Method for producing polytetrafluoroethylene particles

IN595429BActive Publication Date: 2026-07-15DAIKIN INDUSTRIES LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
IN202337088768
Authority / Receiving Office
IN · IN
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-06-30
Filing Date
2023-12-26
Publication Date
2026-07-15
Estimated Expiration
2042-06-30

AI Technical Summary

Technical Problem

The production of polytetrafluoroethylene (PTFE) particles through suspension polymerization often results in a strong acid odor, which is undesirable and stimulates the trigeminal nerve.

Method used

A method involving suspension polymerization of tetrafluoroethylene, followed by washing, crushing, dehydration, and heat treatment at 200°C or higher to reduce the acid odor, while maintaining a water content of 40% or less and achieving a specific particle size and specific gravity, thereby minimizing the presence of acid-forming compounds.

Benefits of technology

The method effectively reduces the acid odor of PTFE particles, improving working conditions and producing particles with desired properties such as reduced fluorine-containing compounds and enhanced handling characteristics.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Provided is a method for producing polytetrafluoroethylene particles which involves producing polytetrafluoroethylene particles by preparing suspension-polymerized particles of polytetrafluoroethylene by suspension-polymerizing tetrafluoroethylene in an aqueous medium, preparing crushed particles by cleaning the suspension-polymerized particles, and thereafter, crushing the same, or cleaning the suspension-polymerized particles while crushing the same, preparing crushed particles having a water content of 40 mass% or less by dehydrating the crushed particles, and heat-treating the dehydrated crushed particles.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present disclosure relates to a method forproducing a polytetrafluoroethylene particle, a method forproducing a polytetrafluoroethylene formed article, and a methodfor producing a polytetrafluoroethylene compression-moldedarticle.BACKGROUND ART

[0002] A known method for producing polytetrafluoroethyleneis an emulsion polymerization method, a suspensionpolymerization method, or the like.

[0003] In an emulsion polymerization method, in general,tetrafluoroethylene is polymerized in an aqueous medium in thepresence of a fluorine-containing surfactant to give an aqueousdispersion in which primary particles of polytetrafluoroethyleneare stably dispersed in the aqueous medium. The primaryparticles in the resulting aqueous dispersion are coagulated anddried to give a polytetrafluoroethylene fine powder.

[0004] On the other hand, in a suspension polymerizationmethod, in general, tetrafluoroethylene is polymerized in anaqueous medium without any fluorine-containing surfactant orwith a small amount of a fluorine-containing surfactant toproduce a suspension-polymerized particle. The resultingsuspension-polymerized particle is recovered and dried to give apolytetrafluoroethylene molding powder.

[0005] For example, Patent Document 1 describes, as a methodfor producing polytetrafluoroethylene by a suspensionpolymerization method, a method for producing apolytetrafluoroethylene molding powder, the method comprising astep of subjecting a monomer containing 99.8% by mass or more oftetrafluoroethylene to suspension polymerization in an aqueousmedium, to produce a granular polymer particle, and a step ofcrushing the granular polymer particle, in which the aqueousmedium contains a compound represented by the following formula(1) at a concentration of 0.5 to 2000 ppm:RF(OCF(X1)CF2)k-1OCF(X2)COO-M+ (1)wherein RF is a perfluorinated monovalent organic group having 1to 10 carbon atoms, X1 and X2 are each independently a fluorineatom or a trifluoromethyl group, k is an integer of 1 or more,and M+ is a hydrogen ion, an ammonium ion, an alkyl-substitutedammonium ion or an alkali metal ion.RELATED ARTPATENT DOCUMENTS

[0006] Patent Document 1: International Publication No. WO2014 / 123075SUMMARY OF THE INVENTIONPROBLEM TO BE SOLVED BY THE INVENTION

[0007] An object of the present disclosure is to provide aproduction method for producing a polytetrafluoroethyleneparticle having a decreased acid odor.MEANS FOR SOLVING THE PROBLEM

[0008] The present disclosure provides a method for producinga polytetrafluoroethylene particle, comprising subjectingtetrafluoroethylene to suspension polymerization in an aqueousmedium to prepare a suspension-polymerized particle of apolytetrafluoroethylene, washing and then crushing thesuspension-polymerized particle or crushing the suspensionpolymerizedparticle with washing to prepare a crushed particle,dehydrating the crushed particle to prepare a crushed particlehaving a water content of 40% by mass or less, and subjectingthe dehydrated crushed particle to heat treatment to produce apolytetrafluoroethylene particle.

[0009] In the production method of the present disclosure, itis preferable that after the crushed particle is dehydrated, thecrushed particle is further dried.In the production method of the present disclosure, it ispreferable that the crushed particle is dried by airflow drying.In the production method of the present disclosure, thetemperature of the heat treatment is preferably 200°C or higher.In the production method of the present disclosure, theheat treatment is preferably performed using a conductive heatreceivingtype dryer.In the production method of the present disclosure, theheat treatment is preferably performed using a material-stirringtype dryer or a material-conveying type dryer.In the production method of the present disclosure, it ispreferable that, in the heat treatment or during transferring ofthe polytetrafluoroethylene particle after the heat treatment,the polytetrafluoroethylene particle is produced by forming asolid-gas mixture containing the polytetrafluoroethyleneparticle generated by the heat treatment and gas, separating thesolid-gas mixture into the polytetrafluoroethylene particle andthe gas, and recovering the polytetrafluoroethylene particle.In the production method of the present disclosure, theaverage particle size of the crushed particle is preferably 100to 800 μm.In the production method of the present disclosure, it ispreferable that after the polytetrafluoroethylene particle isproduced by subjecting the crushed particle to the heattreatment, the polytetrafluoroethylene particle is furthercrushed to produce a polytetrafluoroethylene particle having anaverage particle size of 200 μm or less.In the production method of the present disclosure,tetrafluoroethylene and a modifying monomer are preferablysubjected to suspension polymerization.In the production method of the present disclosure, thestandard specific gravity of the polytetrafluoroethyleneparticle is preferably 2.200 or less.In the production method of the present disclosure, thespecific surface area of the polytetrafluoroethylene particle ispreferably 5.0 m2 / g or less.In the production method of the present disclosure, it ispreferable that the polytetrafluoroethylene particle issubstantially free from a compound represented by the followinggeneral formula (2):General formula (2): [Cn-1F2n-1COO-]M+wherein n represents an integer of 9 to 12 and M+ represents acation.In the production method of the present disclosure, it ispreferable that suspension polymerization is carried out in thepresence or absence of a surfactant, and the amount of thesurfactant is 2000 mass ppm or less based on the aqueous medium.

[0010] The present disclosure also provides a method forproducing a polytetrafluoroethylene formed article, the methodcomprising producing the polytetrafluoroethylene particle by theproduction method, and then forming the polytetrafluoroethyleneparticle to give a formed article.

[0011] The present disclosure also provides a method forproducing a polytetrafluoroethylene compression-molded article,the method comprising producing the polytetrafluoroethyleneparticle by the production method, and then compression moldingthe polytetrafluoroethylene particle to give a compressionmoldedarticle.

[0012] The present disclosure also provides apolytetrafluoroethylene particle obtained by the productionmethod.EFFECTS OF INVENTION

[0013] The present disclosure can provide a production methodfor producing a polytetrafluoroethylene particle having adecreased acid odor.DESCRIPTION OF EMBODIMENTS

[0014] Hereinafter, specific embodiments of the presentdisclosure will now be described in detail, but the presentdisclosure is not limited to the following embodiments.

[0015] The production method of the present disclosurerelates to a method for producing a polytetrafluoroethylene byusing a suspension polymerization method.

[0016] The production of a polytetrafluoroethylene moldingpowder by polymerizing tetrafluoroethylene (TFE), as in theproduction method described in Patent Document 1, has theproblem of generating an acid odor from the resultingpolytetrafluoroethylene molding powder. The acid odor is a"sour" odor of an acidic substance such as formic acid or aceticacid, and is an odor strongly stimulating the trigeminal nerve.

[0017] In the method for producing a polytetrafluoroethyleneparticle of the present disclosure, a suspension-polymerizedparticle of polytetrafluoroethylene is prepared by a suspensionpolymerization method, then the resulting suspension-polymerizedparticle is crushed and the crushed particle is dehydrated, andthe crushed particle is subjected to a heat treatment to producea polytetrafluoroethylene particle. The method for producing apolytetrafluoroethylene particle of the present disclosure hassuch a configuration, and thus can produce apolytetrafluoroethylene particle having a decreased acid odor.

[0018] Next, each step of the production method of thepresent disclosure will be described in detail.

[0019] (Polymerization)In the production method of the present disclosure, first,TFE is subjected to suspension polymerization in an aqueousmedium to prepare a suspension-polymerized particle ofpolytetrafluoroethylene.

[0020] The suspension-polymerized particle ofpolytetrafluoroethylene is obtained by subjecting TFE tosuspension polymerization. The suspension-polymerized particlecannot be present in the state of being dispersed in an aqueousmedium. On the contrary, when the polytetrafluoroethylene isprepared by subjecting TFE to emulsion polymerization, thepolytetrafluoroethylene is obtained in the form of a primaryparticle (emulsion-polymerized particle) dispersed in an aqueousmedium.

[0021] The suspension-polymerized particle usually has alarger average particle size than the emulsion-polymerizedparticle. The average particle size of the suspensionpolymerizedparticle is preferably 200 μm or more, morepreferably 400 μm or more, even more preferably 800 μm or moreand particularly preferably 1 mm or more, and is preferably 100mm or less.

