, polyurethane adhesive layers, epoxy adhesive layers, rubber adhesive layers, other solvent-based adhesive layers, water-based adhesive layers, emulsion adhesive layers, and other adhesives can be used. In the case of dry lamination, the adhesive diluted with an organic solvent is applied to the protective film 104, and after drying, it is pressed and bonded to a pair of protective films 104 through a paper sheet 2 with a first high-hydroxyl concentration region 11 and a second high-hydroxyl concentration region 14 pre-formed using heated rollers.

[0198] Alternatively, in the paper-containing structure 1, as shown in FIG42, the ends of the protective films 104 on both sides may extend on the end faces of the paper-containing sheet 2 to form end-face protective films 105, and the end faces of the paper-containing sheet 2 may be airtightly sealed by the plastic constituting the protective films 104. For the paper-containing structure 1 in which the protective films 104 are attached to both sides of the paper-containing sheet 2 via adhesive layers 103, if the paper-containing structure 1 is cut by irradiating a laser beam using a laser cutter or the like, the protective films 104 (and adhesive layers 103) melt at high temperature and flow along the end face of the paper-containing sheet (page 18 / 23 of the specification, CN 121646554 A 2), forming an end-face protective film 105 that airtightly covers the end faces of the paper-containing sheet 2, thus easily forming the end-face sealing structure of FIG42. However, the paper-containing structure 1 of the ninth embodiment may also have a structure without end-face protective films 105.

[0199] [Tenth Embodiment]

[0200] In the ninth embodiment, a protective film 104 is provided on both sides of the paper sheet 2, but as shown in FIG. 43, the protective film 104 may also be provided only on one side of the paper sheet 2 via the adhesive layer 103. In applications such as applying water droplets only to one side of the paper sheet 2, it is not a problem even if the second side 1b of the paper sheet 2 is exposed.

[0201] In addition, in the ninth and tenth embodiments, instead of providing the protective film 104 on the entire surface of the paper sheet 2, the protective film 104 may be formed only in necessary locations in a certain pattern via the adhesive layer 103. Necessary locations refer to locations that come into contact with water or other liquids, locations that come into contact with items with high water content such as fruits, etc.

[0202] Furthermore, if the material of the protective film 104 is suitable, the adhesive layer 103 may not be provided, and the protective film 104 may be directly heated and softened and then heat-sealed onto the paper sheet 2.

[0203] [Eleventh Embodiment]

[0204] FIG44 is an enlarged cross-sectional view showing the eleventh embodiment of the present invention. In this eleventh embodiment, a protective film 104 is adhered to both sides of the paper sheet 2, on which the first hydroxyl high concentration region 11 and the second hydroxyl high concentration region 14 are pre-formed, via an adhesive layer 103. Then, the protective film 104 on one side is further adhered to the entire surface via an adhesive layer 106.Nonwoven fabric 107. A pair of protective films 104 protect the paper sheet 2 from moisture, maintain the deformability of the paper sheet 2, and make the contact surface with the article soft through the nonwoven fabric 107, thereby achieving the protection of the article and the absorption of excess moisture from the article. The nonwoven fabric 107 can be formed with a certain pattern according to the purpose.

[0205] [Twelfth Embodiment]

[0206] FIG45 is an enlarged cross-sectional view showing the twelfth embodiment of the present invention. In this twelfth embodiment, the structure is as follows: a protective film 104 is attached to both sides of the paper sheet 2, on which a first hydroxyl high concentration region 11 and a second hydroxyl high concentration region 14 are pre-formed, via an adhesive layer 103, and then a circuit layer 108 is provided on one side of the protective film 104, and covered thereon by a protective film 109.

[0207] The circuit layer 108 may have a circuit composed of a metal thin film with high conductivity such as copper or aluminum and arranged in a certain pattern, sensors, resistors, capacitors, integrated circuits, coils, antennas, etc. disposed on the circuit, and combined with the deformability of the paper sheet 2, it performs necessary functions such as sensing, signal processing, and communication.

