Microwave ceramic dielectric filter and processing and forming method therefor

IN598063BActive Publication Date: 2026-08-05SHENZHEN SUNLORD ELECTRONICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
IN202237071242
Authority / Receiving Office
IN · IN
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-05-11
Filing Date
2022-12-09
Publication Date
2026-08-05
Estimated Expiration
2041-02-26

AI Technical Summary

Technical Problem

Current methods for molding microwave ceramic dielectric filters, such as dry pressing, result in nonuniform density distribution, inconsistent dimensional shrinkage, and poor dimensional accuracy, which affects the dielectric properties and increases production costs, making it difficult to produce complex shapes and meet the requirements of modern microwave communication systems.

Method used

The method involves injection molding a mixture of microwave ceramic powder and a ceramic molding agent containing a binder, with specific mass percentages and additives, followed by debinding and segmented heating to achieve uniform density and consistent dielectric properties, allowing for the production of ceramic dielectric filters with improved mechanical and dielectric performance.

Benefits of technology

This approach results in microwave ceramic dielectric filters with uniform density and stable dielectric constants, reducing production costs and enabling mass production of high-performance ceramic components suitable for advanced communication applications.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Disclosed are a processing and forming method for a microwave ceramic dielectric filter and the microwave ceramic dielectric filter prepared by means of the method. The microwave ceramic dielectric filter comprises a ceramic dielectric body and a metal layer attached to the surface of the ceramic dielectric body, and the ceramic dielectric body is formed by mixing microwave ceramic powder with a ceramic forming agent at least containing a binder and then performing injection molding. The present invention can solve the problems of inconsistent dry-pressing molding size shrinkage, a local dielectric constant difference, incapability of molding complex shapes, and non-uniform green body density and the like of the microwave ceramic dielectric filter.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present application relates to the technical field of communications, in particular to a method for processing and molding a microwave ceramic dielectric filter.BACKGROUND

[0002] Filter is an important device in the field of microwave communication. Its main function is to suppress unwanted signals and allow the required signals to pass smoothly. Microwave dielectric ceramics are a new type of functional ceramic powder developed in the past two decades. It refers to ceramic powder used as dielectric powder in microwave frequency (mainly 300MHz-30GHz frequency band) circuits and completes one or more functions. It is the key powder for the manufacture of microwave dielectric filters and resonators. It has excellent properties such as high dielectric constant, low dielectric loss, and small temperature coefficient. It is suitable for manufacturing various microwave components and can meet the requirements of miniaturization, integration, high reliability and low cost of microwave circuits.

[0003] With the advent of the 5G era, it has become a foregone conclusion that microwave ceramic dielectric filters featuring small size, low transmission loss, stable frequency, and low temperature coefficient will replace traditional metal resonators. The mainstream molding method of microwave ceramic dielectric filters is dry pressing molding. Different from structural ceramics, the density distribution of the dry-pressed ceramic body is nonuniform, the shrinkage is inconsistent, the dimensional accuracy is poor, and the sintering deformation is large, resulting in more subsequent flat grinding and CNC machining and high production costs. The nonuniform density distribution also affects the dielectric properties of ceramics, such as the dielectric constant and Qf value, which in turn affects the performance indicators of microwave ceramic dielectric filters. As the design of dielectric filters becomes complicated, dry press molding of dielectric filters of various special-shaped hole and slot structures cannot meet the molding requirements.

[0004] Injection molding of ceramic materials is to form ceramic parts by injecting plastic materials under pressure. This molding method is relatively mature in structural ceramics. However, the ceramic dielectric in the microwave ceramic dielectric filter is a functional ceramic material, and the current injection molding process has not yet met the requirements of functional ceramic parts.SUMMARY OF THE INVENTION

[0005] In order to overcome the deficiencies of the prior art, an objective of the present application is to provide a method for processing and molding a microwave ceramic dielectric filter, which solves the problems of inconsistent dimensional shrinkage, inability to mold complex shapes, and nonuniform density of the green body of microwave ceramic dielectric filters during dry pressing.

[0006] In order to achieve the above objective, the content of the technical solution adopted in the present application is as follows:

[0007] A microwave ceramic dielectric filter, including a ceramic dielectric body and a metal layer attached to a surface of the ceramic dielectric body, wherein the ceramic dielectric body is molded by injection molding a mixture of microwave ceramic powder and a ceramic molding agent containing at least a binder.

[0008] As a further preferred solution of the present application, an amount of the microwave ceramic powder and the ceramic molding agent is respectively 75wt%-90wt% and 10wt%-25wt% by mass percentage.

[0009] As a further preferred solution of the present application, the microwave ceramic powder is one of a calcium magnesium titanate series, a samarium calcium aluminate series, a barium titanate series, and a lanthanum strontium aluminate series, and a particle size of the microwave ceramic powder does not exceed 1.5 μm, and a moisture content does not exceed 0.5%.

[0010] As a further preferred solution of the present application, the ceramic molding agent further includes one or two or more of a plasticizer, a lubricant, a dispersant, and a surfactant.

