Electrode lead, method for producing same, and pouch-type secondary battery

IN597702BActive Publication Date: 2026-08-03LG ENERGY SOLUTION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
IN202217048673
Authority / Receiving Office
IN · IN
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-07
Filing Date
2022-08-26
Publication Date
2026-08-03
Estimated Expiration
2041-03-17

AI Technical Summary

Technical Problem

Pouch type secondary batteries lack effective gas discharge mechanisms and reliable electrical disconnection methods, leading to safety issues such as increased internal pressure, component damage, and potential explosions due to insufficient protection measures.

Method used

A two-stage electrode lead system is introduced, where a first electrode lead is connected to an electrode tab and a second lead protrudes outside the battery case, with a connection part formed by curing an adhesive mixture of conductive materials and solvents, ensuring safe gas discharge and complete electrical disconnection.

Benefits of technology

The two-stage electrode lead system effectively discharges gases externally, ensuring safety and completely cutting off electrical connections, while maintaining low contact resistance and improved electrolyte resistance, thus preventing internal pressure issues and component damage.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

An electrode lead according to an embodiment of the present invention for addressing the problem includes: a first electrode lead having one end connected to an electrode tab protruding from one side of an electrode assembly; a second electrode lead having one end connected to the other end of the first electrode lead and the other end protruding to the outside of a battery case accommodating the electrode assembly; and a connection part that connects the first electrode lead and the second electrode lead to each other. The connection part is formed by curing an adhesive applied between the first electrode lead and the second electrode lead, wherein the adhesive is formed by mixing a conductive material and a solvent. The solvent is formed by mixing a polymer and a diluent and includes 5 wt% to 15 wt% of the diluent.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0002] The present invention relates to an electrode lead, amethod for manufacturing the same, and a pouch type secondarybattery, and more particularly, to an electrode lead, whichis formed in two stages to discharge a gas generated in abattery case to the outside, thereby securing safety, and inwhich the two-stage electrode leads are reliably detached tocompletely cut off electrical connection, a method formanufacturing the same, and a pouch type secondary battery.BACKGROUND ART

[0003] In general, secondary batteries include nickelcadmiumbatteries, nickel-hydrogen batteries, lithium ionbatteries, and lithium ion polymer batteries. Such asecondary battery is being applied to and used in small-sizedproducts such as digital cameras, P-DVDs, MP3Ps, mobilephones, PDAs, portable game devices, power tools, E-bikes,and the like as well as large-sized products requiring highpower such as electric vehicles and hybrid vehicles, powerstorage devices for storing surplus power or renewable energy,andbackuppowerstoragedevices.

[0004] In order to manufacture an electrode assembly, acathode (hereinafter, referred to as a positive electrode), aseparator, and an anode (hereinafter, referred to as anegative electrode) are manufactured and stacked.Specifically, positive electrode active material slurry isapplied to a positive electrode collector, and negativeelectrode active material slurry is applied to a negativeelectrode collector to manufacture a positive electrode and anegative electrode. Also, when the separator is interposedand stacked between the manufactured positive electrode andthe manufactured negative electrode, unit cells are formed.The unit cells are stacked on each other to form an electrodeassembly. Also, when the electrode assembly is accommodatedin a specific case, and an electrolyte is injected, thesecondary battery is manufactured.

[0005] Such a secondary battery is classified into a pouchtype secondary battery and a can type secondary batteryaccording to a material of a battery case accommodating anelectrode assembly. In the pouch type secondary battery, theelectrode assembly is accommodated in a pouch made of aflexible polymer material having a variable shape. Also, inthe can type secondary battery, an electrode assembly isaccommodated in a case made of a metal or plastic materialhaving a predetermined shape.

[0006] The pouch type battery case is manufactured byperforming drawing molding on a pouch film having flexibilityto form a cup part. In addition, when the cup part is formed,an electrode assembly is accommodated in an accommodationspace of the cup part, and then, the battery case is foldedtosealasealingpart,therebymanufacturingasecondarybattery.

[0007] In the secondary battery, a gas in the secondarybattery may be generated by internal short-circuit,overcharging, overdischarging, or the like. Here, the gasmay allow the secondary battery to increase in internalpressure to cause problems such as weakening of bonding forcebetween components, damage of a case of the secondary battery,an early operation of a protection circuit, deformation of anelectrode, internal short-circuit, explosion, and the like.Thus, in the case of the can type secondary battery, aprotection member such as a CID filter and a safety vent isprovided to physically interrupt an electrical connectionwhen an internal pressure of a case increases. However, inthe case of the pouch type secondary battery according to therelated art, the protection member is not sufficientlyprovided.

[0008] (Patent Document 1)

[0009] Korean Patent Publication No. 2019-0059677DISCLOSURE OF THE INVENTIONTECHNICAL PROBLEM

[0010] An object of the present invention is to provide anelectrode lead, which is formed in two stages to discharge agas generated in a battery case to the outside, therebysecuring safety, and in which the two-stage electrode leadsare reliably detached to completely cut off electricalconnection, a method for manufacturing the same, and a pouchtype secondary battery.

[0011] The objects of the present invention are not limitedto the aforementioned object, but other objects not describedherein will be clearly understood by those skilled in the artfrom descriptions below.TECHNICAL SOLUTION

[0012] An electrode lead according to an embodiment of thepresent invention for achieving the above object includes: afirst electrode lead having one end connected to an electrodetab protruding from one side of an electrode assembly; asecond electrode lead having one end connected to the otherend of the first electrode lead and the other end protrudingto the outside of a battery case accommodating the electrodeassembly; and a connection part configured to connect thefirst electrode lead to the second electrode lead, whereinthe connection part is formed by curing an adhesive appliedbetween the first electrode lead and the second electrodelead, the adhesive is formed by mixing a conductor and asolvent, the solvent is formed by mixing a polymer and adiluent, and the solvent contains 5 wt% to 15 wt% of thediluent.