[0022] The polytetrafluoroethylene obtained by suspensionpolymerization is preferably a high molecular weightpolytetrafluoroethylene that is non melt-processible. The term"non melt-processible" means a property that the melt flow ratecannot be measured at a temperature higher than the crystalmelting point in accordance with ASTM D 1238 and D 2116.

[0023] The standard specific gravity (SSG) of thepolytetrafluoroethylene is preferably 2.130 to 2.280. Thestandard specific gravity can be measured according to ASTMD4894. In the present disclosure, when the standard specificgravity (SSG) of the polytetrafluoroethylene is within the aboverange, it is meant that the polytetrafluoroethylene is a highmolecular weight polytetrafluoroethylene.

[0024] The peak temperature of the polytetrafluoroethylene ispreferably 333 to 347°C and more preferably 335 to 347°C. Thepeak temperature can be specified as the correspondingtemperature to the maximum value appearing in a differentialthermal (DTA) curve obtained by heating apolytetrafluoroethylene having no history of being heated to atemperature of 300°C or higher, under the condition of 10°C / minwith TG / DTA (thermogravimetric - differential thermal analyzer).In the present disclosure, when the peak temperature of thepolytetrafluoroethylene is within the above range, it is meantthat the polytetrafluoroethylene is a high molecular weightpolytetrafluoroethylene.

[0025] The polytetrafluoroethylene preferably shows at leastone or more endothermic peak appearing in a range of 333 to347°C on a heat-of-fusion curve obtained by heating apolytetrafluoroethylene having no history of being heated to atemperature of 300°C or higher, at a temperature-increasing rateof 10°C / min with a differential scanning calorimeter [DSC], andhas an enthalpy of fusion of 52 mJ / mg or more at 290 to 350°C,calculated from the heat-of-fusion curve. The enthalpy offusion of the polytetrafluoroethylene is more preferably 55mJ / mg or more and even more preferably 58 mJ / mg or more.

[0026] In the production method of the present disclosure, itis also preferable that TFE and a modifying monomer aresubjected to suspension polymerization. That is to say, thepolytetrafluoroethylene may be a homopolytetrafluoroethylenecontaining only TFE unit, or may be a modifiedpolytetrafluoroethylene containing TFE unit and a modifyingmonomerunit that is based on a modifying monomercopolymerizable with TFE.

[0027] The amount of the modifying monomer added whenpolymerizing TFE is preferably 0.001% by mass or more, morepreferably 0.01% by mass or more, even more preferably 0.03% bymass or more and particularly preferably 0.05% by mass or more,and is preferably 1.0% by mass or less, more preferably 0.8% bymass or less, even more preferably 0.5% by mass or less andparticularly preferably 0.3% by mass or less based on theresulting polytetrafluoroethylene.

[0028] The modifying monomer is not limited as long as it canbe copolymerized with TFE, and examples thereof include afluoromonomer and a non-fluoromonomer. One modifying monomermay be used singly, or multiple modifying monomers may be used.

[0029] The non-fluoromonomer is not limited, and examplesthereof include a monomer represented by general formula:CH2=CRQ1-LRQ2wherein RQ1 represents a hydrogen atom or an alkyl group; Lrepresents a single bond, -CO-O-*, -O-CO-*, or -O-; * representsa bond position with RQ2; and RQ2 represents a hydrogen atom, analkyl group, or a nitrile group.

[0030] Examples of the non-fluoromonomer include methylacrylate, methyl methacrylate, ethyl acrylate, ethylmethacrylate, propyl acrylate, propyl methacrylate, butylacrylate, butyl methacrylate, hexyl methacrylate, cyclohexylmethacrylate, vinyl methacrylate, vinyl acetate, acrylic acid,methacrylic acid, acrylonitrile, methacrylonitrile, ethyl vinylether, and cyclohexyl vinyl ether. Of these, the nonfluoromonomeris preferably butyl methacrylate, vinyl acetate,or acrylic acid.

[0031] Examples of the fluoromonomer include perfluoroolefinssuch as hexafluoropropylene [HFP]; hydrogen-containingfluoroolefins such as trifluoroethylene and vinylidene fluoride[VDF]; perhaloolefins such as chlorotrifluoroethylene;perfluorovinyl ether; (perfluoroalkyl)ethylene; andperfluoroallyl ether.

[0032] The perfluorovinyl ether is not limited, and examplesthereof include a perfluoro unsaturated compound represented bygeneral formula (A):CF2=CF-ORf (A)wherein Rf represents a perfluoro organic group. The "perfluoroorganic group" as used herein means an organic group in whichall hydrogen atoms bonded to the carbon atoms are replaced byfluorine atoms. The perfluoro organic group may have etheroxygen.

[0033] An example of the perfluorovinyl ether is aperfluoro(alkyl vinyl ether) [PAVE] in which Rf in generalformula (A) is a perfluoroalkyl group having 1 to 10 carbonatoms. The perfluoroalkyl group preferably has 1 to 5 carbonatoms.

[0034] Examples of the perfluoroalkyl group in the PAVEinclude a perfluoromethyl group, a perfluoroethyl group, aperfluoropropyl group, a perfluorobutyl group, a perfluoropentylgroup, and a perfluorohexyl group.

[0035] Examples of the perfluoro vinyl ether also includethose represented by general formula (A) in which Rf is aperfluoro(alkoxyalkyl) group having 4 to 9 carbon atoms; thosein which Rf is a group represented by the following formula:

[0036]

[0037] wherein m represents an integer of 0 or 1 to 4; andthose in which Rf is a group represented by the followingformula:CF3CF2CF2-(O-CF(CF3)-CF2)nwhereinn represents an integer of 1 to 4.

[0038] Examples of the hydrogen-containing fluoroolefininclude CH2=CF2, CHF=CH2, CHF=CF2, CH2=CFCF3, CH2=CHCF3, CHF=CHCF3(E isomer), and CHF=CHCF3 (Z isomer).

[0039] The (perfluoroalkyl)ethylene (PFAE) is not limited,and examples thereof include (perfluorobutyl)ethylene (PFBE) and(perfluorohexyl)ethylene.

[0040] Examples of the perfluoroallyl ether include afluoromonomer represented by:General formula: CF2=CF-CF2-ORfwherein Rf represents a perfluoro organic group.

[0041] Rf in the general formula is the same as Rf in generalformula (A). Rf is preferably a perfluoroalkyl group having 1to 10 carbon atoms or a perfluoroalkoxyalkyl group having 1 to10 carbon atoms. The perfluoroallyl ether is preferably atleast one selected from the group consisting of CF2=CF-CF2-O-CF3,CF2=CF-CF2-O-C2F5, CF2=CF-CF2-O-C3F7, and CF2=CF-CF2-O-C4F9, morepreferably at least one selected from the group consisting ofCF2=CF-CF2-O-C2F5, CF2=CF-CF2-O-C3F7, and CF2=CF-CF2-O-C4F9, andeven more preferably CF2=CF-CF2-O-CF2CF2CF3.

[0042] The modifying monomer is preferably at least oneselected from the group consisting of hexafluoropropylene,chlorotrifluoroethylene, vinylidene fluoride, perfluoro(alkylvinyl ether), (perfluoroalkyl)ethylene, and ethylene, and morepreferably a perfluoro(alkyl vinyl ether).

[0043] From the viewpoint of reactivity with TFE, themodifying monomer is preferably at least one selected from thegroup consisting of hexafluoropropylene, perfluoro(alkyl vinylether), and (perfluoroalkyl)ethylene, more preferably at leastone selected from the group consisting of hexafluoropropylene,perfluoro(methyl vinyl ether), perfluoro(propyl vinyl ether),(perfluorobutyl)ethylene, (perfluorohexyl)ethylene, and(perfluorooctyl)ethylene, and even more preferably at least oneselected from the group consisting of perfluoro(methyl vinylether) and perfluoro(propyl vinyl ether).

[0044] The suspension polymerization can be performed, forexample, by charging a reactor with monomers such as TFE, anaqueous medium, and optionally other additives, stirring thecontents of the reactor, retaining the reactor at apredetermined polymerization temperature, and then adding apredetermined amount of a polymerization initiator to initiatethe polymerization reaction. After the polymerization reactionis initiated, the monomers such as TFE, the polymerizationinitiator, and a chain transfer agent may be further addeddepending on the purpose.

[0045] The suspension polymerization can be carried out inthe presence of a polymerization initiator. The polymerizationinitiator is not limited as long as it is a polymerizationinitiator capable of generating radicals within thepolymerization temperature range, and known oil-soluble and / orwater-soluble polymerization initiators can be used. Thepolymerization initiator can also be combined with a reducingagent or the like to form a redox agent and initiatepolymerization. The concentration of the polymerizationinitiator is suitably determined according to the type ofmonomer, the molecular weight of the targetpolytetrafluoroethylene, and the reaction rate.

[0046] The polymerization initiator may be a water-solubleradical polymerization initiator.

[0047] Examples of the water-soluble radical polymerizationinitiator include ionic radical initiators, for example,persulfates such as ammonium persulfate, potassium persulfate,and alkali metal persulfates, and permanganate. Such a radicalpolymerization initiator can also be used as an acidic componentand combined with a reducible component such as hydrazine,diimine, iron(II) sulfate, copper(II) sulfate, oxalates,sulfites, or the like to form an oxidation-reduction typeinitiator. A compound capable of forming a hydrate of iron(II)sulfate, copper(II) sulfate, or the like may be an anhydride ora hydrate.

