Concrete mix composition for 3D printing and method of formulating the same
Patent Information
- Application Number
- IN202421077431
- Authority / Receiving Office
- IN · IN
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2026-10-01
AI Technical Summary
Traditional concrete mixes are not suitable for 3D printing, leading to issues such as inconsistent flowability, inadequate setting times, weak bonding between layers, material waste, and limited design flexibility, which compromise the quality and durability of printed structures.
A specially formulated concrete mix composition for 3D printing, including a balanced mix of cementitious materials, aggregates, water, plasticizers, accelerators, retarders, and fibers, optimized for precise extrusion and controlled setting times to ensure consistent flow, strong bonding, and enhanced structural integrity.
The solution enables precise layering, reduced material waste, improved structural performance, and increased design flexibility, making 3D printed concrete more efficient, sustainable, and cost-effective for construction applications.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present disclosure relates to the field of concrete composition. Inparticular, the present disclosure pertains to concrete mix composition for 3Dprinting and method of formulating the concrete mix composition.BACKGROUND OF THE INVENTION
[0002] The construction industry has long relied on conventional methods ofpouring and molding concrete, which, while effective, come with significantdrawbacks. These traditional techniques are labor-intensive, requiring aconsiderable amount of manpower and time. Additionally, they often lead tosubstantial material waste, as the process of creating molds and pouring concreteis not optimized for material efficiency. This inefficiency not only increases costsbut also has a negative environmental impact due to the overuse of concretematerials.
[0003] The advent of 3D printing technology has sparked interest in itspotential applications within the construction sector, especially for buildingcomplex architectural structures and components. 3D printing offers the promiseof more precise, customizable, and efficient construction processes. However, thesuccessful application of 3D printing in construction hinges on the developmentof concrete compositions that are specifically designed for extrusion through 3Dprinters. Traditional concrete mixes, designed for pouring, often face issues whenadapted for 3D printing, such as inconsistent flowability, inappropriate settingtimes, and reduced structural integrity. These issues can compromise the qualityand durability of printed structures.Following are the problems associated with the traditional concrete mix:- Inconsistent Flowability: Traditional concrete mixes are not designed forthe extrusion process used in 3D printing, often resulting in inconsistentflow and clogging of the printing nozzle.- Inadequate Setting Time: Standard concrete may be set too quickly or tooslowly for 3D printing, leading to poor bonding between layers, whichcompromises the structural integrity of the final product.- Weak Bonding Between Layers: In 3D printed structures, weak interlayeradhesion can lead to cracks and reduced load-bearing capacity.- Material Waste: Conventional construction methods often result insignificant material waste due to overuse or improper application,impacting cost and environmental sustainability.- Limited Design Flexibility: Traditional concrete construction methodsrestrict the complexity and precision of designs, limiting architecturalcreativity.
[0004] To effectively leverage 3D printing technology in construction, thereis a critical need for specially formulated concrete mixes that can addressaforementioned challenges. These mixes must be engineered to ensure consistentflow through the printer nozzle, rapid and controlled setting times, and sufficientstrength to support subsequent layers and the overall structural load.SUMMARY
[0005] In view of the foregoing problems recited above, the present inventionprovides a unique concrete mix composition and method for producing 3D printedconcrete, designed to enhance structural integrity, durability, and ease ofapplication. This concrete mix is specifically formulated to be compatible with 3Dprinting technology, providing optimal flowability and setting time to allowprecise layering without compromising on strength. The composition includes abalanced mix of cementitious materials, aggregates, water, and additives, such asplasticizers, accelerators, and fibers, to improve mechanical properties andresistance to environmental factors.
[0006] The present invention further provides a method of formulatingcomposition involves precise proportioning, thorough mixing, and controlledextrusion through a 3D printer, enabling the creation of complex architecturalforms and structural components with minimal waste.
[0007] The present invention also includes specific guidelines for adjustingthe mix based on environmental conditions and desired properties, ensuringversatility in various construction scenarios. This 3D printed concrete compositionand method offer significant advancements in construction efficiency,sustainability, and design flexibility, making it suitable for both commercial andresidential applications.
[0008] This invention focuses on the composition, preparation, and 3Dprinting process of concrete specifically designed for construction.
[0009] Composition of 3D Printed Concrete: The invention relies on a preciseformulation of concrete suitable for 3D printing. The key components include:
[0010] Cementitious Materials: Portland cement serves as the binder, withoptional supplementary materials like fly ash and silica fume to improveworkability, durability, and environmental performance.
[0011] Aggregates: Fine sand is used to ensure smooth extrusion, with coarseraggregates avoided to prevent nozzle blockages.
[0012] Water: The water-to-cement ratio is carefully controlled for optimalworkability and strength
[0013] Additives and Admixtures:
[0014] Plasticizers: Improve flow ability without compromising strength.
[0015] Accelerators / Retarders: Control the setting time for better printingcontrol.
[0016] Fibers: Enhance tensile strength and bonding between layers.
[0017] Stabilizers: Prevent material separation during the printing process.
[0018] Method of Preparation:
[0019] The preparation method is critical for achieving a high-quality,consistent concrete mix suitable for 3D printing:
[0020] Proportioning: Ingredients are precisely measured to meet specificstructural or environmental needs.
[0021] Mixing: A high-shear mixer ensures uniformity and prevents materialsegregation.
[0022] Quality Control: The mix is tested for flowability, setting time, andstrength to ensure it meets the required standards before printing.
[0023] 3D Printing Process: Once the mix is ready, the printing processinvolves:
[0024] Extrusion: The mix is extruded layer by layer through a nozzle,following a pre-programmed design.
[0025] Layering: Layers are placed with precision, ensuring good bonding andstability between them.
[0026] Curing: After printing, the structure is cured using methods like air orwater curing to maintain moisture and promote strength development.
[0027] Advantages:
[0028] Precision and Customization: Allows for complex and highlycustomized designs, difficult to achieve with traditional methods.
[0029] Efficiency: Reduced waste and faster construction times due to theprecision of the process.
[0030] Enhanced Structural Performance: The inclusion of fibers and carefulcontrol over the mix ensures better tensile strength, ductility, and layer bonding.
[0031] Reduced Labor and Costs: Automation of the building process reduceslabor needs and overall construction costs.