[0208] [Thirteenth Embodiment]

[0209] FIG46 is a top view showing the sensing pad 110 as the twelfth embodiment of the present invention. The sensing pad 110 has a three-dimensional shape suitable for a specific part of a living organism such as a human or animal and a plurality of sensors 111, which perform the following functions: detecting electrical signals, temperature, conductivity, specific substance concentrations, etc. of the living organism through the sensors 111 and processing the signals, and transmitting them to the outside through the cable 112. A protective film 104 may be formed on both sides of the paper sheet 2 via an adhesive layer 103, or it may be a type without a protective film 104.

[0210] The shape of the sensing pad 110 is not limited. The example shown is cross-shaped. A first high-hydroxyl concentration region 11, which is V-shaped when viewed from above, is formed towards the center of the front end of the four extensions extending from the center. A second high-hydroxyl concentration region 14 is formed that crosses the first high-hydroxyl concentration region 11 at the root of the extension. Through the action of these first high-hydroxyl concentration regions 11 and second high-hydroxyl concentration regions 14, if a triggering force is applied, the sensing pad 110 can deform in such a way that the back surface becomes a gently concave surface, for example, it can be placed with the human head 113 with approximately no gap. A plurality of sensors 111 are arranged on the back of the sensing pad 110 and connected to a central cable 112 via electronic circuitry (not shown). If the sensing pad 110 is placed along the curved surface of the head 113, all the sensors 111 will abut against the surface of the head 113, detect electrical signals, and send them out through the cable 112. Therefore, it is possible to detect electrical signals at multiple points on the head 113, for example, for brain diagnosis and analysis.

[0211] [Thirteenth Embodiment]

[0212] Figures 48 and 49 are a top view and a cross-sectional view showing a partially cutaway absorbent pad 120 used as a sanitary napkin or the like according to the thirteenth embodiment of the present invention. As shown in Figure 48, the absorbent pad 120 is, for example, a rectangular shape with rounded corners. As shown in Figure 49, it has a support body 122 containing a paper sheet 2 and absorbent layers 121 covering both sides of the support body 122. Their outer peripheries are pressed and fixed to form a sealing portion 123. In the paper sheet 2, in the areas other than the sealing portion 123, a first high-hydroxyl concentration region 11, a second high-hydroxyl concentration region 14, and an opening 101 are formed in a grid pattern as shown in Figure 37, for which the description refers to Figure 37.

[0213] The absorbent pad 120 is stacked and housed in a housing (not shown). When it is taken out of the housing, the release of compression becomes a triggering force that causes the first high-hydroxyl concentration region 11 and the second high-hydroxyl concentration region 14 to bend, and as shown in Figure 49, the cross-sectional shape becomes a sawtooth shape. As a result, the pair of absorbent layers 121 expand and swell, thereby not only increasing the absorbable capacity of menstrual blood and other liquids and preventing leakage, but also reducing discomfort such as the absorbent layers 121 being too close to the skin due to the unevenness of the support 122.

[0214] [Fourteenth Embodiment]

[0215] FIG50 is a top view showing a conical structure 124 as the fourteenth embodiment of the present invention. The conical structure 124 has a square-shaped paper sheet 2 with a circular central hole 125 formed in the center. On the upper surface of the paper sheet 2, a first hydroxyl high concentration region 11 is formed radially from the central hole 125 at equal intervals at fixed angles. In addition, a weakening line 126 extending radially from the outer periphery to the central hole 125 is formed on a part of the paper sheet 2, which can be easily torn by hand along the weakening line 126. In this fourteenth embodiment, a second hydroxyl high concentration region 14 is not required.