[0011] As a further preferred solution of the present application, the ceramic molding agent includes by mass percentage: binder 50wt%-85wt%; plasticizer 5wt%-15wt%; and surfactant 3wt%-10wt%.

[0012] As a further preferred solution of the present application, the binder is a mixture of one or two or more of paraffin, polyethylene, low density polyethylene, ethylene-vinyl acetate copolymer, polypropylene, random polypropylene, polymethacrylate, and polyaldehyde groups; the plasticizer is a mixture of one or two or more of diethyl phthalate, dibutyl phthalate, dioctyl phthalate, and di-n-butyl phthalate; and the surfactant is a mixture of one or two or more of oleic acid, stearic acid, microcrystalline paraffin, white oil, and silicone oil.

[0013] As a further preferred solution of the present application, the acid is an organic acid or an inorganic acid.

[0014] A method for processing and molding a microwave ceramic dielectricfilter, including:

[0015] a mixing and granulating step: mixing the ceramic molding agent and the microwave ceramic powder uniformly, placing the same in an internal mixer for preheating and melting, kneading and mixing the same uniformly, and then granulating to obtain a microwave ceramic feed;

[0016] an injection molding step: loading the microwave ceramic feed into an injection molding machine for injection molding to obtain a ceramic dielectric green body;

[0017] a debinding step: removing organic matters in the ceramic dielectric green body;

[0018] a sintering and molding step: placing the debinded ceramic dielectric green body in a sintering furnace, and sintering the same using a sintering method of segmented heating to obtain a molded ceramic dielectric; and

[0019] a metallization treatment step: metallizing the ceramic dielectric to obtain a microwave ceramic dielectric filter.

[0020] As a further preferred solution of the present application, in the sintering and molding step, a flow process of the sintering method of segmented heating is as follows: in a first stage, heating up from room temperature to 600-680°C after 1000-1300min, with a heating rate of 0.3-0.7°C / min, and keeping the temperature at 600-680°C for 200-250min; in a second stage, heating up from 600-680°C to 1400-1500°C, with a heating rate of 3-5°C / min; and in a third stage, naturally cooling the temperature after being kept at 1400-1500°C for 3-6 hours.

[0021] As a further preferred solution of the present application, in the injection molding step, an injection pressure is 55MPa-85MPa, and an injection speed is 30mm / s-80mm / s.

[0022] As a further preferred solution of the present application, in the injection molding step, an injection temperature is 135°C-200°C, a mold temperature is 40°C-150°C, and a pressure holding speed is 20mm / s -40mm / s.

[0023] As a further preferred solution of the present application, in the debinding step, a debinding process is one of thermal debinding, solvent debinding or acid debinding.

[0024] As a further preferred solution of the present application, in the debinding step, organic acid catalyzed debinding is adopted, a debinding temperature is 115°C-155°C, a reaction time is 15h-35h, and an amount of acid feeding is 1.5-4.5g / min.

[0025] As a further preferred solution of the present application, in the mixing and granulating step, a preheating temperature of the internal mixer is 150-165°C, a temperature during kneading and mixing is 170°C-200°C, a kneading time is 30min-120min, and a speed of the internal mixer is 5-15r / min.

[0026] As a further preferred solution of the present application, the method for processing and molding a microwave ceramic dielectric filter further includes a step of treating the microwave ceramic powder: drying the microwave ceramic powder at a temperature of 400-500°C, and keeping the temperature at 120-160°C after drying.

[0027] Compared with the prior art, the present application has the following beneficial effects.

[0028] 1. The microwave ceramic dielectric filter according to the present application has uniform density and excellent mechanical properties. Various parts of the green body have stable and consistent dielectric constants and can be used for mass production of ceramic dielectric filters.

[0029] 2. The method for processing and molding a microwave dielectric filter according to the present application can obtain a ceramic dielectric filter green body with uniform dimension shrinkage and small sintering deformation, which can effectively reduce processing difficulty and production costs.

[0030] 3. The method for processing and molding a dielectric filter according to the present application has superior technological conditions, and can realize large-scale mass production, and the obtained ceramic material has superior performance and is suitable for being widely used in the field of communications.

[0031] The above description is merely an overview of the technical solution of the present application. In order to be able to understand the technical means of the present application more clearly, it can be implemented according to the content of the description. In order to make the above and other objectives, features and advantages of the present application more obvious and easy to understand, the following specific preferred examples are described in detail as follows.BRIEF DESCRIPTION OF THE DRAWINGS

[0032] FIG. 1 is a surface electron microscope image of a green body of a ceramic dielectric body in Example 2;

[0033] FIG. 2 is a surface electron microscope image of a sintered body of aceramic dielectric body in Example 2;

[0034] FIG. 3 is a surface electron microscope image of a green body of a ceramic dielectric body in Comparative Example 1; and

[0035] FIG. 4 is a surface electron microscope image of a sintered body of a ceramic dielectric body in Comparative Example 1.DETAILED DESCRIPTION OF THE EXAMPLES

