Copolyester raw material for films, heat-shrinkable polyester films, heat-shrinkable labels, and packages
Patent Information
- Application Number
- IN202247066932
- Authority / Receiving Office
- IN · IN
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-05-12
- Filing Date
- 2022-11-22
- Publication Date
- 2026-08-03
- Estimated Expiration
- 2041-05-10
AI Technical Summary
Heat-shrinkable polyester films with high stretchability and reduced thickness face issues of film breakage due to high stretching ratios, leading to production stoppages and fluctuations in physical properties along the longitudinal direction, caused by segregation of raw materials with different bulk densities during extrusion.
A copolymerized polyester raw material with specific composition requirements, including 5-40 mol% diethylene glycol, 0-5 mol% amorphous components, a glass transition temperature of 73°C or lower, intrinsic viscosity of 0.60-0.85 dl/g, and melt viscosity of 200 Pa·S or less, which reduces segregation and enhances uniformity and stretchability.
The solution provides high stretchability and reduced defects in the film, improving productivity and processability by maintaining consistent physical properties along the film direction, reducing film breakage, and achieving excellent shrinkage ratios without significant changes in heat resistance.
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to a copolymerized polyester raw materialfor film with high stretchability and a heat-shrinkable polyester-based film,a heat-shrinkable label, and a package product using the same.BACKGROUND ART
[0002] In recent years, heat-shrinkable polyester-based labels with high heat-resistance and solvent-resistance, and are easily incinerated produced bypolyester-based heat-shrinkable films have been widely used in labelpackaging, cap sealing, or integrated packaging of glass bottles or PETbottles to protect them and display products' information. The use of thelabels is increasing with an increase in the use of containers such as PET(polyethylene terephthalate) bottles.After use, heat-shrinkable labels are discarded. Recently, the need toreduce the amount of garbage from an environmental standpoint has led tothe use of heat-shrinkable labels with decreased thickness (i.e., thinnerheat-shrinkable labels). Heat-shrinkable films with increased shrinkageratio are highly demanded to cover a variety of containers, therefore, it hasbeen increasing for the heat-shrinkable films to be formed from rawmaterials having increased amorphous content.
[0003] Production of the heat-shrinkable films with high shrinkage ratio forcovering a variety of containers requires high stretching ratio in theshrinkage direction. However, such a high stretching ratio with reduced filmthickness for environmental reasons has a disadvantage in film breakage,resulting in production stoppages due to tear of film during production.PTL 1 discloses the production of heat-shrinkable film with the additionof polybutylene terephthalate or polypropylene terephthalate, which haslower glass transition temperature (hereinafter, merely Tg in some cases)than PET and can decrease stretching stress, allowing the film to haveimproved stretchability. However, polybutylene terephthalate andpolypropylene terephthalate have different bulk density from PET rawmaterials, leading to the segregation of the raw materials on the way to anextruder after mixing the raw materials. This segregation of the rawmaterials causes fluctuation in raw material blend ratio in the longitudinaldirection of the film, resulting in difference in physical properties in thelongitudinal direction of the film.PTL 2 discloses the apparatus related to feeding method of raw materials,by which two or more kinds of raw materials having different bulk densityand angle of repose are fed without segregation for an extrusion process.Thus, produced film has small difference in physical properties in thelongitudinal direction of the film, though such an apparatus undesirablyrequires plant and equipment investments.CITATION LISTPATENT LITERATURE
[0004] PTL1: JP-B2-4552097PTL2: JP-B2-6544492SUMMARY OF THE INVENTIONPROBLEMS TO BE SOLVED BY THE INVENTION
[0005] It is an object of the present invention to provide a raw material forpolyester film with high stretchability. It is also an object to provide a heat-shrinkable polyester film which is produced from the raw material andcapable of reducing troubles during processing such as printing and shrinking.SOLUTION TO THE PROBLEMS
[0006] The present invention that solves the above problem has the followingfeatures.1. A copolymerized polyester raw material for film characterized by satisfyingthe following requirements (1) to (5):(1) the copolymerized polyester raw material comprises 5 mol% or moreand 40 mol% or less of constituent unit derived from diethylene glycol in 100mol% of total glycol component amount in whole polyester resin component;(2) the copolymerized polyester raw material comprises 0 mol% or moreand 5 mol% or less of constituent unit derived from a monomer componentwhich can become an amorphous component in whole polyester resincomponent;(3) the copolymerized polyester raw material has a glass transitiontemperature of 73°C or lower;(4) the copolymerized polyester raw material has an intrinsic viscosity of0.60 dl / g or more and 0.85 dl / g or less; and(5) the copolymerized polyester raw material has a melt viscosity of 200Pa·S or less in a measurement at 255°C and shear rate of 6080 / S.2. The copolymerized polyester raw material for film according the above 1,wherein the copolymerized polyester raw material comprises an acidcomponent consisting of terephthalic acid and a glycol component consistingof ethylene glycol and diethylene glycol in the whole polyester resincomponent.3. A heat-shrinkable polyester film comprising the copolymerized polyesterraw material according to the above 1 or 2,wherein the film satisfies the following requirements (6) to (10):(6) the film has a hot-water heat shrinkage ratio in a main-shrinkingdirection of the film of 40% or more and 85% or less by immersion in hot waterof 98°C for 10 seconds;(7) the film has a hot-water heat shrinkage ratio in a direction orthogonalto the main-shrinking direction of the film of -5% or more and 15% or less byimmersion in hot water of 98°C for 10 seconds;(8) the film has a hot-water heat shrinkage ratio in a direction orthogonalto the main-shrinking direction of the film of -5% or more and 5% or less byimmersion in hot water of 70°C for 10 seconds;(9) the film has an intrinsic viscosity of 0.57 dl / g or more and 0.82 dl / g orless; and(10) the film has an average defects number of 1.1 or less per a film of 100m2 with a defect size of 1 mm or more in a longitudinal direction of the filmor a width direction of the film.4. A heat-shrinkable label, comprising the heat-shrinkable polyester filmaccording to the above 3.5. A package product, characterized in that the package product isproduced by covering at least a part of periphery of an object for packagingwith the heat-shrinkable label according to the above 4, and followed bysubjecting to a heat-shrinking treatment.ADVANTAGEOUS EFFECTS OF THE INVENTION
[0007] The polyester film produced by the copolymerized polyester raw materialsof the present invention has high stretchability and can be stretched at highstretching ratio, leading to excellent productivity. In addition, the heat-shrinkable film using the copolymerized polyester raw materials of thepresent invention has a small difference in shrinkage ratio in the longitudinaldirection of the film, and has fewer foreign substances. These characteristicsof the film can reduce troubles in processing such as printing and shrinking.