[0032] Environmental Benefits: The use of supplementary cementitiousmaterials improves sustainability by reducing the carbon footprint associated withtraditional concrete production.
[0033] Various objects, features, aspects and advantages of the inventivesubject matter will become more apparent from the following detailed descriptionof preferred embodiments, along with the accompanying drawing figures in whichlike numerals represent like components.BRIEF DESCRIPTION OF THE DRAWING
[0034] The accompanying drawings are included to provide a furtherunderstanding of the present disclosure, and are incorporated in and constitute apart of this specification. The drawings illustrate exemplary embodiments of thepresent disclosure and, together with the description, serve to explain theprinciples of the present disclosure.
[0035] FIG. 1 illustrates a perspective view of a three-dimensional (3D)printing system, in accordance with embodiments of the present disclosure.
[0036] FIG. 2 illustrates a perspective view of 3D printed concrete structure,in accordance with embodiments of the present disclosure.
[0037] FIG. 3 illustrates a flow diagram representing a method forformulating a concrete mix suitable for 3D printing, in accordance withembodiments of the present disclosure.
[0038] FIG. 4 illustrates a flow diagram representing a method forconstructing a structure using 3D printing technology, in accordance withembodiments of the present disclosure.DETAILED DESCRIPTION
[0039] The following is a detailed description of embodiments of thedisclosure depicted in the accompanying drawings. The embodiments are in suchdetail as to clearly communicate the disclosure. However, the amount of detailoffered is not intended to limit the anticipated variations of embodiments; on thecontrary, the intention is to cover all modifications, equivalents, and alternativesfalling within the spirit and scope of the present disclosure as defined by theappended claims.
[0040] If the specification states a component or feature "may", "can","could", or "might" be included or have a characteristic, that particular componentor feature is not required to be included or have the characteristic.
[0041] Each of the appended claims defines a separate invention, which forinfringement purposes is recognized as including equivalents to the variouselements or limitations specified in the claims. Depending on the context, allreferences below to the "invention" may in some cases refer to certain specificembodiments only. In other cases, it will be recognized that references to the"invention" will refer to subject matter recited in one or more, but not necessarilyall, of the claims.
[0042] Exemplary embodiments will now be described more fully hereinafterwith reference to the accompanying drawings, in which exemplary embodimentsare shown. This disclosure may however, be embodied in many different formsand should not be construed as limited to the embodiments set forth herein. Theseembodiments are provided so that this disclosure will be thorough and completeand will fully convey the scope of the disclosure to those of ordinary skill in theart. Moreover, all statements herein reciting embodiments of the disclosure, aswell as specific examples thereof, are intended to encompass both structural andfunctional equivalents thereof. Additionally, it is intended that such equivalentsinclude both currently known equivalents as well as equivalents developed in thefuture (i.e., any elements developed that perform the same function, regardless ofstructure).
[0043] Various terms are used herein. To the extent a term used in a claim isnot defined, it should be given the broadest definition persons in the pertinent arthave given that term as reflected in printed publications and issued patents at thetime of filing.
[0044] The term "setting time" in the context of 3D concrete printing refers tothe time it takes for a freshly extruded layer of concrete to harden sufficiently sothat it can support the next layer without deforming or collapsing. The setting timeis crucial in 3D printing because each new layer must be placed on top of theprevious one before it fully cures, ensuring proper bonding and structuralintegrity.
[0045] The term "curing"refers to the process of maintaining adequatemoisture, temperature, and time to allow freshly placed concrete to achieve itsdesired properties, such as strength and durability.
[0046] The present disclosure relates to a concrete mix composition andmethod for producing 3D printed concrete, designed to enhance structuralintegrity, durability, and ease of application. The concrete mix is specificallyformulated to be compatible with 3D printing technology, providing optimalflowability and setting time to allow precise layering without compromising onstrength. The composition includes a balanced mix of cementitious materials,aggregates, water, and additives, such as plasticizers, accelerators, and fibers, toimprove mechanical properties and resistance to environmental factors. Themethod of formulating composition involves precise proportioning, thoroughmixing, and controlled extrusion through a 3D printer, enabling the creation ofcomplex architectural forms and structural components with minimal waste. Theinvention also includes specific guidelines for adjusting the mix based onenvironmental conditions and desired properties, ensuring versatility in variousconstruction scenarios. This 3D printed concrete composition and method offersignificant advancements in construction efficiency, sustainability, and designflexibility, making it suitable for both commercial and residential applications.
[0047] Thus, the present invention solves the problems highlighted in thebackground section as follows:
[0048] Optimized Flowability: The invention introduces a concretecomposition that is specifically formulated to ensure smooth and consistent flowthrough 3D printing nozzles. The inclusion of specific additives, such asplasticizers, helps maintain the right consistency for extrusion without clogging.
[0049] Controlled Setting Time: The concrete mix is designed with abalanced setting time, allowing sufficient time for proper layer bonding whileensuring the structure gains strength quickly. Accelerators or retarders can beadjusted based on the printing speed and environmental conditions.
[0050] Enhanced Interlayer Adhesion: The invention incorporates additivesand fibers that improve the bonding between layers, resulting in a more cohesiveand durable final structure. This addresses one of the primary weaknesses in 3Dprinted concrete, where layers can otherwise separate or crack over time.
[0051] Reduced Material Waste: The precise extrusion and layer-by-layerapproach of 3D printing, combined with the optimized concrete mix, significantlyreduces material waste compared to traditional construction methods. This leadsto more sustainable and cost-effective building processes.
[0052] Increased Design Flexibility: The specially formulated concrete mixallows for the creation of complex and intricate designs that are difficult toachieve with traditional methods. This enables architects and engineers to explorenew possibilities in construction, pushing the boundaries of modern architecture.
[0053] By addressing these key challenges, the invention not only enhancesthe efficiency and effectiveness of 3D printed construction but also contributes tomore sustainable and innovative building practices.
[0054] FIG. 1 illustrates a perspective view of a three-dimensional (3D)printing system 100, in accordance with embodiments of the presentdisclosure.The system 100 may include three primary units: mixing unit 101,pumping unit 102, and the printing unit 103 (interchangeably referred to as printer103).