[0216] According to this conical structure 124, if the weakening line 126 is cut, it becomes a trigger force. Through the stress generated by the first high hydroxyl concentration region 11, the conical structure 124 deforms into a conical shape with the central hole 125 as the apex. Figures 51 and 52 show photographs of the actual fabrication of the conical structure 124 shown in Figure 50. Figure 51 shows the state before the weakening line 126 is cut, and Figure 52 shows the state after the weakening line 126 is cut and deformed into a conical shape. As shown in Figure 42 or Figure 43, the paper sheet 2 preferably has a protective film 104 adhered to at least its upper surface via the adhesive layer 103. The conical structure 124 can also be used as tableware or containers, etc., as long as the tip is facing down and food, containers, etc. are placed in the recess. Alternatively, the tip can be facing up and covering an item as a protective cover, etc.

[0217] In addition, in the examples shown in Figures 51 and 52, a square with a thickness of 153 μm and a length and width of 200 mm is used.The tracing paper is used as the paper sheet 2, and a circular hole with a diameter of 10 mm is formed as the center hole 125. Pure water is used to print a pattern of a first high hydroxyl concentration region 11 with a width of 0.95 mm and a length of 70 mm that is formed radially at an angle of 6° around the center hole 125. About 2 minutes after printing, a protective film 104 made of polyethylene with a thickness of 10 μm is applied to both sides of the paper sheet 2 using an adhesive layer 103 formed by spraying with "3M Spray 55" (3M company trade name) to form a conical structure 124. It can be confirmed that the conical structure 124 is actually deformed into a conical shape.

[0218] [Fifteenth Embodiment]

[0219] FIG53 is a top view showing the catalyst unit 127 as the fifteenth embodiment of the present invention. The catalyst unit 127 has a cylindrical catalyst container 128, a paper sheet 2 disposed in the catalyst container 128, and a catalyst layer 131 fixed to both sides of the paper sheet 2. The catalyst container 128 narrows at both ends in a tapered shape, becoming an inlet 129 and an outlet 130 connected to the outside.

[0220] The paper sheet 2 is a relatively long rectangle, with a first high-hydroxyl concentration region 11, a second high-hydroxyl concentration region 14, and an opening 101 formed in a grid pattern as shown in FIG37, for which FIG37 is referenced. The long paper sheet 2, with catalyst layers 131 fixed on both sides, is rolled into a spiral to form a cylinder, which is then sealed inside the catalyst container 128. Gaps are formed between the layers of the paper sheet 2, and the cross-sectional shape of the paper sheet 2 is serrated, thus allowing the fluid to flow in a zigzag pattern within the gaps, improving the contact efficiency with the catalyst layer 131.

[0221] [Sixteenth Embodiment]

[0222] Figures 54 and 55 are photographs of a cushioning material 100 for arranging small fruits or foods such as strawberries or cherries in a box, before and after deformation, according to the sixteenth embodiment of the present invention. The paper sheet 2 of the cushioning material 100 does not have an adhesive layer 103 or a protective film 104 formed. A first high-hydroxyl concentration region 11 is formed on the surface of the paper sheet 2, and a second high-hydroxyl concentration region 14 with a grid pattern as shown in Figure 37 is formed on the back side, with rectangular openings 101 formed at the intersections of the grid. The paper sheet 2 has dimensions of 420 mm x 297 mm and a thickness of 123 μm, and is formed from tracing paper. The distance between the centers of the openings 101 of the first high-hydroxyl concentration region 11 and the second high-hydroxyl concentration region 14 is 51 mm. The width of the first high-hydroxyl concentration region 11 and the second high-hydroxyl concentration region 14 is 15 mm, formed by printing pure water using an inkjet printer. Figure 54 is a photograph of the printed state, and Figure 55 is a photograph of the state of the cushioning material 100 being compressed from all sides (the state of applying trigger force).