[0008] A non-shrinking direction of the films that heat-shrink in a widthdirection corresponds to a longitudinal direction of the films. Since tensionis applied to films in the longitudinal direction during printing or processing,films are required to have specified tensile elongation at break in thelongitudinal direction of the film for excellent processability of films. Heat-shrinkable polyester-based film produced from the copolymerized polyesterraw material of the present invention has a tensile elongation at break of 20%or more in the non-shrinking direction after aging, allowing the film to haveexcellent processability without film breakage in processing such as printingafter aging.
[0009] Heat-shrinkable polyester-based film of the present invention includes asingle-layer of the present inventive heat-shrinkable polyester film and alaminated heat-shrinkable film comprising the present inventive heat-shrinkable polyester film and a different resin layer.
[0010] A package product covered by a label of the heat-shrinkable polyester-based film of the present invention has excellent appearance.DESCRIPTION OF EMBODIMENTS
[0011] The copolymerized polyester raw material for film of the presentinvention (hereinafter merely "raw material" in some cases) and heat-shrinkable polyester-based film will now be described in detail. Detailedmethod for producing the heat-shrinkable polyester-based film will bedescribed later, and in general, heat-shrinkable film is produced throughconveying and stretching with rolls. The conveying direction of the film isreferred to as a longitudinal direction and the direction orthogonal to thelongitudinal direction is referred to as a width direction of the film.Therefore, in the following, the width direction of the heat-shrinkablepolyester-based film indicates the direction vertical to the roll unwindingdirection, and the longitudinal direction of the film indicates the directionparallel to the roll unwinding direction.
[0012] The raw material of the present invention comprises 5 mol% or more and40 mol% or less of constituent unit derived from diethylene glycol in 100 mol%of total glycol component amount. As described later, the constituent unitderived from diethylene glycol causes generation of foreign substances duringfilm production, so diethylene glycol has been generally contained as little aspossible in terms of film quality. Conversely, the copolymerized polyesterraw material of the present invention has low melt viscosity even at a resintemperature of 250°C, enabling resin extrusion at a lower temperature thanthat of general polyester raw materials. Although the raw material of thepresent invention comprises a large amount of diethylene glycol with 5 mol%or more and 40 mol% or less of the constituent unit derived from diethyleneglycol in 100 mol% of total of glycol component amount, the film, which has40 μm thick, can give a reduced average defects number of 1.1 or less per afilm of 100 m2 with a defect size of 1 mm or more in a longitudinal directionof the film or a width direction of the film.
[0013] It is known that the amount of monomer component constituting the unitwhich can become an amorphous component (hereinafter, merely "amorphouscomponent" in some cases) can be increased in the film having ethyleneterephthalate as a main component, allowing a heat-shrinkable polyester filmto have higher shrinkability. In the production of conventional films bytransverse uniaxial stretching method, as the amount of amorphouscomponent is increased, adequate increase in shrinkage ratio is observed.Unfortunately, neopentylglycol and cyclohexanedimethanol disclosed asamorphous components in PTL 2 are expensive. Addition of neopentylglycolor cyclohexanedimethanol does not lower Tg, so the film may break duringproduction due to fluctuation in the stretching temperature at industriallyhigh stretching ratio, leading to decreased productivity.In order to improve such weaknesses, polybutylene terephthalate orpolypropylene terephthalate, which has lower glass transition temperaturethan PET (polyethylene terephthalate) and is capable of decreasingstretching stress, is added in film production in PTL 2. However,polybutylene terephthalate and polypropylene terephthalate have differentbulk density from PET raw materials, leading to the segregation of the rawmaterials on the way to an extruder after mixing raw materials. Thissegregation of the raw materials causes fluctuation in raw material blendratio in a longitudinal direction of film, resulting in difference in physicalproperties in the longitudinal direction of the film.That led the present inventors to focus on diethylene glycol (hereinaftermerely "DEG" in some cases).
[0014] Increased content of diethylene glycol in films will deteriorate heatresistance and increase in discharge of foreign substances during meltextrusion. For that, diethylene glycol has not been positively used in thepast. Conversely, the inventors found that the use of diethylene glycol as aconstituent unit of polyester resin will lower Tg of the film, decreasestretching stress during film stretching, and further suppress reduction ofshrinkage ratio measured at a low temperature of about 70°C after aging.
[0015] The copolymerized polyester of the present invention, which is used forproducing films such as the heat-shrinkable polyester-based film, preferablyhas an ethylene terephthalate unit as a main constituent component. Theterm "as a main constituent component" indicates that the constituentcomponent is contained in 50 mol% or more of the total constituentcomponents. The film preferably has the ethylene terephthalate unit inamount of 50 mol% or more, more preferably 60 mol% or more, and furtherpreferably 70 mol% or more in 100 mol% of constituent units of the polyester.
[0016] In addition to terephthalic acid, examples of the dicarboxylic acidcomponents constituting the polyester of the present invention includearomatic dicarboxylic acids such as isophthalic acid, orthophthalic acid, and2,6-naphthalenedicarboxylic acid; aliphatic dicarboxylic acids such as adipicacid, azelaic acid, sebacic acid, and decanedicarboxylic acid; and alicyclicdicarboxylic acid such as 1,4-cyclohexanedicarboxylic acid. Preferably, thepolyester of the present invention is free from dicarboxylic acid componentother than terephthalic acid.