[0013] Also, the solvent may contain 5 wt% to 10 wt% of thediluent.

[0014] Also, the diluent may include a glycidyl ester-basedmaterial.

[0015] Also, the adhesive may contain 70 wt% to 85 wt% ofthe conductor and 15 wt% to 30 wt% of the solvent.

[0016] Also, the conductor may include at least one ofgraphite, carbon black, conductive fiber, metal powder,conductive whisker, conductive metal oxide, or conductivematerial.

[0017] Also, the conductor may include silver.

[0018] Also, the polymer may include at least one of anacrylic resin, an epoxy resin, an ethylene propylene dienemonomer (EPDM) resin, a chlorinated polyethylene (CPE) resin,silicone, polyurethane, a urea resin, a melamine resin, aphenol resin, an unsaturated ester resin, polypropylene (PP),polyethylene (PE), polyimide, or polyamide.

[0019] Also, the polymer may include an epoxy resin.

[0020] A pouch type secondary battery according to anembodiment of the present invention for achieving the aboveobject includes: an electrode assembly in which electrodesincluding a positive electrode and a negative electrode andseparators are stacked; a pouch-shaped battery caseconfigured to accommodate the electrode assembly; anelectrode tab connected to the electrodes and protruding fromone side of the electrode assembly; a first electrode leadhaving one end connected to the electrode tab; a secondelectrode lead having one end connected to the other end ofthe first electrode lead and the other end protruding to theoutside of the battery case; and a connection part configuredto connect the first electrode lead to the second electrodelead, wherein the connection part is formed by curing anadhesive applied between the first electrode lead and thesecond electrode lead, the adhesive is formed by mixing aconductive material and a solvent, the solvent is formed bymixing a polymer and a diluent, and the solvent contains 5wt% to 15 wt% of the diluent.

[0021] Also, the pouch type secondary battery may furtherinclude an insulation part configured to surround a portionat which the first and second electrode leads are connectedto each other through the connection part and configured tobond the first and second electrode leads to the battery case.

[0022] Also,bondingforcebetweeneachofthefirstandsecond electrode leads and the connection part may be lessthan that between each of the first and second electrodeleads and the insulation part.

[0023] Also, the insulation part may be made of at least oneof a thermoplastic resin, a thermosetting resin, or aphotocurable resin, which has electrical insulation.

[0024] A method for manufacturing an electrode leadaccording to an embodiment of the present invention forachieving the above object includes: a step of manufacturingeach of a first electrode lead and a second electrode; a stepof applying an adhesive to at least one of the other end ofthe first electrode lead or one end of the second electrodelead; a step of bonding the other end of the first electrodelead to the one end of the second electrode lead to form alead stack; and a step of applying heat to the lead stack tocure the adhesive, thereby forming a connection part 15,wherein the adhesive is formed by mixing a conductivematerial and a solvent, the solvent is formed by mixing apolymer and a diluent, and the solvent contains 5 wt% to 15wt% of the diluent.

[0025] Particularities of other embodiments are included inthe detailed description and drawings.ADVANTAGEOUS EFFECTS

[0026] According to the embodiments of the present invention,there are at least the following effects.

[0027] Since the two-stage electrode leads are provided,even if the gas is generated in the battery case to increasein internal pressure, the gas may be discharged to theoutside to secure the safety.

[0028] In addition, since the two-stage electrode leads arereliably detached, the electrical connection may becompletely cut off.

[0029] In addition, while improving the electrolyteresistance of the adhesive bonding the two-stage electrodeleads to each other, the contact resistance may notsignificantly increase.

[0030] The effects of the prevent invention are not limitedby the aforementioned description, and thus, more variedeffects are involved in this specification.BRIEF DESCRIPTION OF THE DRAWINGS

[0031] FIG. 1 is an assembly view of a secondary batteryaccording to an embodiment of the present invention.

[0032] FIG. 2 is a perspective view of the secondary batteryaccording to an embodiment of the present invention.

[0033] FIG. 3 is a perspective view illustrating a state inwhich the pouch type secondary battery is expanded in volumeaccording to an embodiment of the present invention.

[0034] FIG. 4 is a flowchart illustrating a method formanufacturing an electrode lead according to an embodiment ofthe present invention.

[0035] FIG. 5 is a partial cross-sectional view taken alongline A-A' of FIG. 2 in the pouch type secondary batteryaccording to an embodiment of the present invention.

[0036] FIG. 6 is a partial cross-sectional view taken alongline A-A' of FIG. 2 in a state in which the pouch typesecondary battery is expanded in volume according to anembodiment of the present invention.

[0037] FIG. 7 is a graph illustrating a weight reductionrate of each of electrode lead samples according toManufacturingExample1andComparativeExample1ofthepresent invention.MODE FOR CARRYING OUT THE INVENTION

[0038] Advantages and features of the present invention, andimplementation methods thereof will be clarified throughfollowing embodiments described with reference to theaccompanying drawings. The present invention may, however beembodied in different forms and should not be construed aslimited to the embodiments set forth herein. Rather, theseembodiments are provided so that this disclosure will bethorough and complete, and will fully convey the scope of thepresent invention to those skilled in the art. Further, thepresent invention is only defined by scopes of claims. Likereference numerals refer to like elements throughout.

[0039] Unless terms used in the present invention aredefined differently, all terms (comprising technical andscientific terms) used herein have the same meaning asgenerally understood by those skilled in the art. Also,unless defined clearly and apparently in the description, theterms as defined in a commonly used dictionary are notideally or excessively construed as having formal meaning.

