Self cleaning photocatalyst
Patent Information
- Application Number
- IN202411068911
- Authority / Receiving Office
- IN · IN
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2026-08-05
- Estimated Expiration
- 2044-09-11
AI Technical Summary
Environmental pollution from construction materials like concrete and cementitious building materials leads to the accumulation of pollutants and contaminants on building surfaces, causing damage and requiring frequent cleaning, which is not effectively addressed by existing technologies.
A self-cleaning photocatalyst, specifically Ba2TiMnO6, is developed to impart self-cleaning properties to construction materials, utilizing photo-induced hydrophobicity to remove pollutants through sunlight or UV light, allowing for cleaning via rainfall or manual rinsing, and is synthesized in a powdery form for integration into cement-based composites and paints.
The photocatalyst effectively removes pollutants from building surfaces, achieving complete discoloration within a few days, maintaining the visual integrity of buildings and reducing environmental impact without compromising the compressive strength of the materials.
Abstract
Description
FIELD OF INVENTION:
[0001] The present invention generally relates to the field ofphotocatalysts; more particularly to that of self cleaningphotocatalyst.BACKGROUND OF THE INVENTION:
[0002] Global climate change due to industrialization andurbanization has badly affected our environment. Rapidlydeveloping concrete industry to fulfill human needs also impactedour environment. By selecting eco-friendly materials inconstruction, environmental pollution can be reduced to someextent. Strong sunlight and UV radiation decompose much organicmaterial in natural process. Concrete and cementitious buildingmaterial is generally used in the construction of offices, residentialbuildings, public places area of aesthetic value etc. Dust producedby the construction and demolition of buildings causes pollutionand makes building surfaces look dull and dirty.
[0003] Commonly produced pollutants by these materialsinclude nitrogen oxide (NO2) Sulphur dioxide (SO₂), and volatileorganic compounds (VOCs). These environmental pollutants causethe deposition of organic matter and contaminants which result inexternal damage to the buildings.
[0004] Organic and inorganic substances emanating out ofindustrial, residential exhausts can adhere to and deposit on thesurface of concrete buildings. The contaminants keepaccumulating on the building, in the absence of cleaning actionand also undergo degradation owing to the sunlight and UV rays'exposure. Repeatedly, the building surface will form anaccumulation of pollutants.
[0005] To overcome the above problem, self-cleaningconcrete also known as "Green concrete" are being promoted asthe solution, as it is capable of retaining the visual properties ofbuildings for a longer duration even in highly pollutedenvironments.
[0006] The present invention seeks to address the abovehighlighted issue by providing for a self cleaning photocatalystwhich imparts self cleaning ability to a concrete or a paintformulation, wherein a building can achieve self-cleaning effectthrough natural conditions such as rain and light. The presentinvention enables self cleaning ability to a whole building as abuilding can adapt to self cleaning method to eliminate thepollution and accumulation of dust and grime.OBJECT OF THE INVENTION:
[0007] It is an object of the present invention to provide fora self cleaning photocatalyst.
[0008] It is another object of the present invention to providefor a method of synthesis of photocatalyst in the form of powder.
[0009] It is yet another object of the present invention toprovide for a photocatalytic self-cleaning activity in constructionmaterial.
[0010] It is yet another object of the present invention toprovide for reduction of environmental impact by pollutants.
[0011] It is yet another object of the present invention toprovide for a self-cleaning effect, even achievable by manualrinsing or even rainfall.SUMMARY OF THE INVENTION:
[0012] In an embodiment of the present invention, itdiscloses a self-cleaning photocatalyst for a construction material.
[0013] In a second embodiment, the present inventiondiscloses a method of preparation of the self-cleaningphotocatalyst.
[0014] In a third embodiment, the present invention disclosesmethods of implementation of the self-cleaning photocatalyst.BRIEF DESCRIPTION OF THE DRAWINGS:
[0015] The present invention will be described in more detailhereinafter with the aid of the accompanying drawings. Thedrawings are illustrative of one or more embodiments of theinvention and do not in any manner limit the scope.
[0016] Figure 1 illustrates test data pertaining to self cleaningphotocatalyst at 0.05 gm on OPC composite. The test dataobserved at (a), (b), (c) and (d) indicate the result observed atDay 1 to 4 respectively.
[0017] Figure 2 illustrates test data pertaining to self cleaningphotocatalyst at 0.1 gm on OPC composite. The test data observedat (a), (b), (c) and (d) indicate the result observed at Day 1 to 4respectively.
[0018] Figure 3 illustrates test data pertaining to self cleaningphotocatalyst at 0.2 gm on OPC composite. The test data observedat (a), (b), (c) and (d) indicate the result observed at Day 1 to 4respectively.
