A method for producing ultrafine phase-pure tetragonal and cubic yttria doped-zro2 nanopowder
Patent Information
- Application Number
- IN202331063032
- Authority / Receiving Office
- IN · IN
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2023-09-20
- Publication Date
- 2026-10-23
- Estimated Expiration
- 2043-09-20
AI Technical Summary
Current methods for producing Yttria-Stabilized Zirconia (YSZ) compositions result in low surface area, large particle size, high sintering temperatures, and phase segregation, limiting their widespread application and availability, with a monopoly on high-quality precursors.
A method for producing high surface area, ultrafine, phase-pure tetragonal and cubic Y2O3-doped ZrO2 nanopowders with low temperature sinterability, involving the dissolution of precursor solutions, mixing with alkali, washing, drying, grinding, calcining, and pressureless sintering to achieve near-theoretical density and high hardness.
The method yields nanoparticles with reproducible size and shape, excellent sinterability at low temperatures, and high hardness values, ensuring phase purity and retention without phase segregation, overcoming the limitations of existing YSZ compositions.
Abstract
Description
[0001] The present invention relates to a method for producing ZrO2 nanopowder, in particularly, the present invention relates to method forproducing mass production of high surface area, ultrafine phase-pure tetragonal and cubic yttria doped-ZrO2 nanopowders with low temperature sinterability.BACKGROUND
[0002] Traditionally, among all engineering ceramic products, Yttria-Stabilized 10 Zirconia (YSZ) compositions score very high in terms of their ranges ofapplications, lifetime of devices / instruments, performances and properties, etc. However, the source of these high-quality YSZ precursors is rare and known to have a monopoly with very selected companies. This creates a situation that for making all zirconia components the YSZ precursor has to be imported.
[0003] A conventional solution discloses a low BET surface area (8-40 m2 / g) and larger particle size (0.05-0.25 μm) for 3 mol.% YSZ.
[0004] Another conventional solution discloses partially stabilized zirconia (Phase after sintering- 85% Tetragonal+ 15% Cubic and Monoclinic) ceramics obtained using 0-3 mol.% yttria doping.
[0005] Yet another conventional solution discloses a high sintering temperature (1300 °C-1600 °C) & high grain size (0.1-1 μm).
[0006] Yet another conventional solution discloses a phase separation into high yttrium tetragonal phase and low yttrium tetragonal phase at high sintering temperature (>1500 °C) & high grain size (~0.3μm).
[0007] There is a need for a solution to overcome above-mentioned drawbacks. OBJECTS OF THE DISCLOSURE
[0008] Some of the objects of the present disclosure, which at least one embodiment herein satisfies, are listed below.
[0009] The principle object of the invention is to provide ensure a formation of nanoparticles with reproducible low size, near spherical shape.
[0010] Another objective of the invention is to provide a synthesized powder produced phase pure doped ZrO2 ceramic with fully stabilized tetragonal andcubic phase with near theoretical density and refined grain size 90-200 nm. Both the powders and ceramics may be from monoclinic phase and ensured high temperature phase retention capacities without any phase segregation / separation.
[0011] Another objective of the invention is to provide synthesized powders that show excellent sinterability as a near theoretically dense ceramic that may beobtained a temperature as low as 1150 °C (via pressure less conventional sintering).
[0012] Another objective of the invention is to provide a synthesized ceramic that illustrates remarkable hardness value (13 - 14 GPa).
[0013] This, and other objects and advantages of the present subject matter will 15 be apparent to a person skilled in the art after consideration of the followingdetailed description taken into consideration with accompanying drawings in which preferred embodiments of the present subject matter are illustratedSUMMARY
[0014] Solution to one or more drawbacks of existing technology, and additional advantages are provided through the present subject matter. Additional features and advantages are realized through the technicalities of the present subject matter. Other embodiments and aspects of the subject matter are described in detail herein and are considered to be a part of the claimed subject matter.
