Hydrocarbon adsorbent and hydrocarbon adsorption method

IN598903BActive Publication Date: 2026-08-12TOSOH CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
IN202217058106
Authority / Receiving Office
IN · IN
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-31
Filing Date
2022-10-12
Publication Date
2026-08-12
Estimated Expiration
2041-03-30

AI Technical Summary

Technical Problem

Current hydrocarbon adsorbents used in vehicles lack sufficient heat resistance and high hydrocarbon desorption start temperatures, leading to inefficient hydrocarbon purification, especially during cold start periods, and are costly due to the need for noble metal catalysts.

Method used

A hydrocarbon adsorbent comprising an alkali metal and a zeolite with a ring structure, where the alkali metal is ion-exchangeable and present in specific concentrations, and the zeolite has a high silica to alumina ratio, enhancing heat resistance and desorption start temperature.

Benefits of technology

The proposed adsorbent achieves higher hydrocarbon desorption start temperatures and improved heat resistance, ensuring effective hydrocarbon purification across varying temperature conditions without the need for noble metals, thus enhancing the efficiency and cost-effectiveness of hydrocarbon purification.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

An object is to provide a hydrocarbon adsorbent having a high hydrocarbon desorption start temperature or to provide a method for adsorbing hydrocarbons that uses the hydrocarbon adsorbent. A hydrocarbon adsorbent comprising an alkali metal and a zeolite having a ring structure that includes at least 10 members is used. In the hydrocarbon adsorbent, a content of the alkali metal is 1 to 40 mass% based on a total mass of the hydrocarbon adsorbent, a content of the zeolite having a ring structure that includes at least 10 members is 99 to 60 mass% based on the total mass of the hydrocarbon adsorbent, and at least a portion of the alkali metal is in a state of being ion-exchangeable.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a hydrocarbonadsorbent and a method for adsorbing hydrocarbons.Background Art

[0002] Exhaust gases emitted from internal combustion enginesused in vehicles, such as automobiles and watercrafts,contain large quantities of hydrocarbons. The hydrocarbonsemitted from internal combustion engines are purified with athree-way catalyst. A temperature environment necessary forthe three-way catalyst to function is 200°C or higher.Accordingly, when a temperature is in a range in which thethree-way catalyst does not function, for example, duringthe so-called cold start period, hydrocarbons are adsorbedonto a hydrocarbon adsorbent, and the hydrocarbons arereleased from the adsorbent when the temperature reaches therange in which the three-way catalyst begins to function.The hydrocarbons are then decomposed and purified by thethree-way catalyst. Hydrocarbon adsorbents typically use azeolite-containing composition, and there is a need for thecomposition to have a high hydrocarbon desorption starttemperature. This is because higher hydrocarbon desorptionstart temperatures enable hydrocarbons to be released in astate in which the three-way catalyst has higher activity,which is advantageous for the purification of hydrocarbons.

[0003] Patent Literature 1 proposes a zeolite-containingcomposition that serves as a composition having a highhydrocarbon desorption start temperature; the zeolitecontains at least one kind of ion of an element having anelectronegativity of 1.40 or more.

[0004] Patent Literature 2 proposes a hydrocarbon adsorbentformed of an alkali-metal-containing zeolite.Citation ListPatent Literature

[0005] PTL 1: Japanese Unexamined Patent ApplicationPublication No. 11-005020PTL 2: Japanese Unexamined Patent ApplicationPublication No. 2001-293368Summary of InventionTechnical Problem

[0006] In Patent Literature 1, a composition having a highdesorption start temperature is provided; however, a noblemetal needs to be used as a catalyst material, andconsidering that hydrocarbon adsorbents located upstream ofa three-way catalyst are exposed to a higher temperature,heat resistance necessary for a hydrocarbon adsorbent to bepractically used to purify hydrocarbons emitted frominternal combustion engines is not achieved; in addition,there is a disadvantage in terms of cost. The hydrocarbonadsorbent of Patent Literature 2 presents a problem in thatthe hydrocarbon adsorbent does not have a sufficiently highhydrocarbon desorption start temperature. An object of thepresent disclosure is to provide a hydrocarbon adsorbenthaving a high hydrocarbon desorption start temperature or toprovide a method for adsorbing hydrocarbons that uses thehydrocarbon adsorbent.Solution to Problem

[0007] The present inventors studied adsorption properties ofzeolite-containing compositions. As a result, it wasdiscovered that specific hydrocarbon adsorbents have a highhydrocarbon desorption start temperature.

[0008] Specifically, the present invention is as described inthe claims, and a summary of the present disclosure is asfollows.[1] A hydrocarbon adsorbent comprising an alkali metaland a zeolite having a ring structure that includes at least10 members, characterized in that a content of the alkalimetal is 1 to 40 mass% based on a total mass of thehydrocarbon adsorbent, a content of the zeolite having aring structure that includes at least 10 members is 99 to 60mass% based on the total mass of the hydrocarbon adsorbent,and at least a portion of the alkali metal is in a state ofbeing ion-exchangeable.[2] The hydrocarbon adsorbent according to [1], wherein a content of the alkali metal that is in a state of being ion-exchangeable is 1 mass% or more and 40 mass% or less based on the total mass of the hydrocarbon adsorbent. [3] The hydrocarbon adsorbent according to [1] or [2], wherein the content of the alkali metal that is in a state of being ion-exchangeable is 4 mass% or more and 40 mass% or less based on the total mass of the hydrocarbon adsorbent. [4] The hydrocarbon adsorbent according to any one of [1] to [3], wherein the alkali metal is at least one selected from the group consisting of sodium, potassium, rubidium and cesium. [5] The hydrocarbon adsorbent according to [4], wherein the alkali metal is rubidium and / or cesium. [6] The hydrocarbon adsorbent according to any one of [1] to [5], wherein the zeolite having a ring structure thatincludes at least 10 members has a molar ratio of silica toalumina (SiO2 / Al2O3 ratio) of 5 or more and 35 or less.[7] The hydrocarbon adsorbent according to [6], wherein the zeolite having a ring structure that includes at least 10 members has a molar ratio of silica to alumina (SiO2 / Al2O3 ratio) of 5 or more and 20 or less. [8] The hydrocarbon adsorbent according to any one of [1] to [7], wherein the zeolite having a ring structure thatincludes at least 10 members is a zeolite having at leastone structure selected from a group of a BEA structure, anMFI structure, an MOR structure and an FAU structure.[9] A method for adsorbing a hydrocarbon, the method comprising using the hydrocarbon adsorbent according to any one of [1] to [8].Advantageous Effects of Invention

[0009] With the present disclosure, at least one of thefollowing objects is achieved: to provide a hydrocarbonadsorbent having a high hydrocarbon desorption starttemperature and to provide a method for adsorbinghydrocarbons that uses the hydrocarbon adsorbent.Brief Description of Drawings

[0010] [Fig. 1] A graph illustrates a relationship between ahydrocarbon desorption start temperature and a SiO2 / Al2O3ratio, regarding Examples and a Comparative Example.Description of Embodiments

[0011] A hydrocarbon adsorbent of the present disclosure willbe described below with reference to an exemplaryembodiment. Note that in the present disclosure, when "to"is used to indicate a range, the number preceding "to" andthe number following "to" are included in the range. Forexample, "1 to 40%" is synonymous with "1% or more and 40%or less". Furthermore, in the present disclosure, "A and / orB" is synonymous with "at least one of A and B". Forexample, "rubidium and / or cesium" is synonymous with "atleast one of rubidium and cesium".

