Transition metal doped sodium manganese oxide, a process for its synthesis, and fabrication to anode

IN595231BActive Publication Date: 2026-07-13INDIAN INSTITUTE OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
IN202411083060
Authority / Receiving Office
IN · IN
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-10-30
Publication Date
2026-07-13
Estimated Expiration
2044-10-30

AI Technical Summary

Technical Problem

Existing anode materials for lithium-ion and sodium-ion batteries face challenges such as dendrite formation, safety concerns, low capacity, and structural instability due to Jahn-Teller distortion, limiting their performance and cycle life.

Method used

Transition metal-doped sodium manganese oxides (TMD-NMO) with a layered morphology are synthesized using a solid-state process, incorporating dopants like Co, Ni, Fe, Cr, Cu, Ti, Mo, Zr, and Nb to enhance electronic conductivity and stabilize the structure, fabricated into anodes with a specific composition and morphology.

Benefits of technology

The TMD-NMO anodes exhibit high specific capacity, excellent cycling stability, and long cycle life, delivering over 300 mAh/g at 3C rate with coulombic efficiency above 95%, suitable for next-generation batteries.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Please see the attached
Need to check novelty before this filing date? Find Prior Art

Description

FIELD

[001] The present disclosure pertains to transition metal doped sodium manganese oxide(TMD-NMO) and a process for its synthesis and fabrication to anode. The present disclosurealso provides lithium and sodium-ion batteries comprising the said anode.BACKGROUND

[002] The growing demand for limited non-renewable resources, coupled with advancementsin electric automobiles and portable electronics, has significantly increased interest inrechargeable batteries. Among these, lithium-ion batteries (LIBs) and sodium-ion batteries(SIBs) are particularly notable due to their similar cell chemistries, aside from the mobility oftheir host ions.

[003] Anode materials play a critical role in the performance of LIBs and SIBs, affectingvarious aspects such as energy density, power density, cycle life, safety, and overall efficiency.Therefore, the choice of anode material significantly influences the performance characteristicsof both lithium-ion and sodium-ion batteries. Improvements in anode materials can lead toenhancement in overall effectiveness of the battery, making them a key focus of ongoingresearch and development in battery technology.

[004] In commercial LIBs, graphite is a well-known anode material, but it faces severalchallenges such as dendrite formation, safety concerns, and high polarization during cycling.Hard carbon has been found to be suitable for SIBs but suffers with bottlenecks like poor initialcoulombic efficiency and low discharge plateau leading to safety issues, dendrite formation,etc. Silicon offers a significantly higher theoretical capacity (around 4200 mAh / g) comparedto graphite. However, it suffers from large volume expansion and contraction during cycling,leading to mechanical degradation and capacity loss. Other anodes in SIBs like Na2Ti3O7encounter issues related to poor rate capability and sluggish diffusion kinetics during thesodiation / de-sodiation process, mainly due to the larger size of sodium ions compared tolithium ions (1.02 (Aring) for Na+ and 0.67 (Aring) for Li+).

[005] Durability of the anode plays a key role in influencing rate performance, stabilizing thesolid-electrolyte interface (SEI) layer, and affecting the initial coulombic efficiency (ICE).Achieving high energy density comparable to LIB based anode remains a challenge. As aresult, exploring alternative materials is important for the development of future batterytechnologies.

[006] Na2Mn3O7 (NMO) is a promising candidate due to the large abundance of sodium andmanganese than cobalt, nickel and thus, making it more cost-effective and less-toxic. Itslamellar structure facilitates smooth diffusion kinetics in both LIBs and SIBs. Increase in theinterlayer distance between the Mn3O72- layers of NMO through exfoliation methods has beenreported as an effective approach to stabilize the structure and lower polarization during cycling(Energy Fuels 2021, 35, 14, 11545-11555). Furthermore, transition metal doping within theNMO framework has been shown to enhance electronic conductivity and suppress structuralinstabilities arising from Jahn-Teller distortion during intercalation / deintercalation processes.Despite these advancements, there remains considerable scope for research in transition metal-doped sodium manganese oxides (TMD-NMO) to further optimize their electrochemicalperformance.

[007] NMO has been extensively studied as a cathode material, but stability of manganesetransition metal in various oxidation states suggests it could also be effective in an anodicpotential window as well. However, during cycling, conversion of Mn+4 to M+3 with d4 systemleads to structural disruption caused by Jahn-Teller distortion. Hence, a promising electrodematerial will be one which is based on Mn(IV) and avoidance of Mn(III). Further, NMO lackscapacity retention and low specific capacity at high C-rate, therefore, further development andoptimization of NMO as an anode material is an area of research.

[008] There remains a need for continued research and development to identify and optimizeTMD-NMO-based materials capable of functioning as stable and sustainable anodes forsodium-ion and lithium-ion batteries. To achieve effective anode performance, the intrinsicelectronic structure of NMO must be modified so that the Mn3+ / Mn4+ redox couple, whichtypically operates at high potential, is shifted to lower, anode-relevant voltages (belowapproximately 1.5 V). This requires precise adjustment of transition-metal valence states andoxygen bonding environments through controlled compositional tuning, doping, and defectengineering. These parameters are interdependent and highly sensitive to synthesis conditions,dopant concentration, and particle morphology. Accordingly, systematic investigation intoTMD-NMO compositions and their electrochemical behavior is required to develop stable,reversible, and high-performance anode materials based on this oxide system.OBJECT

[009] One object of the present disclosure is to arrive at a process for the synthesis oftransition metal doped sodium manganese oxides using earth abundant metal-based precursorfor sodium, manganese, and transition metals.

[0010] Another object of the present disclosure is to arrive at transition metal doped sodiummanganese oxides having layered morphology and their fabrication to anode.