[0036] In order to further illustrate the technical means and effects adopted by the present application to achieve the predetermined objective of the present application, below in conjunction with the examples, the specific examples, structures, features and methods and effects thereof according to the present application are described in detail as follows:

[0037] A microwave ceramic dielectric filter according to the present application includes a ceramic dielectric body and a metal layer attached to a surface of the ceramic dielectric body. The ceramic dielectric body is made by injection molding of a mixture of microwave ceramic powder and a ceramic molding agent containing at least a binder. A density of the ceramic dielectric body is not less than 3.0g / cm3 . Preferably, the density of the ceramic dielectric body is 3.0-6.5g / cm3

[0038] A method for processing and molding a microwave ceramic dielectric filter includes:

[0039] a mixing and granulating step: mixing the ceramic molding agent and the microwave ceramic powder uniformly, placing the same in an internal mixer for preheating and melting, kneading and mixing the same uniformly, and then granulating to obtain a microwave ceramic feed;

[0040] an injection molding step: loading the microwave ceramic feed into an injection molding machine for injection molding to obtain a ceramic dielectric green body;

[0041] a debinding step: removing organic matters in the ceramic dielectric green body;

[0042] a sintering and molding step: placing the debinded ceramic dielectric green body in a sintering furnace, and sintering the same using a sintering method of segmented heating to obtain a molded ceramic dielectric; and

[0043] a metallization treatment step: metallizing the ceramic dielectric to obtain a microwave ceramic dielectric filter.

[0044] In the above method, in the mixing and granulating step, the order of feeding will affect the uniformity of mixing. In the present application, the molding agent and the microwave ceramic powder are mixed uniformly first and then preheated and kneaded, and during the heating process, after the colloid is melted, it is mixed uniformly with the molding agent and distributed in the microwave ceramic powder. Considering that a molding agent with a low melting point will volatilize under heating conditions, a molding agent with a high melting point can be mixed with the microwave ceramic powder first, and after reaching a preheating temperature, the molding agent with a low melting point is added, which can effectively avoid the volatilization of the solvent.

[0045] The inventors found in the research that in the injection molding process, the injection pressure and the injection speed have an important influence on the molding of the green body. It is mainly manifested as: due to the existence of a variety of irregular particles in the microwave ceramic feed, there are voids between these particles, which will retain air in the green body. If the injection pressure is too small, the density of the green body may not be able to meet the requirements of the dielectric filter, and the injection molding time of the feed will also be prolonged, which will affect the integrity of the filling process, resulting in incompleteness of the injection molding. Under a certain injection pressure, the blank will first produce elastic deformation under the influence of stress, and as the stress increases and reaches the rheological limit, the blank will produce irreversible pseudoplastic deformation, which is caused by the plastic deformation of the molding agent and the relative displacement of the powder particles. Therefore, coarse particles in the feed push fine particles and ultrafine particles to spread longitudinally and laterally, fine particles enter gaps between coarse particles, and ultrafine particles enter gaps between fine particles and coarse particles, resulting in that the porosity gradually decreases. As the injection pressure increases, the particles of the microwave ceramic powder become more compact, the moisture is compressed from the small pores to the atmosphere, and the air is further compressed and extruded. When the injection pressure reaches a certain limit value, the density of the green body increases and reaches a dense state. If the injection pressure exceeds the limit value, the density of the green body will no longer increase, which will cause flow lines and bubbles. In this case, after the pressure is suddenly removed, the ceramic green body will produce elastic after-effects, which will cause spalling and reduce the density. It can be seen that the control of the injection pressure has a very important influence on the density of the ceramic green body. In order to meet the requirements of the microwave dielectric filter on the density of the ceramic dielectric, in the injection molding step according to the present application, the injection pressure is controlled to be 55MPa-150MPa. Further, the injection speed will also affect the density of the green body, and the injection speed is 30mm / s-80mm / s.

[0046] In a specific example, in the debinding step according to the present application, the debinding process is one of thermal debinding, solvent debinding or catalytic debinding. Among them, thermal debinding is to place a ceramic part in an electric furnace for heating to above 500°C to remove the remaining binder in the green body. During the thermal debinding process, gas molecules are transmitted to the surface of the molded green body by diffusion or penetration. The thermal debinding process is proportional to the thickness of the green body, so it generally takes a longer time for thermal debinding. Solvent debinding is to use non-polar solvents, such as gasoline, chloroform, petroleum ether and other solvents for debinding. The efficiency of solvent debinding is high, and the debinding time is short, but if the process is not controlled well, swelling may appear, resulting in green body cracking. Catalytic debinding is the debinding of a ceramic green body for a binder of a polymerized aldehyde-based system, and a cracking reaction is carried out by acid vapor catalysis in the debinding process. As a further preferred solution of the present application, an acid is used as a catalyst in the debinding step according to the present application, and the acid may be an organic acid or an inorganic acid.