[0019] Figure 4 illustrates test data pertaining to self cleaningphotocatalyst at 0.05 gm on WC composite. The test dataobserved at (a), (b), (c) and (d) indicate the result observed atDay 1 to 4 respectively.
[0020] Figure 5 illustrates test data pertaining to self cleaningphotocatalyst at 0.1 gm on WC composite. The test data observedat (a), (b), (c) and (d) indicate the result observed at Day 1 to 4respectively.
[0021] Figure 6 illustrates test data pertaining to self cleaningphotocatalyst at 0.2 gm on WC composite. The test data observedat (a), (b), (c) and (d) indicate the result observed at Day 1 to 4respectively.
[0022] Figure 7 illustrates test data pertaining to self cleaningphotocatalyst on white paint.DETAILED DESCRIPTION:
[0023] The illustrations of the embodiments described hereinare intended to provide a general understanding of the structureof the various embodiments. The illustrations are not intended toserve as a complete description of all of the elements and featuresof apparatus and systems that utilize the structures or methodsdescribed herein. Many other embodiments may be apparent tothose of skill in the art upon reviewing the disclosure. Otherembodiments may be utilized and derived from the disclosure,such that structural and logical substitutions and changes may bemade without departing from the scope of the disclosure.Additionally, the illustrations are merely representational and maynot be drawn to scale. Certain proportions within the illustrationsmay be exaggerated, while other proportions may be minimized.Accordingly, the disclosure and the figures are to be regarded asillustrative rather than restrictive.
[0024] It is also to be understood that the specific methodillustrated in the attached drawings, and described in the followingspecification are simply exemplary embodiments of the inventiveconcepts defined in the appended claims. Specific dimensionsand / or other physical characteristics relating to the embodimentsdisclosed herein are therefore not to be considered as limiting,unless the claims expressly state otherwise.
[0025] The present invention discloses a photocatalyst.
[0026] In a preferred embodiment, the photocatalyst hasself-cleaning capacity and imparts the same to the constructionmaterial.
[0027] In the present invention, the photocatalyst has a selfcleaning effect due to oxidation promoted by sunlight or UV lightor any other light source.
[0028] In the present invention, the photocatalyst works onthe principle of photo-induced hydrophobicity which induces selfcleaning ability in a construction material to make it look clean.Since the pollutant is organic it causes dirt over the surface. It iseasily removed by rainfall or manual rinsing.
[0029] In a preferred embodiment, in the present inventionwork, the photocatalyst is Ba2TiMnO6 [BTMO]. It has a threedimensional structure with two inequivalent Ba2sites. It is derivedfrom the perovskite structure, which is known for its versatility invarious applications
[0030] In an embodiment, a method of synthesis of thephotocatalyst is disclosed.
[0031] In another embodiment, the photocatalyst isevaluated for its self-cleaning ability at different dosagesinvestigate the self-cleaning and engineering properties ofspecimen prepared with Ordinary Portland Cement (OPC) andwhite cement (WC).
[0032] In the present invention, the photocatalyst wassynthesised to a powdery form.
[0033] For the synthesis, the following constituents wereused.
[0034] BaCO3 (0.5 M) 0.4 gm was dissolved in 10mldeionized water.
[0035] MnCO3 (0.5 M) 0.5 gm was dissolved in 10mldeionized water.
[0036] TiO2 (0.3 M) 0.2 gm was dissolved in 10ml deionizedwater.
[0037] NaOH (8 M) 3.2 gm was dissolved in 10ml deionizedwater.
[0038] The above constituents (in liquid form) were againmixed in 100 ml deionized water to form solution of total volumeof 100 ml. The solution was then magnetically stirred for 45minutes at 800RPM to result in a suspension.
[0039] The suspension was placed in reactor at 1800 C for 12hours. At this stage, the photocatalyst was synthesised in powderform.
[0040] In a first method of implementation, the photocatalystwas mixed with cementitious preparations to prepare bricks. Thecementitious preparations (i.e., a testing material) were pouredinto a wooden mould (50mm x 30mm x 10mm) to obtain cementboard / brick samples.
[0041] In a preferred embodiment, the proportion ofphotocatalyst to the cementitious composition is .05 gm to 0.2 gmby weight of cement.
[0042] In a preferred embodiment, a composition wasprepared for the purposes of testing for the present invention. Thecomposition is merely an illustrative composition and does notpresent any limitation to the extent and scope of the invention.Lime (CaO) 60 to 67%Silica (SiO2) 17 to 25%Alumina (Al2O3) 3 to 8%Iron oxide (Fe2O3) 0.5 to 6%Magnesia (MgO) 0.1 to 4%Sulphur trioxide (SO3) 1 to 3%Soda and / or Potash (Na2O+K2O) 0.5 to 1.3%
[0043] Various dosages of the Ba2 TiMnO6 Nano powderphoto catalyst were added to cement-based compositesseparately which is cast from OPC and White Cement (WC)mortars.