[0011] Yet another object of the present disclosure is to arrive at LIBs and SIBs with improvedperformance.SUMMARY

[0012] In one aspect, the present disclosure provides transition-metal doped sodiummanganese oxides having general formula Na2AxMn3-xO7, (abbreviated as A-NMO) wherein Ais a transition element selected from Co, Ni, Fe, Cr, Cu, Ti, Mo, Zr, V, and Nb, and x can varyfrom 0.1 to 10%. The NMO of the present disclosure when fabricated into anode results inSIBs and LIBs with improved performance.

[0013] In another aspect, the present disclosure provides a solid-state process for the synthesisof transition metal-doped sodium manganese oxide (A-NMO) having the general formulaNa2AxMn3-xO7, wherein A is a transition element selected from Co, Ni, Fe, Cr, Cu, Ti, Mo, Zr,V, and Nb, and x can vary from 0.1 to 10%. The process comprises:a) providing a sodium source, manganese source and a precursor of transition metal A;b) grinding all the components of step a);c) annealing the ground sample obtained in step b); andd) optionally grinding the sample obtained in step c);wherein the ratio of sodium source: manganese source: source of A ranges from 1-5 %: 2-10%:0.01-3% respectively by weight.

[0014] In yet another aspect, the present disclosure provides a process for fabrication of anodefrom A-NMO having general formula Na2AxMn3-xO7 wherein A is a transition element selectedfrom Co, Ni, Fe, Cr, Cu, Ti, Mo, Zr, V, and Nb, and x can vary from 0.1 to 10%. The processcomprises:a) preparing a homogenous slurry of the A-NMO, carbon black, and a binder;b) homogenizing the slurry obtained in step a);c) coating the slurry obtained in step b) onto a current collector;d) drying the coated current collector obtained in step c); ande) punching or compressing the coated current collector obtained in step d) to the desiredgeometry.

[0015] In still another aspect, the present disclosure provides SIBs and LIBs comprising:- a cathode;- an anode comprising A-NMO as described in any of the preceding embodiments; and- an electrolyte disposed between the cathode and anode.BRIEF DESCRIPTION OF ACCOMPANYING DRAWINGS

[0016] The present disclosure will now be described with the help of accompanying diagrams.The figures together with detailed description below, are incorporated into and form part of thespecification, and serve to further illustrate the embodiments and explain various principlesand advantages, in accordance with the present disclosure.Figure 1: 1(a): Powder XRD pattern, (b): FESEM, (c): TEM, (d): EDX mapping, (e): EDXspectrum of Na2AxMn3-xO7, wherein A is Zr, x=3%, and the ratio of Na2CO3, Mn2O3, andZrOCl2.8H2O is 1.00: 2.01: 0.08 by weight.Figure 2: Powder XRD pattern of Na2AxMn3-xO7 wherein A is Zr, x=1%, and the ratio ofNa2CO3, Mn2O3, and ZrOCl2.8H2O is 1.00: 2.02: 0.0 by weight.Figure 3: (a): Powder XRD pattern, (b): FESEM at low magnification, (c): FESEM at highmagnification, (d): EDX mapping, (e): EDX spectrum of Na2AxMn3-xO7, wherein A is Zr,x=3%, and the ratio of Na2CO3, Mn2O3, and ZrO2 is 1.00: 2.01: 0.03: by weight.Figure 4: (a): Powder XRD pattern, (b): FESEM, (c): EDX mapping, (d): TEM of Na2AxMn3-xO7 wherein A is Zr, x=3%, and the ratio of Na2CO3, MnCO3 and ZrOCl2.8H2O is 1.00: 2.93:0.08.Figure 5: (a): Powder XRD pattern, (b): FESEM at low magnification, (c): FESEM at highmagnification, (d): EDX mapping, (e): EDX spectrum of Na2AxMn3-xO7 wherein A is Zr,x=3%, and the ratio of CH3COONa, and (CH3COO)2Mn 4H2O, and ZrOCl2.8H2O is 1.00: 4.03:0.05.Figure 6: (a): Powder XRD pattern, (b) & (c): FESEM at 2 different locations at samemagnification, (d): EDX mapping, (e): EDX spectrum of Na2AxMn3-xO7 A is V, x=1%, and theratio of Na2CO3, MnCO3 and V2O5 is 1.00: 4.03: 0.05.Figure 7: Specific capacity vs. cycle number for (a) A-NMO||Li, and (b) A-NMO||Na.Figure 8: Charge-Discharge profile for (a) A-NMO||Li, and (b) A-NMO||Na.Figure 9: Cyclic Voltammetry for (a): A-NMO||Li, (b) A-NMO||Na.Figure 10: Charge-Discharge profile for (a) A-NMO||Li, and (b) A-NMO||Na of Example 5.DESCRIPTION

[0017] Objective of the present disclosure is to develop a transition metal-doped sodiummanganese oxide (A-NMO) material having a layered morphology that can be efficientlysynthesized, fabricated into an anode, and utilized in lithium-ion and sodium-ion batteries todeliver enhanced electrochemical performance. The invention aims to provide a cost-effective,scalable, and environmentally benign electrode material that overcomes the limitations ofconventional manganese-based oxides.

[0018] The following description includes the preferred best mode of one embodiment of thepresent invention. It will be clear from this description of the invention that the invention is notlimited to these illustrated embodiments but that the invention also includes a variety ofmodifications and embodiments thereto. Therefore, the present description should beillustrative and not limiting. While the invention is susceptible to various modifications andalternative constructions, it should be understood that there is no intention to limit the inventionto the specific form disclosed, but, on the contrary, the invention is to cover all modifications,alternative constructions, and equivalents falling within the spirit and scope of the invention asdefined in the claims.

[0019] The present disclosure can be understood more readily by reference to the followingdescription, taken in conjunction with the accompanying Figures and Examples, all of whichform a part of this disclosure.

[0020] At the very outset of the detailed description, it may be understood that the ensuingdescription only illustrates a particular form of this invention. However, such a particular formis only an exemplary embodiment, and without intending to imply any limitation on the scopeof this invention. Accordingly, the description is to be understood as an exemplary embodimentand teaching of invention and not intended to be taken restrictively.