[0040] In the following description, the technical terms areused only for explaining a specific exemplary embodimentwhile not limiting the present invention. In thisspecification, the terms of a singular form may includeplural forms unless specifically mentioned. The meaning of"comprises" and / or "comprising" does not exclude othercomponents besides a mentioned component.

[0041] Hereinafter, preferred embodiments will be describedin detail with reference to the accompanying drawings.

[0042] FIG.1isanassemblyviewofasecondarybattery1according to an embodiment of the present invention, and FIG.2 is a perspective view of the secondary battery 1 accordingto an embodiment of the present invention.

[0043] As illustrated in FIG. 1, the pouch type secondarybattery 1 according to an embodiment of the present inventionincludes an electrode assembly 10, in which electrodes suchas a positive electrode and a negative electrode andseparators are stacked, and a pouch type battery case 13accommodating the electrode assembly 10 therein.

[0044] To manufacture the pouch type secondary battery 1,first, slurry in which an electrode active material, a binder,and a plasticizer are mixed with each other is applied to apositive electrode collector and a negative electrodecollector to manufacture electrodes such as a positiveelectrode and a negative electrode. The electrodes arestacked on both sides of a separator to manufacture theelectrode assembly 10 having a predetermined shape. Then,the electrode assembly 10 is inserted into the battery case13, and the battery case 13 is sealed after injecting anelectrolyte therein.

[0045] Particularly, the electrode assembly 10 may be astacked structure including two types of electrodes such as apositive electrode and a negative electrode and a separatordisposed between the electrodes to insulate the electrodesfrom each other or disposed at a left or right side of oneelectrode. The stacked structure may have various shapeswithout being limited in shape. For example, the cathode andthe anode, each of which has a predetermined standard, may bestacked with the separator therebetween, or the stackedstructuremaybewoundintheformofajellyroll.Eachofthe two types of electrodes, i.e., the positive electrode andthe negative electrode has a structure in which activematerial slurry is applied to the electrode collector havinga metal foil or metal mesh shape. The slurry may be usuallyformed by agitating a granular active material, an auxiliaryconductor, a binder, and a plasticizer with a solvent added.The solvent may be removed in the subsequent process.

[0046] As illustrated in FIG. 1, the electrode assembly 10includes electrode tabs 11. The electrode tabs 11 arerespectively connected to a positive electrode and a negativeelectrode of the electrode assembly 10 to protrude to theoutside of the electrode assembly 10, thereby providing apath, through which electrons are moved, between the insideand outside of the electrode assembly 10. An electrodecollector of the electrode assembly 10 is constituted by aportion coated with an electrode active material and a distalend, on which the electrode active material is not applied,i.e., a non-coating portion. Also, each of an electrode tabs11 may be formed by cutting the non-coating portion or byconnecting a separate conductive member to the non-coatingportion through ultrasonic welding. As illustrated in FIG. 1,the electrode tabs 11 may protrude from one side of theelectrode assembly 10 in the same direction, but the presentinvention is not limited thereto. For example, the electrodetabs 11 may protrude in directions different from each other.

[0047] In the electrode assembly 10, the electrode lead 12that supplies electricity to the outside of the secondarybattery 1 is connected to the electrode tab 11 through spotwelding. The electrode lead 12 according to an embodiment ofthepresentinventionisprovidedinpluralitytoformtwo-stage electrode leads 12. Also, in the two-stage electrodeleads 12, a first electrode lead 123 (see FIG. 5) isconnected to the electrode tab 11 of the electrode assembly10, and a second electrode lead 124 (see FIG. 5) protrudes tothe outside of a battery case 13. A detailed description ofthe two-stage electrode leads 12 will be described later.

[0048] A portion of the electrode lead 12 is surrounded byan insulation part 14. The insulation part 14 may bedisposed to be limited within a sealing part 134, at which anupper case 131 and a lower case 132 of the battery case 13are thermally fused, so that the electrode lead 12 is bondedto the battery case 13. Also, electricity generated from theelectrode assembly 10 may be prevented from flowing to thebattery case 13 through the electrode lead 12, and thesealing of the battery case 13 may be maintained. Thus, theinsulation part 14 may be a non-conductor having highadhesiveness and non-conductivity by which electricity is notconducted well. Particularly, the insulation part 14 mayinclude at least one of a thermoplastic resin, athermosetting resin, or a photocurable resin, which haselectrical insulation, as a polymer resin. In general,although an insulation tape which is easily attached to theelectrode lead 12 and has a relatively thin thickness ismainly used as the insulation part 14, the present inventionis not limited thereto. For example, various members may beused as the insulation part 14 as long as the members arecapable of insulating the electrode lead 12.

[0049] The electrode leads 12 include a positive electrodelead 121 having one end connected to a positive electrode tab111toextendinadirectioninwhichthepositiveelectrodetab 111 protrudes and a negative electrode lead 122 havingone end connected to a negative electrode tab 112 to extendin a direction in which the negative electrode tab 112protrudes. On the other hand, as illustrated in FIG 1, allof the other ends of the positive electrode lead 121 and thenegative electrode lead 122 protrude to the outside of thebattery case 13. As a result, electricity generated in theelectrode assembly 10 may be supplied to the outside. Also,since each of the positive electrode tab 111 and the negativeelectrode tab 112 is formed to protrude in various directions,each of the positive electrode lead 121 and the negativeelectrode lead 122 may extend in various directions.

[0050] The positive electrode lead 121 and the negativeelectrode lead 122 may be made of materials different fromeach other. That is, the cathode lead 121 may be made of thesame material as the cathode collector, i.e., an aluminum(Al) material, and the anode lead 122 may be made of the samematerial as the anode collector, i.e., a copper (Cu) materialor a copper material coated with nickel (Ni). Also, aportion of the electrode lead 12, which protrudes to theoutside of the battery case 13, may be provided as a terminalpart and electrically connected to an external terminal.