[0017] In the present invention, a monomer unit indicates a repeating unit thatforms a polymer derived from one polyhydric alcohol molecule and onepolycarboxylic acid molecule.
[0018] In case where the polymer comprise the monomer unit derived fromterephthalic acid and ethylene glycol (i.e., ethylene terephthalate unit) as amain monomer unit, examples of the other monomer units include a monomerunit derived from isophthalic acid and ethylene glycol, a monomer unitderived from terephthalic acid and neopentylglycol, a monomer unit derivedfrom terephthalic acid and 1,4-cyclohexanedimethanol, and a monomer unitderived from isophthalic acid and butanediol. Preferably, the polyester ofthe present invention is free from the above-described other monomer units.
[0019] Preferably, the polyester is free from a polycarboxylic acid having three ormore valences such as trimellitic acid, pyromellitic acid, and anhydridethereof. The polyester comprising these polycarboxylic acids will preventthe heat-shrinkable polyester-based film from attaining required highshrinkage ratio.
[0020] In addition to the ethylene terephthalate unit, examples of other diolcomponents constituting the polyester include aliphatic diols such as 1,3-propanediol, 2,2-diethyl-1,3-propanediol, 2-n-butyl-2-ethyl-1,3-propanediol,2,2-isopropyl-1,3-propanediol, 2,2-di-n-butyl-1,3-propanediol, 1,4-butanediol,hexanediol, neopentylglycol, and hexanediol; alicyclic diols such as 1,4-cyclohexanedimethanol; and aromatic diols such as bisphenol A. The diolcomponent constituting the copolymerized polyester of the present inventionother than the ethylene terephthalate unit may be diethylene glycol.
[0021] The copolymerized polyester of the present invention, which is used forproducing films such as the heat-shrinkable polyester-based film, is requiredto comprise the constituent unit derived from diethylene glycol. Thepolyester comprises preferably 5 mol% or more of the constituent unit derivedfrom diethylene glycol, more preferably 7 mol% or more, and furtherpreferably 9 mol% or more in 100 mol% of constituent units of polyester. Theupper limit of the constituent unit derived from diethylene glycol is preferably40 mol% or less, more preferably 38 mol% or less, and further preferably 36mol% or less. The constituent unit derived from diethylene glycol canimprove film formability by decreasing glass transition temperature ofpolyester. Additionally, containing 5 mol% or more of the constituent unitderived from diethylene glycol preferably improves the effects of the presentinvention such as decrease in shrinkage ratio and shrinkage stress measuredat 70°C after aging. In contrast, containing more than 40 mol% of adiethylene glycol component will soften resin and thus cause the resin to stickto cooling rolls during the step of cooling and solidification after meltextrusion, hence the productivity will be undesirably deteriorated.
[0022] Among the monomer components, monomers which can becomeamorphous components are exemplified by neopentylglycol, 1,4-cyclohexanedimethanol, isophthalic acid, 1,4-cyclohexanedicarboxylic acid,2,6-naphthalenedicarboxylic acid, 2,2-diethyl-1,3-propanediol, 2-n-butyl-2-ethyl-1,3-propanediol, 2,2-isopropyl-1,3-propanediol, 2,2-di-n-butyl-1,3-propanediol, and hexanediol. The content of the monomers which canbecome amorphous components is preferably 0 mol% or more and 5 mol% orless in the copolymerized polyester, more preferably 0 mol%, which indicatesthat such monomers are not contained.
[0023] Controlling the content of the constituent unit derived from diethyleneglycol within the above ranged will give the polyester having controlled glasstransition temperature (Tg) of 55 to 73°C. Tg of lower than 55°C will causechange in film physical properties due to moving of molecules in films duringstorage at room temperature in a warehouse, especially in summer. Tg ispreferably 57°C or higher, and further preferably 59°C or higher. Higher Tgwill decrease stretchability during film production, therefore, Tg is preferably71°C or lower, and further preferably 69°C or lower.
[0024] The polyester is preferably free from diol having 8 or more of carbon atomssuch as octanediol, or polyhydric alcohol having three or more valences suchas trimethylolpropane, trimethylolethane, glycerin, and diglycerol. Theheat-shrinkable polyester-based film produced from polyester containingthese diols or polyhydric alcohols may not attain required high shrinkage.Preferably, the polyester comprises as little triethylene glycol andpolyethylene glycol as possible.Diethylene glycol is preferably copolymerized in the polyester. Thecopolymerization will eliminate a concern of segregation of raw materials, andthat will prevent changes in physical properties of the film due to fluctuationof the raw material composition of the film. Moreover, the copolymerizationwill promote transesterification, namely copolymerization will proceedrandomly, resulting in advantages of increased shrinkage ratio in the main-shrinking direction due to decreased crystallinity.
[0025] The resin forming the heat-shrinkable polyester-based film of the presentinvention may contain additives such as waxes, antioxidants, antistaticagents, crystal nucleating agents, viscosity reducing agents, heat stabilizers,coloring pigments, color inhibitor, ultraviolet absorbers, if needed.
[0026] The resin forming the heat-shrinkable polyester-based film of the presentinvention may preferably contain lubricants of fine particles to improveworkability such as slipperiness of the film. Any type of fine particles maybe selected, and the examples of the fine particles include inorganic fineparticles such as silica, alumina, titanium dioxide, calcium carbonate, kaolin,and barium sulfate, and organic fine particles such as acrylic resin particles,melamine resin particles, silicone resin particles, and cross-linkedpolystyrene particles. The fine particles may desirably have an averageparticle diameter ranged within 0.05 to 4 μm measured by Coulter counter, ifneeded.In case where the film contains silica in amount of 50 ppm or more and3000 ppm or less, the average particle diameter of the fine particles can becontrolled within above range. The content of silica is preferably 200 ppmor more, and further preferably 300 ppm or more. Too high content of silicawill impair transparency, and thus the film requiring transparency preferablycontains silica in amount of 2000 ppm or less, and further preferably 1500ppm or less.