[0048] Examples of the oxidation-reduction type initiatorinclude ammonium persulfate / copper(II) sulfate, ammoniumpersulfate / iron(II) sulfate, ammonium persulfate / sodiumsulfite / iron(II) sulfate, ammoniumpersulfate / azodicarbonamide / copper(II) sulfate, ammoniumpersulfate / sodium azodicarboxylate / copper(II) sulfate, ammoniumcarbamate / copper(II) sulfate, ammonium persulfate / ammoniumcarbamate / copper(II) sulfate, and potassiumpermanganate / ammonium oxalate.

[0049] In the case of such a combination of these oxidationreductiontype initiators, it is preferable that any one may beintroduced into a polymerization tank in advance, and then theother may be added intermittently or continuously withpolymerization being performed.

[0050] The amount of the radical polymerization initiatorused is adjusted so as to enable the reaction rate to befavorably controlled. For example, in the case of ammoniumpersulfate, the amount is preferably 1 to 100 ppm, morepreferably 1 to 50 ppm, and most preferably 1 to 10 ppm based onthe aqueous medium.

[0051] The suspension polymerization is carried out bypolymerizing TFE in an aqueous medium under stirring. Theaqueous medium means a liquid containing water. The aqueousmedium is not limited as long as it contains water.

[0052] The suspension polymerization can be carried out inthe presence or absence of a surfactant. The amount of thesurfactant is preferably 2000 mass ppm or less, more preferably1000 mass ppm or less, even more preferably 500 mass ppm or less,particularly preferably 200 mass ppm or less, and mostpreferably 100 mass ppm or less based on the aqueous medium.The amount of the surfactant may be 0 mass ppm.

[0053] The surfactant for use in the suspensionpolymerization is preferably a fluorine-containing surfactant.Examples of the fluorine-containing surfactant include anionicfluorine-containing surfactants. The anionic fluorinecontainingsurfactant may be, for example, a fluorine atomcontainingsurfactant having 20 or fewer carbon atoms in totalin the portion excluding the anionic group.

[0054] The fluorine-containing surfactant may also be afluorine-containing surfactant in which the molecular weight ofthe anionic moiety is 1,000 or less, preferably 800 or less.The "anionic moiety" means a portion of the fluorine-containingsurfactant excluding the cation. For example, in the case ofF(CF2)n1COOM represented by the formula (I) below, the anionicmoiety is the "F(CF2)n1COO" portion.

[0055] Examples of the fluorine-containing surfactant alsoinclude fluorine-containing surfactants having a LogPOW of 3.5or less. The LogPOW of the fluorine-containing surfactant ispreferably 3.4 or less. The LogPOW is a partition coefficientbetween 1-octanol and water, and is represented by LogP, whereinP represents a ratio of the fluorine-containing surfactantconcentration in octanol / the fluorine-containing surfactantconcentration in water attained when an octanol / water (1:1)mixture containing the fluorine-containing surfactant is phaseseparated.

[0056] The LogPOW is calculated by performing HPLC onstandard substances (heptanoic acid, octanoic acid, nonanoicacid, and decanoic acid) having a known octanol / water partitioncoefficient under conditions having column: TOSOH ODS-120Tcolumn (φ4.6 mm x 250 mm, manufactured by Tosoh Corporation),eluent: acetonitrile / 0.6% by mass HClO4 solution = 1 / 1(vol / vol%), flow rate: 1.0 ml / min, sample volume: 300 μL, columntemperature: 40°C, detection light: UV210 nm to construct acalibration curve concerning each elution time and knownoctanol / water partition coefficient, and determining the HPLCelution time of a sample liquid based on the calibration curve.

[0057] Specific examples of the fluorine-containingsurfactant include those described in U.S. Patent ApplicationPublication No. 2007 / 0015864, U.S. Patent ApplicationPublication No. 2007 / 0015865, U.S. Patent ApplicationPublication No. 2007 / 0015866, U.S. Patent ApplicationPublication No. 2007 / 0276103, U.S. Patent ApplicationPublication No. 2007 / 0117914, U.S. Patent ApplicationPublication No. 2007 / 142541, U.S. Patent Application PublicationNo. 2008 / 0015319, U.S. Patent No. 3250808, U.S. Patent No.3271341, Japanese Patent Laid-Open No. 2003-119204,International Publication No. WO 2005 / 042593, InternationalPublication No. WO 2008 / 060461, International Publication No. WO2007 / 046377, Japanese Patent Laid-Open No. 2007-119526,International Publication No. WO 2007 / 046482, InternationalPublication No. WO 2007 / 046345, U.S. Patent ApplicationPublication No. 2014 / 0228531, International Publication No. WO2013 / 189824, and International Publication No. WO 2013 / 189826.

[0058] The anionic fluorine-containing surfactant may be acompound represented by the following general formula (N0):Xn0-Rfn0-Y0 (N0)wherein Xn0 is H, Cl, or F; Rfn0 is a linear, branched, or cyclicalkylene group having 3 to 20 carbon atoms in which some or allof H are replaced by F, the alkylene group optionally containingone or more ether bonds in which some of H are optionallyreplaced by Cl; and Y0 is an anionic group.The anionic group Y0 may be -COOM, -SO2M, or -SO3M, and maybe -COOM or -SO3M.M is H, a metal atom, NR74, optionally substitutedimidazolium, optionally substituted pyridinium, or optionallysubstituted phosphonium, and R7 is H or an organic group.Examples of the metal atom include alkali metals (Group 1)and alkaline earth metals (Group 2), such as Na, K, or Li.R7 may be H or a C1-10 organic group, may be H or a C1-4organic group, and may be H or a C1-4 alkyl group.M may be H, a metal atom, or NR74, may be H, an alkalimetal (Group 1), an alkaline earth metal (Group 2), or NR74, andmay be H, Na, K, Li, or NH4.In the Rfn0, 50% or more of H atoms may be replaced byfluorine atoms.

[0059] Examples of the compound represented by the generalformula (N0) include a compound represented by the followinggeneral formula (N1):Xn0-(CF2)m1-Y0 (N1)(wherein Xn0 is H, Cl, or F, m1 is an integer of 3 to 15, and Y0is as defined above); a compound represented by the followinggeneral formula (N2):Rfn1-O-(CF(CF3)CF2O)m2CFXn1-Y0 (N2)(wherein Rfn1 is a perfluoroalkyl group having 1 to 5 carbonatoms, m2 is an integer of 0 to 3, Xn1 is F or CF3, and Y0 is asdefined above); a compound represented by the following generalformula (N3):Rfn2(CH2)m3-(Rfn3)q-Y0 (N3)(wherein Rfn2 is a partially or fully fluorinated alkyl grouphaving 1 to 13 carbon atoms and optionally containing an etherbond and / or a chlorine atom, m3 is an integer of 1 to 3, Rfn3 isa linear or branched perfluoroalkylene group having 1 to 3carbon atoms, q is 0 or 1, and Y0 is as defined above); acompound represented by the following general formula (N4):Rfn4-O-(CYn1Yn2)pCF2-Y0 (N4)(wherein Rfn4 is a linear or branched, partially or fullyfluorinated alkyl group having 1 to 12 carbon atoms andoptionally containing an ether bond, Yn1 and Yn2 are the same ordifferent and are each independently H or F, p is 0 or 1, and Y0is as defined above); and a compound represented by thefollowing general formula (N5):(wherein Xn2, Xn3, and Xn4 may be the same or different and areeach independently H, F, or a linear or branched, partially orfully fluorinated alkyl group having 1 to 6 carbon atoms andoptionally containing an ether bond, Rfn5 is a linear orbranched, partially or fully fluorinated alkylene group having 1to 3 carbon atoms and optionally containing an ether bond, L isa linking group, and Y0 is as defined above, provided that thetotal number of carbon atoms of Xn2, Xn3, Xn4, and Rfn5 is 18 orless).

[0060] More specific examples of the compound represented bythe above general formula (N0) include a perfluorocarboxylicacid (I) represented by the following general formula (I), anω-H perfluorocarboxylic acid (II) represented by the followinggeneral formula (II), a perfluoroethercarboxylic acid (III)represented by the following general formula (III), aperfluoroalkylalkylenecarboxylic acid (IV) represented by thefollowing general formula (IV), aperfluoroalkoxyfluorocarboxylic acid (V) represented by thefollowing general formula (V), a perfluoroalkylsulfonic acid(VI) represented by the following general formula (VI), an ω-Hperfluorosulfonic acid (VII) represented by the followinggeneral formula (VII), a perfluoroalkylalkylene sulfonic acid(VIII) represented by the following general formula (VIII), analkylalkylene carboxylic acid (IX) represented by the followinggeneral formula (IX), a fluorocarboxylic acid (X) represented bythe following general formula (X), an alkoxyfluorosulfonic acid(XI) represented by the following general formula (XI), acompound (XII) represented by the following general formula(XII), and a compound (XIII) represented by the followinggeneral formula (XIII).

[0061] The perfluorocarboxylic acid (I) is represented by thefollowing general formula (I):F(CF2)n1COOM (I)wherein n1 is an integer of 3 to 14, M is H, a metal atom, NR74,optionally substituted imidazolium, optionally substitutedpyridinium, or optionally substituted phosphonium, and R7 is Hor an organic group.

[0062] The ω-H perfluorocarboxylic acid (II) is representedby the following general formula (II):H(CF2)n2COOM (II)wherein n2 is an integer of 4 to 15, and M is as defined above.

[0063] The perfluoroethercarboxylic acid (III) is representedby the following general formula (III):Rf1-O-(CF(CF3)CF2O)n3CF(CF3)COOM (III)wherein Rf1 is a perfluoroalkyl group having 1 to 5 carbon atoms,n3 is an integer of 0 to 3, and M is as defined above.