[0021] Before the present disclosure or methods of the present disclosure are described ingreater detail, it is to be understood that the specific products, methods, processes, conditionsor parameters, are not limited to particular embodiments described, as such may, of course,vary. It is also to be understood that the terminology used herein is for the purpose of describingparticular embodiments only, and is not intended to be limiting.

[0022] Where a range of values is provided, it is understood that each intervening value, to thetenth of the unit of the lower limit unless the context clearly dictates otherwise, between theupper and lower limit of that range and any other stated or intervening value in that statedrange, is encompassed within the methods. Where the stated range includes one or both of thelimits, ranges excluding either or both of those included limits are also included in the methods.Certain ranges are presented herein with numerical values being preceded by the term "about."The term "about" is used herein to provide literal support for the exact number that it precedes,as well as a number that is near to or approximately the number that the term precedes. Forexample, "about" can mean within one or more standard deviations, or within ± 30%, 25%,20%, 15%, 10% or 5% of the stated value.

[0023] Unless defined otherwise, all technical and scientific terms used herein have the samemeaning as commonly understood by those of ordinary skill in the art to which the inventionbelongs. Although any methods and materials similar or equivalent to those described hereincan be used in the practice or testing of the present invention, preferred methods and materialsare described. For the purposes of the present invention, the following terms are defined below.

[0024] It is appreciated that certain features of the methods, which are, for clarity, described inthe context of separate embodiments, may also be provided in combination in a singleembodiment. Conversely, various features of the methods, which are, for brevity, described inthe context of a single embodiment, may also be provided separately or in any suitable sub-combination. All combinations of the embodiments are specifically embraced by the presentinvention and are disclosed herein just as if each and every combination was individually andexplicitly disclosed, to the extent that such combinations embrace operable processes and / orcomposites / scaffolds.

[0025] The articles "a" and "an" are used herein to refer to one or to more than one (i.e., to atleast one) of the grammatical object of the article. By way of example, "an element" means oneelement or more than one element.

[0026] As used herein, the term "comprises", "comprising", or "comprising of" is generallyused in the sense of include, that is to say permitting the presence of one or more features orcomponents. The term "comprises", "comprising", or "comprising of" when placed before therecitation of steps in a process or method means that the process or method encompasses oneor more steps that are additional to those expressly recited, and that the additional one or moresteps may be performed before, between, and / or after the recited steps.

[0027] Reference throughout this specification to "certain embodiments", "furtherembodiments", "specific embodiments", "further specific embodiment", "one embodiment","a non-limiting embodiment", "an exemplary embodiment", "some instances", or "furtherinstances", means that a particular feature, structure or characteristic described in connectionwith the embodiment may be included in at least one embodiment of the present disclosure.

[0028] As used herein, the terms 'include', 'have', 'comprise', 'contain' etc. or any form ofsaid terms such as 'having', 'including', 'containing', 'comprising' or 'comprises' are inclusiveand will be understood to imply the inclusion of a stated element, integer or step, or group ofelements, integers or steps, but not the exclusion of any other element, integer or step, or groupof elements, integers or steps.

[0029] The use of any and all examples, or exemplary language (e.g., "such as") provided withrespect to certain embodiments herein is intended merely to better illustrate the disclosure anddoes not pose a limitation on the scope of the disclosure otherwise claimed.

[0030] As used herein, the term "invention", "present invention", "disclosure" or "presentdisclosure" as used herein is a non-limiting term and is not intended to refer to any singleembodiment of the particular invention but encompasses all possible embodiments as describedin the specification.

[0031] The terms "process(es)" and "method(s)" are considered interchangeable within thisdisclosure.

[0032] As used herein, the expression "A-NMO" refers to a transition metal-doped sodiummanganese oxide, wherein "A" denotes one or more transition metal elements that areincorporated into the NMO lattice structure. The transition metal "A" is selected from, but notlimited to, Co, Ni, Fe, Cr, Cu, Ti, Mo, Zr, and Nb, or combinations thereof. The expressionsA-NMO, TMD-NMO, transition-metal doped NMO are used interchangeably throughout thespecification.

[0033] In one aspect, the present disclosure provides transition metal-doped sodium metaloxide (A-NMO) having general formula Na2AxMn3-xO7, wherein A is a transition elementselected from Co, Ni, Fe, Cr, Cu, Ti, Mo, Zr, V, and Nb, and x can vary from 0.1 to 10%. Thepartial substitution of manganese sites by the dopant element "A" results in tailoredelectrochemical and structural characteristics. The A-NMO of the present disclosure whenfabricated into anode results in SIBs and LIBs with improved performance.

[0034] In certain embodiments, transition element employed for the purposes of the presentdisclosure can be selected from Co, Ni, Fe, Cr, Cu, Ti, Mo, Zr, V, and Nb. The elements arechosen on the basis of their oxidation potentials, and structural compatibility with the Mn-Oframework, which allow partial substitution without compromising the crystalline integrity.The introduction of such dopants helps to enhance electronic conductivity, and improve theoverall ionic transport properties within the electrode. In a specific embodiment, the dopant isselected from Fe, Mo, Zr, V, Ti, and Nb. In a further specific embodiment, the dopant is Zr, orV.

[0035] In certain embodiments, the components are present in weight ratios consistent with theformula Na2AxMn3-xO7, where x varies from about 0.1 to 10%, preferably, between 1 to 5%, orfrom 1 to 3%. The proportion of the dopant transition metal is carefully controlled, as excessivedoping may distort the lattice and deteriorate electrochemical performance, whereasinsufficient doping may not yield the desired structural stabilization. The stoichiometric ratiodefined is essential for maintaining structural integrity, ensuring reversible redox behavior, andachieving optimal electrochemical performance when used as an anode material.