[0012] The hydrocarbon adsorbent of the present disclosure isone in which a content of an alkali metal is 1 to 40 mass%based on the total mass of the hydrocarbon adsorbent (takenas 100 mass%), and a content of a zeolite having a ringstructure that includes at least 10 members (hereinafteralso referred to as a "large-pore zeolite") is 99 to 60mass% based on the total mass of the hydrocarbon adsorbent(hereinafter, the content of an alkali metal based on thetotal mass of the hydrocarbon adsorbent is also referred toas an "alkali metal content", and the content of a largeporezeolite based on the total mass of the hydrocarbonadsorbent is also referred to as a "zeolite content"). Thatis, the hydrocarbon adsorbent of the present disclosure isone in which an alkali metal is present in an amount of 1 to40 mass% based on the total mass of the hydrocarbonadsorbent, and a large-pore zeolite is present in an amountof 99 to 60 mass% based on the total mass of the hydrocarbonadsorbent. The hydrocarbon adsorbent is preferably one inwhich an alkali metal is present in an amount of 5 to 40mass% based on the total mass of the hydrocarbon adsorbent,and a large-pore zeolite is present in an amount of 95 to 60mass% based on the total mass of the hydrocarbon adsorbent(the alkali metal content is 5 to 40 mass%, and the zeolitecontent is 95 to 60 mass%) and is more preferably one inwhich an alkali metal is present in an amount of 10 to 40mass% based on the total mass of the hydrocarbon adsorbent,and a large-pore zeolite is present in an amount of 90 to 60mass% based on the total mass of the hydrocarbon adsorbent(the alkali metal content is 10 to 40 mass%, and the zeolitecontent is 90 to 60 mass%). Furthermore, the hydrocarbonadsorbent of the present disclosure is one in which at leasta portion of the alkali metal is in a state of being ionexchangeable.

[0013] Note that the alkali metal mentioned above is an alkalimetal element, and the state of the element is notparticularly limited; preferably, the alkali metal is in anionic state.

[0014] Because of the configuration requirements, thehydrocarbon adsorbent of the present disclosure has heatresistance sufficient for use and has a high hydrocarbondesorption start temperature.

[0015] Preferably, the zeolite (large-pore zeolite) that isincluded in the hydrocarbon adsorbent of the presentdisclosure is a crystalline aluminosilicate. Thecrystalline aluminosilicate is a zeolite having a crystalstructure formed of repeating networks containing aluminum(Al) and silicon (Si) with interposed oxygen (O).

[0016] In the present disclosure, the zeolite is a compoundhaving a regular structure in which framework atoms(hereinafter also referred to as "T atoms") are disposedwith interposed oxygen (O), and the T atoms are at least oneof the following: metal atoms, metalloid atoms and atomsother than the foregoing atoms. Examples of the metal atomsinclude atoms of at least one selected from a group of iron(Fe), aluminum (Al), gallium (Ga), tin (Sn) and titanium(Ti), boron (B) atoms and atoms of a different transitionmetal element. Examples of the metalloid atoms includeatoms of at least one selected from a group of boron (B),silicon (Si), germanium (Ge), arsenic (As), antimony (Sb)and tellurium (Te). Examples of the atoms other than theforegoing atoms include phosphorus (P) atoms. The zeoliteof the present disclosure encompasses not onlyaluminosilicates but also metallosilicates, such asferrosilicates and gallosilicates, and zeolite analogues,such as silicoaluminophosphates (SAPO) and aluminophosphates(AlPO).

[0017] The "framework structure" (which is used hereininterchangeably with "crystal structure" and may hereinafteralso be referred to as a "zeolite structure") of the zeoliteis a framework structure determined according to thestructure code specified by the Structure Commission of theInternational Zeolite Association (hereinafter also referredto simply as a "structure code"). The framework structurecan be identified by comparing an XRD pattern of a zeoliteof interest against XRD patterns of zeolite structures shownin Collection of Simulated XRD Powder Patterns for Zeolites,Fifth Revised Edition (2007) (hereinafter also referred toas "reference patterns").

[0018] In the present disclosure, the XRD pattern may be anXRD pattern obtained from an XRD measurement performed underthe following conditions.

[0019] Acceleration current and voltage: 40 mA and 40 kVRadiation source: CuKα radiation (λ=1.5405 Å)Measurement mode: continuous scanningScanning condition: 40° / minuteMeasurement range: 2θ=3° to 43°Vertical divergence limiting slit: 10 mmDivergence / entrance slit: 1°Receiving slit: openReceiving solar slit: 5°Detector: semiconductor detector (D / teX Ultra)Ni filter usedIn the present disclosure, the "ring structure" is aring-shaped framework structure formed of T atoms and oxygenatoms, and the "ring structure that includes at least 10members" is a framework structure formed of at least 10 Tatoms and oxygen atoms. Examples of the ring structureinclude ring structures including 10 members, 12 members, 14members or 18 members.

[0020] In the present disclosure, examples of the large-porezeolite include zeolites having a BEA structure, an MFIstructure, an FAU structure, an FER structure, an MORstructure or the like. From the standpoint of achieving ahigh hydrocarbon desorption start temperature, it ispreferable that the large-pore zeolite be a zeolite having aBEA structure, an MFI structure, an FAU structure or an MORstructure. More preferably, the large-pore zeolite is azeolite having a BEA structure or an MFI structure, and evenmore preferably, a zeolite having an MFI structure. In thepresent disclosure, a zeolite having a specific zeolitestructure is also referred to as a "…-type zeolite". Forexample, a zeolite having a BEA structure, preferably azeolite having only a BEA structure, is also referred to asa "BEA-type zeolite".

[0021] The hydrocarbon adsorbent of the present disclosureincludes an alkali metal. The alkali metal (the type of thealkali metal) of the present disclosure is not particularlylimited and may be, for example, at least one selected froma group of sodium, potassium, rubidium and cesium.Preferably, the alkali metal is rubidium and / or cesium, andmore preferably, cesium. Note that the alkali metal may bein the form of two or more coexisting alkali metals.

[0022] The alkali metal that is included in the hydrocarbonadsorbent of the present disclosure is not particularlylimited and may be an alkali metal included in the largeporezeolite that is included in the hydrocarbon adsorbent.Examples of the alkali metal include an alkali metal alreadypresent in a zeolite derived from a hydrothermal synthesis,which is described later, (resulting from a crystallizationstep) (i.e., an alkali metal incorporated into the zeoliteas a result of crystallization) and an alkali metalincorporated into the zeolite by a post-treatment (e.g., analkali metal incorporated into the zeolite by performing animpregnation treatment on the zeolite with the alkali metalor an alkali metal incorporated into the zeolite by firstperforming ion exchange thereon with hydrogen ions orammonium ions and thereafter performing an impregnationtreatment thereon with the alkali metal.

[0023] The hydrocarbon adsorbent of the present disclosureincludes at least an alkali metal that is supported on thezeolite as a result of a post treatment and is in a state inwhich the alkali metal is not removed by ion exchange. Theinclusion of such an alkali metal is believed to be one ofthe reasons that the hydrocarbon adsorbent of the presentdisclosure is likely to exhibit a higher desorption starttemperature. In this instance, it is sufficient that thepost-treatment and the ion exchange be known methods thatare used to introduce an alkali metal into a zeolite.