[0064] The perfluoroalkylalkylenecarboxylic acid (IV) isrepresented by the following general formula (IV):Rf2(CH2)n4Rf3COOM (IV)wherein Rf2 is a perfluoroalkyl group having 1 to 5 carbon atoms,Rf3 is a linear or branched perfluoroalkylene group having 1 to3 carbon atoms, n4 is an integer of 1 to 3, and M is as definedabove.

[0065] The alkoxyfluorocarboxylic acid (V) is represented bythe following general formula (V):Rf4-O-CY1Y2CF2-COOM (V)wherein Rf4 is a linear or branched, partially or fullyfluorinated alkyl group having 1 to 12 carbon atoms andoptionally containing an ether bond and / or a chlorine atom; Y1and Y2 are the same or different and are each independently H orF; and M is as defined above.

[0066] The perfluoroalkylsulfonic acid (VI) is represented bythe following general formula (VI):F(CF2)n5SO3M (VI)wherein n5 is an integer of 3 to 14, and M is as defined above.

[0067] The ω-H perfluorosulfonic acid (VII) is represented bythe following general formula (VII):H(CF2)n6SO3M (VII)wherein n6 is an integer of 4 to 14, and M is as defined above.

[0068] The perfluoroalkylalkylenesulfonic acid (VIII) isrepresented by the following general formula (VIII):Rf5(CH2)n7SO3M (VIII)wherein Rf5 is a perfluoroalkyl group having 1 to 13 carbonatoms, n7 is an integer of 1 to 3, and M is as defined above.

[0069] The alkylalkylenecarboxylic acid (IX) is representedby the following general formula (IX):Rf6(CH2)n8COOM (IX)wherein Rf6 is a linear or branched, partially or fullyfluorinated alkyl group having 1 to 13 carbon atoms andoptionally containing an ether bond, n8 is an integer of 1 to 3,and M is as defined above.

[0070] The fluorocarboxylic acid (X) is represented by thefollowing general formula (X):Rf7-O-Rf8-O-CF2-COOM (X)wherein Rf7 is a linear or branched, partially or fullyfluorinated alkyl group having 1 to 6 carbon atoms andoptionally containing an ether bond and / or a chlorine atom; Rf8is a linear or branched, partially or fully fluorinated alkylgroup having 1 to 6 carbon atoms; and M is as defined above.

[0071] The alkoxyfluorosulfonic acid (XI) is represented bythe following general formula (XI):Rf9-O-CY1Y2CF2-SO3M (XI)wherein Rf9 is a linear or branched, partially or fullyfluorinated alkyl group having 1 to 12 carbon atoms andoptionally containing an ether bond and optionally containingchlorine; Y1 and Y2 are the same or different and are eachindependently H or F; and M is as defined above.

[0072] The compound (XII) is represented by the followinggeneral formula (XII):wherein X1, X2, and X3 may be the same or different and are eachindependently H, F, or a linear or branched, partially or fullyfluorinated alkyl group having 1 to 6 carbon atoms andoptionally containing an ether bond; Rf10 is a perfluoroalkylenegroup having 1 to 3 carbon atoms; L is a linking group; and Y0is an anionic group.Y0 may be -COOM, -SO2M, or -SO3M, and may be -SO3M or COOM,wherein M is as defined above.Examples of L include a single bond, and a partially orfully fluorinated alkylene group having 1 to 10 carbon atoms andoptionally containing an ether bond.

[0073] The compound (XIII) is represented by the followinggeneral formula (XIII):Rf11-O-(CF2CF(CF3)O)n9(CF2O)n10CF2COOM (XIII)wherein Rf11 is a fluoroalkyl group having 1 to 5 carbon atomscontaining chlorine, n9 is an integer of 0 to 3, n10 is aninteger of 0 to 3, and M is as defined above. Examples of thecompound (XIII) include CF2ClO(CF2CF(CF3)O)n9(CF2O)n10CF2COONH4 (amixture having an average molecular weight of 750, n9 and n10 inthe formula are defined above).

[0074] Thus, examples of the anionic fluorine-containingsurfactant include a carboxylic acid-based surfactant and asulfonic acid-based surfactant.

[0075] The fluorine-containing surfactant may be onefluorine-containing surfactant, or may be a mixture containingtwo or more fluorine-containing surfactants.

[0076] Examples of the fluorine-containing surfactant includecompounds represented by the following formulae. The fluorinecontainingsurfactant may be a mixture of these compounds.F(CF2)7COOM,F(CF2)5COOM,H(CF2)6COOM,H(CF2)7COOM,CF3O(CF2)3OCHFCF2COOM,C3F7OCF(CF3)CF2OCF(CF3)COOM,CF3CF2CF2OCF(CF3)COOM,CF3CF2OCF2CF2OCF2COOM,C2F5OCF(CF3)CF2OCF(CF3)COOM,CF3OCF(CF3)CF2OCF(CF3)COOM,CF2ClCF2CF2OCF(CF3)CF2OCF2COOM,CF2ClCF2CF2OCF2CF(CF3)OCF2COOM,CF2ClCF(CF3)OCF(CF3)CF2OCF2COOM, andCF2ClCF(CF3)OCF2CF(CF3)OCF2COOM,wherein M is H, a metal atom, NR74, optionally substitutedimidazolium, optionally substituted pyridinium, or optionallysubstituted phosphonium. R7 is H or an organic group.

[0077] The suspension-polymerized particle obtained bysuspension polymerization performed in the presence of thefluorine-containing surfactant usually contains, other than thepolytetrafluoroethylene, the fluorine-containing surfactant.Also, the suspension-polymerized particle obtained bypolymerizing the monomers such as TFE and the modifying monomermay contain, other than the polytetrafluoroethylene, a fluorinecontainingcompound produced by polymerizing the monomers. Inthe present disclosure, the fluorine-containing compound is acompound that is not added during suspension polymerization,such as a compound having a structure similar to that of thefluorine-containing surfactant but having a different number ofcarbon atoms.

[0078] The production method of the present disclosure iscapable of producing a polytetrafluoroethylene particle in whichthe content of the fluorine-containing compound produced bypolymerizing the monomers is reduced. The production method ofthe present disclosure is capable of producing apolytetrafluoroethylene particle in which the content of thefluorine-containing surfactant is reduced even when thesuspension polymerization is carried out in the presence of thefluorine-containing surfactant.

[0079] A typical compound as the fluorine-containing compoundin the suspension-polymerized particle is a fluorine-containingcompound having a hydrophilic group, having a molecular weightof 1000 or less, preferably 800 g / mol or less. The productionmethod of the present disclosure is capable of producing apolytetrafluoroethylene particle in which the content of afluorine-containing compound having a hydrophilic group, havinga molecular weight of 1000 or less, preferably 800 g / mol or lessin the suspension-polymerized particle obtained by polymerizingthe monomers such as TFE, is reduced.

[0080] The hydrophilic group in the fluorine-containingcompound is preferably an anionic group such as an acid group,and examples thereof include -NH2, -PO3M, -OPO3M, -SO3M, -OSO3M,and -COOM (wherein M represents a cation). Of these, thehydrophilic group is preferably -SO3M or -COOM, and morepreferably -COOM.

[0081] The suspension-polymerized particle in one embodimentcontains, as the fluorine-containing compound having thehydrophilic group, a compound represented by the followinggeneral formula (1):General formula (1): [X-Rf-A-]iMi+wherein X represents H, Cl, Br, F or I; Rf represents a linearor branched, partially fluorinated or fully fluorinatedaliphatic group, or a linear or branched, partially fluorinatedor fully fluorinated aliphatic group interrupted by at least oneoxygen atom; A- represents an acid group; Mi+ represents a cationhaving a valence of i; and i represents an integer of 1 to 3.

[0082] The suspension-polymerized particle in one embodimentcontains, as the fluorine-containing compound having thehydrophilic group, a compound represented by the followinggeneral formula (2):General formula (2): [Cn-1F2n-1COO-]M+wherein n represents an integer of 9 to 12 and M+ represents acation.

[0083] The compound (perfluoroalkanoic acid) represented bygeneral formula (2) is known to be formed during polymerizationwhen perfluoroalkyl vinyl ether or the like is used as amodifying monomer (see International Publication No. WO2019 / 161153).

[0084] The suspension-polymerized particle in one embodimentcontains, as the fluorine-containing compound having thehydrophilic group, a compound represented by the followinggeneral formula (3):General formula (3): [R1-O-L-CO2-]M+wherein R1 represents a linear or branched, partiallyfluorinated or fully fluorinated aliphatic group, or a linear orbranched, partially fluorinated or fully fluorinated aliphaticgroup interrupted by at least one oxygen atom; L represents alinear or branched non-fluorinated, partially fluorinated orfully fluorinated alkylene group; and M+ represents a cation.

[0085] The suspension-polymerized particle in one embodimentcontains, as the fluorine-containing compound having thehydrophilic group, a compound represented by general formula(4):General formula (4): [H-(CF2)mCO2-]M+wherein m represents an integer of 3 to 19 and M+ represents acation.

[0086] (Crushing)In the production method of the present disclosure, next, acrushed particle is prepared by washing and then crushing theresulting suspension-polymerized particle, or crushing theresulting suspension-polymerized particle with washing theparticle.

[0087] The suspension-polymerized particle obtained bysuspension polymerization is usually obtained in a wet form. Inthe production method of the present disclosure, the suspension polymerizedparticle in a wet form may be crushed, or thesuspension-polymerized particle in a wet form may be dried andthen crushed. The crushing may be wet crushing or dry crushing.