[0047] The inventors also found that during the sintering process of the molded ceramic dielectric green body, the molded green body is heated to a high temperature and kept for an appropriate time, and through material migration and a series of physical and chemical changes, a densification process of enhanced bonding between powder particles, grain growth, and reduction of pores and grain boundaries is completed to eventually forms a solid green body. During the sintering process, the water in the green body is first discharged. With the discharge of the water in the capillary pores in the green body, the particles are drawn together, and the green body shrinks, forming an internal stress. In this process, if the heating rate is too fast and the temperature is too high, the water on the surface of the green body evaporates violently, the surface layer shrinks to the maximum, the capillary tube of the surface layer is shrunk or even closed, it is difficult for the internal water to migrate outward, and the humidity difference between the inside and outside increases. As a result, the surface layer of the green body is under a tensile stress and the inner layer is under a compressive stress. If the internal stress is not uniform, the green body will deform. When the tensile stress exceeds the dry strength of the green body, the green body will crack. Therefore, in the present application, before sintering and heating, the ceramic dielectric green body is heated up from room temperature to 600-680°C in the sintering furnace for 1000-1300min. This stage is a debinding stage, allowing the remaining organic mattersin the green body to come out except the adhesive. In order to prevent the heating rate being too fast, the cracking of the binder being too violent, and the weight loss being too fast to result in nonuniform sintering of the entire green body, it is necessary to control the heating rate. In the present application, the heating rate in a first stage is controlled to 0.3 -0.7°C / min, and the temperature is kept at 600-680°C for 200-250min, which stage is equivalent to the debinding stage. In a second stage, the temperature is raised from 650°C to 1400-1500°C, which stage is a densification process to increase the strength of the green body and form a dense and firm ceramic body, with a heating rate of 3-5°C / min. In a third stage, the temperature is kept at 1400- 1500°C for 3-6 hours to ensure sufficient growth of ceramic grains to complete the ceramic densification process.

[0048] As a further preferred solution of the present application, in the injection molding step according to the present application, if the melting degree of the feed is low, the feed will block the mold during the injection process. If the injection temperature is too high and the feed reaches a completely molten state, the feed will produce the phenomenon of segregation and two-phase separation in the injection process. In addition, the low-melting-point components in the molding agent will be excessively volatilized, which will produce a large number of pores in the green body during the volatilization process and affect the density of the green body. Therefore, in the present application, the injection temperature is 135°C-200°C, preferably 140-160°C. In addition, through further experiments, it was found that the pressure holding speed also affects the density of the green body. If the pressure holding speed is too fast, the pressure holding time will be insufficient, resulting in that the size of the green body will be excessively thick and the density is nonuniform. Therefore, in the present application, in a preferred solution, the pressure holding speed needs to be controlled within a range of 20mm / s-40mm / s. In order to avoid a deformation of the injection-molded green body caused by directly changing from high temperature to low temperature in the mold, the mold needs to be heated. In the present application, the mold temperature is 40°C-150°C, preferably 90-120°C.

[0049] As a further preferred solution of the present application, in the mixing and granulating step according to the present application, in order to prevent the low-melting-point components in the molding agent from volatilizing seriously under the heating effect, the preheating temperature of the internal mixer is 150- 165°C, the temperature during kneading and mixing is 170°C-200°C, the kneading time is 30min-120min, and the speed of the internal mixer is 5-15r / min.

[0050] As a further preferred solution of the present application, the method for processing and molding a microwave ceramic dielectric filter according to the present application further includes a step of treating the microwave ceramic powder: drying the microwave ceramic powder at a temperature of 400-500°C, and keeping the temperature at 12-160°C after drying.

[0051] In the present application, the microwave ceramic powder and the ceramic molding agent are mixed in a certain ratio. Preferably, in the present application, an amount of the microwave ceramic powder and the ceramic forming agent is respectively 75wt%-90%wt% and 10wt%-25wt% by mass percentage. Further preferably, the mass percentages are 75wt%-80wt% and 20wt%-25wt%. Further, the mass percentages may also be 78wt%-82wt% and 18wt%-22wt%.

[0052] As a further preferred solution of the present application, the ceramic powder according to the present application is one of a calcium magnesium titanate series, a samarium calcium aluminate series, a barium titanate series, and a lanthanum strontium aluminate series.

[0053] In the present application, the inventors found that the uniformity of material distribution during mixing is largely determined by the ratio of the density of each component to the particle size of the powder. The closer the density and particle size are, the more likely it is to obtain a mixture of uniform quality. Therefore, in order to obtain a consistent microwave ceramic dielectric, preferably, the particle size of the microwave ceramic powder according to the present application does not exceed 1.5 μm, and the moisture content does not exceed 0.5%.

