Expandable polyolefin composition and method thereof
Reactor-produced propylene-based RACO or terpolymer polyolefins with high comonomer content, combined with blowing agents, enhance foam properties, addressing strength and compatibility issues in polyolefin foams, enabling diverse applications with reduced density and tailored cell structures.
Patent Information
- Application Number
- JP2020569126
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-06-14
- Filing Date
- 2019-06-14
- Publication Date
- 2024-10-28
- Estimated Expiration
- 2039-06-14
AI Technical Summary
Existing polyolefin foams lack improvements in strength, foamability, cell consistency, and temperature resistance without increasing manufacturing costs, and there is a need for compositions compatible with polyolefin recycle streams to reduce the carbon footprint.
Development of reactor-produced propylene-based random copolymer (RACO) or terpolymer polyolefins with high comonomer content, combined with blowing agents and optional nucleating agents, using gas phase polymerization processes to create foamed compositions with improved physical properties.
The foamed compositions exhibit increased flexibility, lower sealing temperatures, and better compatibility with other polyolefins, allowing for a wide range of applications with reduced density and tailored cell structures.
Smart Images

Figure 0007574082000006 
Figure 0007574082000007 
Figure 0007574082000008
Abstract
Description
[Technical field]
[0001] Prior Related Applications This application claims the benefit of U.S. Provisional Patent Application No. 62 / 685,133, filed June 14, 2018, filed under the Patent Cooperation Treaty, which is hereby incorporated by reference in its entirety for all purposes. Field of the Disclosure
[0002] The present disclosure relates to polyolefin compositions, particularly foamed or expanded, reactor-made polyolefin compositions. [Background technology]
[0003] Polyolefins are frequently used in commercial plastics applications due to their outstanding performance and cost characteristics. These polymers can be amorphous or highly crystalline and can behave as thermoplastics, thermoplastic elastomers or thermosets. Polyolefins are therefore easily designed and modified for selected applications by properly selecting their molecular structure and molecular weight distribution(s) to obtain the appropriate balance of stiffness, impact resistance and processability in the extrusion process.
[0004] One area of growing interest in polyolefins is in the formation of foams, which have become a very important part of the polymer industry due to their beneficial properties, including light weight, excellent cushioning, thermal insulation, and resistance to water and chemicals.
[0005] Polyolefin foams are a relatively recent addition to the range of polymer foam materials, first marketed in the early 60's, but are used in almost every industry. Areas of application include packaging, sports and leisure, toys, insulation, automotive, military, aviation, buoyancy, cushioning, etc. This wide range of applications is due to the wide range of physical properties of olefins, ranging from rigid and tough to soft and elastic. Rigid (not brittle) foams are obtained, for example, using high density polyethylene as the base polymer, while softer materials are obtained using ethylene copolymers such as ethylene vinyl acetate (EVA). This ability to change the foam properties by changing the polymer is similar to that seen with polyurethane foams, but the technology is very different, as almost all polyurethane foams result from a liquid technology using in situ polymerization and foaming, while polyolefin foams are produced starting from a base thermoplastic polymer.
[0006] With advanced developments in polymerization techniques, polyolefins are rapidly expanding in foam applications through various chemical and physical forms including crosslinked polyolefins, copolymers, high melt strength (branched) polyolefins and polyolefin blends. However, despite the advances made in foamed polyolefins, there is a continuing need for the development of improved foamable compositions with increased strength, foamability, cell consistency, dimensional stability and temperature resistance without adding cost to the manufacturing process. Ideally, new foamable compositions would also reduce the carbon footprint by being compatible with polyolefin recycle streams. Summary of the Invention [Means for solving the problem]
[0007] The present disclosure provides novel foamed polyolefin compositions with improved physical properties. In particular, the foamable compositions include reactor-made propylene-based random copolymers (RACOs) or terpolymer polyolefins with high comonomer content (greater than about 5 wt. % comonomer) that are foamed by chemical or physical foaming agents. The foamed reactor-made propylene-based random copolymers (RACOs) or terpolymer polyolefins can be used to manufacture a variety of articles.