[0024] In the hydrocarbon adsorbent of the present disclosure,the alkali metal is one in which at least a portion thereofis in a state of being ion-exchangeable. This enables thehydrocarbon adsorbent to exhibit a higher hydrocarbondesorption start temperature. In the present disclosure,"an alkali metal is in a state of being ion-exchangeable"means that a portion or the whole of the alkali metalpresent in the zeolite is in a state of being ionexchangeablewith a different alkali metal (i.e., adifferent type of alkali metal). The hydrocarbon adsorbent,which has an alkali metal having such a state, can beproduced, for example, by using the production methoddescribed later.

[0025] Whether the alkali metal is in a state of being ionexchangeablecan be determined as follows. The hydrocarbonadsorbent of the present disclosure is subjected to ionexchange with an alkali metal of a type not included in thehydrocarbon adsorbent, to examine whether the alkali metaloriginally included in the hydrocarbon adsorbent is lost asa result of the ion exchange (whether the alkali metal ision-exchanged). For example, in instances where 50% of atotal amount of the originally included alkali metal is lost(exchanged) as a result of the ion exchange, it is indicatedthat 50% of the alkali metal, in the total amount of thealkali metal, is in a state of being ion-exchangeable.Furthermore, in instances where the total amount of theoriginally included alkali metal is lost (exchanged) as aresult of the ion exchange, it is indicated that 100% of thealkali metal, in the total amount of the alkali metal, ision-exchangeable.

[0026] In the total amount (taken as 100 mol%) of the alkalimetal included in the hydrocarbon adsorbent of the presentdisclosure, a proportion of the alkali metal that is ionexchangeablewith a different type of alkali metal, that is,a proportion of the alkali metal that is in a state of beingion-exchangeable in the hydrocarbon adsorbent of the presentdisclosure, may be within a range of 30 to 100 mol%. Thisis preferable from the standpoint of achieving a highhydrocarbon desorption start temperature. More preferably,the proportion may be within a range of 50 to 95 mol%. Thatis, in the hydrocarbon adsorbent of the present disclosure,it is preferable that 30 to 100 mol% of the total amount ofthe alkali metal be in a state of being ion-exchangeable,and it is more preferable that 50 to 95 mol% of the totalamount of the alkali metal be in a state of being ionexchangeable.

[0027] The alkali metal that is included in the hydrocarbonadsorbent of the present disclosure may be, for example, atleast one selected from a group of sodium, potassium,rubidium and cesium. Preferably, the alkali metal isrubidium and / or cesium.

[0028] In this instance, it is preferable that the rubidiumand / or cesium included in the hydrocarbon adsorbent of thepresent disclosure be ion-exchangeable with sodium and / orpotassium. In the total amount (100 mol%) of the rubidiumand / or cesium, it is preferable that 30 to 100 mol% thereofbe in a state of being ion-exchangeable, and it is morepreferable that 50 to 95 mol% thereof be in a state of beingion-exchangeable.

[0029] In another embodiment, it is preferable that the alkalimetal that is included in the hydrocarbon adsorbent of thepresent disclosure be sodium and / or potassium.

[0030] In this instance, it is preferable that the sodiumand / or potassium included in the hydrocarbon adsorbent ofthe present disclosure be ion-exchangeable with rubidiumand / or cesium. In the total amount (100 mol%) of the sodiumand / or potassium, it is preferable that 30 to 100 mol%thereof be in a state of being ion-exchangeable, and it ismore preferable that 50 to 95 mol% thereof be in a state ofbeing ion-exchangeable.

[0031] In the present disclosure, the amount of the alkalimetal can be measured by inductively coupled plasma emissionspectroscopy (ICP-AES), and the amount of the alkali metalthat is in a state of being ion-exchangeable can bequantitatively determined with the method described in theExamples section.

[0032] Furthermore, the amount of the alkali metal that is ina state of being ion-exchangeable in the hydrocarbonadsorbent formed of the alkali-metal-containing large-porezeolite can be quantitatively determined with the followingmethod. Specifically, an aqueous solution is passed throughthe hydrocarbon adsorbent formed of a large-pore zeolitecontaining an alkali metal (e.g., cesium (Cs)). The aqueoussolution contains a different type of alkali metal (e.g.,sodium (Na)), other than the first-mentioned alkali metal.The aqueous solution may be used in an amount such that alarge excess of the alkali metal (Na) is present relative tothe amount of the aluminum in the large-pore zeoliteincluded in the hydrocarbon adsorbent (e.g., in an amountsuch that Na is present in an amount of 5 molar equivalentsrelative to the amount of the aluminum of the large-porezeolite). After the passing of the solution, a sufficientamount (e.g., an amount that is 8 to 12 times the mass ofthe hydrocarbon adsorbent) of warm water (50 to 70°C) ispassed through the hydrocarbon adsorbent to wash thehydrocarbon adsorbent. After the washing, the hydrocarbonadsorbent is dried in air at 110°C. Accordingly, theoriginally included alkali metal (Cs) is replaced with adifferent type of alkali metal (Na).

[0033] By determining the molar ratios of the alkali metal(Cs) to the aluminum in the hydrocarbon adsorbent before thepassing of the solution and after the drying, the proportion(molar proportion) of the alkali metal that is in a state ofbeing ion-exchangeable can be determined, according to thefollowing equation.

[0034] R = [{Me / Al (before) - Me / Al (after)} / Me / Al (before)] x 100In the equation, R is a proportion (mol%) of the ionexchangeablealkali metal, Me / Al (before) is a molar ratioof the alkali metal to the aluminum in the hydrocarbonadsorbent before the passing of the solution and Me / Al(after) is a molar ratio of the alkali metal to the aluminumin the hydrocarbon adsorbent after the drying, where thealkali metal (Me) in Me / Al (before) and the alkali metal(Me) in Me / Al (after) are both the same type of alkali metalas the alkali metal present in the hydrocarbon adsorbentbefore the passing of the solution.

[0035] A content of the ion-exchangeable alkali metal in thehydrocarbon adsorbent of the present disclosure ispreferably 0.01 mass% or more and 40 mass% or less, morepreferably 1 mass% or more and 40 mass% or less and evenmore preferably 4 mass% or more and 40 mass% or less, basedon the total mass of the hydrocarbon adsorbent.

[0036] The content (mass%) of the alkali metal that is in astate of being ion-exchangeable can be determined bymultiplying the alkali metal content (mass%) of the largeporezeolite that is included in the hydrocarbon adsorbentof the present disclosure, by the proportion (%) of thealkali metal that is in a state of being ion-exchangeable inthe alkali metal present therein.

[0037] The large-pore zeolite that is included in thehydrocarbon adsorbent of the present disclosure has a molarratio of silica to alumina (hereinafter also referred to asa "SiO2 / Al2O3 ratio"), which is not particularly limited andmay be specified to be 5 or more and 40 or less or 5 or moreand 35 or less, from the standpoint of achieving a highhydrocarbon desorption start temperature. The molar ratiois more preferably 5 or more and 30 or less, even morepreferably 5 or more and 20 or less, still more preferably 5or more and 18 or less, still further more preferably 5 ormore and 15 or less and particularly preferably 5 or moreand 10 or less.