[0054] In the present application, in the injection molding process, the binder is one of the key factors. When selecting the binder, the fluidity of the binder should be considered first, and the viscosity should be moderate. If the viscosity is too high, the ceramic powder cannot be effectively dispersed in the binder, increasing the difficulty of mixing, and the obtained ceramic feed is nonuniform. If the viscosity is too low, delamination will appear between the ceramic powder and the binder, affecting the consistency of the ceramic green body. Secondly, the wettability of the binder to the powder should also be considered, in order to increase the fluidity of the powder, and facilitate injection molding. In addition, in order to ensure the thermal conductivity and thermal expansion coefficient of the functional ceramics, the added binder should avoid thermal stress making the green body defective. The binder that may be selected in the present application is a mixture of one or two or more of paraffin, polyethylene, low density polyethylene, ethylene-vinyl acetate copolymer, polypropylene, random polypropylene, polymethacrylate, polyaldehyde, etc. In the present application, the preferably adopted binders contain at least a polyaldehyde group binder, which has good compatibility with the ceramic powder. The molded green body has high strength and can meet the performance requirements of functional ceramics, and the product pass rate is high. The polyacetal group binder can be specifically selected from but not limited to polyoxymethylene. When a polyoxymethylene binder is adopted, the microwave ceramic filter according to the present application adopts an acid-catalyzed debinding process during the molding process. Specifically, it can be organic acid catalyzed debinding or inorganic acid debinding. The listed organic acids may be selected from but not limited to oxalic acid. The inorganic acid may be selected from but not limited to nitric acid. In the present application, oxalic acid is preferably used as a catalyst for debinding. In the present application, the debinding efficiency of oxalic acid is high and the time is short. In the oxalic acid catalysis process, the reaction temperature is lower than the melting point of the polyoxymethylene resin, and the liquid phase is avoided, thereby avoiding softening of the green body or deformation due to gravity. Therefore, it will not affect the morphology of the molded ceramic green body and the yield of sintering. In the present application, the amount of acid feeding is also a factor affecting the quality of the green body. The larger the amount of acid feeding, the faster the reaction rate will be. However, too much acid will affect the morphology of the ceramic green body, and it will not help the reaction of removing the binder. In addition, if the debinding time is short, the debinding will be incomplete, and the ceramic will crack during sintering. If the debinding time is too long, the production efficiency will be low. In the present application, by controlling the time of the debinding reaction and the amount of acid feeding, the two influencing factors are synergized with each other to achieve an optimal effect. Therefore, as a preferred solution, in the debinding step according to the present application, the temperature of the acid catalyzed debinding is 115°C-155°C, the reaction time is 15h-35h, and the amount of acid feeding is 1.5-4.5g / min.

[0055] In the present application, the molding agent can improve the fluidity of the ceramic powder during molding, increase the bonding force between particles, and improve the mechanical strength of the green body. Therefore, the main function of the molding agent not only includes a bonding effect (which is achieved by the binder), but also sometimes needs to include a plasticizing effect, which is usually achieved by adding a plasticizer. However, the adsorption effect of the binder and the plasticizer with the surface of the microwave ceramic powder will be affected. In order to improve this effect, it can be solved by adding a small amount of surfactant. Therefore, the ceramic molding agent according to the present application contains not only a binder, but also one or two or more of a plasticizer, a lubricant, a dispersant, and a surfactant. In the present application, a preferred combination mode of the ceramic molding agent that can be implemented includes a binder, a plasticizer, and a surfactant. Alternatively, there may be a second combination mode including a plasticizer, a lubricant, and a dispersant. Also, there may be a third combination mode including a binder, a plasticizer, a lubricant, a dispersant, and a surfactant. A fourth combination mode includes a binder, a plasticizer, a lubricant, and a surfactant. Of course, the present application is not limited to the above combination modes. In a specific solution, the plasticizer may be selected from a mixture of one or two or more of diethyl phthalate, dibutyl phthalate, dioctyl phthalate, di-n-butyl phthalate, etc. The surfactant may be selected from a mixture of one or two or more of oleic acid, stearic acid, microcrystalline paraffin, white oil, silicone oil, etc.

[0056] During specific implementation, as an implementation, the ceramic molding agent according to the present application includes by mass percentage: binder 60wt%-85wt%; plasticizer 5wt%-25wt%; and surfactant 3wt%-15wt%. As another implementation, the mass percentage of the microwave ceramic powder is 75%-90%, the mass percentage of the binder is 10%-20%, the mass percentage of the plasticizer is 1%-4%, and the mass percentage of the surfactant is 0.5% %-3%.

[0057] Hereinafter, the present application will be further explained and illustrated in detail with specific preferred examples, but the scope of protection of the present application is not limited to the content of the following examples.

[0058] Example 1

[0059] A microwave ceramic dielectric filter includes a ceramic dielectric body and a metal layer attached to a surface of the ceramic dielectric body. Feed materials for preparing the ceramic dielectric body include 24kg of microwave ceramic powder, 4.2kg of polyoxymethylene, 0.9kg of polypropylene, 0.6kg of paraffin wax, 0.012kg of dioctyl phthalate, 0.06kg of oleic acid, and 0.06kg of silicone oil.