[0223] [Seventeenth Embodiment]

[0224] Figures 56 and 57 are photographs showing a cushioning material 133 with a protective film, formed as the seventeenth embodiment of the present invention, in which a protective film 104 is adhered to both sides of a paper sheet 2 formed in the same manner as in the sixteenth embodiment, and then an opening 101 is formed. The shape of the cushioning material 133 with the protective film, the printing pattern of the first high-hydroxyl concentration region 11 and the second high-hydroxyl concentration region 14, and the size and arrangement of the opening 101 are the same as those of the cushioning material 100, except that the adhesive layer 103 and the protective film 104 are formed on both sides of the paper sheet 2. Furthermore, no opening 101 is formed in the adhesive layer 103 and the protective film 104. It is manufactured as follows. After printing pure water on the paper sheet 2 using an inkjet printer, about 10 minutes later, a protective film 104 made of polyethylene with a thickness of about 10 μm is pasted on both sides of the paper sheet 2 using an adhesive layer 103 formed by spraying a commercially available spray adhesive (3M product name: 3M Spray Adhesive 55). The blank part is cut off with a laser cutter, and the end face of the protective film 104 is melted to form an end face protective film 105, sealing the cross-section of the paper sheet 2. The protective film 104 is further heated at 90°C for 5 minutes with an electric heater, so that the protective film 104 deforms according to the thermoplasticity of the paper sheet 2. It is then adjusted and bent by hand to obtain a cushioning material 133 with a protective film.

[0225] Figure 56 is a photograph of the state after the protective film 104 is pasted, and Figure 57 is a photograph of the state of the cushioning material 133 with the protective film compressed from all sides (the state of applying trigger force). A comparison of Figures 55 and 57 shows that when the protective film 104 is fixed to both sides of the cushioning material 133 with the protective film using the adhesive layer 103, the same deformation occurs as in the cushioning material 100 without the protective film 104.

[0226] Figure 58 is a photograph of the cushioning material 133 with the protective film of Figure 57 compressed and placed in a strawberry packaging box (117mm x 210mm x 50mm), with strawberries placed in the central recess (bag). The cushioning material 133 with the protective film, which has a complex three-dimensional shape, can be easily manufactured by inkjet printing, and a moisture-proof protective film 104 is formed on the cushioning material 133, thus allowing the strawberries to be preserved with good flavor for a long time.

[0227] [Moisture Absorption Experiment]

[0228] Samples were taken from the cushioning material 100 of the sixteenth embodiment without a protective film 104 formed on the paper sheet 2 and the cushioning material 133 of the seventeenth embodiment with a protective film 104 formed on it. The difference in moisture absorption of the samples was investigated. The surface area (one side) of the cut samples was 150 cm2. The lids of the two airtight containers with an internal volume of 430 cm3 were opened. (See page 21 / 23 of the instruction manual, CN 121646554 A)The samples were placed in an environment with constant temperature and humidity. The temperature was set to room temperature. The constant humidity environment was conditioned using a saturated salt method with high humidity NaCl, with a relative humidity of approximately 75%. After the temperature and humidity stabilized, each sample and the humidity sensor were sealed together in an airtight container, and the humidity of the humidity sensor was measured over time. The results are shown in Figure 60.

[0229] As shown in Figure 60, in the sample of the sixteenth embodiment without the protective film 104, the relative humidity decreased to approximately 60% after approximately 1000 seconds. In contrast, in the sample of the seventeenth embodiment with the protective film 104, the relative humidity was approximately 73% after approximately 1000 seconds, which was approximately constant. It can be seen that the protective film 104 can prevent the paper sheet 2 from absorbing moisture.

[0230] The embodiments of the present invention have been described above, but the present invention is not limited to the above embodiments. The structural elements of the above embodiments can be combined with each other, and other known structures can also be combined.