[0044] In a second method of implementation, 2gm of thephotocatalyst was added in 30ml of white Paint (a commerciallyavailable variety was procured for testing purposes) to result in atesting material and used directly for application.
[0045] The efficacy of the photocatalyst in self-cleaningability was performed by subjecting the bricks (obtained from firstmethod of implementation) and the paint (obtained from thesecond method of implementation) to a discoloration test.
[0046] For the purposes of having a realistic simulation of thetest, Rhodamine B dye was selected as the pollutant and the effectof the photocatalyst in removing the pollutant from the samplesprepared were observed and studied.
[0047] A Rhodamine B solution with a concentration of 0.005g / L was prepared by adding 1.5 mg of RhB powder to 30 mL ofdeionized water and allowed to dissolve.
[0048] The brick samples prepared from OPC and WC weredipped in the Rhodamine solution for a time period of 1-2 minutesand then exposed to UV irradiation lamp (LUMILUX T8, 18 W). Thetest was conducted for 4 days and the observation readings weretaken every 3 hours. Figures 1-6 identify the different stages ofthe bricks and its discolouration, obtained at differentconcentrations of the photocatalyst. The a, b, c and d indicationsin the Figures 1-6 identify the readings taken at Day 1, 2, 3 and 4respectively. The compressive strength of the specimens was thesame even at different dosages of photocatalyst. It is concludedthat the specimen prepared with 0.2g of Ba2TiMnO6 gives betterresults in self-cleaning than other specimens.
[0049] Figures 1-6 identify the gradual self-cleaning effect onthe bricks. Day 1 is the first day of testing and therefore, thecolour of the pollutant on the bricks is sharp and bright. However,on Day 2 itself a remarkable effect is observed, wherein thepollutant has been leached or removed from the brick.
[0050] Further, on Days 3 and 4, the cleaning actioncontinues to take place, thereby indicating that the effect of thecatalyst is continuing and has not stopped prematurely.
[0051] On Day 4 of the test period, the bricks are completelyremoved off the pollutant and have achieved a colourless effect;thereby indicating the effectiveness of the photocatalyst on apollutant and exhibiting its self-cleaning effect.
[0052] For the second method of implementation, theRhodamine B solution was mixed with the paint formulation. Thepaint formulation (as described in the second method ofimplementation) was used directly on a building surface andexposed to sunlight. Figure 7 identifies the various stages ofdiscolouration obtained due to the use of the photocatalyst.
[0053] Similar to that of Figures 1-6, it is observed that thereis gradual discolouration effect achieved on the brick, and that atthe end of 5th day, the optimum discolouration effect was achievedand thereafter, the effect of photocatalyst was further prevalentto achieve a complete discoloration.
[0054] The present invention has therefore achieved a selfcleaning effect due to oxidation promoted by sunlight and / or UVirradiation.
[0055] The invention as described above refers to a preferredembodiment. Naturally, while the principle of the inventionremains the same, the details of construction and theembodiments may widely vary with respect to what has beendescribed and illustrated purely by way of the example, withoutdeparting from the scope of the present invention.
Claims
1. A method of preparation of a photocatalyst, comprising: Dissolving BaCO3 (0.5 M) 0.4 gm in 10 ml deionized water; Dissolving MnCO3 (0.5 M) 0.5 gm in 10 deionized water; Dissolving TiO2 (0.3 M) 0.2 gm in 10 deionized water; Dissolving NaOH (8 M) 3.2 gm in 10 deionized water; Mixing the above constituents in 100 ml deionized water; Magnetic stirring for 45 minutes to result in a suspension; and Heating the suspension in a reactor at 1800 C for 12 hours.
2. The method as claimed in claim 1, wherein the resulting photocatalyst is in powder form.
3. A method of testing the photocatalyst, comprising the following steps: Mixing the photocatalyst with a test material to result in a testing material; Application of a pollutant on the testing material; Subjecting the test material to a photo source such as sunlight, UV irradiation.
4. The method as claimed in claim 3, wherein the pollutant is Rhodamine B dye.
5. The method as claimed in claim 3, wherein the concentration of the pollutant is 0.005 g / L.
6. A self-cleaning photocatalyst, wherein the photocatalyst is in powder form; and wherein the photocatalyst is prepared by a method disclosed in claim 1.
7. The photocatalyst as claimed in claim 1, wherein the photocatalyst is Ba2TiMnO6.