[0060] Its preparation process is as follows:

[0061] Mixing and granulating step: a ceramic molding agent is placed in an internal mixer for preheating and melting, the mixing temperature is 165°C, and the speed is 5r / min; the microwave ceramic powder is added for kneading, the kneading temperature is 185°C, and the speed is 25r / min; a milky white mud mass is obtained after kneading and mixing uniformly, and then granulated with a granulator to obtain a microwave ceramic feed.

[0062] Injection molding step: the above microwave ceramic feed is loaded into an injection molding machine for injection molding to obtain a ceramic dielectric green body, the injection temperature is 155°C, the mold temperature is 125°C, the injection speed is 40mm / s, and the pressure holding speed is 20mm / s.

[0063] Debinding step: organic matters in the ceramic dielectric green body are removed using oxalic acid catalyzed debinding, and the debinding parameters are as follows: the temperature is 125°C, the time is 18h, and the amount of acid feeding is 1.8g / min.

[0064] Sintering and molding step: the above debinded ceramic dielectric green body is placed into a sintering furnace for sintering with a heat-up system in which it is heated up to 650°C at a heating rate of 0.5°C / min, kept at 650°C for 240 minutes, and then heated up from 650°C to 1480°C at a rate of 5°C / min, and kept at the highest temperature for 5 hours, and a molded ceramic dielectric is obtained after the sintering is completed.

[0065] Metallization treatment step: the above ceramic dielectric is metallized to obtain a microwave ceramic dielectric filter after debugging.

[0066] In this example, in order to further verify the influence of the injection pressure on the green body and the molded microwave ceramic dielectric, property effects of the green body and the microwave ceramic dielectric under different injection pressures in a range of 10-100 MPa were investigated. The results are shown in Table 1.

[0067] In the range of 10-100 MPa, the inventors made green bodies using 5 MPa as a step interval, and found that when the injection pressure was below 35 MPa, the filling of the green bodies was not tight, about 23% of the obtained green bodies could not meet the requirements, and more than 30% of the green bodies will collapse when sintered. In the morphology of a sample with a lower injection pressure, the surface appears concave and uneven, and the cross section has obvious 25 defects such as cracking and voids. Due to a high defective rate of green bodies and sintered bodies at a lower injection pressure, green bodies under an injection pressure below 35MPa were not sintered and their properties were not analyzed. Similarly, it was found that after the injection pressure exceeds 160MPa, because the pressure is too high, the green bodies cool too fast, about 25% of the green bodies will deform, and after being sintered, 21% of the sintered bodies will have cracks. Therefore, green bodies under an injection pressure exceeding 95MPa will not be sintered and its property analysis will not be carried out.

[0068] Table 1: Effects of injection pressure on properties of microwave ceramic green bodies and sintered bodies pressure is in the range of 55-150MPa, both the green body and the sintered body can meet the requirements in terms of density and bending strength. When the injection pressure is 65-80MPa, the density and the bending strength both have excellent performance. When the injection pressure is in the range of 55-150MPa, the sintered body obtained has excellent thermal conductivity. After being processed into a microwave dielectric filter, the Q value is excellent.

[0070] Example 2

[0071] A microwave ceramic dielectric filter includes a ceramic dielectric body and a metal layer attached to a surface of the ceramic dielectric body. Feed materials for preparing the ceramic dielectric body include 24.6 kg of microwave ceramic powder, 3.51 kg of polyoxymethylene, 1.08 kg of low-density polyethylene, 0.54kg of paraffin wax, 0.108kg of dioctyl phthalate, 0.081kg of oleic acid, 0.054kg of sorbitan monostearate, and 0.027kg of polyamide.

[0072] Its preparation process is as follows:

[0073] Pretreatment of microwave ceramic powder: the microwave ceramic powder is dried at 500°C for 2 hours, and the temperature is kept at 150°C.

[0074] Mixing and granulating step: a ceramic molding agent and the microwave ceramic powder are mixed uniformly and then placed into an internal mixer for preheating and melting, the preheating temperature is 165°C, and the speed is 5r / min; after reaching the preheating temperature, they are heated up and kneaded, the kneading temperature is 180°C, and the speed is 25r / min; and a milky white mud mass is obtained after kneading and mixing uniformly, and then granulated with a granulator to obtain a microwave ceramic feed.

[0075] Injection molding step: the above microwave ceramic feed is loaded into 2an injection molding machine for injection molding to obtain a ceramic dielectric green body, the injection temperature is 195°C, the injection pressure is 65MPa, the mold temperature is 120°C, the injection speed is 40mm / s, and the pressure holding speed is 25mm / s.

[0076] Debinding step: organic matters in the ceramic dielectric green body are removed using oxalic acid catalyzed debinding, and the debinding parameters are as follows: the temperature is 125°C, the time is 18h, and the amount of acid feeding is 1.8g / min.

[0077] Sintering and molding step: the above debinded ceramic dielectric green body is placed into a sintering furnace, heated up from room temperature to 650°C after 1300min, then to 680°C at a heating rate of 0.3°C / min, and kept at 680°C for 240min, then heated up from 680°C to 1480°C at a rate of 3°C / min, and kept at the highest temperature for 5 hours, and after the sintering was completed, a molded ceramic dielectric was obtained.