[0051] The battery case 13 is a pouch made of a flexiblematerial, which accommodates the electrode assembly 10therein. Hereinafter, the case in which the battery case 13is the pouch will be described. When a pouch film 135 havingflexibility is drawn by using a punch or the like, a portionof the pouch film 135 is stretched to form a cup part 133including a pocket-shaped accommodation space 1331, therebymanufacturingthebatterycase13.Thebatterycase13accommodates the electrode assembly 10 so that a portion ofthe electrode lead 12, i.e., the terminal part is exposed andthen is sealed. As illustrated in FIG. 1, the battery case13 includes the upper case 131 and the lower case 132. Anaccommodation space 1331 in which a cup part 133 is formed toaccommodate the electrode assembly 10 may be provided in thelower case 132, and upper case 131 may cover an upper side ofthe accommodation space 1331 so that the electrode assembly10 is not separated to the outside of the battery case 13.Also, the sealing part 134 is sealed to seal theaccommodation space 1331. Here, the cup part 133 having theaccommodation part 1331 may be formed in the upper case 131to accommodate the electrode assembly 10 in the upper portion.As illustrated in FIG. 1, one side of the upper case 131 andone side of the lower case 132 may be connected to each other.However, the present invention is not limited thereto. Forexample, the upper case 131 and the lower case 132 may beseparately manufactured to be separated from each other.

[0052] When an electrode lead 12 is connected to theelectrode tab 11 of the electrode assembly 10, and theinsulation part 14 is provided on a portion of the electrodelead 12, the electrode assembly 10 may be accommodated in theaccommodation space 1331 provided in the cup part 133 of thelower case 132, and the upper case 131 may cover theaccommodation space from the upper side. Also, theelectrolyte is injected, and the sealing part 134 extendingoutward from edges of the upper case 131 and the lower case132 is sealed. The electrolyte may move lithium ionsgenerated by electrochemical reaction of the electrode duringcharginganddischargingofthesecondarybattery1.Theelectrolyte may include a non-aqueous organic electrolytethat is a mixture of a lithium salt and a high-purity organicsolvent or a polymer using a polymer electrolyte. Asillustrated in FIG. 2, the pouch type secondary battery 1 maybe manufactured through the above-described method.

[0053] FIG. 3 is a perspective view illustrating a state inwhich the pouch type secondary battery 1 is expanded involume according to an embodiment of the present invention.

[0054] In general, the pouch type secondary battery 1 mayabnormally generate a large amount of gases due to heatgeneration due to an internal short circuit, overcharge,overdischarge, etc., by an external impact of the electrodeassembly 10, and also due to electrolyte decomposition and athermal runaway phenomenon by the heat generation. Inaddition, when the secondary battery is stored at a hightemperature, an electrochemical reaction between anelectrolyte and an electrode active material is quicklypromoted by the high temperature to generate a gas.

[0055] In order to manufacture the pouch type battery case13, the pouch film 135 having the flexibility is drawn usinga punch or the like. The drawing is performed by insertingthe pouch film 135 into a press and applying a pressure tothe pouch film 135 through the punch to stretch the pouchfilm 135. As described above, the pouch film 135 isstretched to form the recessed cup part 133, therebymanufacturing the battery case 13. The pouch film 135 isformed by stacking a surface protection layer made of a nylonresin or polyethylene terephthalate (PET), a gas barrierlayer mainly made of a thin aluminum film (Al foil), and asealantlayermainlymadeofapolymersuchaspolypropylene(PP) or polyethylene (PE).

[0056] However, if the gas is generated in the battery case13, since all the layers have the flexibility in the batterycase 13, the internal pressure of the secondary battery 1increases by the generated gas to expand a volume of thesecondary battery 1 as illustrated in FIG. 3. In addition,there are problems such as weakening of bonding force betweencomponents, damage of the case of the secondary battery 1, anearly operation of a protection circuit, deformation of anelectrode, internal short circuit, explosion, and the like.

[0057] FIG. 4 is a flowchart illustrating a method formanufacturing an electrode lead 12 according to an embodimentof the present invention.

[0058] According to an embodiment of the present invention,since two-stage electrode leads 12 are formed, even if a gasis generated in a battery case to increase in internalpressure, the gas may be discharged to the outside to securesafety. In addition, since the two-stage electrode leads 12are reliably detached, electrical connection may becompletely cut off. In addition, while improving electrolyteresistance of an adhesive bonding the two-stage electrodeleads 12 to each other, contact resistance may notsignificantly increase.

[0059] For this, a method for manufacturing an electrodelead 12 according to an embodiment of the present inventionincludes: a step of manufacturing each of a first electrodelead 123 and a second electrode 12; a step of applying anadhesive to at least one of the other end of the firstelectrode lead 123 or one end of the second electrode lead124;astepofbondingtheotherendofthefirstelectrodelead 123 to the one end of the second electrode lead 124 toform a lead stack; and a step of applying heat to the leadstack to cure the adhesive, thereby forming a connection part15. Here, the adhesive is formed by mixing a conductor and asolvent, the solvent is formed by mixing a polymer and adiluent, and the solvent contains 5 wt% to 15 wt% of thediluent.

[0060] The electrode lead 12 manufactured in this mannerincludes: a first electrode lead 123 having one end connectedto an electrode tab 11 protruding from one side of anelectrode assembly 10; a second electrode lead 124 having oneend connected to the other end of the first electrode lead123 and the other end protruding to the outside of a batterycase 13 accommodating the electrode assembly 10; and aconnection part 15 configured to connect the first electrodelead 123 to the second electrode lead 124. Here, theconnection part 15 is formed by curing an adhesive appliedbetween the first electrode lead 123 and the second electrodelead 124, the adhesive is formed by mixing a conductor and asolvent, the solvent is formed by mixing a polymer and adiluent, and the solvent contains 5 wt% to 15 wt% of thediluent.