[0015] The present disclosure provides method for preparing high surface area (~100-160 m2 / g) Y2O3-doped-zirconia nanoparticles. The method includes dissolving a first predetermined amount of a first precursor solution with a second predetermined amount of deionized water to produce a first solution. The method includes mixing the first solution into a third predetermined amount of alkalisolution to produce a first product. The method includes washing the first product with a fourth predetermined amount of an alcohol. The method includes drying the first product for a first predetermined amount of time (10-12 hrs) at a first predetermined temperature. The method includes grinding the dried first product 5 into a powder. The method includes calcining the powder to produce one or more ceramic pellets, by simultaneous application of a pressure less sintering. The method includes grinding the one or more ceramic pellets for a second predetermined amount of time.
[0016] In an aspect of the present subject matter, the method further includes 10 polishing the one or more ceramic pellets for the second predetermined amountof time, and performing a thermal etching at a second predetermined temperature for a third predetermined amount of time upon grinding.
[0017] In an aspect of the present subject matter, the first predetermined amount of the first precursor solution and the second predetermined amount of deionizedwater are stirred magnetically for a predetermined amount of time for producing the first solution.
[0018] In an aspect of the present subject matter, the first product is collected after waiting for a fourth predetermined amount of time prior to washing and a centrifuge.
[0019] In an aspect of the present subject matter, the third predetermined amount of alkali solution is mixed with the first solution to change a pH value of the first solution from a first value to a second value, further wherein the second value ranges between 8.5-11.5.
[0020] In an aspect of the present subject matter, the pressure less sintering is performed at a third predetermined temperature.
[0021] In an aspect of the present subject matter, the first predetermined amount of a first precursor solution ranges between 30 mMol-60 mMol, the second predetermined amount of deionized water ranges between 100 -150 ml, the thirdpredetermined amount of alkali solution ranges between 100-150 ml, the fourth predetermined amount of an alcohol ranges between 150-200 ml.
[0022] In an aspect of the present subject matter, the predetermined amount of time ranges between 15 minutes to 30 minutes, the first predetermined amountof time ranges between 10 hours to 12 hours, the second predetermined amount of time ranges between 100 minutes to 130 minutes, the third predetermined amount of time ranges between 10 minutes to 30 minutes, and the fourth predetermined amount of time ranges between 30 minutes to 45 minutes.
[0023] In an aspect of the present subject matter, the first predetermined 10 temperature ranges between 100 °C - 120 °C, the second predeterminedtemperature ranges between 950 °C-1050 °C, the third predetermined temperature ranges between 1050 °C -1250 °C.
[0024] In an aspect of the present subject matter, the Y2O3-doped-zirconia ceramics comprises a density of at least 99.5 %, and a high hardness valueranging between 14 GPa-15 GPa.
[0025] Various objects, features, aspects, and advantages of the inventive subject matter will become more apparent from the following detailed description of preferred embodiments, along with the accompanying drawing figures in which like numerals represent like components.BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The illustrated embodiments of the subject matter will be best understood by reference to the drawings, wherein like parts are designated by like numerals throughout. The following description is intended only by way of example, andsimply illustrates certain selected embodiments of devices, systems, and methods that are consistent with the subject matter as claimed herein, wherein:
[0027] Fig 1a illustrates a graphical representation 100a depicting an XRD pattern of 1.5 mol.% Yttria-doped zirconia powder, in accordance with an existing prior-art; and
[0028] Fig. 1b illustrates a graphical representation depicting the XRD pattern of 1.5 mol.% Yttria-doped zirconia ceramics, in accordance with an embodiment of the present invention;
[0029] Fig. 2 illustrates a schematic block diagram depicting a method for a 5 preparing high surface area Y2O3-doped-zirconia nanoparticles, in accordancewith an embodiment of the present subject matter;
[0030] Fig. 3 illustrates an operational flow diagram depicting a process for a preparing high surface area Y2O3-doped-zirconia nanoparticles, in accordance with an embodiment of the present subject matter
[0031] Fig 4 illustrates a graphical representation depicting Raman spectra of 1.5 mol.% Yttria-doped zirconia ceramics, in accordance with an embodiment of the present invention;
[0032] Fig 5 illustrates an image depicting FESEM micrograph of fracture surface of 1.5YSZ sintered pellet, in accordance with an embodiment of the presentinvention; and
[0033] Fig. 6 illustrates an image depicting FESEM micrograph of indent at 1 kgf sintered pellet showing ~14 GPa hardness value, in accordance with an embodiment of the present invention.DETAILED DESCRIPTION
[0034] The following is a detailed description of embodiments of the disclosure depicted in the accompanying drawings. The embodiments are in such detail as to clearly communicate the disclosure. However, the amount of detail offered is not intended to limit the anticipated variations of embodiments; on the contrary, theintention is to cover all modifications, equivalents, and alternatives falling within the scope of the present disclosure as defined by the appended claims.