[0055] In an embodiment, the mixing unit 101 may include one or morehoppers 101-1 and a mixer 101-2 such as high shear mixer. The hoppers 101-1may include containers that can hold the raw materials needed for the concretemix, such as cement, sand, aggregates, fibers and any additives. These materialsare fed into the mixer 101-2 through the hoppers. The hoppers store the drycomponents, such as cement, aggregates, and fibers. When these materials are fedinto the mixer, water is simultaneously added to achieve the desired consistencyof the concrete mix. The water content is a crucial component of the mix as itactivates the cement and facilitates the chemical reactions needed for the concreteto set and harden.
[0056] In an embodiment, a dry mix composition can include cementitiousmaterials and aggregates. The cementitious materials comprisesPortland cementand supplementary cementitious materials. Portland cement is the primary binder,providing the necessary strength and durability. The Portland cement can vary inan amount ranging between 30-60 % by weight of dry mix composition. In apreferred embodiment, the Portland cement can vary between 40-52% by weightof dry mix composition.
[0057] Supplementary cementitious materials (SCMs) like fly ash, slag, orsilica fume may be included to enhance specific properties such as workability,durability, and environmental performance. In an embodiment, supplementarycementitious materials (SCMs) can vary in an amount ranging between 0-30 % byweight of dry mix composition. In a preferred embodiment, supplementarycementitious materials (SCMs) can vary in an amount ranging between 2 to 8 %by weight of dry mix composition.
[0058] In an embodiment, aggregates can vary in an amount ranging between0-30 % by weight of dry mix composition. In a preferred embodiment, aggregatescan vary in an amount ranging between 10-22 % by weight of dry mixcomposition.Fine aggregates, such as sand, are used in the mix. The size, shape,and grading of the aggregates are carefully controlled to ensure a smoothextrusion process. Coarser aggregates are generally avoided to prevent nozzleblockages. The maximum size of the particles of aggregates can vary between 0.1mm to 2 mm. In a preferred embodiment, the maximum size of the particles canbe less than 1 mm to ensure smooth extrusion.
[0059] In an embodiment, the dry mix composition can also include additives(interchangeably referred to as admixtures), which play a crucial role in enhancingthe properties of the concrete mix composition, especially in applications like 3Dprinting. These substances are added in small quantities to the concrete mix tomodify its characteristics, improving performance and making it suitable forspecific conditions.
[0060] In some embodiments, additives can be pre-mixed with the dryingredients in the hoppers before being transferred to the mixer. Alternatively,additives can be directly introduced into the mixer along with the other materialsand water. This ensures that the additives are uniformly distributed throughout themix.
[0061] There are different types of additives that can be added to dry mixcomposition such as:1. Plasticizersincrease the workability of concrete without adding extra water.This is particularly important in 3D printing, where a fluid yet stable mix isneeded to ensure smooth extrusion through the nozzle.In other words, theplasticizers reduce the water content needed for the mix, improvingflowability without compromising strength. The plasticizer can vary in anamount ranging between 0.5% to 2.5% by weight of cement.2. Acceleratorscan speed up the setting and hardening process of concrete,allowing better control over the printing process. They are useful in situationswhere rapid strength development is needed, such as in environments wherequick construction is essential or when working in cold weather conditionsthat could slow down the curing process.The accelerators can vary in anamount ranging between0.1% to 2% by weight of cement.3. Retarderscan delay the setting time of concrete, allowing for more workingtime before the concrete begins to harden. In 3D printing, retarders can helpmanage the timing of layer placement, ensuring that previous layers remainworkable and bond well with subsequent layers. The retarders can vary in anamount ranging between 0.1% to 1.5% by weight of cement.4. Stabilizerscan prevent the separation of the components in the concrete mix(e.g., aggregates, cement, water). This is important because segregation canlead to uneven strength and texture in the printed structure. By increasing thecohesiveness of the mix, stabilizers ensure that the fine particles (cement andfine aggregates) remain uniformly distributed with the coarse aggregates andwater. The stabilizer can vary in an amount ranging between 0.1% to 1% byweight of cement.
[0062] In an embodiment, the dry mix composition can include fiber such asPolypropylene, glass, or steel fibers added to improve tensile strength, ductility,and interlayer bonding. The fiber can vary in an amount ranging from 0.5% to 3%by volume of the concrete mix. The length of fiber ranges between 3 mm to 20mm. In a preferred embodiment, the length of the fiber ranges between 6 mm to12 mm.
[0063] In an embodiment, when the dry mix composition can be fed into themixer, water is simultaneously added to achieve the desired consistency of theconcrete mix. The ratio of water content to the cement ranges between 0.25 to0.45. In a preferred embodiment, the ratio of water content to the cement rangesbetween 0.30 to 0.40 for optimal flowability and strength. The water-to-cementratio is critical for the mix's workability and strength. A lower water-to-cementratio is preferred to reduce the risk of segregation and to ensure the mix has thenecessary flow characteristics for 3D printing. Thus, the ingredients are carefullymeasured and proportioned to meet the desired properties. This involves adjustingthe ratios of cement, aggregates, water, and admixtures to suit specificrequirements, such as the load-bearing capacity of the structure or environmentalconditions.
[0064] In an embodiment, the mixer 101-2 may receive the materials from thehoppers 101-1 and thoroughly combine them to create a homogeneous concretemix. This ensures that the concrete has the right consistency and properties for 3Dprinting. Within the mixer 101-2, the water-to-cement ratio and amount ofadditives for concrete mix composition are adjusted to control the flowability andsetting time of the mix. The mixture is tested for its flowability, curing time, andmechanical strength prior to the printing process.
[0065] In an embodiment, the pumping unit 102 may include a concretepump 102-1. After the concrete mix composition is prepared in the mixing unit101, it is transferred to the concrete pump 102-1. The pump 102-1 is responsiblefor moving the concrete mix from the mixer to the printing unit. It ensures that theconcrete mix is delivered at the correct pressure and flow rate, necessary forconsistent extrusion through the nozzle.
[0066] The slump of concrete is a measure of its flowability or workability,indicating how easily the concrete can flow and be placed in formwork. It is a keyparameter in evaluating the consistency of a concrete mix. The slump test is asimple, standardized method used to assess the flowability of fresh concrete.