[0231] For example, in addition to the embodiments described above, from the viewpoint of maintaining an appropriate distance from the object through deformation of the paper sheet 2, the present invention can also be applied to skin care products (cosmetics), electrostatic adhesive pads, wristbands, tourniquets, etc. From the viewpoint of increasing surface area, in addition to catalyst units, it can also be applied to filters, etc. From the viewpoint of imparting a curved shape, it can be applied to filters, speakers, ultrasonic components, displays, hats, helmets, shoe insoles, etc. From the viewpoint of compactness through deformation, it can be applied to space shelters, furniture, tableware, parachutes, etc. From the viewpoint of changes in optical properties brought about by deformation, it can be applied to the construction of windows and walls that prevent peeping. From the viewpoint of cushioning function, it can be applied to helmets, protectors for drone equipment, propellers, etc. From the viewpoint of changes in heat insulation and heat resistance effects caused by deformation, it can be applied to beverage sleeves, etc. Based on the pop-out effect caused by deformation, it can be applied to picture books. From the viewpoint of folding, it can be applied to stickers, labels, office equipment, etc.

[0232] Industrial Applicability

[0233] According to the present invention, by applying a triggering force to a portion of a paper-containing structure having a first high-hydroxyl concentration region and a second high-hydroxyl concentration region, the antagonistic balance between tensile stress and resistance to deformation within the paper-containing structure changes, switching between a first shape and a second shape in at least one direction. Through this switching action, various functions can be achieved, thus enabling industrial application.