[0036] In certain embodiments, the A-NMO adopts a layered structure. The compound mayfurther include particle size variations, surface coatings, or morphological modifications toenhance cycling stability, excellent rate capability typically above 3 C, stable cyclingperformance over more than 300 cycles, and electrode compatibility.

[0037] In certain embodiments, when the A-NMO of the present disclosure is fabricated as ananode in a CR2016 coin-cell, it has ability to exhibit about 300 to about 900 mAh / g specificcapacity (CE> 95%) even at about ~3 C rate between the potential window 0.01-3 V in CR2016coin-cell configuration and has a long cycle life. The cell exhibits excellent cycling stability,retaining a significant portion of its capacity over prolonged charge-discharge cycles. Theenhanced performance is attributed to the synergistic effect of transition-metal doping andoptimized electrode microstructure, which collectively reduce internal resistance and facilitaterapid ion transport.

[0038] In certain embodiments, the A-NMO of the present disclosure when fabricated as A-NMO||Li cell, exhibits an initial capacity of about ~498 mAh / g, which decreases to about ~153mAh / g after about 150 cycles, ultimately delivering a capacity of about ~115 mAh / g after 300cycles, maintaining the coulombic efficiency (CE) remains above 95%. This performancedemonstrates excellent charge retention of the doped NMO material under extended cycling.The material's stability and sustained electrochemical activity highlight its potential as a high-performance anode for next-generation LIBs and SIBs.

[0039] The above embodiments collectively establish that transition metal-dopedNa2AxMn3-xO7 compounds of the present disclosure provide a versatile platform for the designof advanced anode materials. By tuning the dopant type, and concentration. The resulting A-NMO exhibits a balance of high capacity at high C-rate, and long cycle life, making it suitablefor integration into rechargeable ion batteries for portable electronics, electric vehicles, andgrid-scale energy storage applications.

[0040] In another aspect, the present disclosure provides a solid-state route to arrive at A-NMOhaving formula Na2AxMn3-xO7, wherein A is a transition element selected from Co, Ni, Fe, Cr,Cu, Ti, Mo, Zr, V, and Nb, and x can vary from 0.1 to 10%. The process comprises:a) providing a sodium source, manganese source and a precursor of transition metal A;b) grinding all the components of step a);c) annealing the ground sample obtained in step b); andd) optionally grinding the sample obtained in step c);wherein the ratio of sodium source: manganese source: source of A ranges from 1-5 %: 2-10%:0.01-3% respectively by weight.

[0041] In certain embodiments, the sodium source employed in step a) for the purposes of thepresent disclosure is selected from sodium acetate (CH3COONa), sodium sulphate (Na2SO4),sodium bicarbonate (NaHCO3), sodium carbonate (Na2CO3), and sodium hydroxide (NaOH).In a specific embodiment, the sodium source is sodium carbonate or sodium acetate.

[0042] In certain embodiments, the manganese source used in the present disclosure may beselected from, but is not limited to, manganese oxides, carbonates, nitrates, or acetates.Examples include manganese dioxide (MnO2), manganese(III) oxide (Mn2O3), manganesecarbonate (MnCO3), manganese nitrate (Mn(NO3)2), and manganese acetate tetrahydrate(Mn(CH3COO)2(mid dot)4H2O). In a specific embodiment, the manganese source is Mn2O3, MnCO3,or Mn(CH3COO)2(mid dot)4H2O.

[0043] In certain embodiments, the transition element can be selected from Co, Ni, Fe, Cr, Cu,Ti, Mo, Zr, V, and Nb, preferably, Fe, Mo, Zr, V, Ti, and Nb. Precursors of transition metalssuch as oxides, oxy-hydroxides, nitrates, oxy-chlorides, nitrites, sulphates, oxalates etc. can beemployed for the purposes of the present invention. Examples include, but are not limited toiron nitrate (Fe(NO3)3(mid dot)9H2O or Fe(NO3)2(mid dot)4H2O), iron acetate (Fe(CH3COO)3(mid dot)xH2O), ironchloride (FeCl3(mid dot)6H2O); titanium isopropoxide (Ti(OCH(CH3)2)4), titanium nitrate (Ti(NO3)4),MoON (Molybdenumoxynitride) Co2ON (Cobalt oxynitride), ZrO2, ZrOCl2.xH2O (Zirconiumoxychloride), VOCl (Vandium oxychlride), FeOCl (Iron oxychlorides), CuO (Copper oxide),MoO3 (Molybdenum trioxide), Niobium oxalate, Vanadyl isopropoxide (VO(O-iPr)3), Nickelsulphate, TiO2 nickel oxalate, and V2O5. In a specific embodiment, the transition metalprecursor employed is ZrO2, ZrOCl2.xH2O, or V2O5.

[0044] In certain embodiments, the components are taken in weight ratios consistent with theformula Na2AxMn3-xO7, where x varies from about 0.1 to 10%, preferably, between 1 to 5%,or from 1 to 3%.

[0045] In certain embodiments, the precursors of transition metals are typically mixed withmanganese source and a sodium source to form the desired doped NMO.

[0046] In certain embodiments, ratio of the sodium source, manganese precursor, and sourceof transition metal ranges from 1-5 %: 2-10%: 0.01-3% by weight, which includes a range of1-2%: 2-5%: 0.01-1%, and 1-2%: 2-3%: 0.03-1% by weight.

[0047] In certain embodiments, grinding in step b) is carried out for a period ranging between15 to 120 mins using methods such as mortar and pestle, ball mill, jet milling, vibratory millingetc. The time and speed of grinding using different methods can vary. Grinding usingconventional methods such as mortar and pestle can be carried out for several minutes to hours.Grinding using ball mill, jet mill vibratory mill etc. can be carried out for one hour to severalhours and speed of grinding can range from about 50 to 400 rpm in a ball mill, about 400 to800 m / s in a jet mill, and the frequency of vibration in a vibratory mill may range from about50 to 100 Hz. The mixture is ground to ensure homogeneity. This step is crucial for achievinga uniform distribution of the transition metal dopant throughout the manganese oxide matrix.