[0067] In an embodiment, the slump of the concrete mix is typicallymeasured after the completion of the mixing processbutbefore pumping of theconcrete in the printing unit 103. This means the slump is calculated during orimmediately after the mixing unitstep, before the concrete is transferred to thepumping unit. Once the mixing is complete, a sample of the concrete mix is takento perform the slump test. This test is done to check the flowability andworkability of the mix. If the slump falls within the desired range, the mix isconsidered suitable for 3D printing.
[0068] If the slump is too high (indicating the mix is too fluid) or too low(indicating it's too stiff), adjustments can be made by adding more water,plasticizers, or other admixtures to achieve the required flowability. The slump,measured from the slump test or similar methods, indicating the flowability canvary between 10 mm to 100 mm.
[0069] Once the desired slump is confirmed, the mixed composition (alsoreferred to as "mix") is then pumped through the pumping unit 102 to the printingunit 103 for extrusion.
[0070] In an embodiment, the printing unit 103 may include a hose pipe 103-1, a nozzle 103-2, and a frame 103-3. The hose pipe 103-1 may connect theconcrete pump 102-1 to the nozzle 103-2, allowing the concrete mix compositionto flow from the pump 102-1 to the printing area. The hose pipe 103-1 must beflexible and durable to handle the flow of concrete without blockages.
[0071] In an embodiment, the nozzle 103-2 is a crucial component of theprinting unit 103. It controls the extrusion of the concrete mix composition,shaping it as it is deposited layer by layer to form the structure. The design of thenozzle 103-2 affects the precision and quality of the printed layers.
[0072] In an embodiment, the frame 103-2 provides the structural support forthe 3D printing process. It guides the movement of the nozzle, ensuring that eachlayer is accurately aligned with the previous one. The frame must be sturdy andprecise to maintain the integrity of the printed structure. In an embodiment, aheight of layer ranges between 5 mm to 20 mm, whereas a diameter of the nozzleranges between 10 mm to 50 mm. In another embodiment, a speed at which theconcrete mix composition is extruded through the nozzle, can vary between20mm / s to 150 mm / s.
[0073] The printed structure is associated with compressing strengthindicating the maximum amount of compressive force the concrete can bearbefore it fails or cracks. This is a crucial property for any concrete structure,particularly in construction, where the material must support weight and resistexternal pressures. The compressive strength of the concrete determines the loadbearing capacity of the printed structure. High compressive strength is essentialfor ensuring that the structure can support the intended loads without collapsing ordeforming. The compressive strengthof the printed structure can vary between 20MPa to 60 MPa after 28 days of curing.
[0074] The environmental conditions such as temperature, humidity etc., alsoaffect the composition of concrete mix. In particular, water-to-cement ratio, andamount of additives can be modified based on ambient temperature. Lowertemperatures may require accelerators, while higher temperatures may needretarders. Further, curing time may be increased or composition may be adjustedwithin the prescribed range for more rapid setting in low-humidity environmentsto avoid cracking.
[0075] FIG. 2 illustrates a perspective view of 3D printed concrete structure200, in accordance with embodiments of the present disclosure. Once the concretemix composition is prepared, it is loaded into the 3D printer for extrusion. Theprinting process includes extrusion, layering, and curing.
[0076] In an embodiment, in the step of extrusion, the mix is extrudedthrough a nozzle, typically layer by layer, following a pre-programmed design.The nozzle's size and shape are optimized to maintain a consistent flow and toprevent blockages. In an embodiment, a height of layer ranges between 5 mm to20 mm, whereas a diameter of the nozzle ranges between 10 mm to 50 mm. Inanother embodiment, a speed at which the concrete mix composition is extrudedthrough the nozzle, can vary between20 mm / s to 150 mm / s.
[0077] In the process of layering, each layer is precisely placed on top of theprevious one. The mix's setting time is carefully controlled to ensure goodbonding between layers, while also supporting the weight of subsequent layerswithout deformation.There are two types of setting time as follows:- Initial setting time: This is the time required for the concrete to beginhardening. For 3D printed concrete, this typically ranges from 30 minutes to 2hours, adjustable depending on the printing speed and environmentalconditions.- Final Setting Time: This is the time at which the concrete has hardenedenough to hold its shape and support subsequent layers. This can takeanywhere from 2 hours to 6 hours.
[0078] In an embodiment, in the process of curing, after printing, thestructure is allowed to cure. In 3D concrete printing, curing is particularlyimportant because it ensures that each printed layer develops the necessarystrength to support subsequent layers and the overall structure. The importantparameters associated with the curing are temperature and relative humidity.- Relative humidity - Concrete gains strength through a chemical reactioncalled hydration, which requires water. If the concrete loses moisture tooquickly, the hydration process can be incomplete, leading to weaker concrete.The relative humidity may range between 50% to 100% - higher humiditypreferred for proper curing.- Temperature plays a critical role in the rate of hydration. If the concrete is toocold, the curing process will be slow, potentially compromising thedevelopment of strength. If it is too hot, it might set too quickly, leading tocracks. The temperature may range between 10°C to 35°C to avoid rapiddrying or freezing.
[0079] In an embodiment, curing methods such as natural air curing, watercuring, or the use of curing compounds can be implemented to maintain moistureand promote strength development.
[0080] FIG. 3 illustrates a flow diagram representing a method 300 forformulating a concrete mix suitable for 3D printing, in accordance withembodiments of the present disclosure. The method 300 starts with step 302. Theformulation method is crucial to achieving the mix that is consistent and suitablefor 3D printing.
[0081] At step 302, cementitious materials, fine aggregates, water,plasticizers, and fibers are combined in the proportion as defined above to create aconcrete mix composition. The ingredients are carefully measured andproportioned to achieve the desired properties. This includes adjusting the ratiosof cement, aggregates, water, and admixtures to match specific requirements, suchas the structure's load-bearing needs or environmental conditions.
[0082] At step 303, the concrete mix composition is mixed using a high-shearmixer to ensure uniformity and to prevent the formation of clumps or segregationof materials. The mixing time and speed are carefully controlled to achieve ahomogeneous mix.