[0035] As used in the description herein and throughout the claims that follow, the meaning of "a," "an," and "the" includes plural reference unless the context clearlydictates otherwise. Also, as used in the description herein, the meaning of "in" includes "in" and "on" unless the context clearly dictates otherwise.
[0036] Fig 1a illustrates a graphical representation 100a depicting an X-Ray Diffraction (XRD) pattern of 1.5 mol.% Yttria-doped zirconia powder, inaccordance with an existing prior-art.
[0037] Fig. 1b illustrates a graphical representation depicting the XRD pattern of 1.5 mol.% Yttria-doped zirconia ceramics showing full tetragonal phase, in accordance with an embodiment of the present invention.
[0038] Fig. 2 illustrates a schematic block diagram depicting a method 200 for a 10 preparing high surface area Y2O3-doped-zirconia nanoparticles, in accordance withan embodiment of the present subject matter.
[0039] At block 202, the method 200 includes dissolving a first predetermined amount of a first precursor solution with a second predetermined amount of deionized water to produce a first solution.
[0040] At block 204, the method 200 includes mixing the first solution into a third predetermined amount of alkali solution to produce a first product.
[0041] At block 206, the method 200 includes washing the first product with a fourth predetermined amount of an alcohol.
[0042] At block 208, the method 200 includes drying the first product for a first 20 predetermined amount of time at a first predetermined temperature.
[0043] At block 210, the method 200 includes grinding the dried first product into a powder.
[0044] At block 212, the method 200 includes calcining the powder to produce one or more ceramic pellets, by simultaneous application of a pressure less sintering.
[0045] At block 214, the method 200 includes grinding the one or more ceramic pellets for a second predetermined amount of time.
[0046] Fig. 3 illustrates an operational flow diagram depicting a process 300 for a preparing high surface area Y2O3-doped-zirconia nanoparticles, in accordance withan embodiment of the present subject matter. In a preferred embodiment of the present subject matter, the high surface area may range between 100-160 m2 / g. Among a number of engineering ceramic products, Yttria Stabilized Zirconia (YSZ) compositions score high in terms of a range of applications, lifetime of 5 devices / instruments, performances and properties, and the like. The process 300 may be an industrially scalable synthesis process for obtaining high surface area the ultrafine phase-pure tetragonal and cubic yttria doped-zirconia (YSZ) nanoparticles. The high surface area doped-zirconia nanoparticles may be obtained without the addition of any surfactant and / or ligands and without any compromise 10 on the properties. The high surface area doped-zirconia nanoparticles may confirm a stabilization of tetragonal phase with a minimum / optimized doping, a phase retention at high temperature (>1400 °C) and a near-theoretical (>99.5%) density at low sintering temperature (<1150 °C). The process 300 may ensure a specific improvement over an existing YSZ compositions in the way that the tetragonal 15 phase may be stabilized at a much lower doping of yttria (<2 mol.%).
[0047] Furthermore, the high surface area doped-zirconia nanoparticles may also include a phase pure tetragonality and cubicity for both low and high doped YSZ compositions, and the high surface area and ultrafine size refinement in the nanoscale to ensure a grain size of the sintered ceramics within 100 nm, or the like.