[0038] The large-pore zeolite may have a BET specific surfacearea of 200 m2 / g or more and 800 m2 / g or less, which ispreferable from the standpoint of achieving a highhydrocarbon desorption start temperature. The BET specificsurface area is more preferably 300 m2 / g or more and 700 m2 / gor less.

[0039] The hydrocarbon adsorbent of the present disclosure mayinclude, if necessary, one or more components other thanthose described above. Examples of the components otherthan those described above include, but are not limited to,binders.

[0040] In the present disclosure, examples of preferredhydrocarbon adsorbents include a hydrocarbon adsorbentincluding an alkali metal and a zeolite, in which the alkalimetal is one of sodium, potassium, rubidium or cesium; thezeolite is at least one selected from a group of BEA-typezeolites, FAU-type zeolites, MOR-type zeolites and MFI-typezeolites and having a SiO2 / Al2O3 ratio of 5 or more and 40 orless; a content of the alkali metal is 1 mass% or more andadsorbent, and a content of the zeolite is 70 mass% or moreand 99 mass% or less based on the total mass of thehydrocarbon adsorbent; and 20 mass% or more and 98 mass% orless of the alkali metal is in a state of being ionexchangeable.

[0041] Examples of hydrocarbon adsorbents that exhibit ahigher desorption start temperature include a hydrocarbonadsorbent including cesium and a zeolite, in which thezeolite is at least one selected from a group of BEA-typezeolites, FAU-type zeolites, MOR-type zeolites and MFI-typezeolites and has a SiO2 / Al2O3 ratio of 5 or more and 30 orless; a content of the cesium is 8 mass% or more and 30mass% or less based on the total mass of the hydrocarbonadsorbent, and a content of the zeolite is 70 mass% or moreand 92 mass% or less based on the total mass of thehydrocarbon adsorbent; and 40 mass% or more and 98 mass% orless of the alkali metal is in a state of being ionexchangeable.

[0042] Examples of hydrocarbon adsorbents that exhibit an evenhigher desorption start temperature include a hydrocarbonadsorbent including cesium and a zeolite, in which thezeolite is at least one selected from a group of BEA-typezeolites, FAU-type zeolites, MOR-type zeolites and MFI-typezeolites and has a SiO2 / Al2O3 ratio of 5 or more and 20 ormass% or less based on the total mass of the hydrocarbonadsorbent, and a content of the zeolite is 70 mass% or moreand 90 mass% or less based on the total mass of thehydrocarbon adsorbent; and 20 mass% or more and 96 mass% orless of the alkali metal is in a state of being ionexchangeable.

[0043] Examples of hydrocarbon adsorbents that exhibit aparticularly high desorption start temperature include ahydrocarbon adsorbent including cesium and a zeolite, inwhich the zeolite is at least one selected from a group ofFAU-type zeolites, MOR-type zeolites and MFI-type zeolitesand has a SiO2 / Al2O3 ratio of 5 or more and 17 or less; acontent of the cesium is 10 mass% or more and 30 mass% orless based on the total mass of the hydrocarbon adsorbent,and a content of the zeolite is 70 mass% or more and 90mass% or less based on the total mass of the hydrocarbonadsorbent; and 20 mass% or more and 95 mass% or less of thealkali metal is in a state of being ion-exchangeable.

[0044] Now, methods for producing the hydrocarbon adsorbent ofthe present disclosure will be described.

[0045] Methods for producing the hydrocarbon adsorbent of thepresent disclosure are not limited. Production methods thatcan be used to obtain the hydrocarbon adsorbent of theincluding an alkali metal incorporation step in which analkali metal is incorporated into a large-pore zeolite; anda production method including a crystallization step inwhich a composition containing a silica source, an aluminasource, an alkali source and water (hereinafter alsoreferred to as a "raw material composition") is subjected toa hydrothermal treatment to yield a crystallized product andincluding an alkali metal incorporation step in which analkali metal is incorporated into the crystallized product.These production methods also correspond to methods forproducing the large-pore zeolite that is included in thehydrocarbon adsorbent of the present disclosure. Note thatin the crystallization step, a structure directing agent(hereinafter also referred to as an "SDA") may beadditionally used, if necessary, that is, a raw materialcomposition containing an SDA may be subjected to ahydrothermal treatment. From the standpoint of simplifyingproduction operation, it is preferable not to use any SDA,whereas, from the standpoint of extending a productioncontrol limit, it is preferable to use an SDA.

[0046] The silica source is at least one of silica and aprecursor thereof. For example, the silica source may be atleast one from the group consisting of colloidal silica,amorphous silica, sodium silicate, tetraethyl orthosilicateand an aluminosilicate gel. In particular, the silicasource is preferably at least one of colloidal silica andamorphous silica or is colloidal silica or amorphous silica.

[0047] The alumina source is at least one of alumina and aprecursor thereof. For example, the alumina source may beat least one from the group consisting of aluminum nitrate,aluminum sulfate, sodium aluminate, aluminum hydroxide,aluminum chloride, an aluminosilicate gel and metalaluminum. In particular, the alumina source is preferablyat least one of aluminum hydroxide and aluminum sulfate oris aluminum hydroxide or aluminum sulfate.

[0048] The alkali source may be, for example, at least onefrom the group consisting of various salts, such ashydroxides, halides and carbonate salts of lithium, sodium,potassium, rubidium, cesium, francium, magnesium, calcium,strontium or ammonium. In particular, the alkali source ispreferably at least one hydroxide selected from a group ofhydroxides of sodium, hydroxides of potassium and hydroxidesof ammonium or is a hydroxide of sodium, potassium orammonium.

[0049] The raw material composition may include an SDA ifnecessary. The structure directing agent may be, forexample, at least one selected from the group consisting oftetraethylammonium hydroxide (hereinafter also referred toas "TEAOH"), tetraethylammonium bromide, tetrapropylammoniumhydroxide, tetrapropylammonium bromide and adimethyldipropylammonium salt (hereinafter also referred toas "Me2Pr2N+"). Examples of the dimethyldipropylammoniumsalt include, but are not limited to,dimethyldipropylammonium hydroxide, dimethyldipropylammoniumchloride and dimethyldipropylammonium bromide.

[0050] In the methods for producing the zeolite of the presentdisclosure, it is desirable that the raw materialcomposition include a seed crystal of a zeolite (hereinafteralso referred to simply as a "seed crystal"). The use of aseed crystal accelerates the crystallization of the zeolite,which shortens the time necessary for the production of thezeolite and, in addition, improves the yield.

[0051] It is desirable that the seed crystal be analuminosilicate having an LTL structure, an LTA structure,an MOR structure, an MFI structure, a BEA structure, an FAUstructure, a CHA structure or a YFI structure.

[0052] The SiO2 / Al2O3 molar ratio of the seed crystal isdesirably 2 to 100 and more desirably 3 to 60.

[0053] It is desirable that an amount of addition of the seedcrystal (i.e., a content of the seed crystal in the rawmaterial composition) be small. On the other hand, in termsof a reaction rate, an impurity-inhibiting effect and thelike, it is desirable that the content of the seed crystalbe 0.1 to 60 mass% relative to a mass of the silicacomponent included in the raw material composition. Moredesirably, the content of the seed crystal is 0.5 to 40mass%.