[0088] Examples of the method for crushing the suspension polymerizedparticle include a crushing method with a crusher.Examples of the crusher include impact type crushers such as ahammer mill, a pin mill, a high-speed rotation mill, and a jetmill, and grinding type crushers for crushing due to the shearforce generated by a rotary blade and a peripheral stator(stationary knife), such as a cutter mill, a feather mill, and acolloid mill. A combination of a plurality of crushing devicesmay be used in crushing.

[0089] The temperature at which crushing treatment is carriedout is preferably -200 to 50°C, more preferably 1°C or higher,more preferably 40°C or lower, and even more preferably 30°C orlower.

[0090] Examples of the method for crushing the suspension polymerizedparticle with washing the particle include a methodinvolving crushing the suspension-polymerized particle in wateror an organic solvent. For example, water or an organic solventand the suspension-polymerized particle may be simultaneouslyfed to a grinding type crusher such as a cutter mill to crushthe suspension-polymerized particle, or water or an organicsolvent and the suspension-polymerized particle may be mixed inadvance and the mixture may be fed to the crusher to crush thesuspension-polymerized particle.

[0091] The suspension-polymerized particle may be washedbefore the suspension-polymerized particle is crushed. Water oran organic solvent can be used for washing the suspensionpolymerizedparticle. The washing may be carried out once ormultiple times.

[0092] Examples of the organic solvent used in such washinginclude ether, halogenated hydrocarbon, aromatic hydrocarbon,pyridine, nitrile, a nitrogen-containing polar organic compound,dimethylsulfoxide, and alcohol.

[0093] The crushing may be carried out once or may berepeatedly carried out until a crushed particle having a desiredaverage particle size or a desired particle size distributioncan be prepared.

[0094] The crushed particle obtained by crushing is usuallyobtained in a wet form. The water content in the crushedparticle after crushing and before dehydration is, for example,more than 40% by mass. In the production method of the presentdisclosure, a wet crushed particle is dehydrated, and subjectedto heat treatment described below. Examples of the method fordehydrating the wet crushed particle include a dehydrationmethod with a dehydrator. Examples of the dehydrator include avibrating dehydrator, a filtering dehydrator, and a centrifugaldehydrator. The dehydration is preferably performed at lowerthan 50°C. The dehydration temperature is the temperature ofthe atmosphere around the crushed particle.

[0095] The wet crushed particle is dehydrated and furtherdried, and then may be subjected to heat treatment describedbelow. The drying is carried out for removal of water from thecrushed particle obtained by crushing. Examples of the methodfor drying the wet crushed particle include a drying method witha dryer.

[0096] Examples of the dryer include a hot air heat-receivingtype dryer, a conductive heat-receiving type dryer, a radiationheat-transfer type dryer, and a high-frequency heat-transfertype dryer. Examples of the dryer include a material-standingtype dryer, a material-transfer type dryer, a material-stirringtype dryer, and a material-conveying type dryer.

[0097] Examples of material-standing type dryer and materialtransfertype dryer which are of hot air heat-receiving typeinclude a box type dryer, a tunnel dryer, a band dryer, a turbovertical dryer, a vertical dryer, and a belt dryer.Examples of the material-stirring type dryer which is ofhot air heat-receiving type include a fluidized bed dryer, adraft rotary dryer, a ditch type stirring dryer, and a multistagedisk dryer.Examples of the material-conveying type dryer which is ofhot air heat-receiving type include an airflow dryer and aspraying dryer (jet dryer, spray dryer).

[0098] Examples of the material-standing type dryer and thematerial-transfer type dryer which are of conductive heatreceivingtype include a vacuum box type dryer, a cylindricaldryer, a vibrating dryer, a vacuum heat treatment dryer, afreeze dryer, and a drum dryer.Examples of the material-stirring type dryer which is ofconductive heat-receiving type include a cylinder type dryer, aditch type dryer, an inverse-cone type dryer, an extrusion dryer,and a steam heating tube bundle rotation dryer.

[0099] Examples of the material-standing type dryer and thematerial-transfer type dryer which are of radiation heattransfertype include an infrared dryer and a superheated steamdryer.

[0100] Examples of the material-standing type dryer and thematerial-transfer type dryer which are of high-frequency heattransfertype include a high-frequency dryer and a microwavedryer.

[0101] In one embodiment of the production method of thepresent disclosure, the crushed particle is dried by airflowdrying. The airflow drying can be carried out using an airflowdryer.

[0102] After the crushed particle is dried by the airflowdrying, a solid-gas mixture containing the crushed particledried and gas may be separated into the crushed particle and thegas by using a cyclone or the like to recover the crushedparticle.

[0103] The temperature for drying the crushed particle ispreferably lower than 300°C, more preferably 280°C or lower,even more preferably 250°C or lower, yet even more preferablylower than 200°C, particularly preferably lower than 180°C andmost preferably lower than 160°C, and is preferably 50°C orhigher and more preferably 100°C or higher. The dryingtemperature is the temperature of the atmosphere around thecrushed particle, and can be specified by measuring thetemperature of hot air in the case of use of hot air in drying.The temperature of hot air can be measured at a feed portthrough which hot air is fed to the dryer or an exhaust portthrough which hot air is exhausted from the dryer, and ispreferably measured at the exhaust port.

[0104] The water content in the crushed particle ispreferably 40% by mass or less, more preferably 20% by mass orless, and even more preferably 10% by mass or less, and thelower limit is not limited, and may be 0.01% by mass or more.The water content in the crushed particle can be adjusted by,for example, dehydrating or drying the crushed particle. Thewater content in the crushed particle can be determined by, forexample, heating and thus sufficiently drying the crushedparticle at 150°C for 3 hours, measuring the mass of the crushedparticle before and after heating, and performing calculationaccording to the following expression.Water content (% by mass) = [(Mass (g) of crushed particlebefore heating) - ((Mass (g) of crushed particle afterheating)] / (Mass (g) of crushed particle after heating) x 100

[0105] After the suspension-polymerized particle is crushed,the resulting crushed particle may be classified by a knownmethod such as airflow classification. The classification canremove any fine particle having a very small particle size andany coarse particle having a very large particle size, to give acrushed particle having a desired average particle size or adesired particle size distribution.

[0106] The average particle size of the crushed particle ispreferably 800 μm or less, more preferably 600 μm or less andeven more preferably 400 μm or less, and is preferably 1 μm ormore, more preferably 5 μm or more, even more preferably 10 μmor more, yet even more preferably 100 μm or more, particularlypreferably 150 μm or more and most preferably more 200 μm.

[0107] (Heat treatment)In the production method of the present disclosure, next, apolytetrafluoroethylene particle is produced by subjecting theresulting crushed particle to heat treatment. The heattreatment is carried out for removal of an acid odor from thecrushed particle obtained by crushing.

[0108] The heat treatment of the crushed particle may bebatch type heat treatment or continuous heat treatment.

[0109] The temperature of the heat treatment is preferably160°C or higher, more preferably 180°C or higher and even morepreferably 200°C or higher, and is preferably 340°C or lower,more preferably 310°C or lower and even more preferably 300°C orlower.

[0110] The heat treatment time is preferably 1 second or more,more preferably 2 seconds or more, even more preferably 1 minuteor more and particularly preferably 3 minutes or more, and ispreferably 24 hours or less, more preferably 2 hours or less andeven more preferably 1 hour or less.

[0111] The heat treatment can be performed, for example, inair or in an inert gas. The heat treatment can be performed,for example, in a gas not containing any active gas such asfluorine gas. The heat treatment can be performed under normalpressure or reduced pressure.

[0112] The heat treatment can be carried out using a dryer.

[0113] Examples of the dryer include a hot air heat-receivingtype dryer, a conductive heat-receiving type dryer, a radiationheat-receiving type dryer, and a high-frequency heat-receivingtype dryer. Examples of the dryer include a material-standingtype dryer, a material-transfer type dryer, a material-stirringtype dryer, and a material-conveying type dryer.

[0114] Examples of the material-standing type dryer and thematerial-transfer type dryer which are of hot air heat-receivingtype include a box type dryer, a tunnel dryer, a band dryer, aturbo vertical dryer, a vertical dryer, and a belt dryer.Examples of the material-stirring type dryer which is ofhot air heat-receiving type include a fluidized bed dryer, adraft rotary dryer, a ditch type stirring dryer, and a multistagedisk dryer.Examples of the material-conveying type dryer which is ofhot air heat-receiving type include an airflow dryer and aspraying dryer (jet dryer, spray dryer).

[0115] Examples of the material-standing type dryer and thematerial-transfer type dryer which are of conductive heat-receiving type include a vacuum box type dryer, a cylindricaldryer, a vibrating dryer, a vacuum heat treatment dryer, afreeze dryer, and a drum dryer.Examples of the material-stirring type dryer which is ofconductive heat-receiving type include a cylinder type dryer, aditch type dryer, an inverse-cone type dryer, an extrusion dryer,and a steam heating tube bundle rotation dryer.

[0116] Examples of the material-standing type dryer and thematerial-transfer type dryer which are of radiation heatreceivingtype include an infrared dryer and a superheated steamdryer.

[0117] Examples of the material-standing type dryer and thematerial-transfer type dryer which are of high-frequency heatreceivingtype include a high-frequency dryer and a microwavedryer.

[0118] The heat treatment of the crushed particle may beperformed by subjecting the crushed particle to fluidization(stirring or conveying) and heat treatment, or may be performedwith the crushed particle being left to still stand. The heattreatment method of the crushed particle is, in particular,preferably a method involving subjecting the crushed particle tofluidization and heat treatment because the heat treatmentefficiency is higher. The method involving subjecting thecrushed particle to fluidization and heat treatment can becarried out using a material-stirring type dryer or a materialconveyingtype dryer. The method involving heat treatment withthe crushed particle being left to still stand can be carriedout using a material-standing type dryer or a material-transfertype dryer.