[0027] The fine particles may be added to the resin forming the heat-shrinkablepolyester-based film at any step during polyester resin production. The fineparticles are added preferably in the form of a slurry dispersed in ethyleneglycol during the step of esterification or after the finish of transesterificationand before the start of polycondensation, and polycondensation reactionproceeds. Preferably, the fine particles are blended with the polyester resinraw materials in the form of a slurry dispersed in ethylene glycol or waterwith vented kneading extruder, or dried fine particles are blended with thepolyester resin raw materials with kneading extruder.
[0028] The heat-shrinkable polyester-based film of the present invention may besubjected to surface treatment such as corona treatment, coating treatment,or flame treatment to enhance adhesiveness of the film surface.
[0029] Characteristics of the copolymerized polyester raw material and the heat-shrinkable polyester-based film of the present invention will be described.
[0030] The copolymerized polyester raw material of the present inventionpreferably has the intrinsic viscosity of 0.60 dl / g or more and 0.85 dl / g or less.This range of intrinsic viscosity under the melt extrusion conditions describedbelow enables the intrinsic viscosity of the heat-shrinkable polyester-basedfilm to be controlled to 0.57 dl / g or more and 0.82 dl / g or less. The intrinsicviscosity of less than 0.57 dl / g of the heat-shrinkable polyester-based film willundesirably lead to tensile elongation at break of less than 5% in thelongitudinal direction of the film after aging. The heat-shrinkable polyester-based film has the intrinsic viscosity of preferably 0.60 dl / g or more, and morepreferably 0.63 dl / g or more. Since there is little demand for the heat-shrinkable polyester-based film with an intrinsic viscosity more than 0.82 dl / g,the upper limit of the hot-water heat shrinkage ratio is determined to be 0.82dl / g.
[0031] Amorphous copolymerized polyester raw material of the presentinvention has the melt viscosity of preferably 200 Pa · S or less in ameasurement at 255°C and shear rate of 6080 / S. Resin having high meltviscosity requires high resin temperature for extrusion, otherwise extrusionwill be difficult. However, such a high resin temperature of presentinventive raw material containing high amount of diethylene glycolundesirably causes more foreign substances in the film or sheet afterextrusion. Accordingly, the resin temperature is preferably 265°C or lower,and further preferably 260°C or lower. Lower resin temperature ispreferable; however, too low resin temperature will cause unmelted materials.Therefore, the lower limit of the resin temperature is 235°C or lower.The melt viscosity of 200 Pa·S or more in the measurement at 255°Cincreases pressure load on an extruder of melted raw materials, undesirablyleading to the requirement for larger equipment. The melt viscosity ispreferably 190 Pa·S or less, and further preferably 180 Pa·S or less.Too low melt viscosity undesirably will cause thickness nonuniformity dueto reduced shear stress at discharge part for melted resin. The melt viscositymeasured at 255°C is preferably 100 Pa·S or more, and further preferably110 Pa·S or more.
[0032] The heat-shrinkable film produced from the copolymerized polyester rawmaterial of the present invention, which has, for example, 40 μm thick, maypreferably has the defects number of 1.1 or less per a film of 100 m2 with adefect size of 1 mm or more in a longitudinal direction or a width direction ofthe film. The film having more than 1.1 of defects causes blanking of inkson the spots of defects or foreign substances during printing, resulting in poorappearance of the label after printing. The number of defects per a film of100 m2 in a longitudinal direction or a width direction of the film is morepreferably 1 or less, and further preferably 0.5 or less.
[0033] The heat-shrinkable polyester-based film of the present invention isimmersed in hot water of 98°C with no load for 10 seconds, and immediatelyafter the first immersion, the film is further immersed in water of 25°C±0.5°Cfor 10 seconds. The heat shrinkage ratio, that is, the hot-water heatshrinkage ratio at 98°C, in the width direction as the main-shrinkingdirection of the film is calculated from the length before and after shrinkageaccording to the following Equation 1. The hot-water heat shrinkage ratioat 98°C is 40% or more and 85% or less.Equation 1: heat shrinkage ratio = {(length before shrinkage-length aftershrinkage) / length before shrinkage} x 100 (%)
[0034] The heat-shrinkable polyester-based film with hot-water heat shrinkageratio at 98°C in the main-shrinking direction of less than 40% cannot meetthe demand for a high-shrinkage film that covers the entire container (so-called full label). In addition, a label made from such a film will have strain,shrinkage insufficiency, wrinkles, or sagging after heat-shrinking due tosmall amount of shrinkage. The hot-water heat shrinkage ratio at 98°C ispreferably 45% or more, and more preferably 50% or more. Since there islittle demand for the film with hot-water heat shrinkage ratio at 98°C in themain-shrinking direction of more than 85%, the upper limit of the hot-waterheat shrinkage ratio is determined to be 85%.
[0035] The heat-shrinkable polyester-based film of the present invention has thehot-water heat shrinkage ratio at 98°C in a direction orthogonal to the main-shrinking direction of the film, i.e., the longitudinal direction, of -5% or moreand 15% or less, which is measured in the same manner as the above. Thehot-water heat shrinkage ratio at 98°C in the direction orthogonal to themain-shrinking direction of less than -5% causes too much elongation of thefilm upon heating, undesirably leading to poor appearance as labels forcontainers. In contrast, the hot-water heat shrinkage ratio at 98°C in thedirection orthogonal to the main-shrinking direction of more than 15% causeslabel shortening due to a decrease in label height after heat-shrinkage,leading to a decrease in label area. Therefore, the film is unsuitable as labelfor a full label. In addition, the label made from such a film undesirably willhave strain after heat-shrinkage. The upper limit of the hot-water heatshrinkage ratio at 98°C in the direction orthogonal to the main-shrinkingdirection is preferably 12% or less, and more preferably 9% or less.