[0054] The content of the seed crystal (hereinafter alsoreferred to as the "seed crystal content") in the rawmaterial composition can be determined according to thefollowing equation, where the mass of the silicon (Si)included in the raw material composition is calculated asSiO2.

[0055] Seed crystal content (mass%) = (mass of SiO2 of seedcrystal) / (mass of SiO2 of raw material composition) x 100A preferred composition of the raw material compositionis the following composition (molar composition), forexample.

[0056] SiO2 / Al2O3 ratio = 3 or more and 40 or lessSDA / SiO2 ratio = 0 or more and 0.50 or lessMe / SiO2 ratio = 0 or more and 0.50 or lessH2O / SiO2 ratio = 3 or more and 100 or lessIn the above equations, Me represents an alkali metalelement.

[0057] The crystallization step can crystallize the rawmaterial composition with a hydrothermal treatment. Theconditions for the hydrothermal treatment are notparticularly limited as long as the conditions are thoseunder which a large-pore crystallized zeolite can beobtained. Examples of the conditions include the followingconditions.

[0058] Crystallization temperature: 80°C or higher and200°C or lowerCrystallization time: 1 hour to 10 daysCrystallization pressure: autogenous pressureThis crystallization step can produce a large-porezeolite. After the crystallization step, the resultinglarge-pore zeolite may be subjected to the steps ofcollection, washing, drying and calcination that areperformed with any method, and in addition, a dealuminationtreatment may be performed to achieve a desired SiO2 / Al2O3ratio.

[0059] From the standpoint of increasing the hydrocarbondesorption start temperature, it is preferable that, afterthe crystallization step, the resulting large-pore zeolitebe subjected to a calcination step.

[0060] The calcination step is a step for removing the SDAfrom the large-pore zeolite. The conditions for thecalcination are not limited, and examples of the conditionsfor the calcination include an oxidizing atmosphere, acalcination temperature of 400°C or higher and 800°C or lessand a calcination time of 0.5 hours or more and 12 hours orless.

[0061] The production methods of the present disclosureinclude an alkali metal incorporation step. The alkalimetal incorporation step is a step for contacting an alkalimetal with the large-pore zeolite, thereby incorporating thealkali metal into the zeolite. This enables theincorporation of the alkali metal while also enabling atleast a portion of the alkali metal to be placed in a stateof being ion-exchangeable. In the alkali metalincorporation step, the alkali metal is incorporated in amanner that intentionally creates a state in which thealkali metal is not coordinated at some of the ion exchangesites (alkali metal coordination sites) of the framework ofthe large-pore zeolite (zeolite structure). As a result,presumably, at least a portion of the alkali metal that isincluded in the resulting large-pore zeolite and thehydrocarbon adsorbent is placed in a state of being ionexchangeable,which, consequently, increases the hydrocarbondesorption start temperature.

[0062] The alkali metal to be incorporated is not particularlylimited and may be at least one selected from a group ofsodium, potassium, rubidium and cesium. The alkali metal ispreferably rubidium and / or cesium and more preferablycesium. Note that two or more alkali metals may beincorporated simultaneously, sequentially or intermittently.

[0063] In instances where sodium, potassium, rubidium orcesium is to be incorporated into the large-pore zeolite ofthe present disclosure, it is preferable to use a compoundof sodium, potassium, rubidium or cesium, and it is morepreferable to use an inorganic salt containing sodium,potassium, rubidium or cesium or use at least one from thegroup consisting of sulfate salts, nitrate salts, acetatesalts, hydroxides and chlorides that contain sodium,potassium, rubidium or cesium.

[0064] It is sufficient that the alkali metal incorporationstep be a method that incorporates an alkali metal into atleast one of the ion exchange sites and the pores, of thelarge-pore zeolite. Specifically, the method may be atleast one from the group consisting of ion exchange,evaporation to dryness and incipient wetness impregnation.Preferably, the method is incipient wetness impregnation,particularly, a method in which an aqueous solutioncontaining an alkali metal compound is mixed with thezeolite.

[0065] Note that in the alkali metal incorporation step, thealkali metal is incorporated in a manner that intentionallycreates a state in which the alkali metal is not coordinatedat some of the ion exchange sites (alkali metal coordinationsites) of the framework of the large-pore zeolite. That is,the alkali metal incorporation step is one that causes atleast a portion of the alkali metal that is included in thehydrocarbon adsorbent to be placed in a state of being ionexchangeable.Methods therefor are not particularlylimited, and examples of the methods include the methoddescribed in the Examples section of the present disclosure(a method in which the zeolite is used as a fixed bed, and asolution of an alkali metal is passed through the fixed bedto cause the alkali metal to be supported thereon). Aspecific method for the alkali metal incorporation step maybe a method in which a zeolite bed obtained by filtering azeolite-containing slurry is used as a fixed bed, and analkali metal solution is passed through the fixed bed fromabove sequentially or intermittently. A water content ofthe zeolite bed may be, for example, 35 mass% or more and 75mass% or less, 40 mass% or more and 75 mass% or less, 40mass% or more and 70 mass% or less or 50 mass% or more and70 mass% or less. A density of the zeolite bed may be 0.25g / cm3 or more and 0.9 g / cm3 or less or 0.3 g / cm3 or more and0.7 g / cm3 or less.

[0066] Note that the production methods of the presentdisclosure may include at least one of a washing step, adrying step or an activation step, which is performed afterthe alkali metal incorporation step.

[0067] The washing step after the alkali metal incorporationstep is a step for removing impurities and the like from thezeolite, and the washing may be performed with any washingmethod. For example, the large-pore zeolite may be washedwith a sufficient amount of purified water.

[0068] The drying step after the alkali metal incorporationstep is a step for removing water from the zeolite, and theprocess (drying) may be performed, for example, in air at atemperature of 100°C or higher and 200°C or lower orpreferably a temperature of 110°C or higher and 190°C orlower. The process time is not limited and may be, forexample, 1 hour or more and 2 hours or less.

[0069] The activation step after the alkali metalincorporation step is a step for removing organic matterfrom the zeolite, and the process (activation) may beperformed, for example, in air at a temperature of higherthan 200°C and 600°C or lower or preferably in air at atemperature of higher than 300°C and 600°C or lower. Theprocess time is not limited and may be, for example, 1 houror more and 2 hours or less.

[0070] The hydrocarbon adsorbent of the present disclosure isa hydrocarbon adsorbent including a large-pore zeoliteobtained as described above and may be a hydrocarbonadsorbent formed of the large-pore zeolite containing analkali metal.

[0071] The hydrocarbon adsorbent of the present disclosure mayhave any shape depending on the intended use. Preferably,the hydrocarbon adsorbent may be at least one of a powderand a molded body. A specific shape of the molded body mayshapes, generally spherical shapes, elliptical shapes, discshapes, cylindrical shapes, polyhedral shapes, irregularshapes and petaloid shapes.

[0072] In instances where the hydrocarbon adsorbent isemployed as a powder, the hydrocarbon adsorbent may be mixedwith a solvent, such as water or alcohol, to form a slurry,and the slurry may be coated onto a substrate to form anadsorbent member.

[0073] In instances where the hydrocarbon adsorbent of thepresent disclosure is used as a molded body, the hydrocarbonadsorbent may be mixed with a binder, if necessary, and maybe molded with any method. Preferably, the binding agentmay be, for example, at least one from the group consistingof silica, alumina, kaolin, attapulgite, montmorillonite,bentonite, allophane and sepiolite. A method for themolding may be, for example, at least one from the groupconsisting of tumbling granulation, press molding, extrusionmolding, injection molding, slip casting and sheet molding.