[0061] A pouch type secondary battery 1 including such anelectrode lead 12 according to an embodiment of the presentinvention includes: an electrode assembly 10 in whichelectrodes including a positive electrode and a negativeelectrode and separators are stacked; a pouch-shaped batterycase 13 configured to accommodate the electrode assembly 10;an electrode tab 11 connected to the electrodes andprotrudingfromonesideoftheelectrodeassembly10;afirst electrode lead 123 having one end connected to theelectrode tab 11; a second electrode lead 124 having one endconnected to the other end of the first electrode lead 123and the other end protruding to the outside of the batterycase 13; and a connection part 15 configured to connect thefirst electrode lead 123 to the second electrode lead 124.Here, the connection part 15 is formed by curing an adhesiveapplied between the first electrode lead and the secondelectrode lead, the adhesive is formed by mixing a conductorand a solvent, the solvent is formed by mixing a polymer anda diluent, and the solvent contains 5 wt% to 15 wt% of thediluent.

[0062] Hereinafter, each of the steps illustrated in theflowchart of FIG. 4 will be described with reference to FIGS.5 and 6.

[0063] FIG. 5 is a partial cross-sectional view taken alongline A-A' of FIG. 2 in the pouch type secondary batteryaccording to an embodiment of the present invention.

[0064] According to an embodiment of the present invention,an electrode lead 12 is formed in two stages. That is, theelectrode lead 12 includes a first electrode lead 123 havingone end connected to an electrode tab 11 of an electrodeassembly 10 and a second electrode 124 having one endconnected to the other end of the first electrode lead 123and the other end protruding to the outside of a battery case13. Also, one surface of the other end of the firstelectrode lead 123 and one surface of one end of the secondelectrode lead 124 may adhere to each other through aconnection part 15 and thus be connected to each other.

[0065] Inordertomanufacturetheelectrodelead12,first,the first electrode lead 123 and the second electrode lead124 are separately manufactured (S401). It is preferablethat each of both the first electrode lead 123 and the secondelectrode lead 124 have a rectangular shape. Also, in orderto be easily bonded to each other later, it is preferablethat the first electrode lead 123 and the second electrodelead 124 have the same width.

[0066] An adhesive is applied to at least one of the otherend of the manufactured first electrode lead 123 and one endof the manufactured second electrode lead 124 (S402). Then,the other end of the first electrode lead 123 and the one endof the second electrode lead 124 are bonded to each other toform a lead stack (S403).

[0067] The adhesive includes a material having conductivity.As a result, electricity generated from the electrodeassembly 10 may be easily discharged to the outside. Forthis, it is preferable that the adhesive is formed by mixinga conductor and a solvent, and the solvent is formed bymixing a polymer and a diluent.

[0068] The conductor may include at least one of: natural orartificial graphite; carbon black such as carbon black,acetylene black, Ketjen black, channel black, furnace black,lamp black, and summer black; conductive fiber such as carbonfiber or metal fiber; metal powders such as carbon fluoride,aluminum, nickel, gold, silver, and copper powder; powderhaving a core / shell structure coated with a different kind ofmetal on one kind of metal; conductive whiskey such as zincoxide and potassium titanate; conductive metal oxide such astitanium oxide; or conductive materials such as polyphenylenederivatives,inparticular,maymostpreferablyincludesilver. It is preferable that the conductor contained in theadhesive is contained at 70 wt% to 85 wt%.

[0069] The polymer may include at least one of an acrylicresin, an epoxy resin, an ethylene propylene diene monomer(EPDM) resin, a chlorinated polyethylene (CPE) resin,silicone, polyurethane, a urea resin, a melamine resin, aphenol resin, an unsaturated ester resin, polypropylene (PP),polyethylene (PE), polyimide, or polyamide, in particular,may most preferably include an epoxy or acrylic resin. It ispreferable that the polymer contained in the adhesive iscontained at 15 wt% to 30 wt%.

[0070] In order to increase in user convenience by reducingviscosity of the adhesive and improving fluidity, a diluentis added to the polymer. Here, the diluent may be aglycidylester-based material, for example, may include atleast one of n-butyl glycidyl ether, allyl glycidyl ether, 2-ethylhexyl glycidyl ether, styrene oxide, phenylglycidylether, cresyl glycidyl ether, glycidyl methacrylate, tertiarycarboxylic acid glycidyl ester, monoepoxides such as vinylcyclohexene monoepoxide, butanediol glycidyl ether, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidylether, (poly) ethylene glycol diglycidyl ether, (poly)propylene glycol diglycidyl ether, or diepoxides such asvinyl cyclohexene dioxide.

[0071] Also, the diluent is added to a rate of 5 wt% to 15wt%, preferably 5 wt% to 10 wt%. If the addition ratio ofthe diluent is less than 5 wt%, viscosity is excessively high,and thus, it almost impossible to apply the adhesive, or evenif it is possible, there is a problem in that it takes toomuchtimeandefforttoapplytheadhesive.Conversely,ifthe addition ratio of the diluent is greater than 15 wt%,electrolyte resistance of the connection part 15 formed bycuring the adhesive decreases. As a result, there is aproblem that the two-stage electrode leads 12 are detached byan electrolyte after the secondary battery 1 is manufactured.