[0234] Explanation of Reference Numerals

[0235] 1 Paper-containing structure

[0236] 1a First surface

[0237] 1b Second surface

[0238] 2 Paper-containing sheet

[0239] 5 Upper fold line

[0240] 6 Lower fold line

[0241] 9 Water

[0242] 11 First high-hydroxyl concentration region

[0243] 14 Second high-hydroxyl concentration region

[0244] 20, 30, 40, 50, 60, 70, 80, 90, 100 Paper-containing structure

[0245] 22 Weakening line

[0246] 61 Opening

[0247] 62 Annular protrusion

[0248] 70 UAV grip

[0249] 71 Roll deformation part

[0250] 73 Opening instruction manual 22 / 23 pages 25 CN 121646554 A

[0251] 74 UAV

[0252] 75 Support

[0253] 77 Article

[0254] 80 Cushioning material

[0255] 81 Opening

[0256] 82 Cylinder wall part

[0257] 83 Support part

[0258] 90 Cushioning material

[0259] 91 92. Opening

[0260] 93. Cylinder Wall

[0261] 94. Support

[0262] 105. Buffer Material

[0263] 106. Opening

[0264] 107. Undulated Section

[0265] 108. Adhesive Layer

[0266] 109. Protective Film

[0267] 100. End Face Protective Film

[0268] 101. Adhesive Layer

[0269] 102. Non-woven Fabric

[0270] 103. Circuit Layer

[0271] 104. Protective Film

[0272] 110. Sensing Pad

[0273] 111. Sensor

[0274] 112. Cable

[0275] 113. Head

[0276] 120. Absorbent Pad

[0277] 121. Absorbent Layer

[0278] 122 Support body

[0279] 123 Sealing part

[0280] 124 Conical structure

[0281] 125 Central hole

[0282] 126 Weakening line

[0283] 127 Catalyst unit

[0284] 128 Catalyst container

[0285] 129 Inlet part

[0286] 130 Outlet part

[0287] 131 Catalyst layer

[0288] 132 Passage

[0289] 133 Buffer material with protective film Specification 23 / 23 pages 26 CN 121646554 A Figure 1A Figure 1B Figure 1C Figure 2 Specification drawing 1 / 42 pages 27 CN 121646554 A Figure 3 Figure 4A Figure 4B Specification drawing 2 / 42 pages 28 CN 121646554 A Figure 5 Instruction manual, Figure 6 (page 3 / 42, CN 121646554 A), Figure 7 (page 30, CN 121646554 A), Figure 8 (page 31, CN 121646554 A). Description.Figure 9 of the instruction manual, page 32 of page 6 / 42, CN 121646554 A; Figure 10 of the instruction manual, page 33 of page 7 / 42, CN 121646554 A; Figure 11 of the instruction manual, page 34 of page 8 / 42, CN 121646554 A; Figure 12 of the instruction manual, page 13 of page 9 / 42, CN 121646554 A; Figure 14 of the instruction manual, page 15 of page 10 / 42, CN 121646554 A; Figure 16 of the instruction manual, CN 121646554 A; Figure 17A of the instruction manual, page 17B; Figure 18 of the instruction manual, page 37 of page 11 / 42, CN 121646554 A; Figure 19 of the instruction manual, page 38 of page 12 / 42, CN 121646554 A; Figure 20 of the instruction manual, page 39 of page 13 / 42, CN 121646554 A; Figure 21 of the instruction manual, page 40 of page 14 / 42, CN 121646554 A. Figure 15 / 42, page 41, CN 121646554 A, Figure 22, Figure 23; Figure 16 / 42, page 42, CN 121646554 A, Figure 24; Figure 17 / 42, page 43, CN 121646554 A, Figure 25; Figure 18 / 42, page 44, CN 121646554 A, Figure 26; Figure 19 / 42, page 45, CN 121646554 A, Figure 27; Figure 20 / 42, page 46, CN 121646554 A, Figure 28; Figure 21 / 42, page 47, CN 121646554 A, Figure 29; Figure 22 / 42, page 48, CN 121646554 A, Figure 30; Figure 23 / 42, page 49, CN 121646554 A, Figure 31; Figure 24 / 42 Page 50 CN 121646554 A Figure 32 Description drawing 25 / 42 Page 51 CN 121646554 A Figure 33 Description drawing 26 / 42 Page 52 CN 121646554 A Figure 34 Description drawing 27 / 42 Page 53 CN 121646554 A Figure 35 Figure 36 Description drawing 28 / 42 Page 54 CN 121646554 A Figure 37 Description drawing 29 / 42 Page 55 CN 121646554 A Figure 38 Description drawing 30 / 4256 CN 121646554 A Figure 39 Figure 40 Appendix to the Specification Page 31 / 42 57 CN 121646554 A Figure 41 Figure 42 Figure 43 Appendix to the Specification Page 32 / 42 58 CN 121646554 A Figure 44 Figure 45 Appendix to the Specification Page 33 / 42 59 CN 121646554 A Figure 46 Figure 47 Appendix to the Specification Page 34 / 42 60 CN 121646554 A Figure 48 Figure 49 Appendix to the Specification Page 35 / 42 61 CN 121646554 A Figure 50 Figure 51 Appendix to the Specification Page 36 / 42 62 CN 121646554 A Figure 52 Appendix to the Specification Page 37 / 42 63 CN 121646554 A Figure 53 Appendix to the Specification Page 38 / 42 64 CN 121646554 A Figure 54 Figure 55 Appendix to the Instruction Manual, Page 39 / 42, 65 CN 121646554 A Figure 56 Figure 57 Appendix to the Instruction Manual, Page 40 / 42, 66 CN 121646554 A Figure 58 Appendix to the Instruction Manual, Page 41 / 42, 67 CN 121646554 A Figure 59 Figure 60 Appendix to the Instruction Manual, Page 42 / 42, 68 CN 121646554 A

Claims

1. A paper-containing structure, characterized in that, formed of a paper-containing sheet in a dry state including paper, the paper-containing sheet has a first face and a second face which mutually form surface back faces, a first hydroxyl high concentration region in which the density of hydroxyl groups is higher than other parts of the first face is formed on the first face, a second hydroxyl high concentration region in which the density of hydroxyl groups is higher than other parts of the second face is formed on the second face, tensile stress is respectively generated in the first hydroxyl high concentration region and the second hydroxyl high concentration region, the tensile stress of the first hydroxyl high concentration region of the first face and the tensile stress of the second hydroxyl high concentration region of the second face are balanced with the deformation resistance of the paper-containing sheet when the paper-containing structure is in a first shape to form a first stable state, and are able to maintain the first shape, and also are balanced with the deformation resistance of the paper-containing sheet when the paper-containing structure is in a second shape to form a second stable state, and are able to maintain the second shape, the first shape and the second shape are switched to at least one direction by applying a trigger force to a part of the paper-containing structure.