[0074] The hydrocarbon adsorbent of the present disclosure ispreferably a hydrocarbon adsorbent for adsorbinghydrocarbons at 160°C or less and more preferably ahydrocarbon adsorbent for adsorbing hydrocarbons at 160°C orless and desorbing the adsorbed hydrocarbons at higher than160°C. Further, more preferably, the hydrocarbon adsorbentis a hydrocarbon adsorbent for adsorbing hydrocarbons at170°C or lower and desorbing the adsorbed hydrocarbons athigher than 170°C or is a hydrocarbon adsorbent foradsorbing hydrocarbons at 180°C or lower and desorbing theadsorbed hydrocarbons at higher than 180°C. The hydrocarbonadsorbent of the present disclosure can be used in a methodfor adsorbing hydrocarbons.

[0075] The hydrocarbon adsorbent of the present disclosure canadsorb hydrocarbons with a method including a step ofcontacting a hydrocarbon-containing fluid with thehydrocarbon adsorbent of the present disclosure.

[0076] The hydrocarbon-containing fluid may be, for example, ahydrocarbon-containing gas or a hydrocarbon-containingliquid.

[0077] The hydrocarbon-containing gas is a gas containing atleast one hydrocarbon and preferably a gas containing two ormore hydrocarbons. The hydrocarbon present in thehydrocarbon-containing gas may be at least one from thegroup consisting of paraffins, olefins and aromatichydrocarbons. It is sufficient that the number of carbonatoms of the hydrocarbon be 1 or more. Preferably, thenumber of carbon atoms is 1 or more and 15 or less.Preferably, the hydrocarbon present in the hydrocarboncontaininggas is at least two from the group consisting ofmethane, ethane, ethylene, propylene, butane, linearparaffins having 5 or more carbon atoms, linear olefinshaving 5 or more carbon atoms, benzene, toluene and xylene.The hydrocarbon is preferably at least two from the groupconsisting of methane, ethane, ethylene, propylene, butane,benzene, toluene and xylene and more preferably at least onefrom the group consisting of methane, ethane, ethylene andpropylene and at least one from the group consisting ofbenzene, toluene and xylene. The hydrocarbon-containing gasmay contain at least one from the group consisting of carbonmonoxide, carbon dioxide, hydrogen, oxygen, nitrogen,nitrogen oxides, sulfur oxides and water. Specific examplesof the hydrocarbon-containing gas include combustion gases,such as exhaust gases from internal combustion engines.

[0078] Preferably, a contact temperature for the step is roomtemperature to 200°C.EXAMPLES

[0079] The hydrocarbon adsorbent of the present disclosurewill be described in more detail below with reference toexamples. The present disclosure is not limited to theexamples.

[0080] (Determination of Crystal Structure)An XRD measurement was performed on a sample with atypical X-ray diffractometer (instrument name: Ultima IVProtectus, manufactured by Rigaku Corporation). Theradiation source used was CuKα radiation (λ=1.5405 Å), andthe measurement was performed over a 2θ measurement range of3° to 43°. The obtained XRD pattern was compared against areference pattern to determine the crystal structure.Specific measurement conditions are shown below.

[0081] Acceleration current and voltage: 40 mA and 40 kVRadiation source: CuKα radiation (λ=1.5405 Å)Measurement mode: continuous scanning (2θ / θscanning)Scanning condition: 40° / minuteMeasurement range: 2θ=3° to 43°Vertical divergence limiting slit: 10 mmDivergence / entrance slit: 1°Receiving slit: openReceiving solar slit: 5°Detector: D / teX UltraNi filter used(Composition Analysis)A sample solution for a measurement was prepared bydissolving the sample into a mixed aqueous solution ofhydrofluoric acid and nitric acid, and the sample solutionwas measured by inductively coupled plasma emissionspectroscopy (ICP-AES) with a typical ICP instrument(instrument name: Optima 5300 DV, manufactured byPerkinElmer, Inc.). From the obtained measured values of Si,Al and the alkali metal (e.g., Cs and Na), the compositionwas determined regarding the SiO2 / Al2O3 ratio of the sample,the content (mass%) of the alkali metal and the like.

[0082] More specifically, the preparation of the samplesolution for the measurement was performed as follows.Specifically, an aqueous mixed acid solution was obtained bymixing together 48% hydrofluoric acid, 60% nitric acid andwater in a volume ratio of 1:1:50. Approximately 0.01 g ofthe sample was dissolved into 10 mL of the obtained aqueousmixed acid solution in a manner such that a concentration ofeach of the measurement target elements falls within acalibration curve concentration range. In this manner, themeasurement solution was prepared. The calibration curveconcentration and the measurement wavelength of each of themeasurement target elements are shown in Table 1.

[0083] [Table 1]

[0084] Example 1(Synthesis of Large-Pore Zeolite (BEA-type zeolite))A 35 mass% aqueous solution of TEAOH, a 48 mass%aqueous solution of potassium hydroxide, purified water andan amorphous aluminosilicate (SiO2 / Al2O3 ratio=18.2) weremixed together, and subsequently, 1.5 mass% of a zeolite β(product name: HSZ-930NHA, manufactured by TosohCorporation), which was used as a seed crystal, was added tothe mixture to produce a raw material composition having thefollowing molar composition.

[0085] SiO2 / Al2O3 ratio = 18.2TEAOH / SiO2 ratio = 0.12K / SiO2 ratio = 0.12H2O / SiO2 ratio = 12.0Seed crystal = 1.5 mass%The raw material composition was loaded into a sealedcontainer, and the container was rotated at 55 rpm to allowthe raw material composition to undergo a reaction at 150°Cfor 48 hours to yield a crystallized product. The resultingcrystallized product was subjected to solid-liquidseparation and washing with purified water. Subsequently,the resultant was dried in air at 110°C for 24 hours andthen collected. The resulting crystallized product wascalcined in air at 600°C for 2 hours to form a calcinedproduct. The calcined product was mixed with a 20% aqueoussolution of ammonium chloride, which was used in an amountsuch that a large excess of NH4, namely, in an amount of 30molar equivalents relative to the amount of Al of thecalcined product, was present. The mixed aqueous solutionwas subjected to a stirring and mixing process in which anoperation of stirring the mixed aqueous solution at 80°C for24 hours and subsequently filtering the mixed solution wasperformed twice. Subsequently, the resultant was dried inair at 110°C overnight. In this manner, a large-porezeolite (BEA-type zeolite) in which SiO2 / Al2O3 was 18, andthe type of the cation was NH4 was obtained. Theconcentrations of Na and K in the obtained BEA-type zeolitewere less than or equal to the detection limits.

[0086] (Impregnation of Alkali Metal (Cs))A 2 mass% aqueous solution of cesium chloride wasprepared with cesium chloride (manufactured by Fujifilm WakoPure Chemical Corporation (special grade)). For theincorporation (impregnation) of the alkali metal, theaqueous solution of cesium chloride was used in an amountsuch that the alkali metal (Cs) was present in an amount of4 molar equivalents relative to the amount of Al of theobtained BEA zeolite (large-pore zeolite).