[0072] After forming the lead stack, heat is applied to thelead stack using an oven or the like (S404). Then, theadhesive is dried and cured to form the connection part 15,and the connection part 15 also includes a conductor and aconductive polymer. Thus, as illustrated in FIG. 5, twostage electrode leads 12 in which the first electrode lead123 and the second electrode lead 124 are connected to eachother may be completely manufactured.

[0073] When the battery case 13 is normal, the first andsecond electrode leads 123 and 124 have to be stablyconnected to each other. When the secondary battery 13 isexpanded, the first and second electrode leads 123 and 124have to be easily detached from each other. Thus it ispreferable that the first and second electrode leads 123 and124 are disposed on different planes so that upper and lowersurfaces thereof are connected to each other instead that thefirst and second electrode leads 123 and 124 are disposed onthe same plane so that side surfaces thereof are connected toeach other.

[0074] It is preferable that the connection part 15connecting the first electrode lead 123 to the secondelectrode lead 124 has a very thin thickness of 1 μm to 500μm. Therefore, even if the first electrode lead 123 and thesecond electrode lead 124 form a stepped portion therebetween,asizeofthesteppedportionmaynotbeexcessivelylarge.

[0075] As described above, a portion of the electrode lead12, in particular, the portion at which the first electrodelead 123 and the second electrode lead 124 are connected toeach other through the connection part 15, is surrounded bythe insulation part 14. Also, the first and second electrodeleads 123 and 124 are bonded to the battery case 13 throughthe insulation part 14. In a process of sealing the uppercase 131 and the lower case 132, a relatively high pressuremay be applied to a portion contacting the electrode lead 12to damage the sealant layer of the battery case 13. Sincethe sealant layer directly contacts the electrode assembly 10as described above, the sealant layer may have insulationproperties. However, if the sealant layer is damaged,electricity may flow to the battery case 13 through theelectrode lead 12. Particularly, since the gas barrier layerof the battery case 13 is made of a metal such as aluminum,if the sealant layer is partially damaged to expose the gasbarrier layer, the electricity may easily flow due to thecontact with the electrode lead 12.

[0076] Thus, the insulation part 14 may be made of anonconductor having non-conductivity, which is notelectrically conductive. Also, the insulation part 14 hashigh mechanical strength and heat resistance. Thus, theinsulation part 14 may include, for example, a polyolefinbased resin such as polypropylene (PP) or polyethylene (PE).Particularly, polypropylene (PP) is excellent in mechanicalproperties such as tensile strength, rigidity, surfacehardness, abrasion resistance, heat resistance, and the like,and chemical properties such as corrosion resistance and thelikeandthusismainlyusedformanufacturingtheinsulationpart 14. Furthermore, acid-treated polypropylene may beprovided to improve bonding force of the insulation part 14.For example, the acid-treated polypropylene and normalpolypropylene may be mixed with each other, polypropylene maybe further mixed, or only the acid-treated polypropylene maybe provided simply. Here, the acid-treated polypropylene maybe maleic anhydride polypropylene (MAH PP).

[0077] Thus, when the upper case 131 and the lower case 132are thermally fused, the insulation part 14 may be maintainedin shape to prevent the electrode lead 12 and the gas barrierlayer from contacting each other even through a portion ofthe sealant layer is damaged. Thus, the electricitygenerated from the electrode assembly 10 may be preventedfrom flowing to the battery case 13 through the electrodelead 12.

[0078] As illustrated in FIG. 5, the insulation part 14 maysurround all of the first electrode lead 123, the connectionpart 15, and the second electrode lead 124. If the firstelectrode lead 123 or the connection part 15 is notsurrounded by the insulation part 14, repulsive force may notbe applied to the first electrode lead 123 and the secondelectrode 124 even though the battery case 13 is expanded.

[0079] FIG. 6 is a partial cross-sectional view taken alongline A-A' of FIG. 2 in a state in which the pouch typesecondary battery is expanded in volume according to anembodiment of the present invention.

[0080] As described above, when the internal pressure of thepouch type secondary battery 13 increases, the pouch typesecondary battery 1 is expanded in volume. Thus, asillustratedinFIG.6,anouterwallofthebatterycase13moves outward. Here, upper and lower walls of the outer wallof the battery case 13 may have a large area and be notsealed, resulting in higher flexibility. Thus, the upperwall of the battery case 13 may move upward, and the lowerwall of the battery case 13 may move downward. The outerwall of the battery case 13 may move outward to apply therepulsive force to the first electrode lead 123 and thesecond electrode 124 connected through the insulation part 14.Thus, as the internal pressure of the battery case 13gradually increases, moving force of the outer wall of thebattery case 13 may more increase, and the repulsive forceapplied to the first electrode lead 123 and the secondelectrode lead 124 more increase.

[0081] When the bonding force between the first electrodelead 123 and the second electrode lead 124 is greater thanthe repulsive force, as illustrated in FIG. 6, the firstelectrode lead 123 and the second electrode lead 124 may bedetached from each other. Thus, the electrical connectionmay be physically interrupted so that the electricity doesnot flow ever. Here, the detachment may mean that adsorbedor attached portions are separated from each other. However,the bonding force between the first and second electrodeleads 123 or 124 and the connection part 15 may be less thanthat between the first and second electrode leads 123 and 124and the insulation part 14. Thus, when the repulsive forceis applied to the first electrode lead 123 and the secondelectrode lead 124, the bonding force between the first andsecond electrode leads 123 and 124 and the insulation part 14may be maintained to maintain the sealing of the battery case13,butthefirstandsecondelectrodeleads123and124maybe detached from each other.

[0082]

[0083] Manufacturing Example 1

[0084] A nickel-plated copper plate having a thickness of200 μm was cut to manufacture each of a first electrode leadhaving a length of 40 mm and a width of 45 mm and a secondelectrode lead having a length of 10 mm and a width of 45 mm.