[0083] At step 304, the water-to-cement ratio and amount of the additivesforthe mixed concrete mix composition are adjusted to control the flowability andsetting time of the mixed concrete composition.
[0084] At step 306, the control mix composition is tested for analysis ofproperties, comprising flowability, setting time, and compressive strength, prior to3D printing. Adjustments to the mix can be made based on these tests to ensureoptimal performance. The mixture is tested for its flowability, curing time, andmechanical strength prior to the printing process. Adjustments are made to ensureoptimal print quality.Table 1
[0085] Table 1 represents a detailed report on the mechanical properties ofthe 3D printed concrete, including compressive strength, tensile strength, anddurability under various conditions.
[0086] FIG. 4 illustrates a flow diagram representing method 400 forconstructing a structure using 3D printing technology, in accordance withembodiments of the present disclosure.
[0087] At step 402, a concrete mix composition is dispensed into a 3Dprinter.
[0088] At step 404, the composition may be extruded through a nozzle insuccessive layers, with each layer being aligned with the preceding layer.
[0089] At step 406, one or more parameters comprising at least one of aspeed of the extrusion, and temperature of the nozzle may be controlled to ensureoptimal bonding between layers;
[0090] At step 408, a printed structure is cured using the one or morecontrolled parameters to attain the particular strength and durability.Working ExamplesExample 1: Residential Wall Construction- Composition: A concrete mix with Portland cement (for example between30-60% by wt, preferably 40% by wt), fly ash (a supplementarycementitious material (SCM)) (for example between 8-10% by wt,preferably 8% by wt), silica sand(for example between 10-12% by wt,preferably 12% by wt), slag (for example between 9-10% by wt,preferably 10% by wt), and binder concretes such as plasticizer (forexample between 0.5-2.5% by wt, preferably 1% by wt), accelerators (forexample between 01.-2% by wt, preferably 05% by wt), retarder (forexample between 0.1-0.5% by wt, preferably 0.4% by wt), stabilizer (forexample between 0.1-1% by wt, preferably 0.3% by wt), and fibers likepolypropylene (for example between 0.5-3% by wt, preferably 2% by wt),length 3 to 20 mm, preferably 8 mm.- Apart from the above following is used as per requirements: a water(forexample between 0.1-2% by wt, preferably 0.15% by wt), andpolypropylene fibers was prepared.Creating a concrete mix using the specified components and proportions can yielda high-performance concrete suitable for various applications. Below are realworld examples that align with your specified concrete mix composition,including the use of Portland cement, fly ash, silica sand, slag, and variousadditives.1. Infrastructure Projects- Example: Highway Overpasses or Bridgeso Concrete Composition:- Portland Cement: 40% by weight- Fly Ash: 8% by weight- Silica Sand: 12% by weight- Slag: 10% by weight- Plasticizer: 1% by weight- Accelerator: 0.5% by weight- Retarder: 0.4% by weight- Stabilizer: 0.3% by weight- Polypropylene Fibers: 2% by weight, 8 mm in length- Water: 0.15% by weightReason for Use: This concrete mix would provide enhanced durability andworkability for structures subjected to heavy loads and environmentalstressors, like highway overpasses.2. Commercial Construction- Example: High-Rise Buildingso Concrete Composition:- Portland Cement: 40% by weight- Fly Ash: 8% by weight- Silica Sand: 12% by weight- Slag: 10% by weight- Plasticizer: 1% by weight- Accelerator: 0.5% by weight- Retarder: 0.4% by weight- Stabilizer: 0.3% by weight- Polypropylene Fibers: 2% by weight, 10 mm in length- Water: 0.15% by weightReason for Use: In high-rise buildings, the inclusion of fly ash and slagenhances the strength and sustainability of the concrete, while theplasticizer ensures better flowability for pouring in forms.3. Pavement and Road Construction- Example: Airport Runwayso Concrete Composition:- Portland Cement: 40% by weight- Fly Ash: 8% by weight- Silica Sand: 12% by weight- Slag: 10% by weight- Plasticizer: 1% by weight- Accelerator: 0.5% by weight- Retarder: 0.4% by weight- Stabilizer: 0.3% by weight- Polypropylene Fibers: 2% by weight, 8 mm in length- Water: 0.15% by weightReason for Use: This mix can withstand the stresses and thermal variationsof an airport runway while minimizing cracking and enhancing longevity.4. Residential Applications- Example: Driveways and Patioso Concrete Composition:- Portland Cement: 40% by weight- Fly Ash: 8% by weight- Silica Sand: 12% by weight- Slag: 10% by weight- Plasticizer: 1% by weight- Accelerator: 0.5% by weight- Retarder: 0.4% by weight- Stabilizer: 0.3% by weight- Polypropylene Fibers: 2% by weight, 8 mm in length- Water: 0.15% by weightReason for Use: Using this mix for driveways or patios enhances theresistance to cracking and improves the aesthetics of the concrete surface.- Proportioning: The water-to-cement ratio was set at 0.35, with a plasticizerdosage of 1% by weight of cement.- Printing: The mix was extruded to form a layer-by-layer deposition ofconcrete which sets immediately when comes out of the nozzle. The layerformation is shown in the figure below.- Results: The printed wall demonstrated excellent layer adhesion andmaintained its shape during printing. After 28 days of curing, thecompressive strength was measured at 40 MPa, suitable for residentialload-bearing walls.Example 2: Complex Architectural Feature- Composition: A mix of Portland cement, fly ash, fine sand, water, glassfibers, and retarders was used.- Proportioning: The water-to-cement ratio was 0.32, with fly ashcomprising 20% of the cementitious material.- Printing: The mix was used to create a freeform architectural element withintricate curves and overhangs.- Results: The structure exhibited high precision in detail, with no visiblecracks or delamination between layers. The use of fly ash improved theworkability, and the final compressive strength was 40 MPa.
[0091] The present invention offers several advantages. For instance, theoptimized mixing of concrete mix composition allows for faster construction withminimal human intervention, reducing labor costs and construction time.In theprocess of the preparation of the concrete mix composition, material wasteisreduced as compared to the traditional concrete composition and the potentialinclusion of recycled materials (left over material after the composition is formed)contributes to the environmental sustainability of construction projects.