[0087] The obtained BEA-type zeolite was mixed with water, andsubsequently, the mixture was filtered for solid-liquidseparation to produce a cake of the obtained zeolite. Theaqueous solution of cesium chloride was passed through thecake, and subsequently, hot water (60°C) in a mass amount 10times that of the zeolite (cake) was passed through the caketo wash the cake. After the washing, the cake was dried at110°C in air for 24 hours to carry out the impregnation ofthe alkali metal (Cs). Accordingly, a Cs-containing BEAtypezeolite was obtained and designated as a hydrocarbonadsorbent of the present Example. ICP analysis wasperformed on the obtained hydrocarbon adsorbent to determinethe content (mass%) of the alkali metal (Cs, in the presentExample) and the Cs / Al molar ratio (before treatment) of thehydrocarbon adsorbent.

[0088] (Quantitative Determination of Amount of Alkali Metalin State of Being Ion-Exchangeable)The amount of the alkali metal that was in a state ofbeing ion-exchangeable was determined as follows.

[0089] The Cs-containing BEA-type zeolite (hydrocarbonadsorbent of the present Example) was additionallyimpregnated with Na. A 2 mass% aqueous solution of sodiumchloride was prepared with sodium chloride (manufactured byManac Incorporated). The aqueous solution of sodiumchloride was used for impregnation, that is, ion exchange ofCs with Na. The amount of use of the solution was such thatthe alkali metal (Na) was present in an amount of 5 molarequivalents relative to the amount of Al of the hydrocarbonadsorbent (zeolite) obtained by impregnation with Cs asdescribed above.

[0090] The obtained Cs-containing BEA-type zeolite was mixedwith water, and subsequently, the mixture was filteredthrough a funnel to produce a cake of the obtained zeolite.The aqueous solution of sodium chloride was passed throughthe cake, and subsequently, hot water (60°C) in a massamount 10 times that of the obtained zeolite was passedthrough the cake to carry out washing. After the washing,the cake was dried at 110°C in air, and, accordingly, a Naadditionallyimpregnated product was obtained. ICP analysiswas performed on the obtained additionally impregnatedproduct to determine a Cs / Al molar ratio (after treatment).The amount (%) of ion-exchangeable cesium, that is, cesiumthat was in a state of being ion-exchangeable, in the totalamount of cesium in the hydrocarbon adsorbent was calculatedaccording to the following equation.

[0091] [Chem. 1]

[0092] Furthermore, the content (mass%) of the alkali metalthat was in a state of being ion-exchangeable included inthe BEA-type zeolite, which was included in the hydrocarbonadsorbent of the present Example, was calculated bymultiplying the content (mass%) of the alkali metaldetermined as described above by the content (%) of thealkali metal that was in a state of being ion-exchangeable.The results are shown in Table 2.

[0093] Example 2A hydrocarbon adsorbent of the present Example wasobtained as in Example 1, except that an FAU-type zeoliteSiO2 / Al2O3=6) was used instead of a BEA-type zeolite. Thecontent (mass%) of the alkali metal (Cs, in the presentExample) and the amount of ion-exchangeable cesium werequantitatively determined.

[0094] Example 3A hydrocarbon adsorbent of the present Example wasobtained as in Example 1, except that an FAU-type zeolite(product name: HSZ-341NHA, manufactured by Tosoh Corporation,SiO2 / Al2O3=7) was used instead of a BEA-type zeolite. Thecontent (mass%) of the alkali metal (Cs, in the presentExample) and the amount of ion-exchangeable cesium werequantitatively determined.

[0095] Example 4A hydrocarbon adsorbent of the present Example wasobtained as in Example 1, except that an MOR-type zeolite(product name: HSZ-610HOA, manufactured by Tosoh Corporation,SiO2 / Al2O3=11) was used instead of a BEA-type zeolite. Thecontent (mass%) of the alkali metal (Cs, in the presentExample) and the amount of ion-exchangeable cesium werequantitatively determined.

[0096] Example 5A hydrocarbon adsorbent of the present Example wasobtained as in Example 1, except that an MFI-type zeolite(product name: HSZ-820NHA, manufactured by Tosoh Corporation,SiO2 / Al2O3=23) was used instead of a BEA-type zeolite. Thecontent (mass%) of the alkali metal (Cs, in the presentExample) and the amount of ion-exchangeable cesium werequantitatively determined.

[0097] Example 6A hydrocarbon adsorbent of the present Example wasobtained as in Example 1, except that a BEA-type zeolite(product name: HSZ-931HOA, manufactured by Tosoh Corporation,SiO2 / Al2O3=28) was used instead of the BEA-type zeolite usedin Example 1. The content (mass%) of the alkali metal (Cs,in the present Example) and the amount of ion-exchangeablecesium were quantitatively determined.

[0098] Example 7A hydrocarbon adsorbent of the present Example wasobtained as in Example 1, except that an MFI-type zeolite(product name: HSZ-830NHA, manufactured by Tosoh Corporation,SiO2 / Al2O3=28) was used instead of a BEA-type zeolite. Thecontent (mass%) of the alkali metal (Cs, in the presentExample) and the amount of ion-exchangeable cesium werequantitatively determined.

[0099] Example 8A hydrocarbon adsorbent of the present Example wasobtained with a method similar to that of Example 5, exceptthat the impregnation of an alkali metal was performed withthe following method. Specifically, a 5 mass% aqueoussolution of cesium chloride was used in an amount such thatCs was present in an amount of 2 molar equivalents relativeto the amount of Al of the zeolite. The aqueous solution ofcesium chloride and the zeolite were mixed together, and anoperation of stirring the mixed aqueous solution at 80°C for24 hours and subsequently filtering the mixed solution wasperformed twice. Water (60°C) in a mass amount 10 timesthat of the obtained zeolite was passed through the zeolite,and the resultant was washed. After the washing, theresultant was dried at 110°C in air to carry out theimpregnation of the alkali metal (Cs).

[0100] Example 9A hydrocarbon adsorbent of the present Example wasobtained as in Example 8, except that an MFI-type zeolite(product name: HSZ-840NHA, manufactured by TosohCorporation, SiO2 / Al2O3=39) was used instead of the MFI-typezeolite used in Example 8.

[0101] Example 10A hydrocarbon adsorbent of the present Example wasobtained as in Example 1, except that an MFI-type zeolite(product name: HSZ-840NHA, manufactured by TosohCorporation, SiO2 / Al2O3=39) was used instead of a BEA-typezeolite.

[0102] Example 11A hydrocarbon adsorbent of the present Example wasobtained as in Example 10, except that a 10 mass% aqueoussolution of sodium chloride (manufactured by Fujifilm WakoPure Chemical Corporation) was used instead of an aqueoussolution of cesium chloride, and the process of impregnationof an alkali metal (impregnation of Na) was performed withthe solution in an amount such that Na was present in anamount of 50 molar equivalents relative to the amount of Alof the zeolite.

[0103] Example 12A hydrocarbon adsorbent of the present Example wasobtained as in Example 10, except that a 2 mass% aqueoussolution of potassium chloride (manufactured by KantoChemical Co., Inc.) was used instead of an aqueous solutionof cesium chloride, and the process of impregnation of analkali metal (impregnation of K) was performed with thesolution in an amount such that K was present in an amountof 10 molar equivalents relative to the amount of Al of thezeolite.