[0036] The hot-water heat shrinkage ratio at 98°C in the direction orthogonal tothe main-shrinking direction of less than -5% causes an increase in labelheight after heat-shrinkage, undesirably leading to baggy label's excess orwrinkles. Therefore, the lower limit is determined to be -5%.
[0037] The heat-shrinkable polyester-based film of the present invention isimmersed in hot water of 70°C with no load for 10 seconds, and immediatelyafter the first immersion, the film is further immersed in water of 25°C±0.5°Cfor 10 seconds. The heat shrinkage ratio, that is, the hot-water heatshrinkage ratio at 70°C, in the direction orthogonal to the main-shrinkingdirection, i.e., longitudinal direction, is calculated from the length before andafter shrinkage according to the following Equation 1. And the hot-waterheat shrinkage ratio at 70°C is -5% or more and 5% or less.The hot-water heat shrinkage ratio at 70°C in the direction orthogonal tothe main-shrinking direction of less than -5% causes too much elongation ofthe film upon heating, undesirably leading to poor appearance as labels forcontainers. In contrast, the hot-water heat shrinkage ratio at 70°C in thedirection orthogonal to the main-shrinking direction of more than 5%undesirably causes strain of the label after heat-shrinkage. The upper limitof the hot-water heat shrinkage ratio at 70°C in the direction orthogonal tothe main-shrinking direction is preferably 4% or less, and more preferably 3%or less.
[0038] Thickness of the heat-shrinkable polyester-based film of the presentinvention is not particularly limited, and the thickness is preferably 10 μm ormore and 60 μm or less. The lower limit of the thickness is more preferably15 μm.
[0039] For the production of the heat-shrinkable polyester-based film of thepresent invention, the polyester raw material is melt-extruded from anextruder to form an unstretched film, and the unstretched film is thenstretched in the width direction. The polyester is produced throughpolycondensation reactions of appropriate dicarboxylic acid components anddiol components by known method, and the polyester in chip form is generallyused as raw materials for film.
[0040] Polyester materials are preferably dried with a hopper dryer, a paddledryer, or a vacuum dryer for melt extrusion of raw material resin. The driedpolyester raw materials are melted at 235 to 265°C and extruded into a filmwith an extruder.In the process with an extruder, prevention of degrading raw materialsand causing foreign substance, stable discharge of resin from a die atappropriate melt viscosity, and progression of transesterification areimportant. The resin raw material is extruded at the temperature of 235 to265°C to reduce foreign substances caused by degrading resin as describedabove. The melt viscosity at 235 to 265°C and shear rate of 5000 to 8000 / Sis preferably controlled to 100 Pa·S or more and 200 Pa·S or less. Asdescribed above, this range can reduce the load of an extruder and preventthickness nonuniformity from getting worse. The shear rate wasdetermined according to the following Equation (2). The resin can have theshear rate within the above range by controlling the discharge rate of the rawmaterial and lip gap of die.
[0041] Shear rateEquation (2): Y=6Q / (W x H2)γ; shear rate (sec-1)Q; discharge rate of raw material from extruder (cm3 / sec)W; width of die's opening at exit (cm)H; lip gap of die (cm)
[0042] In general, transesterification can be accelerated by raising thetemperature of an extruder or increasing the residence time of resin, however,these methods will cause foreign substances due to resin degradation.Therefore, an extrusion screw with shafts of 2 or more to 32 or less ispreferably used to accelerate transesterification in a short period of time.The shear force during kneading is increased with an increase in the numberof screws, leading to an accelerated transesterification. Increased numberof screws can accelerate transesterification; however, too high number ofscrews requires labor for machine maintenance. Therefore, the upper limitis determined to be 32.
[0043] An unstretched film is produced by rapidly cooling sheet-shaped meltedresin after extrusion. In the preferred method of cooling melted resin, theresin is cast on rotating drums from a nozzle and then rapidly cooled andsolidified to form substantially unoriented resin sheet.
[0044] (Transverse stretching and relaxation after transverse stretching)The following methods (1) and (2) can more desirably developperformances of the copolymerized polyester of the present invention. Fromthe viewpoint of simplifying production facilities, it is preferable to form thefilm by transverse uniaxial stretching.
[0045] (1) Control of transverse stretching conditionsThe film is preheated to a temperature ranged from Tg+10°C or higherand Tg+40°C or lower while both ends in the width direction of the film beinggrasped by clips in a tenter for transverse stretching. After that, the film isstretched in the width direction preferably by 3.5 to 6 times while the filmbeing cooled so that the film temperature becomes Tg-5°C or higher andTg+10°C or lower. Stretching in the width direction with cooling canincrease the stress ratio in a stress-strain curve (calculated by dividing tensilestress by upper yield stress in final stretching) resulting in decreasedthickness nonuniformity in the width direction. The film is then heattreated preferably at a temperature stretching temperature +1°C tostretching temperature +15°C after transverse stretching. If the heattreatment temperature is lower than the stretching temperature, molecularorientation cannot be sufficiently relaxed, and this insufficient relaxationdisadvantageously leads to high shrinkage of the film products during storagein a warehouse (so called natural shrinkage). The higher heat treatmenttemperature than the stretching temperature +15°C disadvantageously leadsto decreased shrinkage ratio in the width direction.
[0046] (2) Relaxation in the width direction after transverse stretchingIn the heat treatment step, the film is relaxed in the width directionpreferably by 0% to 5% while both ends in the width direction of the film isgrasped by clips in a tenter. Relaxation by 0% means that the film is notrelaxed. Relaxation of the film will slightly decrease shrinkage ratio in thewidth direction; however, molecular orientation will be relaxed in the widthdirection, and that can decrease shrinkage stress and natural shrinkage ratio.In addition, heat treatment at a temperature higher than the stretchingtemperature in the final heat treatment step will lead to relaxed molecularorientation, enabling the film to have decreased shrinkage stress and naturalshrinkage ratio.