[0092] Moreover, the extrusion process of the proposed invention providesthe ability to print complex shapes and structures.In addition, the inclusion offibers and additives within the concrete mix composition enhances the durabilityand longevity of the structures, making them suitable for a wide range ofapplications, from residential to commercial construction.
[0093] Thus, the present disclosure provides following key aspects of theinvention:
[0094] The development of a concrete mix suitable for 3D printing involvescareful balancing of various components, including cement, aggregates, water,and additives along with nozzle extrusion and layer bonding.
[0095] While 3D printing in construction is an emerging field, the specificchallenges associated with concrete extrusion, such as achieving the rightflowability, setting time, and interlayer adhesion, are addressed in presentinvention.
[0096] The use of additives and fibers enhances the properties of the concretemix, particularly for 3D printing applications.
[0097] Following are the real-world examples based on the claimsmentioned:
[0098] Concrete Composition: Scenario: Building a 3D Printed ModularHouse A construction company plans to build modular houses using a concretemix suitable for 3D printing. The dry mix for the project contains:Portland cement: 50% by weight of the dry mix composition to ensuresufficient strength for the structure.Supplementary Cementitious Materials (SCMs): 15% fly ash is addedto improve the mix's environmental performance and durability.Aggregates: 25% fine sand ensures smooth extrusion through theprinter without clogging.Water content: The water-to-Portland cement ratio is set at 0.35 toachieve the right balance between workability and structural integrity for efficientprinting.This mix provides high strength and ensures workability for 3Dprinting in a construction site.
[0099] Additives in the Concrete Mix: Scenario: Construction of a 3D PrintedPedestrian Bridge In a project to build a pedestrian bridge using 3D printedconcrete, additives are added to ensure optimal performance:Plasticizers: 1.5% plasticizers by weight of cement are used toimprove flowability without increasing the water content, ensuring smooth andeven layers.Accelerators: 0.5% accelerators help reduce the setting time, allowingrapid construction in cold weather conditions.Retarders: 0.2% retarders are added in warmer conditions to slow thesetting process, giving enough time for precise layer placement.Stabilizers: 0.3% stabilizers maintain mix cohesion, preventingsegregation of the materials as they are extruded from the printer.This results in a concrete mix with enhanced flow, quick curing, andstability during printing, vital for the bridge's layered structure.
[00100] Inclusion of Fibers: Scenario: High-Strength 3D Printed RetainingWall for an Urban Project A retaining wall needs to be built for a new urbandevelopment, requiring enhanced tensile strength to resist ground movement. Theconcrete mix includes:Fibers: 2% by volume of steel fibers, providing the required strengthand flexibility for the retaining wall.Fiber size: Fibers with a length of 12 mm are used, ensuring theydistribute evenly throughout the mix.Aggregate size: The aggregate particles are between 0.1 mm to 2 mm,ensuring smooth extrusion and strong bonding between layers.This mix results in a high-strength, durable wall capable ofwithstanding lateral pressure from the surrounding soil.
[00101] Specific Fiber Length: Scenario: 3D Printed Parking Garage Rampswith Improved Durability For a parking garage, ramps need to be durable andhandle significant traffic loads. To improve tensile strength and flexibility:Fibers: 1% polypropylene fibers are added, with a fiber lengthbetween 6 mm and 12 mm, helping to reinforce the layers without disrupting thesmooth flow of the material through the printer.The fibers enhance the ramp's load-bearing capacity whilemaintaining smooth printing and strong bonding between layers.These real-world applications showcase how the claimed concretecomposition can be adapted for various construction needs, providing structuralintegrity, ease of application, and environmental benefits.
[00102] Following are the real-world examples for a method for formulating aconcrete mix composition for 3d printing.
[00103] Scenario 1: Construction of a 3D Printed Affordable Housing Unit ina Tropical Climate: A construction company is tasked with building affordablehousing units using 3D printed concrete. The process follows a specific method toensure that the mix is suitable for the local climate and project requirements.Proportioning (302): The team begins by selecting materials that willwork well in a humid, tropical environment. They proportion:Cementitious materials: Portland cement at 45% and supplementarymaterials like fly ash at 10% to reduce environmental impact.Fine aggregates: Sand makes up 25% to ensure a smooth extrusionprocess.Water: The water content is adjusted to maintain flowability withoutcompromising strength.Plasticizers: 1.5% is added to reduce the water requirement whileensuring smooth flow through the printer.Fibers: 1.5% polypropylene fibers by volume are added to improvetensile strength and bonding between printed layers.Mixing (304): The concrete mix composition is thoroughly mixedusing a high-shear mixer to ensure uniformity, preventing segregation ofmaterials. This step is critical to maintaining consistency during the extrusionprocess.Adjusting (306): The water-to-cement ratio is optimized at 0.35,ensuring the right balance between flowability and strength. The flowability isadjusted so that the slump falls within the range of 60 mm, which is ideal for thetropical environment where high flow is necessary due to humidity.The setting time is carefully controlled:Initial setting time: Adjusted to 1 hour, allowing enough time to printeach layer at a speed suitable for the local weather.Final setting time: Set to 4 hours to provide a stable structure withoutcausing delays in the construction process.Testing (308): Before beginning the 3D printing, the mix is tested for:Flowability: A slump test is conducted to ensure the concrete can flowthrough the printer and maintain layer consistency.Setting time: The mix is tested for initial and final setting times toensure the concrete remains workable during printing and develops strengthwithin the desired time frame.Compressive strength: Test samples are cured and checked to ensurethe housing units meet structural safety standards.This method ensures that the concrete mix is suitable for the tropicalenvironment, allowing efficient and high-quality 3D printing of affordable homes.