[0104] Example 13A hydrocarbon adsorbent of the present Example wasobtained as in Example 10, except that a 2 mass% aqueoussolution of rubidium chloride (manufactured by KantoChemical Co., Inc.) was used instead of an aqueous solutionof cesium chloride, and the process of impregnation of analkali metal (impregnation of Rb) was performed with thesolution in an amount such that Rb was present in an amountof 2 molar equivalents relative to the amount of Al of thezeolite.

[0105] Comparative Example 1A hydrocarbon adsorbent of the present ComparativeExample was obtained as in Example 1, except that an MFItypezeolite (product name: HSZ-840NHA, manufactured byTosoh Corporation, SiO2 / Al2O3=39) was used instead of a BEAtypezeolite, and the impregnation of an alkali metal wasnot performed.

[0106] Measurement Example 1(Preparation and Pretreatment of Measurement Sample)The hydrocarbon desorption start temperature of thehydrocarbon adsorbents obtained in the Examples and theComparative Example was measured. Each of the hydrocarbonadsorbents of the Examples and the Comparative Example waspressure-molded and ground to form an irregular-shapedmolded body having an aggregate size of 20 to 30 mesh. Theresulting molded bodies were designated as respectivemeasurement samples of the Examples and the ComparativeExample. A pretreatment was performed as follows. 1 g ofeach of the measurement samples was loaded into a normalpressurefixed bed flow reactor and treated at 500°C for 1hour under a nitrogen flow, and subsequently, themeasurement sample was cooled to 50°C.

[0107] (Adsorption of Hydrocarbons)A hydrocarbon-containing gas was flowed through each ofthe hydrocarbon adsorbents treated by the pretreatment, andadsorbed hydrocarbons were measured over a range of 50°C to600°C, to determine an amount of adsorbed hydrocarbons. Acomposition of the hydrocarbon-containing gas and themeasurement conditions are shown below.

[0108] Hydrocarbon-containing gas:toluene 3000 volume ppmC (equivalent methaneconcentration)Water 3 vol%Nitrogen balanceGas flow rate: 200 mL / minuteMeasurement temperature: 50 to 600°CHeating rate: 10°C / minute(Measurement of Hydrocarbon Desorption StartTemperature)Hydrocarbons in the gas after the gas passed throughthe hydrocarbon adsorbent were quantitatively analyzedcontinuously with a flame ionization detector (FID). Thefollowing hydrocarbon concentrations were measured: ahydrocarbon concentration of the hydrocarbon-containing gason an inlet side of a normal-pressure fixed bed flow reactor(an equivalent methane concentration, hereinafter referredto as an "inlet concentration"); and a hydrocarbonconcentration of the hydrocarbon-containing gas on an outletside of the normal-pressure fixed bed flow reactor (anequivalent methane concentration, hereinafter referred to asan "outlet concentration").

[0109] An integral value of the inlet concentrations wasdesignated as an amount of hydrocarbons that passed throughthe hydrocarbon adsorbent. By determining a value resultingfrom the subtraction of an integral value of the outletconcentrations (equivalent methane concentrations) from theamount of hydrocarbons, the amount of adsorbed hydrocarbonsin each of the adsorbents was determined as an amount ofdesorbed hydrocarbons per mass of the hydrocarbon adsorbent(μmolC / g). In association with the increase in thetemperature of the measurement sample, the temperature atwhich the amount of desorbed hydrocarbons reached 0 μmolC / gin the shortest time was designated as the desorption starttemperature.

[0110] The hydrocarbon desorption start temperatures ofMeasurement Example 1 are shown in the table below.Furthermore, a relationship between the SiO2 / Al2O3 ratio andthe desorption start temperature is shown in Fig. 1.

[0111] [Table 2]

[0112] In Table 2, "Me" represents an alkali metal, "Totalcontent of Me" represents a total amount of the alkali metalincluded in the hydrocarbon adsorbent, "Proportion of ionexchangeableMe" represents a proportion of the alkali metalthat was in a state of being ion-exchangeable in the alkalimetal present in the zeolite and "Content of ionexchangeableMe" represents a content (mass%) of the alkalimetal that was included in the zeolite and was in a state ofbeing ion-exchangeable.

[0113] As shown in Table 2, the hydrocarbon adsorbents of theExamples had hydrocarbon desorption start temperatureshigher than that of the hydrocarbon adsorbent of ComparativeExample 1 and retained hydrocarbons until a highertemperature was reached. In each of the Examples, there wasa tendency for the hydrocarbon desorption start temperatureto increase as the content of the alkali metal that was in astate of being ion-exchangeable increased.

[0114] Furthermore, the hydrocarbon adsorbents of Examples 11to 13, which contained Na, K or Rb as the alkali metal, alsohad higher hydrocarbon desorption start temperatures thanthe hydrocarbon adsorbent of Comparative Example 1, as withthe hydrocarbon adsorbents of Examples 1 to 10.

[0115] Furthermore, referring to Fig. 1, the hydrocarbondesorption start temperature had a linear relationship withthe SiO2 / Al2O3 ratio, and there was a tendency for thehydrocarbon desorption start temperature to increase as theSiO2 / Al2O3 ratio decreased, independently of the structure ofthe zeolite.

[0116] The entire contents of the specification, claims,drawing and abstract of Japanese Patent Application No.2020-064909, filed on March 31, 2020, is incorporated hereinby reference as a disclosure of the specification of thepresent disclosure.

Claims

1. A hydrocarbon adsorbent comprising: an alkali metal; and a zeolite having a ring structure that includes at least 10 members, wherein a content of the alkali metal is 1 to 40 mass% based on a total mass of the hydrocarbon adsorbent, a content of the zeolite having a ring structure that includes at least 10 members is 99 to 60 mass% based on the total mass of the hydrocarbon adsorbent, and at least a portion of the alkali metal is in a state of being ion-exchangeable.

2. The hydrocarbon adsorbent according to Claim 1, wherein a content of the alkali metal that is in a state of being ion-exchangeable is 1 mass% or more and 40 mass% or less based on the total mass of the hydrocarbon adsorbent.

3. The hydrocarbon adsorbent according to Claim 2, wherein the content of the alkali metal that is in a state of being ion-exchangeable is 4 mass% or more and 40 mass% or less based on the total mass of the hydrocarbon adsorbent.

4. The hydrocarbon adsorbent according to any one of Claims 1 to 3, wherein the alkali metal is at least one selected from the group consisting of potassium, sodium, rubidium and cesium.

5. The hydrocarbon adsorbent according to Claim 4, wherein the alkali metal is rubidium and / or cesium.

6. The hydrocarbon adsorbent according to any one of Claims 1 to 5, wherein the zeolite has a molar ratio of silica to alumina (SiO2 / Al2O3 ratio) of 5 or more and 35 or less.

7. The hydrocarbon adsorbent according to Claim 6, wherein the zeolite has a molar ratio of silica to alumina (SiO2 / Al2O3 ratio) of 5 or more and 20 or less.

8. The hydrocarbon adsorbent according to any one of Claims 1 to 7, wherein the zeolite having a ring structure that includes at least 10 members is a zeolite having at least one structure selected from a group of a BEA structure, an MFI structure, an MOR structure and an FAU structure.

9. A method for adsorbing a hydrocarbon, the method comprising using the hydrocarbon adsorbent according to any one of Claims 1 to 8.