[0048] Both powders and ceramics may be free from a monoclinic phase and ensure high temperature phase retention capacities without a phase segregation / separation. The synthesized powders may disclose an excellent sinterability as a near-theoretically dense (>99.5%) ceramic may be obtained at a temperature as low as 1100 °C (via pressure less, and conventional sintering). The synthesized ceramic 25 may also include a remarkably high hardness value (14-15 GPa).
[0049] At step 302, the process 300 may include dissolving a first predetermined amount of a first precursor solution with a second predetermined amount of deionized water to produce a first solution. The first precursor solution may be made up of chloride, nitrate and sulphate precursors of zirconium and yttrium. The first 30 predetermined amount of the first precursor solution and the second predeterminedamount of deionized water may be stirred magnetically for a predetermined amount of time for producing the first solution in glass beakers. The predetermined amount of time may range between 15 minutes to 30 minutes. In a preferred embodiment, the first predetermined amount of the first precursor solution may range between a 5 stoichiometric amount of 30 mMol-60 mMol and the second predetermined amount of deionized water may range between 100 ml-150 ml.
[0050] At step 304, the process 300 may include mixing the first solution into a third predetermined amount of alkali solution to produce a first product. The alkali solution may be ammonia solution. In a preferred embodiment, the thirdpredetermined amount of alkali solution may range between 100 ml-150ml.
[0051] The first product may be collected after waiting for a fourth predetermined amount of time prior to washing and a centrifuge for precipitating the first product. The fourth predetermined amount of time may range between 30 minutes to 45 minutes. The third predetermined amount of alkali solution may be mixed with thefirst solution to change a pH value of the first solution from a first value to a second value. In a preferred embodiment, the second value may range between 8.5-11.5.
[0052] At step 306, the process 300 may include washing the first product with a fourth predetermined amount of an alcohol. In a preferred embodiment, fourth predetermined amount of the alcohol may range between 150 ml-200 ml. Examplesof the alcohol may include, but are not limited to, ethanol and / or butanol, propanol.
[0053] At step 308, the process 300 may include drying the first product for a first predetermined amount of time at a first predetermined temperature. The first predetermined amount of time may range between 10 hours-12 hours. In a preferred embodiment, the first predetermined temperature may range between 100 °C - 12025 °C.
[0054] At step 310, the process 300 may include grinding the dried first product into a powder.
[0055] At step 312, the process 300 may include calcining the powder to produce one or more ceramic pellets, by simultaneous application of a pressure lesssintering. The pressure less sintering may be performed at a third predetermined temperature. In a preferred embodiment, the third predetermined temperature may range between 1050 °C -1250 °C. A range of temperature of calcination may be 500-700 °C and an environment of calcination is air. The calcination may be done 5 for obtaining the crystalline and phase pure tetragonal and cubic Y2O3-doped-zirconia nanoparticles. After obtaining the crystalline powder, the sintering may be performed on the green pellets (cylindrical pellets with a diameter of 10 mm made by compacting the calcined nanopowders via uniaxial pressing at 375 MPa) by conventional sintering in muffle furnace at 1050 °C-1250 °C temperature.
[0056] At step 314, the process 300 may include grinding the one or more ceramic pellets for a second predetermined amount of time. In a preferred embodiment, the second predetermined amount of time may range between 100 minutes to 130 minutes.
[0057] At step 316, the process 300 may include polishing the one or more ceramicpellets for the second predetermined amount of time.
[0058] At step 318, the process 300 may include performing a thermal etching at a second predetermined temperature for a third predetermined amount of time upon grinding. In a preferred embodiment, the second predetermined temperature may range between 950 °C-1050 °C. Further, in a preferred embodiment, the third predetermined amount of time may range between 10 minutes to 30 minutes.