2. The paper-containing structure according to claim 1, wherein In the first and second high-hydroxyl concentration regions, the transmittance of infrared light is lower than in the other regions when the infrared absorption spectrum of the surface portion of the paper-containing structure is measured by total reflection measurement using infrared light of a wave number of 3331 cm -1 -1.

3. The paper-containing structure according to claim 1 or 2, wherein one or more notched portions through which the first stable state and the second stable state can be formed are formed on the paper-containing sheet.

4. The paper-containing structure according to claim 1 or 2, wherein the trigger force is generated by penetration of water into the paper-containing structure, change in humidity of an environment in which the paper-containing structure is placed, local compression of the paper-containing structure, heating of the paper-containing structure, cooling of the paper-containing structure, cutting of a part of the paper-containing structure, or application of an external force to the paper-containing structure.

5. The paper-containing structure according to claim 1 or 2, wherein the first shape and the second shape are bidirectionally switched by applying the trigger force to a part of the paper-containing structure.

6. A holding member characterized by comprising: a paper-containing structure according to claim 1 or 2 is used for holding an article, the first shape is an article release shape in which end portions are opened, the second shape is an article holding shape in which the end portions are narrowed, the trigger force is generated by collision of the holding member with an article or contact of the holding member with a support surface on which an article is supported, whereby the paper-containing structure changes from the article release shape to the article holding shape to hold the article.

7. A holding member for a drone, characterized by a holding member according to claim 6 has a fixing portion in a central portion of the holding member which is fixed to a support portion of a drone.

8. A cushioning material characterized by, a paper-containing structure according to claim 1 or 2 is used for arranging one or more articles therein, the paper-containing structure has a paper folding structure, the first shape is a reduced shape in which the paper-containing structure is folded without having a bag or a flat shape in which the paper-containing structure is unfolded, the second shape is an unfolded shape in which the paper-containing structure is unfolded to form one or more bags, the change from the reduced shape or the flat shape to the unfolded shape is made by applying a trigger force to a part of the paper-containing structure.

9. A paper folding device, characterized by a paper-containing structure according to claim 1 or 2 and at least one of an electronic element and a wiring provided to at least one of the first face and the second face of the paper-containing structure.

10. A cushioning material characterized by, The paper-containing structure according to claim 1 or 2, for arranging one or a plurality of articles therein, The paper-containing structure has a paper-folding structure, The first shape is a reduced shape in which the paper-containing structure is folded without having a bag, or a flat shape in which the paper-containing structure is unfolded, The second shape is an unfolded shape in which the paper-containing structure is unfolded to have one or a plurality of bags, The change from the reduced shape or the flat shape to the unfolded shape is made by applying a trigger force to a portion of the paper-containing structure.

11. A cushioning material characterized by, The paper-containing structure according to claim 1 or 2, The paper-containing structure has one or a plurality of opening portions and the first and second high-hydroxyl regions arranged around the opening portions, The first shape is a flat shape in which the paper-containing structure is unfolded, The second shape is a three-dimensional shape in which the paper-containing structure has a cylindrical wall portion that stands around a periphery of the opening portion and a support portion that extends from the cylindrical wall portion, The change from the flat shape to the three-dimensional shape is made by applying a trigger force to a portion of the paper-containing structure.

12. A method for manufacturing a paper-containing structure, which manufactures the paper-containing structure according to claim 1 or 2, characterized by, The process has the following steps: A liquid containing water is applied to portions of the first and second faces of the paper-containing sheet that are to form the first and second high-hydroxyl regions; and The liquid is dried.

13. The paper-containing structure according to claim 1 or 2, wherein A protective film having flexibility is attached to at least a portion of at least one of the first and second faces of the paper-containing sheet.

14. The paper-containing structure according to claim 1 or 2, wherein Protective films having flexibility are attached to the first and second faces of the paper-containing sheet, respectively.