[0048] In certain embodiments, annealing in step c) is conducted at temperatures of about 600to 900°C for about 8 to 14 hours. The heating rate may vary from about 50 to 100°C per hour.The annealing process results in the formation of the transition metal-doped sodium manganeseoxide phase. After the annealing is completed, the reaction mixture is cooled to roomtemperature. The cooling rate may take place at about 50 to 100°C per hour.

[0049] In certain embodiments the annealed product obtained in step d) is optionally re-groundto achieve a uniform particle size and improved surface area. This step may involve manualgrinding, high-energy ball milling, or jet milling to obtain particles in the size range of 100 nmto several micrometers. The re-ground A-NMO powder can be sieved to obtain the desired sizedistribution and ensure uniform electrode coating when used in battery fabrication.

[0050] In certain embodiments, the method of the present disclosure employs a single-stepsolid-state process. This simplification not only makes the method more efficient but alsoenvironmentally friendly by avoiding the complexities and potential hazards associated withsolvent use. The process ensures reproducible synthesis, minimal impurity formation, andexcellent phase purity of the resultant A-NMO material.

[0051] In certain embodiments, the process can be easily adapted for large-scale production,making it suitable for commercial manufacturing of electrode materials for sodium-ion andlithium-ion batteries. In certain embodiments, the synthesized A-NMO may undergo post-treatment, such as carbon coating, conductive polymer coating, or partial reduction treatment,to further enhance electronic conductivity and electrochemical performance.

[0052] In yet another aspect, the present invention provides a process for fabrication of anodefrom A-NMO having general formula Na2AxMn3-xO7 wherein A is a transition element selectedfrom Co, Ni, Fe, Cr, Cu, Ti, Mo, Zr, V, and Nb, and x can vary from 0.1 to 10%. The processcomprises:a) preparing a homogenous slurry of the A-NMO, carbon black, and a binder;b) homogenizing the slurry obtained in step a);c) coating the slurry obtained in step b) onto a current collector;d) drying the coated current collector obtained in step c); ande) punching or compressing the coated current collector obtained in step d) to the desiredgeometry.

[0053] In certain embodiments, the TMD-NMO, and carbon black serve as the active material,and conductive additive respectively in step a). The binder acts as a mechanical adhesive thatensures uniform coating and strong adhesion of the active layer to the current collector. Thebinder may be selected from polyvinylidene fluoride (PVDF) / Carboxymethyl cellulose(CMC) / Styrene butadiene rubber (SBR). The composition of the slurry may vary dependingon the electrode design, but typically contains:- 70-90 wt% active A-NMO material,- 5-15 wt% conductive carbon, and- 5-10 wt% binder.

[0054] In a specific embodiment, A-NMO employed in step a) has general formula Na2AxMn3-xO7, wherein A is Zr or V, wherein x has ranged from 1 to 3%.

[0055] In certain embodiments, the slurry mixture in step b) is homogenized to ensure auniform dispersion of particles and consistent rheological properties. Homogenization may becarried out by vigorous magnetic or mechanical stirring, ultrasonic agitation, or a combinationthereof, for about 1-3 hours at a temperature of 40-60°C. This ensures thorough mixing of thebinder with the particulate materials, enhances slurry fluidity, and prevents agglomeration ofA-NMO particles or carbon black.

[0056] In certain embodiments, the homogenized mixture in step c) is coated onto a batterygrade current collector which may be selected from but not limited to nickel foam, carbon cloth,Al, Cu foil or the like. This is done using techniques like doctor blade coating, slot-die coating,or roll-to-roll coating. The thickness of coating may range from about 350-500 μm, yielding adry film thickness of about 50-150 μm after solvent removal.

[0057] In certain embodiments, the coated foil in step d) is dried in an oven to remove thesolvent and solidify the coating. Drying may be carried out for about 12-15 hours at about 40-70°C in a vacuum oven, convection oven, or inert-atmosphere chamber. This drying stepensures complete evaporation of residual solvent (such as NMP or water) and promotes bindercuring and particle-particle cohesion.

[0058] In certain embodiments, the coated material in step e) is punched, or compressed toensure a uniform thickness and good contact with the current collector. Compression may beperformed at moderate pressures of about 1-5 MPa to reduce surface roughness, improveelectrode density, and ensure consistent contact between the active material, conductiveadditive, and current collector. The electrodes are typically punched into circular discs of about10-20 mm diameter, suitable for coin-cell or half-cell configurations.

[0059] In certain embodiments, after punching, the electrodes are assembled to a battery. In anembodiment, it is assembled in an argon-filled glove box with lithium and sodium counterelectrodes for use in lithium-ion batteries (LIB) and sodium-ion batteries (SIB), respectively.

[0060] In still another aspect, the present disclosure provides SIBs and LIBs comprising:- a cathode;- an anode comprising A-NMO as described in any of the preceding embodiments; and- an electrolyte disposed between the cathode and anode.

[0061] In certain embodiments, the cathode may be selected from conventional cathodematerials suitable for SIBs and LIBs. For lithium-ion batteries, the cathode may comprise oneor more lithium-based compounds such as lithium foil, lithium cobalt oxide (LiCoO2), lithiumiron phosphate (LiFePO4), lithium manganese oxide (LiMn2O4), lithium nickel manganesecobalt oxide (LiNixMnyCozO2; NMC), or lithium nickel cobalt aluminum oxide(LiNixCoyAl_zO2; NCA). For sodium-ion batteries, the cathode may comprise sodium foil,sodium transition metal oxides, NaxFePO4, Na3V2(PO4)3 and other layered / polyanionicsodium-based compounds known for reversible sodium intercalation. In a specificembodiment, the A-NMO material of the present disclosure may act as cathode.