[0078] Metallization treatment step: the above ceramic dielectric is metallized, and a microwave ceramic dielectric filter is obtained after debugging.

[0079] The inventors observed the surfaces of the green body and the sintered body of the ceramic dielectric body of Example 2 with an electron microscope, and the results of the electron microscope are shown in FIGS. 1 and 2. The results in FIGS. 1 and 2 show that the surfaces of the green body and the sintered body are characterized by compactness and consistency.

[0080] Example 3

[0081] A microwave ceramic dielectric filter includes a ceramic dielectric body and a metal layer attached to a surface of the ceramic dielectric body. Feed materials for preparing the ceramic dielectric body include 24kg of microwave ceramic powder, 4.2kg of polyacetal group, 0.9kg of polypropylene, 0.6kg of paraffin wax, 0.012kg of dioctyl phthalate, 0.06kg of oleic acid, and 0.06kg of silicone oil.

[0082] Its preparation method is as follows:

[0083] Mixing and granulating step: a ceramic molding agent is placed into an internal mixer for preheating and melting, the mixing temperature is 165°C, and the speed is 5r / min; the microwave ceramic powder is added for kneading, the kneading temperature is 185°C, and the speed is 25r / min; a milky white mud mass is obtained after kneading and mixing uniformly, and then granulated with a granulator to obtain a microwave ceramic feed.

[0084] Injection molding step: the above microwave ceramic feed is loaded into an injection molding machine for injection molding to obtain a ceramic dielectric green body, the injection temperature is 195°C, the injection pressure is 65MPa, the mold temperature is 125°C, the injection speed is 40mm / s, and the pressure holding speed is 20mm / s.

[0085] Debinding step: organic matters in the ceramic dielectric green body are removed using oxalic acid catalyzed debinding, and the debinding parameters are as follows: the temperature is 145°C, the time is 12h, and the amount of acid feeding is 3.5g / min.

[0086] Sintering and molding step: the above debinded ceramic dielectric green body is placed into a sintering furnace for sintering with a heat-up system in which it is heated up from room temperature to 650°C after 1300min and to 650°C at a heating rate of 0.7°C / min, kept at 650°C for 240 minutes, and then heated up from 650°C to 1480°C at a rate of 5°C / min, and kept at the highest temperature for 5 hours, and a molded ceramic dielectric is obtained after the sintering is completed.

[0087] Metallization treatment step: the above ceramic dielectric is metallized, and a microwave ceramic dielectric filter is obtained after debugging.

[0088] Comparative Example 1

[0089] In this comparative example, effects of the settings of the sintering and molding step and the sintering temperature procedure on the properties of the green body, the sintered body, and the microwave ceramic filter are mainly compared. In this comparative example, steps the same as those in Example 4 are adopted. The difference lies in that the sintering and molding step adopts vacuum sintering directly in the sintering furnace, and the sintering temperature is 1480°C. The sintered body in the comparative example was observed by a surface electron microscope, and the surface electron microscope diagram is shown in FIG. 3.

[0090] Performance comparison

[0091] Properties of the green bodies, the sintered bodies, and the microwave ceramic dielectric filters obtained in Example 2, Example 3, and Comparative Example are compared. Table3 shows comparison property items and results. The quantity of each group of samples in Examples 2 and 3 and Comparative Example 1 is 20 pieces.

[0092] Table3: Property comparison results of Examples 2, 3 and Comparative Example 1

[0093] According to the results in Table 2 above, it can be seen that the sintering temperature procedure mainly affects the pass rate, the density, the compactness, and the bending strength of the sintered body. It can be seen from the properties that the pass rate, density, compactness, and bending strength of the sintered body in Examples 2 and 3 are significantly higher than those in Comparative Example 1. FIG. 3 shows that the surface of the sintered body has pores and depressions.

[0094] Comparative Example 2

[0095] According to the raw material ratio in Example 3 above, effects of the feeding sequence of the ceramic powder and the ceramic molding agent on the properties of the green body, the sintered body, and the microwave ceramic dielectric filter in the mixing and granulating step was investigated. In this comparative example, other steps are the same as in Example 3. The difference lies in that the mixing and granulating step is as follows: firstly mixing the ceramic molding agent and the microwave ceramic powder uniformly, and then kneading the same according to the same steps as in Example 3. The green body in Comparative Example 2 was observed with an electron microscope, and an electron microscope diagram is shown in FIG. 4.

[0096] Performance comparison

[0097] The properties of the green body, the sintered body, and the microwave ceramic dielectric filter in the above Example 2, Example 3 and Comparative Example 2 were compared. The quantity of each group of samples in Examples 2 and 3 and Comparative Example 2 is 20 pieces.