[0047] The package product of the present invention includes the packageproduct produced by covering at least a part of periphery of object forpackaging with perforated or notched heat-shrinking the label prepared fromthe heat-shrinkable polyester-based film of the present invention. Theobject for packaging is exemplified by various bottles such as PET bottles forbeverages, cans, plastic containers for confectionery or packed lunch, andpaper boxes. The attachment of the labels prepared from the heat-shrinkable polyester-based film to these objects generally requires heatshrinkage of the labels by approximately 5 to 70%, and the labels are closelyattached to the objects. The labels for covering the objects for packaging maybe or may not be printed.
[0048] The following two methods can be suggested for preparing labels from theheat-shrinkable polyester-based film of the present invention. In onemethod, organic solvents are applied slightly inward from an end of one sideof a rectangular-shaped film, and the film is immediately rolled up to form alabel by overlapping and adhering both ends. In the other method, organicsolvents are applied slightly inward from an end of one side of a wound filmin a roll, then the film is immediately rolled up to overlap and adhere bothends, and thus obtained tubular film is cut to labels. The organic solventsfor the adhesion are preferably exemplified by cyclic ethers such as 1,3-dioxolane or tetrahydrofuran; mixtures of these solvents with amorphousresins; aromatic hydrocarbons such as benzene, toluene, xylene,trimethylbenzene; halogenated hydrocarbons such as methylene chloride andchloroform; phenols such as phenol; or mixtures thereof. The film can alsobe label shape by applying heat and thermally bonding, so-called by heatsealing or fusion sealing.EXAMPLES
[0049] The present invention will be now described specifically with Examplesand Comparative Examples, but the present invention is not limited to theembodiments, and can be appropriately modified within the scope notdeparting from the gist of the present invention. The evaluation methods ofthe film are described below.
[0050] [Heat shrinkage ratio (hot-water heat shrinkage ratio)]The film was cut into 10 cm x 10 cm squares and immersed in hot waterof prescribed temperature (°C) ±0.5 (°C) for 10 seconds with no load to be heat-shrunk. After that, the film sample was immersed in water of 25°C ± 0.5°Cfor 10 seconds and pulled out of the water to measure the dimension of thefilm both in longitudinal and transverse directions. Heat shrinkage ratio ofthe film was determined according to the following Equation (1).Equation (1): Heat shrinkage ratio = {(length before shrinkage - lengthafter shrinkage) / length before shrinkage} x 100(%)
[0051] [Tensile elongation at break in longitudinal direction after aging]After the aging of the film for 672 hours in an environmental test chamberset to a temperature of 40°C and a humidity of 65%, the film was made tostrip-shaped test pieces having the size of 140 mm in the longitudinaldirection of the film and 20 mm in the direction orthogonal to themeasurement direction, i.e., the width direction of the film. The test pieceswere grasped at both ends by chucks by 20 mm respectively with the distancebetween the chucks of 100 mm, and tensile test was conducted with auniversal tensile strength tester "DSS-100" (manufactured by ShimadzuCorporation) under the conditions of ambient temperature of 23°C and tensilespeed of 200 mm / min. Elongation at break was defined as tensile elongationat break and evaluated as follows from the measurement of 10 test pieces.Good: 9 or 10 test pieces have elongation at break of 30% or more.Bad: 8 or more test pieces have elongation at break of less than 30%.
[0052] [Melt viscosity]Melt viscosity was measured with Capirograph 1D PMD-C (manufacturedby Toyo Seiki Seisakusho, Ltd) under conditions of resin temperature of 255°Cand shear rate 6080 / S in accordance with JIS K7199.
[0053] [Intrinsic viscosity (IV)] Intrinsic viscosity was measured at 30°C with an Ostwald viscometer forthe polyester (0.2 g) prepared by dissolving into a mixed solvent (50 ml) ofphenol / 1,1,2,2-tetrachloroethane (60 / 40, weight ratio). Measurementresults were expressed in the unit of dl / g.
[0054] [Counting method of defects]The film was cut into a sample with the size of 0.5 m in the width directionand 5 m in the longitudinal direction. Then the sample was placed on a desk-top film orientation viewer (manufactured by Unitika), and polarized lightwas applied thereto. After that, the number of defects having the size of 1mm or more was counted using a loupe with a magnification 10x. Thenumber of defects was counted for a totally 80 films (200 m2) in the samemanner. An average defects number per 100 m2 of film was determinedaccording to the following Equation 3.Equation 3: average defects number = total defects number / 2(defects / 100 m2)
[0055] [Diethylene glycol content]The heat-shrinkable film was cut with a razor blade for sampling, andsampled film (about 5 mg) was dissolved into mixed solution (0.7 ml) ofdeuterochloroform and trifluoroacetic acid (9 / 1, volume ratio). An existingamount of the diethylene glycol unit was calculated with 1H-NMR (UNITY50, manufactured by Varian), and the measured value was expressed in mol%.
[0056] [Tg (glass transition temperature)]Tg was measured from -40°C to 120°C at a heating rate of 10°C / min witha differential scanning calorimeter (type: DSC220; manufactured by SeikoElectronic Industry) using unstretched film (5 mg). In the endothermiccurve, the glass transition temperature (Tg) was determined at a crossingpoint temperature of an extended base line lower than the glass transitiontemperature and a tangent line having the maximum slope in a transitionpart.
[0057] [Shrinkage finish property]The heat-shrinkable film was printed in three colors with grass, gold, andwhite inks (manufactured by TOYO INK CO., LTD.) in advance. Then, bothends of the printed film were adhered with a solution of 1,3-dioxolane mixedwith 10% of PET resin (Vylon200, manufactured by TOYOBO CO., LTD.) toform cylindrical labels, which has the main-shrinking direction of the heat-shrinkable film as a circumferential direction. After that, the label was cutand had a diameter in a label shrinkage direction of 70 mm. The labels werethen heat-shrunk and attached to a PET bottle (500 ml, a trunk diameter: 62mm, a minimum neck diameter: 25 mm) at a zone temperature of 90°C withpassing time of 4 seconds with a steam tunnel (type: SH-1500-L,manufactured by Fuji Astec Inc.). In the neck portion of a bottle, the labelwas attached with adjustment so that one end of the label came on a bottleportion of 45 mm in diameter. Shrinkage finish property was visuallyevaluated according to the following criteria.