[0059] In a preferred embodiment of the present subject, the pure doped zirconia ceramic nanopowders with fully stabilized tetragonal (< 2 mol.% Yttria doping) and cubic zirconia with refined grain size and free from monoclinic phase having high temperature phase retention is disclosed. Phase purity of nanoparticles / ceramics may be checked by X-ray diffraction using 2 degree / min. scan rate and step size may be fixed at 0.02 degree. Raman analysis using 514 nm excitation wavelength may be performed. Microstructural analyses of the polished ceramics may be done using scanning electron microscopy. The Vickers micro-indentation technique may be employed to determine the hardness (H) of the sintered ceramics. A 1 kgf loadand a dwell time of 10 seconds were applied.
[0060] Fig 4 illustrates a graphical representation 400 depicting aRaman spectra of 1.5 mol.% Yttria-doped zirconia ceramics showing full tetragonal phase, in accordance with an embodiment of the present invention.
[0061] Fig 5 illustrates an image 500 depicting a FESEM micrograph of fracture 5 surface of 1.5YSZ sintered pellet showing the grains size < 100 nm, in accordancewith an embodiment of the present invention.
[0062] Fig. 6 illustrates an image 600 depicting FESEM micrograph of indent at 1 kgf sintered pellet showing 14 GPa hardness value, in accordance with an embodiment of the present invention.
[0063] While the detailed description describes various embodiments of the invention, other and further embodiments of the invention may be devised without departing from the basic scope thereof. The scope of the invention is determined by the claims that follow. The invention is not limited to the described embodiments, versions, or examples, which are included to enable a person having ordinary skill 15 in the art to make and use the invention when combined with information and knowledge available to the person having ordinary skill in the art.
Claims
1. A method for preparing high surface area Y2O3-doped-zirconia nanoparticles, the method comprising: dissolving a first predetermined amount of a first precursor solution 5 with a second predetermined amount of deionized water to produce a first solution; mixing the first solution into a third predetermined amount of alkali solution to produce a first product; washing the first product with a fourth predetermined amount of an alcohol; drying the first product for a first predetermined amount of time at a first predetermined temperature; grinding the dried first product into a powder; calcining the powder to produce one or more ceramic pellets, by simultaneous application of a pressure less sintering; and; grinding the one or more ceramic pellets for a second predetermined amount of time.
2. The method as claimed in claim 1, further comprising: polishing the one or more ceramic pellets for the second predetermined amount of time; and performing a thermal etching at a second predetermined temperature for a third predetermined amount of time upon grinding.
3. The method as claimed in claim 1, wherein the first predetermined amount of the first precursor solution and the second predetermined amount of deionized water are stirred magnetically for a predetermined amount of time for producing the first solution.
4. The method as claimed in claim 1, wherein the first product is collected after waiting for a fourth predetermined amount of time prior to washing and a centrifuge.
5. The method as claimed in claim 1, wherein the third predetermined amount of alkali solution is mixed with the first solution to change a pH value of the first solution from a first value to a second value, further wherein the second value ranges between 8.5-11.5.
6. The method as claimed in claim 1, wherein the pressure less sintering is performed at a third predetermined temperature.
7. The method as claimed in claim 1, wherein the first predetermined amount of a first precursor solution ranges between 30 mMol-60 mMol, the second predetermined amount of deionized water ranges between 100 ml-150 ml, the third predetermined amount of alkali solution ranges between 100 ml-150 ml, the fourth predetermined amount of an alcohol ranges between 150 ml-200 ml.
8. The method as claimed in claim 1-4, wherein the predetermined amount of time ranges between 15 minutes to 30 minutes, the first predetermined amount of time ranges between 10 hours to 12 hours, the second predetermined amount of time ranges between 100 minutes to 130 minutes, the third predetermined amount of time ranges between 10 minutes to 30 minutes, and the fourth predetermined amount of time ranges between 30 minutes to 45 minutes.
9. The method as claimed in claim 1 or 2, wherein the first predetermined temperature ranges between 100 °C - 120 °C, the second predetermined temperature ranges between 950 °C-1050 °C, the third predetermined temperature ranges between 1050 °C -1250 °C.
10. The method as claimed in claim 1 wherein the Y2O3-doped-zirconia ceramics comprises a density of at least 99.5 %, and a high hardness value ranging between 14 GPa-15 GPa.