[0085] 30 g of first silver powder having a particle size of5 μm or less and 30 g of second silver powder having aparticle size of 2 μm or less were mixed at a 1:1 weightratio. Also, 1 g of glycidyl ester as a diluent was added to9 g of liquid epoxy to prepare a solvent. In addition, 7.8 gof the mixed silver powder was dissolved in 2.2 g of thesolvent to prepare an adhesive containing 78 wt% silver and22 wt% solvent. Here, the glycidyl ester that is the diluentis added to the epoxy in 10 wt% and thus occupies 2.2 wt% inthe total adhesive.

[0086] The prepared adhesive was applied to an area from oneend of the second electrode lead up to a distance of 5 mm,and the other end of the first electrode lead was bonded toform a lead stack. Also, the lead stack was put into an oven,and the adhesive was dried and cured at a temperature of180°C for 1 hour to manufacture two-stage electrode leads.

[0087]

[0088] Manufacturing Example 2

[0089] Two-stage electrode leads were manufactured in thesame method as in Manufacturing Example 1, except that 0.5 gof glycidyl ester that is the diluent is added to 9.5 g ofliquid epoxy to prepare a solvent. Here, the glycidyl esterthatisthediluentisaddedtotheepoxyin5wt%andthusoccupies 1.1 wt% in the total adhesive.

[0090]

[0091] Comparative Example 1

[0092] Two-stage electrode leads were manufactured in thesame method as in Manufacturing Example 1, except that 3 g ofglycidyl ester that is the diluent is added to 7 g of liquidepoxy to prepare a solvent. Here, the glycidyl ester that isthe diluent is added to the epoxy in 30 wt% and thus occupies6.6 wt% in the total adhesive.

[0093]

[0094] Comparative Example 2

[0095] Two-stage electrode leads were manufactured in thesame method as in Manufacturing Example 1, except that 5 g ofglycidyl ester that is the diluent is added to 5 g of liquidepoxy to prepare a solvent. Here, the glycidyl ester that isthe diluent is added to the epoxy in 50 wt% and thus occupies11 wt% in the total adhesive.

[0096] [Table 1]

[0097] Method for measuring physical property - 1. Tongterm reliability

[0098] First, each of two-stage electrode lead samplesmanufactured in Manufacturing Example 1, ManufacturingExample 2, Comparative Example 1, and Comparative Example 2was accommodated together with 30 ml of an electrolyte(prepared by dissolving lithium salt (LiPF6) 1M, and ethylenecarbonate (EC): ethylmethyl carbonate (EMC): dimethylcarbonate (DMC), which are contained at a ratio of 3:3:4) ina 125 ml polyethylene (PE) bottle, and then, an inlet wassealed with paraffin. Then, each of the bottles were sealedwith an aluminum wrapper and stored for 16 weeks in a spacehaving a temperature of 60°C and a relative humidity of 90%RH. After every 1, 2, 4, 8, and 16 weeks elapse, the twostage electrode lead samples were put out to completelyremove the electrolyte, and a terminal was connected to eachof both ends to measure resistance by using a resistancemeter (model name: HIOKI 3560).

[0099]

[00100] Result obtained by measuring physical property - 1.Tong-term reliability[Table 2]

[00101] As described in [Table 2], when comparingManufacturing Examples 1 and 2 to Comparative Examples 1 and2 according to the present invention, the electrode leadsaccording to Manufacturing Examples 1 and 2 were notseparated into the first electrode lead and the secondelectrode lead even though a period of 16 weeks elapses. Onthe other hand, in the electrode leads according toComparative Examples 1 and 2, the first electrode lead andthe second electrode lead were separated from each other bythe electrolyte when only two weeks elapse.

[00102] As described above, in the case of the electrodeleads according to Manufacturing Examples 1 and 2, bondingforce of the connection part was not significantly reduced bythe electrolyte, but in the case of the electrode leadsaccording to Comparative Examples 1 and 2, bonding force ofthe connection part was significantly reduced. That is, itis seen that the electrode leads according to ManufacturingExamples 1 and 2 have electrolyte resistance that is superiorto that of the electrode leads according to ComparativeExamples 1 and 2.

[00103] In the electrode lead according to ManufacturingExample 1, the resistance increased by 12.7% from 0.150 mΩthat is initial resistance to 0.169 mΩ after 16 weeks. Onthe other hand, in the electrode lead according toManufacturing Example 2, the resistance increased by only0.74% from 0.136 mΩ that is initial resistance to 0.137 mΩafter 16 weeks.

[00104] As described above, it is seen that the electrodelead according to Manufacturing Example 2 did not have alarger increase in resistance than the electrode leadaccording to Manufacturing Example 1.

[00105]

[00106] Methodformeasuringphysicalproperty-2.Weightreduction rate

[00107] The two-stage electrode lead samples manufactured inManufacturing Example 1 and Comparative Example 1 were putinto a simultaneous thermogravimetric analyzer (Manufacturer:HITACHI, Model Name: STA7200). Then, heat was applied in anenvironment of a nitrogen (N2) gas at a temperature from 30°Cto 400°C at a heating rate of 4°C / min. Then, a changed masscompared to an initial mass was calculated to a weightreduction rate.

[00108]

[00109] Result obtained by measuring physical property - 2.Weight reduction rate[Table 3]

[00110] FIG. 7 is a graph illustrating a weight reductionrate of each of electrode lead samples according toManufacturing Example 1 and Comparative Example 1 of thepresent invention.