[0119] The heat treatment of the crushed particle may beperformed by allowing hot air to act on the crushed particle(hot air heat-receiving type), or bringing the crushed particleinto contact with a heat-transfer medium other than hot air. Ofthese, a method involving bringing the crushed particle intocontact with a heat-transfer medium other than hot air ispreferable because the heat efficiency is good. The methodinvolving bringing the crushed particle into contact with aheat-transfer medium other than hot air can be carried out usinga conductive heat-receiving type dryer.

[0120] The crushed particle is subjected to heat treatmentand, if desired, cooled, to give a polytetrafluoroethyleneparticle. The resulting particle can be transferred using gasfrom a dryer to a device where the next step is to be performed.

[0121] When the heat treatment is carried out using hot air,when the crushed particle (polytetrafluoroethylene particle) istransferred by using a gas, or the like, a solid-gas mixturecontaining the crushed particle (polytetrafluoroethyleneparticle) and the gas can be formed. The solid-gas mixtureformed may be separated into the crushed particle(polytetrafluoroethylene particle) and the gas by using acyclone or the like, to recover the crushed particle(polytetrafluoroethylene particle).

[0122] The resulting polytetrafluoroethylene particle may befurther crushed to adjust the particle size of thepolytetrafluoroethylene particle.

[0123] When the polytetrafluoroethylene particle is furthercrushed, such crushing may be wet crushing or dry crushing.Examples of the method for crushing the particle include acrushing method with a crusher. Examples of the crusher includeimpact type crushers such as a hammer mill, a pin mill, a high-speed rotation mill, and a jet mill, and grinding type crushersfor crushing due to the shear force generated by a rotary bladeand a peripheral stator (stationary knife), such as a cuttermill, a feather mill, and a colloid mill.

[0124] The temperature at which the crushing is carried outis preferably -200 to 50°C, more preferably 1°C or higher, morepreferably 40°C or lower, and even more preferably 30°C or lower.

[0125] The resulting polytetrafluoroethylene particle may beclassified by a known method such as airflow classification.The classification can remove any fine particle having a verysmall particle size and any coarse particle having a very largeparticle size, to give a polytetrafluoroethylene particle havinga desired average particle size or a desired particle sizedistribution.

[0126] The average particle size of thepolytetrafluoroethylene particle is preferably 200 μm or less,more preferably 100 μm or less, even more preferably less than100 μm, yet even more preferably 70 μm or less, particularlypreferably 50 μm or less and most preferably 30 μm or less, andis preferably 1 μm or more, more preferably 5 μm or more andeven more preferably 10 μm or more. If the average particlesize of the polytetrafluoroethylene particle is too large,formability of the polytetrafluoroethylene particle easilydeteriorates and forming defects easily occur in a formedarticle. If the average particle size of thepolytetrafluoroethylene particle is too small, handleabilitytends to be inferior.

[0127] The average particle size of thepolytetrafluoroethylene particle is a 50% cumulative particlesize measured by a laser diffraction method. In the presentdisclosure, the average particle size of any other particle, forexample, the suspension-polymerized particle, is also a 50%cumulative particle size measured by a laser diffraction method.

[0128] The content of a high-temperature volatile substancein the polytetrafluoroethylene particle is preferably 0.050% bymass or less, more preferably 0.030% by mass or less and evenmore preferably 0.020% by mass or less, and is preferably 0.001%by mass or more, more preferably 0.003% by mass or more and evenmore preferably 0.005% by mass or more, based on the mass of thepolytetrafluoroethylene particle.

[0129] The content of the high-temperature volatile substancein the polytetrafluoroethylene particle can be determined bymeasuring the mass of the polytetrafluoroethylene particleheated at 370°C for 2 hours according to JIS K 6891, andperforming calculation according to the following expression.High-temperature volatile substance (% by mass) = [(Mass(g) of polytetrafluoroethylene particle before heating) - (Mass(g) of polytetrafluoroethylene particle after heating)] / (Mass(g) of polytetrafluoroethylene particle before heating) x 100

[0130] The standard specific gravity of thepolytetrafluoroethylene particle may be 2.130 to 2.280, and ispreferably 2.200 or less and more preferably 2.135 or more.

[0131] The standard specific gravity of thepolytetrafluoroethylene particle can be measured according toASTM D4894.

[0132] The specific surface area of thepolytetrafluoroethylene particle is preferably 5.0 m2 / g or less,more preferably 4.5 m2 / g or less and even more preferably 4.0m2 / g or less, and is preferably 0.1 m2 / g or more and morepreferably 1.0 m2 / g or more.

[0133] The specific surface area of thepolytetrafluoroethylene particle can be measured according tothe BET method, based on JIS Z8830, by using a mixed gas of 30%of nitrogen and 70% of helium, as a carrier gas, and cooling thegas with liquid nitrogen.

[0134] The apparent density of the polytetrafluoroethyleneparticle is preferably 0.55 g / cm3 or less, more preferably 0.50g / cm3 or less and even more preferably 0.45 g / cm3 or less, andis preferably 0.15 g / cm3 or more, more preferably 0.20 g / cm3 ormore and even more preferably 0.25 g / cm3 or more.

[0135] The apparent density of the polytetrafluoroethyleneparticle can be measured according to JIS K 6891.

[0136] The polytetrafluoroethylene contained in thepolytetrafluoroethylene particle may be ahomopolytetrafluoroethylene containing only TFE unit, or may bea modified polytetrafluoroethylene containing TFE unit and amodifying-monomer unit that is based on a modifying monomercopolymerizable with TFE.

[0137] Examples of the modifying monomer forming themodifying-monomer unit include a modifying monomer used in theproduction method of the present disclosure, and the samemodifying monomer as that used in the production method of thepresent disclosure is preferable.

[0138] The content of the modifying-monomer unit inpolytetrafluoroethylene is preferably 0.001% by mass or more,more preferably 0.01% by mass or more, even more preferably0.03% by mass or more and particularly preferably 0.05% by massor more, and is preferably 1.0% by mass or less, more preferably0.8% by mass or less, even more preferably 0.5% by mass or lessand particularly preferably 0.3% by mass or less, based on allpolymerization units constituting polytetrafluoroethylene.

[0139] In the present disclosure, the content of each of themonomer units constituting polytetrafluoroethylene can becalculated by appropriately combining NMR, FT-IR, elementalanalysis, and X-ray fluorescence analysis in accordance with thetypes of the monomers. The content of each of the monomer unitsconstituting polytetrafluoroethylene can also be determined bycalculation from the amount of the modifying monomer added, usedin polymerization.

[0140] The polytetrafluoroethylene particle in one embodimentcontains a fluorine-containing compound.

[0141] The polytetrafluoroethylene particle in one embodimentis substantially free from a fluorine-containing compound. Thefluorine-containing compound is a compound not added insuspension polymerization, as described above. A typicalcompound as the fluorine-containing compound is a fluorinecontainingcompound having a hydrophilic group, having amolecular weight of 1000 or less, preferably 800 g / mol or less.

[0142] The polytetrafluoroethylene particle in one embodimentis substantially free from, as the fluorine-containing compoundhaving the hydrophilic group, a compound represented by thefollowing general formula (1):General formula (1): [X-Rf-A-]iMi+wherein X is H, Cl, Br, F, or I; Rf is a linear or branched,partially fluorinated or fully fluorinated aliphatic group, or alinear or branched, partially fluorinated or fully fluorinatedaliphatic group interrupted by at least one oxygen atom; A- isan acid group; Mi+ is a cation having a valence of i; and irepresents an integer of 1 to 3.

[0143] The polytetrafluoroethylene particle in one embodimentis substantially free from, as the fluorine-containing compoundhaving the hydrophilic group, a compound represented by thefollowing general formula (2):General formula (2): [Cn-1F2n-1COO-]M+wherein n is an integer of 9 to 12, and M+ represents a cation.

[0144] The compound (perfluoroalkanoic acid) represented bygeneral formula (2) is known to be formed during polymerizationwhen perfluoroalkyl vinyl ether or the like is used as amodifying monomer (see International Publication No. WO2019 / 161153).

[0145] The polytetrafluoroethylene particle in one embodimentis substantially free from, as the fluorine-containing compoundhaving the hydrophilic group, a compound represented by thefollowing general formula (3):General formula (3): [R1-O-L-CO2-]M+wherein R1 represents a linear or branched, partiallyfluorinated or fully fluorinated aliphatic group, or a linear orbranched, partially fluorinated or fully fluorinated aliphaticgroup interrupted by at least one oxygen atom; L represents alinear or branched non-fluorinated, partially fluorinated orfully fluorinated alkylene group; and M+ represents a cation.

[0146] The polytetrafluoroethylene particle in one embodimentis substantially free from, as the fluorine-containing compoundhaving the hydrophilic group, a compound represented by generalformula (4):General formula (4): [H-(CF2)mCO2-]M+wherein m represents an integer of 3 to 19, and M+ represents acation.

[0147] In the present disclosure, "substantially free fromthe fluorine-containing compound (fluorine-containing compoundhaving the hydrophilic group)" means that the content of thefluorine-containing compound (fluorine-containing compoundgenerated by polymerizing the monomers) in thepolytetrafluoroethylene particle is 1 mass ppm or less based onpolytetrafluoroethylene. The content of the fluorine-containingcompound (fluorine-containing compound having the hydrophilicgroup) in the polytetrafluoroethylene particle is preferably 100mass ppb or less, more preferably 50 mass ppb or less, even morepreferably 10 mass ppb or less, even more preferably 5 mass ppbor less and particularly preferably 1 mass ppb or less, and thecontent of the fluorine-containing surfactant is most preferablyless than the detection limit in measurement by liquidchromatography-mass spectrometry (LC / MS).