[0098] Table4: Property comparison results of Examples 2, 3 and Comparative Example 2

[0099] From the results in Table 3 above, it can be seen that the pass rate of green body, the density of green body, the pass rate of sintered body, the density of sintered body, and the compactness of sintered body in Examples 2 and 3 are significantly higher than those in Comparative Example 2. It can also be seen from FIG. 4 that the surface of the green body is uneven and the particle distribution is nonuniform.

[00100] The above examples are merely preferred examples of the present application, and are not intended limit the scope of protection of the present application. Any insubstantial changes and substitutions made by those skilled in the art on the basis of the present application belong to the scope of protection of the present application.

Claims

1. A microwave ceramic dielectric filter, comprising a ceramic dielectric body and a metal layer attached to a surface of the ceramic dielectric body, wherein the ceramic dielectric body is molded by injection molding a mixture of microwave ceramic powder and a ceramic molding agent containing at least a binder.

2. The microwave ceramic dielectric filter according to claim 1, wherein an amount of the microwave ceramic powder and the ceramic molding agent is respectively 75wt%-90wt% and 10wt%-25wt% by mass percentage.

3. The microwave ceramic dielectric filter according to claim 1, wherein the microwave ceramic powder is one of a calcium magnesium titanate series, a samarium calcium aluminate series, a barium titanate series, and a lanthanum strontium aluminate series, and a particle size of the microwave ceramic powder does not exceed 1.5 μm, and a moisture content does not exceed 0.5%.

4. The microwave ceramic dielectric filter according to claim 1, wherein the ceramic molding agent further comprises one or two or more of a plasticizer, a lubricant, a dispersant, and a surfactant.

5. The microwave ceramic dielectric filter according to claim 4, wherein the ceramic molding agent comprises by mass percentage: binder 50wt%-85wt%; plasticizer 5wt%-15wt%; and surfactant 3wt%-10wt%.

6. The microwave ceramic dielectric filter according to claim 4 or 5, wherein the binder is a mixture of one or two or more of paraffin, polyethylene, low density polyethylene, ethylene-vinyl acetate copolymer, polypropylene, random polypropylene, polymethacrylate, and polyaldehyde groups; the plasticizer is a mixture of one or two or more of diethyl phthalate, dibutyl phthalate, dioctyl phthalate, and di-n-butyl phthalate; and the surfactant is a mixture of one or two or more of oleic acid, stearic acid, microcrystalline paraffin, white oil, and silicone oil.

7. The microwave ceramic dielectric filter according to claim 1, wherein a density of the ceramic dielectric body is 3.0-6.5g / cm38. A method for processing and molding the microwave ceramic dielectric filter according to any one of claims 1-7, comprising: a mixing and granulating step: mixing the ceramic molding agent and the microwave ceramic powder uniformly, placing the same in an internal mixer for preheating and melting, kneading and mixing the same uniformly, and then granulating to obtain a microwave ceramic feed; an injection molding step: loading the microwave ceramic feed into an injection molding machine for injection molding to obtain a ceramic dielectric green body; a debinding step: removing organic matters in the ceramic dielectric green body; a sintering and molding step: placing the debinded ceramic dielectric green body in a sintering furnace, and sintering the same using a sintering method of segmented heating to obtain a molded ceramic dielectric; and a metallization treatment step: metallizing the ceramic dielectric to obtain a microwave ceramic dielectric filter.

9. The processing and molding method according to claim 8, wherein, in the sintering and molding step, a flow process of the sintering method of segmented heating is as follows: in a first stage, heating up from room temperature to 600- 680°C after 1000-1300min, with a heating rate of 0.3-0.7°C / min, and keeping the temperature at 600-680°C for 200-250min; in a second stage, heating up from 600- 680°C to 1400-1500°C, with a heating rate of 3-5°C / min; and in a third stage, naturally cooling the temperature after being kept at 1400-1500°C for 3-6 hours.

10. The processing and molding method according to claim 8, wherein, in the injection molding step, an injection pressure is 55MPa-150MPa, and an injection speed is 30mm / s-80mm / s.

11. The processing and molding method according to claim 8, wherein, in the injection molding step, an injection temperature is 135°C-200°C, a mold temperature is 40°C-150°C, and a pressure holding speed is 20mm / s-40mm / s.

12. The processing and molding method according to claim 8, wherein, in the mixing and granulating step, a preheating temperature of the internal mixer is 150- 165°C, a temperature during kneading and mixing is 170°C-200°C, a kneading time is 30min-120min, and a speed of the internal mixer is 5-15r / min.

13. The processing and molding method according to claim 8, wherein, in the debinding step, a debinding process is one of thermal debinding, solvent debinding or acid debinding.

14. The processing and molding method according to claim 13, wherein, in the debinding step, organic acid catalyzed debinding is adopted, a debinding temperature is 115°C-155°C, a reaction time is 15h-35h, and an amount of acid 1feeding is 1.5-4.5g / min.

15. The processing and molding method according to any one of claims 8-14, further comprising a step of treating the microwave ceramic powder: drying the microwave ceramic powder at a temperature of 400-500°C, and keeping the temperature at 120-160°C after drying.