[00111] As illustrated in FIG. 7, as the temperatureincreases, a weight of the electrode lead according toComparative Example 1 decreased more rapidly compared to theelectrode lead according to Manufacturing Example 1.Particularly, as described in [Table 3], the electrode leadaccording to Manufacturing Example 1, which is manufacturedat a temperature of 300°C, had a weight reduction ratio ofonly -0.4 wt%, but the electrode lead according toComparative Example 1 had a weight reduction ratio of -1.4wt%. The high weight reduction rate means that a containedamount of diluent and a residual amount of moisture containedin the diluent itself are large. However, when the adhesiveis dried and cured, the diluent and the moisture contained inthe diluent itself are not sufficiently evaporated in theelectrode lead according to Comparative Example 1 rather thanin the electrode lead according to Manufacturing Example 1,and thus, an amount of diluent and a residual amount ofmoisture are larger. If the amount of diluent and theresidual amount of moisture are large, reactivity with theelectrolyte is high, and when the amount of diluent and theresidual amount of moisture are small, reactivity with theelectrolyte is low.

[00112] As described above, since the electrode leadaccording to Manufacturing Example 1 of the present inventionhas less weight at a high temperature than the electrode leadaccording to Comparative Example 1, it is seen that theamount of diluent and the residual amount of moisture issmall, and thus, the electrolyte resistance is more excellent.

[00113]

[00114] Those with ordinary skill in the technical field ofthe present invention pertains will be understood that thepresent invention can be carried out in other specific formswithout changing the technical idea or essential features.Therefore, the above-disclosed embodiments are to beconsidered illustrative and not restrictive. Accordingly,the scope of the present invention is defined by the appendedclaims rather than the foregoing description and theexemplary embodiments described therein. Variousmodificationsmadewithinthemeaningofanequivalentoftheclaims of the invention and within the claims are to beregarded to be in the scope of the present invention.

[00115] [Description of the Symbols]

[00116] 1: Secondary battery 10: Electrode assembly

[00117] 11: Electrode tab 12: Electrode lead

[00118] 13: Battery case 14: Insulation part

[00119] 15: Connection part 111: Positive electrode tab

[00120] 112: Negative electrode tab 121: Positiveelectrode lead

[00121] 122: Negative electrode lead 123: First electrodelead

[00122] 124: Second electrode lead 131: Upper case

[00123] 132: Lower case 133: Cup part

[00124] 134: Sealing part 135: Pouch film

[00125] 1331: Accommodation space.

Claims

1. An electrode lead comprising: a first electrode lead having one end connected to an electrode tab protruding from one side of an electrode assembly; a second electrode lead having one end connected to the other end of the first electrode lead and the other end protruding to the outside of a battery case accommodating the electrode assembly; and a connection part configured to connect the first electrode lead to the second electrode lead, wherein the connection part is formed by curing an adhesive applied between the first electrode lead and the second electrode lead, the adhesive is formed by mixing a conductor and a solvent, the solvent is formed by mixing a polymer and a diluent, and the solvent contains 5 wt% to 15 wt% of the diluent.

2. The electrode lead of claim 1, wherein the solvent contains 5 wt% to 10 wt% of the diluent.

3. The electrode lead of claim 1, wherein the diluent comprises a glycidyl ester-based material.

4. The electrode lead of claim 1, wherein the adhesive contains 70 wt% to 85 wt% of the conductor and 15 wt%to30wt%ofthesolvent.

5. The electrode lead of claim 1, wherein the conductor comprises at least one of graphite, carbon black, conductive fiber, metal powder, conductive whisker, conductive metal oxide, or conductive material.

6. The electrode lead of claim 5, wherein the conductor comprises silver.

7. The electrode lead of claim 1, wherein the polymer comprises at least one of an acrylic resin, an epoxy resin, an ethylene propylene diene monomer (EPDM) resin, a chlorinated polyethylene (CPE) resin, silicone, polyurethane, a urea resin, a melamine resin, a phenol resin, an unsaturated ester resin, polypropylene (PP), polyethylene (PE), polyimide, or polyamide.

8. The electrode lead of claim 7, wherein the polymer comprises an epoxy resin.

9. A pouch type secondary battery comprising: an electrode assembly in which electrodes comprising a positive electrode and a negative electrode and separators are stacked; a pouch-shaped battery case configured to accommodate the electrode assembly; an electrode tab connected to the electrodes and protruding from one side of the electrode assembly; a first electrode lead having one end connected to the electrodetab; a second electrode lead having one end connected to the other end of the first electrode lead and the other end protruding to the outside of the battery case; and a connection part configured to connect the first electrode lead to the second electrode lead, wherein the connection part is formed by curing an adhesive applied between the first electrode lead and the second electrode lead, the adhesive is formed by mixing a conductive material and a solvent, the solvent is formed by mixing a polymer and a diluent, and the solvent contains 5 wt% to 15 wt% of the diluent.

10. The pouch type secondary battery of claim 9, further comprising an insulation part configured to surround a portion at which the first and second electrode leads are connected to each other through the connection part and configured to bond the first and second electrode leads to the battery case.

11. The pouch type secondary battery of claim 10, wherein bonding force between each of the first and second electrode leads and the connection part is less than that between each of the first and second electrode leads and the insulation part.

12. The pouch type secondary battery of claim 10, wherein the insulation part is made of at least one of a thermoplasticresin,athermosettingresin,oraphotocurable resin, which has electrical insulation.

13. A method for manufacturing an electrode lead, the method comprising: a step of manufacturing each of a first electrode lead and a second electrode lead; a step of applying an adhesive to at least one of the other end of the first electrode lead or one end of the second electrode lead; a step of bonding the other end of the first electrode lead to the one end of the second electrode lead to form a lead stack; and a step of applying heat to the lead stack to cure the adhesive, thereby forming a connection part 15, wherein the adhesive is formed by mixing a conductive material and a solvent, the solvent is formed by mixing a polymer and a diluent, and the solvent contains 5 wt% to 15 wt% of the diluent.