[0148] The content of the fluorine-containing compound(fluorine-containing compound having the hydrophilic group) canbe quantified by a known method. For example, the content canbe quantified by LC / MS analysis.First, methanol is added to the polytetrafluoroethyleneparticle to perform extraction, and the resulting extract issubjected to LC / MS analysis. In order to further improve theextraction efficiency, treatment by Soxhlet extraction,ultrasonic treatment, or the like may be performed.Molecular weight information is extracted from theresulting LC / MS spectrum to confirm agreement with thestructural formula of the candidate fluorine-containing compound(fluorine-containing compound having the hydrophilic group).Thereafter, aqueous solutions having five or more differentcontent levels of the confirmed fluorine-containing compound(fluorine-containing compound having the hydrophilic group) areprepared, and the LC / MS analysis is carried out on the aqueoussolutions with the respective content levels, and therelationship between the content level and the areacorresponding to that content level is plotted to draw acalibration curve.Then, using the calibration curve, the area of the LC / MSchromatogram of the fluorine-containing compound (fluorinecontainingcompound having the hydrophilic group) in the extractcan be converted to the content of the fluorine-containingcompound (fluorine-containing compound having the hydrophilicgroup).

[0149] The polytetrafluoroethylene particle in one embodimentcontains a fluorine-containing surfactant. Thepolytetrafluoroethylene particle in one embodiment contains thefluorine-containing compound and a fluorine-containingsurfactant.

[0150] The polytetrafluoroethylene particle in one embodimentis substantially free from a fluorine-containing surfactant.

[0151] In the present disclosure, "substantially free from afluorine-containing surfactant" means that the content of thefluorine-containing surfactant in the polytetrafluoroethyleneparticle is 1 mass ppm or less. The content of the fluorinecontainingsurfactant in the polytetrafluoroethylene particle ispreferably 100 mass ppb or less, more preferably 50 mass ppb orless, even more preferably 10 mass ppb or less, even morepreferably 5 mass ppb or less and particularly preferably 1 massppb or less, and the content of the fluorine-containingsurfactant is most preferably less than the detection limit inmeasurement by liquid chromatography-mass spectrometry (LC / MS).

[0152] The content of the fluorine-containing surfactant canbe quantified by a known method. For example, the content canbe quantified by LC / MS analysis.First, methanol is added to the polytetrafluoroethyleneparticle to perform extraction, and the resulting extract issubjected to LC / MS analysis. In order to further improve theextraction efficiency, treatment by Soxhlet extraction,ultrasonic treatment, or the like may be performed.Molecular weight information is extracted from theresulting LC / MS spectrum to confirm agreement with thestructural formula of the candidate fluorine-containingsurfactant.Thereafter, aqueous solutions having five or more differentcontent levels of the confirmed fluorine-containing surfactantare prepared, and the LC / MS analysis is carried out on theaqueous solutions with the respective content levels, and therelationship between the content level and the areacorresponding to that content level is plotted to draw acalibration curve.Then, using the calibration curve, the area of the LC / MSchromatogram of the fluorine-containing surfactant in theextract can be converted to the content of the fluorinecontainingsurfactant.

[0153] (Forming)The present disclosure also relates to apolytetrafluoroethylene particle obtained by the productionmethod. The polytetrafluoroethylene particle obtained by theproduction method is usually obtained as a powder including aplurality of polytetrafluoroethylene particles.

[0154] The polytetrafluoroethylene particle obtained by theproduction method of the present disclosure can be formed togive a polytetrafluoroethylene formed article. Thepolytetrafluoroethylene particle obtained by the productionmethod of the present disclosure has a decreased acid odor, andthus the polytetrafluoroethylene particle can be used tosignificantly improve a working environment during forming.

[0155] Examples of the method for forming thepolytetrafluoroethylene particle include compression molding,ram extrusion forming, and isobaric compression molding. Theforming method is, of these, preferably compression molding.The polytetrafluoroethylene particle is compression molded,thereby providing a polytetrafluoroethylene compression-moldedarticle.

[0156] In compression molding, in general, thepolytetrafluoroethylene particle is placed in a mold andcompressed to prepare a preform, and the resulting preform isloaded in a furnace, sintered, and cooled, thereby providing acompression-molded article.

[0157] The compression molding can be performed by, forexample, placing the polytetrafluoroethylene particle in a mold,compressing the polytetrafluoroethylene particle at 1 to 100 MPa,and heating and sintering a preform obtained by compression, at345 to 400°C.

[0158] A formed article having a desired shape may beprepared by processing the polytetrafluoroethylene formedarticle by machining such as cutting. For example, apolytetrafluoroethylene sheet can be obtained by cutting thepolytetrafluoroethylene formed article. The resultingpolytetrafluoroethylene sheet can be used in lining sheets,packings, gaskets, and diaphragm valves. The resultingpolytetrafluoroethylene sheet can also be used in heat-resistantelectric wires, heat-resistant insulating tapes for vehiclemotors / generators, release sheets, and the like.

[0159] The polytetrafluoroethylene formed article can also beused in sealants, casing, sleeves, bellows, hoses, piston rings,butterfly valves, square tanks, wafer carriers, and the like.

[0160] The polytetrafluoroethylene particle obtained by theproduction method of the present disclosure and thepolytetrafluoroethylene particle of the present disclosure canalso be used in raw materials for granulation, and raw materialsfor compounds. The polytetrafluoroethylene particle obtained bythe production method of the present disclosure and thepolytetrafluoroethylene particle of the present disclosure maybe granulated by a known granulation method. A filler may beappropriately compounded to the polytetrafluoroethylene particleobtained by the production method of the present disclosure andthe polytetrafluoroethylene particle of the present disclosure.Furthermore, a powder for forming, to which a filler iscompounded, may be granulated by a known granulation method.The resulting granulated product and material for forming may beformed in the same manner as in the method for forming thepolytetrafluoroethylene particle.

[0161] While embodiments have been described above, it willbe understood that various changes in form and details can bemade without departing from the gist and scope of the claims.EXAMPLES

[0162] Next, embodiments of the present disclosure will nowbe described by way of Examples, but the present disclosure isnot limited only to the Examples.

[0163] Various numerical values in the Examples were measuredby the following methods.

[0164] <Water content>The water content was determined by, heating and thussufficiently drying a crushed particle ofpolytetrafluoroethylene at 150°C for 3 hours, measuring the massof the crushed particle before and after heating, and performingcalculation according to the following expression.Water content (% by mass) = [(Mass (g) of crushed particlebefore heating) - (Mass (g) of crushed particle afterheating] / (Mass (g) of crushed particle after heating) x 100

[0165] <Average particle size (50% cumulative particle size)>The average particle size was determined by the followinglaser diffraction method. The method was performed in a drymanner by using HELOS & RODOS system (trade name, manufacturedby Sympatec GmbH). The shade of a measurement powder dispersedby compressed air at a dispersion pressure of 2 bar wasreflected by laser and detected by a measurement sensor portion,thereby computing the particle size distribution of themeasurement powder, and thus the value of the average particlesize (50% cumulative particle size) d50 was determined on avolume basis. The d50 was equal to the particle sizecorresponding to 50% in cumulative particle size distributionaccumulation.

[0166] <Hydrogen fluoride concentration>10 kg of the polytetrafluoroethylene particle was added toa plastic bag made of PET, having a volume of 60 L, and left tostill stand at room temperature in a cold dark place for 10 days.The gas in the bag was suctioned by using a hydrogen fluoridedetector tube, according to the method recommended by themanufacturer, and the hydrogen fluoride concentration in the bagwas determined from an indicated value. The detection limit was0.05 mass ppm.

[0167] <Standard specific gravity (SSG)>Using a sample formed in accordance with ASTM D4894, theSSG was measured by the water replacement method in accordancewith ASTM D792.

[0168] <Specific surface area>The specific surface area of the polytetrafluoroethyleneparticle was measured according to the BET method (flow method,one-point method), based on JIS Z8830, by using a mixed gas of30% of nitrogen and 70% of helium, as a carrier gas, and coolingthe gas with liquid nitrogen. The equipment here used wasMacsorb HM Model-1210.

[0169] <Content of perfluoro(propyl vinyl ether) (PPVE)>The content of PPVE in polytetrafluoroethylene wasdetermined by press-forming the polytetrafluoroethylene particleto produce a thin film, subjecting the thin film disk to FT-IRmeasurement to provide the infrared absorbance, and multiplyingthe ratio of absorbance at 995 cm-1 / absorbance at 935 cm-1 by0.14.

[0170] <Measurement of fluorine-containing compound havinghydrophilic group>[Method for measuring content of compound represented by generalformula (2)]Extraction from polytetrafluoroethylene particle10 mL of methanol was added to 0.30 g of thepolytetrafluoroethylene particle, ultrasonic treatment wasperformed with warming to 60°C for 120 minutes, and asupernatant including a compound represented by general formula(2) was extracted.General formula (2): [Cn-1F2n-1COO-]M+(wherein n represents an integer of 9 to 12 and M+ represents acation.)

[0171] Measurement of content of compound represented bygeneral formula (2), contained in extractCalibration curveFive concentration levels of methanol standard solutions ofperfluorononanoic acid (PFNA), perfluorodecanoic acid (PFDA),perfluoroundecanoic acid (PFUnDA), and perfluorododecanoic acid(PFDoDA) having known concentrations were prepared in each ofconcentration ranges of 0.03 to 0.5 ng / mL, 0.5 to 5 ng / mL, and 5to 50 ng / mL, and measurement was made using a liquidchromatograph-mass spectrometer. First-order approximation wasused to create calibration curves from the sample concentrationsand peak integral values thereof. The lower limit ofquantification was 1 ppb / polymer.