[0008] Propylene-based RACOs and terpolymers with high comonomer content have improved properties for sealing applications due to their low seal initiation temperature, optical properties, good processability, and lack of tack. Reactor-made RACOs and terpolymers with high comonomer content were selected as the propylene-based polyolefins to be foamed because of their improved properties compared to conventional propylene-based RACO polyolefins. The gas-phase reactor polymerization process allows the incorporation of higher comonomer contents (e.g., ethylene and / or butene) that provide improved physical properties such as increased flexibility, high gloss, lower seal temperature, and improved compatibility with other polyolefins compared to conventional propylene-based RACOs and terpolymers.
[0009] The reactor-made propylene-based RACO or terpolymer base resin for the foam composition described herein is composed of A) a propylene-based RACO or terpolymer having a high comonomer content, B) a foaming agent, and C) optionally one or more nucleating agents. Any reactor-made propylene-based random copolymer or terpolymer polyolefin having a high comonomer content of greater than about 5 wt% can be used as component A. Alternatively, the reactor-made propylene-based random copolymer or terpolymer polyolefin selected can have a high comonomer content of greater than about 8 wt%, or greater than about 13 wt%. These higher comonomer polyolefins (about 8 wt% or greater) can be selected because of improved physical properties such as increased flexibility, high gloss, lower sealing temperature, and improved compatibility with other polyolefins compared to comonomer polyolefins with less than 5 wt% comonomer. Exemplary comonomers include ethylene and C4-C8 alpha-olefins.
[0010] In some embodiments, the reactor-made polyolefin in the foam composition is a random copolymer of propylene and ethylene having a high ethylene content. In other embodiments, the reactor-made polyolefin is a terpolymer having ethylene, propylene and butene comonomers. In some embodiments, the reactor-made polyolefin is a blend of random copolymers and terpolymers. In still other embodiments, the reactor-made propylene-based RACO or terpolymer is prepared using a multi-stage gas phase polymerization process.
[0011] To obtain the foamed polyolefin compositions and articles made from the foamed polyolefin compositions of the present disclosure, the selected reactor-produced propylene-based RACO or terpolymer is foamed using processes and foaming agents known in the art, including both physical and chemical types.
[0012] Any physical blowing agent (PBA), also known as a physical foaming agent, can be used to foam the reactor-made propylene-based RACO or terpolymer-based resin, including, but not limited to, highly pressurized CO, N, air, propane, isobutane, butane, CFC derivatives, and / or argon.
[0013] The PBAs can be metered into the base resin melt during foam extrusion or foam injection molding. The PBAs can be injected or introduced into the molten polymer mass in the extruder away from the point where the solid polymer is fed, where the polymer is found to be molten and homogeneous. If pressurized PBAs are injected directly into the melt, they will expand when returning to atmospheric pressure, forming fine bubbles within the polymer.
[0014] To promote cell formation when using PBA as a foaming agent, a masterbatch containing at least one nucleating agent can be combined with the reactor-made propylene-based RACO or terpolymer. Nucleating agents are useful for polypropylene-based resins because they can provide enhanced properties, improved molding or extrusion productivity, and increased clarity to the reactor-made propylene-based RACO or terpolymer. To ensure proper dispersion of the nucleating agent, the masterbatch uses a carrier resin that is compatible with at least one polymer or monomer in the polyolefin, such as polyethylene or polypropylene. For example, a polyethylene carrier resin will be compatible with the comonomers of the RACO or terpolymer. This allows for consistent cell morphology with controlled size distribution throughout the extruded and foamed reactor-made propylene-based RACO or terpolymer.
[0015] In another embodiment, reactor-made propylene-based RACO or terpolymer-based resin is foamed using at least one chemical foaming agent (CFA). The CFA produces / releases gas when decomposed, imparting cellular structure to the material. The CFA gas remains dissolved in the polymer melt while the melt is under pressure. When the melt is injected or extruded into a mold, the pressure is released, allowing the gas to expand the polymer.
[0016] Similar to a nucleating agent, a masterbatch can be used to ensure proper dispersion of the CFA(s) and the carrier resin in the masterbatch is compatible with at least one monomer in the reactor-made propylene-based RACO or terpolymer-based resin.