[0062] In certain embodiments, the electrolyte comprises a liquid, solid, or gel-type ionicconductor that facilitates ion transport between the anode and cathode. The electrolyte mayinclude for LIBs, a lithium salt such as LiPF6, LiClO4, LiBF4, or LiTFSI, dissolved in an organicsolvent mixture such as ethylene carbonate (EC), dimethyl carbonate (DMC), diethyl carbonate(DEC), propylene carbonate (PC), or combinations thereof; for SIBs, a sodium salt such asNaPF6, NaClO4, NaBF4, or NaTFSI, dissolved in a suitable organic solvent such as ethylenecarbonate, propylene carbonate, dimethyl carbonate, or diethyl carbonate or combinationsthereof.

[0063] In certain embodiments, the electrolyte may further comprise additives such asfluoroethylene carbonate (FEC), vinylene carbonate (VC), or tris(trimethylsilyl)phosphate(TMSP) to enhance solid-electrolyte interphase (SEI) stability and cycle life.

[0064] In certain embodiments, the electrolyte may be a solid-state electrolyte selected fromoxide-based like LiSr1.65Zr1.3Ta1.7O9, Na-β-Al2O3, or polymer-based ionic conductors likeLi4Al0.33Si0.33P0.33O4 , Na3Zr2Si2PO12.

[0065] In certain embodiments, the cells are fabricated by sequential stacking of the A-NMO-based anode, separator, electrolyte-soaked separator, and lithium or sodium counter electrode,followed by sealing under vacuum using crimping machine.

[0066] In certain embodiments, the punched and compressed electrodes are incorporated intoCR2016 coin-cell assemblies. The resulting coin cells exhibit excellent electrochemicalstability, with specific capacities in the range of 300-900 mAh g-1 and coulombic efficiencyexceeding 95% over extended cycling. The superior performance is attributed to the layeredstructure, homogeneous dopant distribution, and optimized electrode microstructure achievedthrough the disclosed fabrication process.

[0067] In certain embodiments, the punched and compressed electrodes are incorporated intoA-NMO||Li cell. The cells exhibit an initial capacity of about 498.15 mAh / g, which decreasedto about 153.75 mAh / g after about 150 cycles, ultimately delivering a capacity of about 115.62mAh / g. Throughout the 300 cycles, the coulombic efficiency (CE) remains above 95%. In thecase of the A-NMO||Na cell, the initial specific capacity is about 401.37 mAh / g. The celldelivers specific capacities of about 611 mAh / g and about 883 mAh / g at the end of the 150thand 300th cycles, respectively, with CE exceeding about 97%.

[0068] In a specific embodiment, the present disclosure provides SIB comprising- Sodium foil as cathode;- A-NMO having general formula Na2AxMn3-xO7, wherein A is Zr or V, wherein x hasranged from 1 to 3%; and- an electrolyte comprising NaPF6 in EC & DMC (1:1 ratio, v / v%) with 2% FEC additive

[0069] In a further specific embodiment, the present disclosure provides a LIB comprising- Lithium foil as cathode;- A-NMO having general formula Na2AxMn3-xO7, wherein A is Zr or V , wherein x hasranged from 1 to 3%; and- electrolyte comprising LiPF6 in EC & DMC (1:1 ratio, v / v%)

[0070] The present disclosure provides an alternative anode material, transition metal-dopedNa2Mn3O7 (A-NMO), which exhibits exceptional performance metrics. Specifically, A-NMOdemonstrates a high specific capacity of over 300 mAh / g with a cycle count exceeding 300cycles at approximately 3C in sodium-ion batteries (SIBs). the A-NMO||Li system shows arespectable specific capacity of over 100 mAh / g for 300 cycles at around 3C. These resultsindicate superior battery parameters compared to those reported in the literature.

[0071] The present disclosure focuses on the design of A-NMO, it features a layeredmorphology, making it suitable for application in both LIBs and SIBs. A-NMO anode exhibitshigh specific capacity, delivering values greater than 100 mAh g-1 in lithium-ion batteries(LIBs) and greater than 300 mAh g-1 in sodium-ion batteries (SIBs), both under over 3C formore than 300 cycles.