[00104] Scenario: 3D Printing of Custom Garden Structures in a TemperateClimate: A landscaping company is creating custom garden structures using 3Dprinted concrete. The method of formulating the concrete mix is adapted to suitboth aesthetic and functional requirements for outdoor use in a temperate climate.Proportioning (302): The company starts by proportioning:Cementitious materials: Portland cement at 40% and silica fume at 5%to improve durability.Fine aggregates: Sand makes up 30%, ensuring the mix is smoothenough for intricate designs.Plasticizers: 1% is used to reduce water content and improveflowability without compromising strength.Fibers: 2% glass fibers to enhance tensile strength and resistance tocracking in outdoor conditions.Mixing (304): The mix is processed using a high-shear mixer to ensurethe materials are evenly distributed and prevent segregation during printing,which is especially important for creating fine, detailed structures.Adjusting (306):Water-to-cement ratio: Adjusted to 0.40 for increased workability,important for the intricate designs and slower printing speeds.Flowability: The mix's slump is kept at 40 mm to ensure that thelayers can be precisely extruded without collapsing.Setting time: Adjusted to suit outdoor printing in cooler temperatures:Initial setting time: 45 minutes to allow adequate time to print beforethe concrete begins to set.Final setting time: 3 hours to provide enough strength whilemaintaining structural integrity.Testing (308): The control mix undergoes testing for:Flowability: Ensuring the concrete can handle the delicate structureswithout nozzle blockages.Setting time: Testing shows that the mix meets the timeframes neededto ensure the layers bond well without sagging.Compressive strength: The structures are tested to ensure they canwithstand outdoor weather conditions, including rain and temperature changes.By using this method, the company ensures that the garden structuresare both aesthetically pleasing and durable enough to withstand the outdoorenvironment.This method highlights the flexibility of 3D printed concrete fordifferent applications, ensuring the right balance of workability, strength, andenvironmental adaptability.
[00105] Following is the real-world examples for method for constructing astructure using a 3D Printer.
[00106] Scenario: 3D Printing a Custom Pavilion for an Outdoor Exhibition: Adesign firm is tasked with building a custom pavilion for an outdoor exhibitionusing a 3D printed concrete structure. The method follows:Dispensing (402): The concrete mix is prepared following thecomposition specified in previous claims (e.g., Portland cement, fibers, andadditives). It is dispensed into the 3D printer designed for large-scaleconstruction.Extruding (404): The concrete is extruded through a nozzle insuccessive layers, with each layer carefully aligned to match the previous one,ensuring precision in the pavilion's intricate design.Controlling (406):The extrusion speed is controlled at 80 mm / s, ensuring smoothprinting for the pavilion's large walls.Nozzle temperature is kept within a suitable range to optimize thebonding between layers, which is critical for ensuring structural integrity duringthe build process.Curing (408): Once the printing process is completed, the pavilion iscured under controlled conditions, ensuring the material reaches the requiredstrength and durability.
[00107] Controlled Curing Conditions: Scenario: 3D printing an outdoor restarea in a desert environment.In a desert location, an outdoor rest area is being 3D printed using thecontrolled curing method. The construction team ensures the curing processoccurs within the correct environmental conditions:Temperature: The operating temperature is maintained between 25°Cand 30°C to facilitate even curing, despite the higher daytime temperatures.Humidity: Since the desert air is dry, a relative humidity of 50% ismaintained around the printed structure using misting systems to prevent theconcrete from drying out too quickly and to ensure proper hydration and strengthdevelopment.This controlled curing process ensures the structure reaches optimalstrength, resisting environmental wear in the harsh desert conditions.
[00108] Compressive Strength Target: Scenario: 3D printed foundation for awind turbine: A wind turbine foundation is being constructed using 3D printing.The printed concrete must achieve a compressive strength between 40 MPa and60 MPa after 28 days of curing to ensure the foundation can support the heavystructure of the turbine.The curing process is closely monitored to maintain theproper conditions, ensuring the concrete mix develops the necessary strengthwithin the specified time frame. After curing, compressive strength tests confirmthat the foundation has achieved 45 MPa, making it strong enough to support thedynamic loads exerted by the wind turbine during operation.
[00109] Layer height, nozzle diameter, and extrusion speed: Scenario: 3Dprinting urban planters with custom patterns.A city park is being revitalized withthe installation of custom-designed urban planters. These planters are printedusing 3D concrete printing technology:Layer Height and Nozzle Diameter: The design requires smoothcurves, so the layer height is set to 10 mm, ensuring precision. The nozzlediameter is 30 mm, allowing for a balance between speed and detail in theprinting process.Extrusion Speed: To maintain high production efficiency whilepreserving the aesthetic details, the extrusion speed is adjusted to 60 mm / s. Thisspeed ensures that the printer can maintain the intricate patterns required for theplanters' surface while maintaining structural integrity.By controlling these parameters, the company achieves high-qualityprints that meet the design and structural requirements for the project.
[00110] These real-world examples demonstrate how the method of 3Dprinting with concrete is adapted to meet diverse construction needs, ensuringoptimal performance in different environments and applications, from aestheticurban structures to high-strength foundations.
[00111] In an example, following is technical composition of a 3D-printableconcrete mix based on the parameters provided, focusing on an optimal balance ofworkability, strength, and flowability:
[00112] 3D Printable Concrete Material Composition:
[00113] Cementitious Materials:
[00114] Portland Cement: 50% by weight of the dry mix composition. Thisensures sufficient strength and durability for the printed structure.
[00115] Supplementary Cementitious Materials (SCMs):
[00116] Fly Ash: 10% by weight of the dry mix composition. Fly ash improvesworkability, reduces heat generation during curing, and enhances long-termstrength development.
[00117] Aggregates:
[00118] Fine Sand: 20% by weight of the dry mix composition. Fine sandensures smooth extrusion and reduces the risk of nozzle blockages during the 3Dprinting process.
[00119] Water Content:
[00120] Water-to-Portland Cement Ratio: 0.35. This ratio provides an optimalbalance between flowability and strength, ensuring the concrete mix can flowsmoothly through the nozzle while maintaining structural integrity after extrusion.
[00121] Effect of this Material Composition:
[00122] Workability and Extrusion: The selected water-to-cement ratio (0.35)combined with the plasticizing effect of fly ash results in a highly workable mix.This ensures smooth extrusion through the 3D printer nozzle without blockages,and good layer adhesion during the printing process.
[00123] Strength: Portland cement at 50% ensures that the material has a highcompressive strength once cured, while fly ash contributes to durability andimproves the material's resistance to environmental factors like moisture ortemperature changes.
[00124] Flowability: The composition ensures sufficient flowability, with atarget slump range between 50-70 mm, ideal for 3D printing applications wherethe mix must flow smoothly but retain its shape after each layer is deposited.