[0058] [Strain by shrinkage in label]Strain of the attached label was evaluated based on a gauge measurementfor shrinkage finish property. The label was measured with a gauge in 360-degree direction at lower and upper portions of the attached label, and themaximum strain values of the lower and upper portions were respectivelydetermined. Strain of the label was evaluated according to the followingcriteria.Good: maximum strain is less than 3 mm.Bad: maximum strain is 3 mm or more.
[0059] [Shrinkage insufficiency of label]Shrinkage state of the label were evaluated according to the followingcriteria.Good: attached label is shrunk with no sagging between the label andcontainers.Bad: attached label is shrunk with sagging due to insufficient shrinkagebetween the label and containers.
[0060] [Wrinkles of label]Wrinkling state of label was evaluated under the same measurementconditions with the strain by shrinkage in label according to the followingcriteria.Good: the number of wrinkles in a size of 2 mm or more is 2 or less.Bad: the number of wrinkles in a size of 2 mm or more is 3 or more.
[0061] [Productivity]Productivity was judged in accordance with the number of breaks during2 hours of film formation according to the following criteria.Good: one time of break or less per 2 hoursBad: two times of break or more per 2 hours
[0062] <Preparation of polyester raw materials >Raw materials A to H were prepared by a conventional method ofpolycondensation via transesterification from dimethyl terephthalate (DMT)and the following glycol components.Raw material A: polyester consisting of 40 mol% of diethylene glycol, 60mol% of ethylene glycol, and terephthalic acid. Intrinsic viscosity is 0.831dl / g. Melt viscosity is 170 Pa·S at shear rate of 6080 / S·255°C.Raw material B: polyester consisting of 7 mol% of diethylene glycol, 93mol% of ethylene glycol, and terephthalic acid. Intrinsic viscosity is 0.631dl / g. Melt viscosity is 100 Pa·S at shear rate of 6080 / S·255°C.Raw material C: polyester consisting of 30 mol% of diethylene glycol, 70mol% of ethylene glycol, and terephthalic acid. Intrinsic viscosity is 0.731dl / g. Melt viscosity is 130 Pa·S at shear rate of 6080 / S·255°C.
[0063] Raw material D: polyester consisting of 20 mol% of diethylene glycol, 80mol% of ethylene glycol, and terephthalic acid. Intrinsic viscosity is 0.731dl / g. Melt viscosity is 140 Pa·S at shear rate of 6080 / S·255°C.Raw material E: polyester consisting of 3 mol% of diethylene glycol, 97mol% of ethylene glycol, and terephthalic acid. Intrinsic viscosity is 0.731dl / g. Melt viscosity is 170 Pa·S at shear rate of 6080 / S·255°C.Raw material F: polyester consisting of 20 mol% of diethylene glycol, 80mol% of ethylene glycol, and terephthalic acid. Intrinsic viscosity is 0.91 dl / g.Melt viscosity is 215 Pa·S at shear rate of 6080 / S·255°C.Raw material G: polyester consisting of 30 mol% of diethylene glycol, 70mol% of ethylene glycol, and terephthalic acid. Intrinsic viscosity is 0.551dl / g. Melt viscosity is 88 Pa·S at shear rate of 6080 / S·255°C.
[0064] Raw material H: polyester consisting of 60 mol% of diethylene glycol, 40mol% of ethylene glycol, and terephthalic acid. Intrinsic viscosity is 0.651dl / g. Melt viscosity is 110 Pa·S at shear rate of 6080 / S·255°C.Raw material I: polyester consisting of 60 mol% of diethylene glycol, 40mol% of ethylene glycol, and terephthalic acid. Intrinsic viscosity is 0.651dl / g. Melt viscosity is 105 Pa·S at shear rate of 6080 / S·255°C.
[0065] For the production of polyester raw materials A to G, a lubricant of SiO2(Silysia 266, manufactured by FUJI SILYSIA CHEMICAL LTD) was added tothe polyester by a proportion of 700 ppm. Similar silica was added to rawmaterial I by a proportion of 7200 ppm. In Table 1, TPA representsterephthalic acid, EG represents ethylene glycol, and DEG representsdiethylene glycol. Each polyester was prepared in the form of chips, ifneeded.
[0066] Tables 1 and 2 show the composition of polyester raw materials used inExamples and Comparative Examples and resin composition andmanufacturing conditions of films in Examples and Comparative Examples.
[0067] [Table 1]
[0068] [Table 2]
[0069] Example 1Raw material A was fed into an extruder. The resin was melted at 255°Cand extruded from a T-die, then quenched by winding the resin aroundrotating metal rolls cooled to a surface temperature of 30°C to form anunstretched film having a thickness of 152 μm at taking-up speed of theunstretched film (i.e., a rotational speed of the metal rolls) of 30 m / min. Theunstretched film had Tg of 62°C. The unstretched film was then introducedto a tenter, and preheated at film surface temperature of 120°C, and stretched4 times in the width direction while the film being cooled so that a surfacetemperature became 75°C. Then the film was relaxed in the width directionby 5% while the film being heated so that a surface temperature became 76°C.After that, the film was cooled and cut to remove both ends, and rolled up toproduce uniaxially oriented film having a width of 500 mm and a thickness of40 μm continuously over a predetermined length. Properties of thusobtained film was evaluated by the method described above. Table 3 showsthe evaluation results, and the results were excellent.
[0070] Example 2The film having a thickness of 40 μm was produced in the same manneras Example 1 except that raw material A was changed to raw material B.Table 3 shows the evaluation results, and the results were excellent similarlywith Example 1.