[0072] The foregoing outlines features of several embodiments so that those skilled in the artbetter understand the aspects of the present disclosure. Those skilled in the art should appreciatethat they may readily use the present disclosure as a basis for designing or modifying otheranodes and cathodes. Those skilled in the art should also realize that such equivalentconstructions do not depart from the spirit and scope of the present disclosure, and that theymay make various changes, substitutions, and alterations herein.EXAMPLES:Example 1: Synthesis of Na2AxMn3-xO7, wherein A is Zr, x=3% via solid state route.Synthesis of Na2AxMn3-xO7 was carried through solid state route. Na2CO3, Mn2O3, andZrOCl2.8H2O were taken in exact ratios of 1.00: 2.01: 0.08 by weight. The precursors wereground well using mortar-pestle and were annealed at 600°C for 8-12 hrs at the rate 50°C perhour.Figure 1 represents analytical data for the obtained sample. The XRD (Fig. 1(a)), and FESEM(Fig. 1(b)), confirm the successful synthesis with phase purity of > 95%, which is well matchedwith JCPDS no. 78-0193, and layered morphology of the Zr-NMO, respectively. TEMindicates towards a layer of A-NMO formed due to sonication during sample preparation asshown in Fig. 1(c). EDX mapping shows the uniform presence of all the elements such as Na,Mn, Zr, O as shown in Fig. 1(d). Additionally, Fig. 1(e) confirms the presence Zr dopant inNMO sample.Example 2: Synthesis of Na2AxMn3-xO7 wherein A is Zr, x=1% via solid state route:Synthesis of Na2AxMn3-xO7 was carried through solid state route. Na2CO3, Mn2O3, andZrOCl2.8H2O were taken in exact ratios of 1.00: 2.02: 0.0 by weight. The precursors wereground well using mortar-pestle and was annealed at 600°C for 8-12 hrs at the rate 50°C perhour.Figure 2 represents analytical data for the obtained sample. It shows the XRD with phase purityof >95% which is well matched with the JCPDS No. 78-0193 and also good crystallinity.Example 3: Synthesis of Na2AxMn3-xO7 wherein A is Zr, x=3% via solid state route:Synthesis of Na2AxMn3-xO7 was carried through solid state route, Na2CO3, Mn2O3, and ZrO2were taken in exact ratios of 1.00: 2.01: 0.03: by weight. The precursors were ground wellusing mortar-pestle and was annealed at 600°C for 8-12 hrs at the rate 50°C per hour.Figure 3 represents analytical data for the obtained sample. The XRD (Fig. 3(a)), and FESEM(Fig. 3(b-c)), confirm the successful synthesis with phase purity of > 95%, which is wellmatched with JCPDS no. 78-0193, and layered morphology of the Zr-NMO at two differentmagnifications, respectively. The morphology of Zr-NMO has larger size of agglomeratedparticles with closely stacked layers as compared to Example 1. EDX mapping shows theuniform presence of all the elements such as Na, Mn, Zr, O as shown in Fig.3(d). Fig.3(e) alsoconfirms the presence successful Zr doping in NMO sample.Example 4: Synthesis of Na2AxMn3-xO7 wherein A is Zr, x=3% via solid state route:Synthesis of Na2AxMn3-xO7 was carried through solid state route. Na2CO3, MnCO3 andZrOCl2.8H2O were taken in exact ratios of 1.00: 2.93: 0.08 by weight. The precursors wereground well using mortar-pestle and was annealed at 600°C for 10-12 hrs at the rate 50°C perhour.Figure 4 represents analytical data for the obtained sample. The XRD (Fig. 4(a)), and FESEM(Fig. 4(b)), confirm the successful synthesis with phase purity of > 95%, which is well matchedwith JCPDS no. 78-0193, and layered morphology of the Zr-NMO with particle size of 2 um,respectively. Here, the agglomeration is comparatively lesser than Example 1 and Example 3.EDX mapping shows the uniform presence of all the elements such as Na, Mn, Zr, O as shownin Fig.4(c). TEM indicates towards a pebble like morphology made up of multiple layer of ZrNMO as shown in Fig.4(d).Example 5: Synthesis of Na2AxMn3-xO7 wherein A is Zr, x=3% via solid state route:Synthesis of Na2AxMn3-xO7 was carried through solid state route. CH3COONa, and(CH3COO)2Mn.4H2O, and ZrOCl2.8H2O were taken in exact ratios of 1.00: 4.03: 0.05 byweight. The precursors were ground well using mortar-pestle and was annealed at 600°C for10-12 hrs at the rate 50°C per hour.Figure 5 represents analytical data for the obtained sample.Figure 5 shows the schematic representation of Zr-NMO (Example 5) synthesis via the solid-state route. The XRD (Fig. 5(a)), and FESEM (Fig. 5(b)), confirm the successful synthesis withphase purity of > 95%, which is well matched with JCPDS no. 78-0193, and elongated platelike morphology of the Zr-NMO with particle length of 1-2 um and thickness of 200-300 nm,respectively. The morphology is quite different from other Examples 1 to 4. EDX mappingshows the uniform presence of all the elements such as Na, Mn, Zr, O as shown in Fig.5(c).Fig.5(d) also confirms the presence successful Zr doping in NMO sample.Example 6: Synthesis of Na2AxMn3-xO7 wherein A is V, x=1% via solid state route:Synthesis of Na2AxMn3-xO7 was carried through solid state route. Na2CO3, MnCO3 and V2O5were taken in exact ratios of 1.00: 4.03: 0.05 by weight. The precursors were ground well usingmortar-pestle and was annealed at 750°C for 12-14 hrs at the rate 100°C per hour.Figure 6 represents analytical data for the obtained sample. The XRD (Fig. 6(a)), and FESEM(Fig. 6(b-c)), confirm the successful synthesis with phase purity of 100%, which is wellmatched with JCPDS no. 78-0193, and the morphology found to be irregular shaped particleswith size ranging from 200-400 nm, respectively. The morphology of V-NMO is completelydifferent from above mentioned Example 1 to Example 5. This observation further suggeststhat the uniquely close-packed layers in Zr-NMO arise from Zr doping as well as the reactionconditions employed in Examples 1 to 5. EDX mapping shows the uniform presence of all theelements such as Na, Mn, V, O as shown in Fig.6(d). Fig.6(e) also confirms the presencesuccessful V doping in NMO sample.Example 7: Fabrication of electrodes:Electrode fabrication for the electrode material obtained in Example 1 and Example 5 is asfollows: The active material Zr -NMO, Super-P carbon black (CB) and Polyvinylidene fluoride(PVDF, average Mw=5,34,000) as a binder were taken in 7:2:1 ratio by weight. The slurry wasprepared in 1.5-3mL of N-Methyl-2-Pyrrolidone (NMP) solvent. The mixture was thoroughlymixed twice using a vacuum mixer for 10 min each. The resultant slurry was coated on Cu foil(thickness(symbol) 80 um) using thin film coater and dried in a vacuum oven at 50°C for 12 h. Theprepared film was cut into discs of 10 mm. The mass loading, approximately 1.4-2mg / cm2, waskept the same throughout the cell testing. Sodium foil (Sigma-Aldrich, battery grade) was takenas a counter electrode, and the electrolyte was 1 M NaPF6 in ethylene carbonate and dimethylcarbonate with 1% FEC (1:1, v / v ratio, Sigma-Aldrich, battery grade) for SIB. Lithium foil(Sigma-Aldrich, battery grade) was taken as a counter electrode, and the electrolyte was 1 MLiPF6 in ethylene carbonate and dimethyl carbonate (1:1, v / v ratio, Sigma-Aldrich, batterygrade) for LIB. Whatman GF (glass fibre) / D (battery grade) separator was used. The cellassembly of CR2016 was done in an Ar-filled glove box.Electrochemical testing:A-NMO was tested within a potential window of 0.01-3V in CR2016 half-cell configurationfor both LIB and SIB applications. Figure 7 illustrates the galvanostatic charge-discharge(GCD) performance of the A-NMO half-cell at a 3C rate over 300 cycles. The A-NMO||Li cellexhibited an initial capacity of 498.15 mAh / g, which decreased to 153.75 mAh / g after 150cycles, ultimately delivering a capacity of 115.62 mAh / g. Throughout the 300 cycles, thecoulombic efficiency (CE) remained above 95%. In the case of the A-NMO||Na cell, the initialspecific capacity was 401.37 mAh / g. It was observed that the specific capacity graduallyincreased, likely due to the expansion of interlayer spacing within the A-NMO structure,facilitating the mobility of the larger Na+ ions. The cell delivered specific capacities of ~611mAh / g and ~883 mAh / g at the end of the 150th and 300th cycles, respectively, with CEexceeding 97%. Figure 8 depicts the charge-discharge profile for A-NMO||Li and A-NMO||Naat 2nd and 300th cycle. Figure 9 depicts the CV profiles of A-NMO electrodes in half-cellconfigurations against Li / Li+ and Na / Na+, respectively, recorded at varying scan rates of 0.1,and 1mV / s. For the A-NMO||Li (Fig. (9a)), the CV curves exhibit broad anodic at 1.22V andsharp elongated cathodic peak at 0.27V primarily corresponding to Li+ intercalation / de-intercalation into the layered structure. A-NMO||Na (Fig. (9b)) shows distinct anodic andcathodic peaks at 2.33V and 2.05V apart from multiple redox couples between 2.5-3V owingto various oxidation state of Mn ion.For Example, 5, Figure 10 depicts the charge-discharge profile for Zr-NMO||Li and Zr-NMO||Na at 0.5C. Zr-NMO||Li exhibited 407.29 and 228.86 mAh / g at 2nd and 10th cyclerespectively as in Fig.10a. Zr-NMO||Na exhibited 209.40 and 78.45 mAh / g at 2nd and 10th cyclerespectively as in Fig.10b. The capacity retention can be improved by optimizing electrodefabrication process.Comparative Examples:

[0073] Table 1 presents a review of the electrochemical performance of reported NMO-basedelectrodes. The study demonstrates the highest specific capacity with a high cycle count (>300cycles) under high C-rate conditions (~3C).

[0074] Table 1: Comparative study from published research articles of cell performance ofNa2Mn3O7 based anode.References:1. Energy Fuels 2021, 35, 14, 11545-115502. Chem. Mater. 2017, 29, 11, 4645-46483. Journal of Alloys and Compounds 918 (2022): 1657654. ACS Applied Materials & Interfaces 2022, 14 (34) , 38769-38777

Claims

1. A transition metal doped sodium manganese oxide having general formula Na2AxMn3-xO7, (A-NMO) wherein A is a transition element selected from Co, Ni, Fe, Cr, Cu, Ti, Mo, Zr, V, and Nb, and x can vary from 0.1 to 10%.

2. The A-NMO as claimed in claim 1, wherein A is Zr, or V.

3. The A-NMO as claimed in claim 1, wherein x ranges from 1 to 3%.

4. The transition metal doped NMO as claimed in claim 1, wherein the A-NMO adopts a layered structure.

5. A solid-state process for the synthesis of transition metal-doped sodium manganese oxide (A-NMO) as claimed in claim 1 having general formula Na2AxMn3-xO7, wherein A is a transition element selected from Co, Ni, Fe, Cr, Cu, Ti, Mo, Zr, V, and Nb, and x can vary from 0.1 to 10%, the process comprising: a) providing a sodium source, manganese source and a precursor of transition metal A; b) grinding all the components of step a); c) annealing the ground sample obtained in step b); and d) optionally grinding the sample obtained in step c); wherein the ratio of sodium source: manganese source: source of A ranges from 1-5 %: 2-10%: 0.01-3% respectively by weight.

6. The process as claimed in claim 5, wherein the source of sodium is sodium carbonate or sodium acetate, source of manganese is Mn2O3, MnCO3, or (CH3COO)2Mn 4H2O, and source of transition metal is ZrO2, ZrOCl2.xH2O, or V2O5, and they are present in a ratio of 1-2%: 2- 5%: 0.01-1%, or 1-2%: 2-3%: 0.03-1% by weight respectively.

7. A process for fabrication of anode from A-NMO having general formula Na2AxMn3-xO7 as claimed in claim 1, the process comprising: a) preparing a homogenous slurry of the A-NMO, carbon black, and a binder; b) homogenizing the slurry obtained in step a); c) coating the slurry obtained in step b) onto a current collector; d) drying the coated current collector obtained in step c); and e) punching or compressing the coated current collector obtained in step d) to the desired geometry.

8. The process as claimed in claim 7, wherein A-NMO has the general formula Na2AxMn3-xO7, wherein A is Zr or V, wherein x has ranged from 1 to 3%.

9. SIBs and LIBs comprising: - a cathode; - an anode comprising A-NMO as claimed in claim 1; and - an electrolyte disposed between the cathode and anode.

10. SIBs and LIBs as claimed in claim 9, wherein, the SIB comprises Sodium foil as cathode; A-NMO having general formula Na2AxMn3-xO7, wherein A is Zr or V, wherein x has ranged from 1 to 3%; and electrolyte comprising NaPF6 in EC & DMC (1:1 ratio, v / v%) with 2% FEC additive; and the LIB comprises Lithium foil as cathode; A-NMO having general formula Na2AxMn3-xO7, wherein A is Zr or V, wherein x has ranged from 1 to 3%; and electrolyte comprising LiPF6 in EC & DMC (1:1 ratio, v / v%).