[0172] Measuring instrument configuration and LC-MSmeasurement conditions[Table 1]

[0173] SRM measurement parameters[Table 2]

[0174] Content of compound represented by general formula (2),contained in extractThe compound represented by general formula (2) wasmeasured using a liquid chromatograph-mass spectrometer.Concerning the liquid phase extracted, the peak area of thecompound represented by general formula (2) with respect to eachnumber of carbon atoms was determined by an SRM method, and thecontent of the compound represented by general formula (2)contained in the polytetrafluoroethylene particle was determined.

[0175] Production Example 1Polymerization of tetrafluoroethylene was performed by themethod described in Production Example 3 of InternationalPublication No. WO 2003 / 035724. In the polymerization, theamount of PPVE was 85 g, and no surfactant was used. Theresulting suspension-polymerized particle ofpolytetrafluoroethylene was taken out and washed with pure watertwice, and washed and simultaneously crushed by a high-speedrotation mill, to an average particle size of 350 μm, therebyproviding a crushed particle. The resulting crushed particlewas dehydrated by a vibrating dehydrate, to a water content of5% by mass, thereby providing a dehydrated crushed particle.Then, a solid-gas mixture containing the crushed particle andgas was formed, then airflow dried under temperature adjustmentso that the temperature measured at an exhaust port of hot airwas 130°C, and separated into the crushed particle and the gas,thereby providing a crushed particle dried. The averageparticle size of the resulting crushed particle was 350 μm.

[0176] Example 1A solid-gas mixture containing the crushed particleobtained in Production Example 1 and gas was formed, and thencrushed by an air jet mill and separated into the crushedparticle and the gas, thereby providing apolytetrafluoroethylene particle. The average particle size ofthe resulting polytetrafluoroethylene particle was 26 μm. Anacid odor was felt and the hydrogen fluoride concentration was4.8 mass ppm. The standard specific gravity was 2.171. Thespecific surface area was 3.5 m2 / g. The content of PPVE inpolytetrafluoroethylene was 0.062% by mass.

[0177] Example 2The crushed particle obtained in Production Example 1 wasfed to a vibrating dryer as a material-conveying type dryerwhich was of conductive heat-receiving type, and heat treatmentat 250°C for 12 minutes was performed. Then, a solid-gasmixture containing the crushed particle and gas was formed, andthen crushed by an air jet mill and separated into the crushedparticle and the gas, thereby providing apolytetrafluoroethylene particle. The average particle size ofthe resulting polytetrafluoroethylene particle was 30 μm. Noacid odor was felt. The hydrogen fluoride concentration was 1.0mass ppm. The standard specific gravity was 2.171. Thespecific surface area was 3.4 m2 / g.

[0178] Example 3The crushed particle obtained in Production Example 1 wasfed to an inverse-cone type dryer as a material-stirring typedryer which was of conductive heat-receiving type, and heattreatment at 250°C for 6 hours was performed. Then, a solid-gasmixture containing the crushed particle and gas was formed, andthen crushed by a feather mill and separated into the crushedparticle and the gas, thereby providing apolytetrafluoroethylene particle. The average particle size ofthe resulting polytetrafluoroethylene particle was 29 μm. Noacid odor was felt and the hydrogen fluoride concentration was0.3 mass ppm. The standard specific gravity was 2.171. Thespecific surface area was 3.7 m2 / g.

[0179] Example 4The crushed particle obtained in Production Example 1 wasfed to a fluidized bed dryer as a material-stirring type dryerwhich was of hot air heat-receiving type, and heat treatment at250°C for 1.5 hours was performed. Then, a solid-gas mixturecontaining the crushed particle and gas was formed, and thencrushed by an air jet mill and separated into the crushedparticle and the gas, thereby providing apolytetrafluoroethylene particle. The average particle size ofthe resulting polytetrafluoroethylene particle was 26 μm. Noacid odor was felt and the hydrogen fluoride concentration was0.5 mass ppm. The standard specific gravity was 2.171. Thespecific surface area was 3.7 m2 / g.

[0180] Example 5Polymerization of tetrafluoroethylene was performed by themethod described in Production Example 3 of InternationalPublication No. WO 2003 / 035724. In the polymerization, theamount of PPVE was 85 g, and no surfactant was used. Theresulting suspension-polymerized particle ofpolytetrafluoroethylene was taken out, washed and simultaneouslycrushed by a high-speed rotation mill and furthermore crushed bya colloid mill, to an average particle size of 300 μm, therebyproviding a crushed particle. The resulting crushed particlewas dehydrated by vibrating dehydration to a water content of 5%by mass, thereby providing a dehydrated crushed particle. Thecrushed particle was fed to a vibrating dryer as a materialconveyingtype dryer which was of conductive heat-receiving type,and heat treatment at 250°C for 15 minutes was performed. Then,a solid-gas mixture containing the crushed particle and gas wasformed, and then crushed by an air jet mill and separated intothe crushed particle and the gas, thereby providing apolytetrafluoroethylene particle. The average particle size ofthe resulting polytetrafluoroethylene particle was 21 μm. Noacid odor was felt. The hydrogen fluoride concentration was 0mass ppm. The standard specific gravity was 2.171. Thespecific surface area was 3.6 m2 / g. The content of PPVE inpolytetrafluoroethylene was 0.062% by mass.

[0181] Example 6The crushed particle obtained in Production Example 1 wasfed to a vibrating dryer as a material-conveying type dryerwhich was of conductive heat-receiving type, and heat treatmentat 260°C for 10 minutes was performed. Here, hot air at 260°Cwas entrained. Then, a solid-gas mixture containing the crushedparticle and gas was formed, and then crushed by an air jet milland separated into the crushed particle and the gas, therebyproviding a polytetrafluoroethylene particle. The averageparticle size of the resulting polytetrafluoroethylene particlewas 23 μm. No acid odor was felt. The hydrogen fluorideconcentration was 0.3 mass ppm. The standard specific gravitywas 2.171. The specific surface area was 3.4 m2 / g.

[0182] The content of the compound represented by generalformula (2) is shown in Table 3.[Table 3]

Claims

1. A method for producing a polytetrafluoroethylene particle, comprising: subjecting tetrafluoroethylene to suspension polymerization in an aqueous medium to prepare a suspension-polymerized particle of a polytetrafluoroethylene; washing and then crushing the suspension-polymerized particle or crushing the suspension-polymerized particle with washing to prepare a crushed particle; dehydrating the crushed particle to prepare a crushed particle having a water content of 40% by mass or less; and subjecting the dehydrated crushed particle to heat treatment to produce a polytetrafluoroethylene particle.

2. The production method according to claim 1, the method comprising, after dehydrating the crushed particle, further drying the crushed particle.

3. The production method according to claim 2, wherein the crushed particle is dried by airflow drying.

4. The production method according to any one of claims 1 to 3, wherein a temperature of the heat treatment is 200°C or higher.

5. The production method according to any one of claims 1 to 4, wherein the heat treatment is performed using a conductive heat-receiving type dryer.

6. The production method according to any one of claims 1 to 4, wherein the heat treatment is performed using a materialstirring type dryer or a material-conveying type dryer.

7. The production method according to any one of claims 1 to 6, the method comprising, in the heat treatment or during transferring of the polytetrafluoroethylene particle after the heat treatment, forming a solid-gas mixture containing the polytetrafluoroethylene particle generated by the heat treatment and gas, separating the solid-gas mixture into the polytetrafluoroethylene particle and the gas, and recovering the polytetrafluoroethylene particle to produce the polytetrafluoroethylene particle.

8. The production method according to any one of claims 1 to 7, wherein an average particle size of the crushed particle is 100 to 800 μm.

9. The production method according to any one of claims 1 to 8, the method comprising, after subjecting the crushed particle to the heat treatment to produce the polytetrafluoroethylene particle, further crushing the polytetrafluoroethylene particle to produce a polytetrafluoroethylene particle having an average particle size of 200 μm or less.

10. The production method according to any one of claims 1 to 9, wherein tetrafluoroethylene and a modifying monomer are subjected to suspension polymerization.

11. The production method according to any one of claims 1 to 10, wherein a standard specific gravity of the polytetrafluoroethylene particle is 2.200 or less.

12. The production method according to any one of claims 1 to 11, wherein a specific surface area of the polytetrafluoroethylene particle is 5.0 m2 / g or less.

13. The production method according to any one of claims 1 to 12, wherein the polytetrafluoroethylene particle is substantially free from a compound represented by the following general formula (2): General formula (2): [Cn-1F2n-1COO-]M+ wherein n represents an integer of 9 to 12 and M+ represents a cation.

14. The production method according to any one of claims 1 to 13, wherein suspension polymerization is carried out in the presence or absence of a surfactant, and an amount of the surfactant is 2000 mass ppm or less based on the aqueous medium.

15. A method for producing a polytetrafluoroethylene formed article, the method comprising producing the polytetrafluoroethylene particle by the production method according to any one of claims 1 to 14, and then forming the polytetrafluoroethylene particle to give a formed article.

16. A method for producing a polytetrafluoroethylene compression-molded article, the method comprising producing the polytetrafluoroethylene particle by the production method according to any one of claims 1 to 14, and then compression molding the polytetrafluoroethylene particle to give a compression-molded article.

17. A polytetrafluoroethylene particle obtained by the production method according to any one of claims 1 to 14.