[00125] This concrete mix is ideal for 3D printing structural elements inconstruction, such as walls or modular components, where both workability andstrength are critical.
[00126] Following is a comparison between the selected 3D printable concretematerial composition and a more traditional 3D printable concrete mix,highlighting improvements, efficiency, and the synergistic effects of theoptimized mix.
[00127] Traditional 3D Printable Concrete Composition: Portland Cement:60% by weight. SCMs (Fly Ash, Silica Fume, or Slag): 5% by weight. FineAggregates: 30% by weight. Water-to-Cement Ratio: 0.45. This traditional mixfocuses on a higher cement content to achieve strength and durability, but itcompromises workability and sustainability due to the higher Portland cementcontent.
[00128] The 3D Printable Material Composition of the present invention:Portland Cement: 50% by weight. SCMs (Fly Ash): 10% by weight. FineAggregates: 20% by weight. Water-to-Cement Ratio: 0.35.
[00129] Comparison in Key Aspects:
[00130] Synergistic Effect of SCMs and Reduced Cement Content: By using10% fly ash, the optimized mix of the present invention reduces the need for highamounts of Portland cement, improving the sustainability of the material. Fly ashalso enhances workability and long-term strength, creating a more resilientstructure with less risk of cracking and shrinkage.
[00131] Improved Workability and Flowability: The selected mix of thepresent invention improves flowability due to the reduced water-to-cement ratioand the reduced aggregate content. This enhances the overall efficiency of the 3Dprinting process, as the material can be extruded more smoothly and precisely,minimizing delays caused by nozzle blockages.
[00132] Enhanced Strength and Durability: While the traditional mix reliesheavily on Portland cement for strength, the optimized mix of the presentinvention achieves similar or improved strength by utilizing the synergisticproperties of fly ash and a lower water content. This also leads to improveddurability, as fly ash contributes to better resistance against environmentaldegradation (e.g., moisture and temperature changes).
[00133] Sustainability and Environmental Efficiency: The optimized mix of thepresent invention significantly lowers the carbon footprint by reducing cementcontent and incorporating SCMs like fly ash, a byproduct of coal combustion.This makes the selected composition eco-friendlier and more aligned with modernsustainable building practices.
[00134] The selected optimized 3D printable concrete composition of thepresent invention offers clear improvements over traditional compositions interms of workability, strength, durability, and environmental impact. Thesynergistic effect of combining lower cement content with a higher proportion offly ash enhances both the material's performance in 3D printing applications andits long-term sustainability.
[00135] While the foregoing describes various embodiments of the invention,other and further embodiments of the invention may be devised without departingfrom the basic scope thereof. The scope of the invention is determined by theclaims that follow. The invention is not limited to the described embodiments,versions or examples, which are included to enable a person having ordinary skillin the art to make and use the invention when combined with information andknowledge available to the person having ordinary skill in the art.
Claims
1. A concrete composition comprising: a dry mix composition having: cementitious materials, wherein the cementitious materials comprising Portland cement in an amount ranging between 30-60 % by weight of dry mix composition and supplementary cementitious materials (SCMs) in an amount ranging between 0-30 % by weight of dry mix composition, and aggregates in an amount ranging between 0-30 % by weight of dry mix composition; and water content, wherein a ratio of water content to the Portland cement ranges between 0.25 to 0.45.
2. The concrete composition as claimed in claim 1, wherein the dry mix composition comprises additives, the additives comprising: plasticizers in an amount ranging between 0.5% to 2.5% by weight of cement, accelerators in an amount ranging between 0.1% to 2% by weight of cement, retarders in an amount ranging between 0.1% to 1.5% by weight of cement, and stabilizers in an amount ranging between 0.1% to 1% by weight of cement.
3. The concrete composition as claimed in claim 2, wherein the dry mix composition comprising fiber in an amount ranging from 0.5% to 3% by volume of the concrete mix, wherein a type of fibre comprises at least one of Polypropylene, glass, or steel fibers, and wherein a length of fiber ranges between 3 mm to 20 mm, and wherein size of the particles in the aggregates ranges between 0.1 mm to 2 mm.
4. The concrete composition as claimed in claim 3, wherein the length of the fiber ranges between 6 mm to 12 mm.
5. A method (300) for formulating a concrete mix composition for 3D printing, the method comprising: proportioning (302) Cementitious materials, fine aggregates, water, plasticizers, and fibers to create a concrete mix composition as claimed in any of claims 1-4; mixing (304) the concrete mix composition using a mixer (101-2) to achieve a mixed concrete mix composition having uniformity that prevents segregation; adjusting (306) the water-to-cement ratio and a number of additives within the mixed concrete mix composition to control a flowability and setting time of the mix, wherein the flowability of the mixed concrete mix composition is determined by a slump ranging between 10 mm to 100 mm, and wherein the setting time comprises an initial setting time that ranges between 30 minutes to 2 hours and depends on the printing speed and environmental conditions, and a final setting time that ranges between 2 hours to 6 hours; and testing (308) the control mix composition for analysis of properties, comprising flowability, setting time, and compressive strength, prior to 3D printing.
6. A method (400) for constructing a structure using 3D printer (103), the method comprising: dispensing (402) a concrete mix composition as claimed in any of claims 1-4into the 3D printer (103); extruding (404) the composition through a nozzle (103-2) in successive layers, with each layer being aligned with the preceding layer; controlling (406) one or more parameters comprising at least one of a speed of the extrusion, and temperature of the nozzle (103-2)to ensure optimal bonding between layers; and curing (408) a printed structure (200) using the one or more controlled parameters to attain the particular strength and durability.
7. The method (400) as claimed in claim 6, wherein the curing is performed at an operating temperature ranging between 10°C to 35°C, and a relative humidity ranging between 50% to 100% 8. The method (400) as claimed in claim 6, wherein compressive strength associated with the printed structure (200) ranges between 20 MPa to 60 MPa after 28 days of curing.
9. The method (400) as claimed in claim 6, wherein a height of layer ranges between 5 mm to 20 mm, and a diameter of the nozzle (103-2) ranges between 10 mm to 50 mm, and wherein a speed at which extrusion is performed, ranges between 20 mm / s to 150 mm / s.