[0071] Example 3The film having a thickness of 40 μm was produced in the same manneras Example 1 except that raw material A was changed to raw material C.Table 3 shows the evaluation results, and the results were excellent similarlywith Example 1.
[0072] Example 4The film having a thickness of 40 μm was produced in the same manneras Example 1 except that raw material A was changed to raw material D.Table 3 shows the evaluation results, and the results were excellent similarlywith Example 1.
[0073] Example 5Raw material A was fed into an extruder. The resin was melted at 255°Cand extruded from a T-die, then quenched by winding the resin aroundrotating metal rolls cooled to a surface temperature of 30°C to form anunstretched film having a thickness of 198 μm at taking-up speed of theunstretched film (i.e., rotational speed of the metal rolls) of 30 m / min. Theunstretched film had Tg of 62°C. The unstretched film was then introducedto a tenter, and preheated at film surface temperature of 125°C, and stretched6 times in the width direction while the film being cooled so that a surfacetemperature became 78°C. Then the film was relaxed in the width directionby 5% while the film being heated so that a surface temperature became 79°C.After that, the film was cooled and cut to remove both ends, and rolled up toproduce uniaxially oriented film having a width of 500 mm and a thickness of40 μm continuously over a predetermined length. Properties of thusobtained film was evaluated by the method described above. Table 3 showsthe evaluation results, and the results were excellent.
[0074] Example 6The film having a thickness of 40 μm was produced in the same manneras Example 5 except that raw material A was changed to raw material B.Table 3 shows the evaluation results, and the results were excellent similarlywith Example 5.
[0075] Comparative Example 1The film was produced in the same manner as Example 5 except that rawmaterial A was changed to raw material E. However, productivity was notstable due to occasional breakage during film production. Table 3 shows theevaluation results of the film. Compared to Example 5, the film ofComparative Example 1 had lower shrinkage ratio in the width direction andhigher shrinkage ratio in the longitudinal direction, resulting in poorshrinkage finish property.
[0076] Comparative Example 2The film having a thickness of 40 μm was produced in the same manneras Example 1 except that raw material A was changed to raw material F.The high melt viscosity of raw material F increased pressure load on theextruder, so the resin temperature in the extruder was also changed byraising it from 255°C to 280°C. Table 3 shows the evaluation results of thefilm. Compared to Example 1, the film of Comparative Example 2 hadhigher number of defects and was inferior as a heat-shrinkable film requiringprinting.
[0077] Comparative Example 3The film having a thickness of 40 μm was produced in the same manneras Example 1 except that raw material A was changed to raw material G.Table 3 shows the evaluation results of the film. The low tensile elongationat break in the longitudinal direction after aging caused continuous breakageduring printing process, resulting in poor productivity of film roll.
[0078] Comparative Example 4The film having a thickness of 40 μm was produced in the same manneras Example 1 except that raw material A was changed to raw material H andI (raw material H: raw material I = 90:10 (weight ratio)). Table 3 shows theevaluation results of the film. Compared to Example 1, the film ofComparative Example 4 had higher number of defects and was inferior as aheat-shrinkable film requiring printing. The high shrinkage ratio at 70°Cin the main-shrinking direction disadvantageously led to poor shrinkagefinish property with wrinkles.
[0079] [Table 3]*-indicates that film was not evaluated due to impossibility of printing.INDUSTRIAL APPLICABILITY
[0080] The copolymerized polyester raw material of the present invention issuitable for film to be shrunk or molded, such as heat-shrinkable film. Theheat-shrinkable polyester film produced from the copolymerized polyesterraw material is inexpensive and has high productivity and shrinkage finishproperty. The package product of a container covered and fixed with the filmas a label has excellent appearance.
Claims
1. A copolymerized polyester raw material for film characterized by satisfying the following requirements (1) to (5): (1) the copolymerized polyester raw material comprises 5 mol% or more and 40 mol% or less of constituent unit derived from diethylene glycol in 100 mol% of total glycol component amount in whole polyester resin component; (2) the copolymerized polyester raw material comprises 0 mol% or more and 5 mol% or less of constituent unit derived from a monomer component which can become an amorphous component in whole polyester resin component; (3) the copolymerized polyester raw material has a glass transition temperature of 73°C or lower; (4) the copolymerized polyester raw material has an intrinsic viscosity of 0.60 dl / g or more and 0.85 dl / g or less; and (5) the copolymerized polyester raw material has a melt viscosity of 200 Pa-S or less in a measurement at 255°C and shear rate of 6080 / S.
2. The copolymerized polyester raw material for film according to claim 1, wherein the copolymerized polyester raw material comprises an acid component consisting of terephthalic acid and a glycol component consisting of ethylene glycol and diethylene glycol in the whole polyester resin component.
3. A heat-shrinkable polyester film comprising the copolymerized polyester raw material according to claim 1 or 2, wherein the film satisfies the following requirements (6) to (10): (6) the film has a hot-water heat shrinkage ratio in a main-shrinking direction of the film of 40% or more and 85% or less by immersion in hot water of 98°C for 10 seconds; (7) the film has a hot-water heat shrinkage ratio in a direction orthogonal to the main-shrinking direction of the film of -5% or more and 15% or less by immersion in hot water of 98°C for 10 seconds; (8) the film has a hot-water heat shrinkage ratio in a direction orthogonal to the main-shrinking direction of the film of -5% or more and 5% or less by immersion in hot water of 70°C for 10 seconds; (9) the film has an intrinsic viscosity of 0.57 dl / g or more and 0.82 dl / g or less; and (10) the film has an average defects number of 1.1 or less per a film of 100 m2 with a defect size of 1 mm or more in a longitudinal direction of the film or a width direction of the film.
4. A heat-shrinkable label, comprising the heat-shrinkable polyester film according to claim 3.
5. A package product, characterized in that the package product is produced by covering at least a part of periphery of an object for packaging with the heat-shrinkable label according to claim 4, and followed by subjecting to a heat-shrinking treatment.