[0017] The CFA(s) may be endothermic or exothermic. Endothermic is desirable because CFAs tend to be more stable in blends and do not decompose or produce gas until exposed to heat in the extrusion process. Additionally, the CFA(s) may also act as nucleating agents to promote bubble formation in reactor-made propylene-based RACOs or terpolymer-based resins. Nucleating chemical foaming agents are useful for resins with polypropylene components because the nucleating agents can provide enhanced properties, improved molding or extrusion productivity, and increased clarity to reactor-made propylene-based RACOs or terpolymers. However, nucleating ability is not a requirement for CFAs.
[0018] The masterbatch used to distribute the CFA includes at least one chemical foaming agent, but can also have a mixture of chemical foaming agents at various concentrations. In some embodiments, the masterbatch can have CFA(s) and an optional nucleating agent separate from the CFA(s). Alternatively, a mixture of both nucleating and non-nucleating chemical foaming agents can be used in the masterbatch to fine-tune the resulting foam characteristics, such as cell size, cell distribution, and cell stability, for a selected application. In yet another option, multiple masterbatches can be combined to provide the desired CFA(s) and optional nucleating agent.
[0019] The articles formed using the foam compositions described herein are not limited to any particular architecture. The foam can be extruded in-line during processing of many shapes, including sheets, strands, tubes, containers, or specialized profiles specific to a particular application, eliminating the need and additional expense for a second processing step. Alternatively, the foam can be injection molded. In yet another option, the foam can be layered or combined with other polyolefin resins, if required for a particular application. For example, foam articles made from reactor-made RACO or terpolymers can be used as a central layer with one or more outer layers made of solid polyolefin. Thus, the physical properties of polyolefins, the ability to tailor the foam's cell structure using mixtures of CFA, PBA, and optional nucleating agents, and the wide range of architectures available combine synergistically to allow for a wide range of applications. In either case, the gas should be fully dissolved in the polymer melt and maintained under appropriate pressure until released from the die.
[0020] The present disclosure includes any of the following embodiments in any combination or combinations.
[0021] A foamable composition (MFR values are measured according to ASTM D 1238L) comprising a propylene-based polyolefin having a melt flow rate between 2 and 15 g / 10 min, and a masterbatch having at least one chemical foaming agent. The propylene-based polyolefin has a semi-crystalline propylene copolymer composition having: (A) a propylene / ethylene copolymer comprising 1-7 wt. % ethylene, a copolymer of propylene and one or more C4-C8 alpha-olefins comprising 2-10 wt. % C4-C8 alpha-olefins, or a terpolymer of propylene and ethylene and one or more C4-C8 alpha-olefins comprising 0.5-4.5 wt. % ethylene and 2-6 wt. % C4-C8 alpha-olefins, provided that the ethylene and C4-C8 alpha-olefins in the terpolymer are not mixed. and (B) 20 to 80 wt. % of one or more propylene-based components selected from the group consisting of copolymers of propylene and one or more C4 to C8 alpha-olefins containing more than 10 wt. % to 30 wt. % of C4 to C8 alpha-olefins, or terpolymers of propylene and ethylene and one or more C4 to C8 alpha-olefins containing 1 to 7 wt. % of ethylene and 6 to 15 wt. % of C4 to C8 alpha-olefins. A precursor composition containing the same components (A) and (B) in the above proportions has an MFR value (MFR(1)) of 0.3 to 5 g / 10 min, and an MFR value (MFR(2)) obtained by subjecting the precursor composition to precursor composition decomposition is 2 to 15 g / 10 min, the ratio of MFR(2) to MFR(1) being 2:20.
[0022] A foamed polyolefin composition comprising a reactor-produced propylene-based RACO having a melt flow rate between 2 and 15 g / 10 min (MFR values are measured according to ASTM D 1238L). A propylene-based polyolefin having a crystalline propylene copolymer composition having: (A) a propylene / ethylene copolymer comprising 1-7 wt% ethylene, a copolymer of propylene and one or more C4-C8 alpha-olefins comprising 2-15 wt% C4-C8 alpha-olefins, or a terpolymer of propylene and ethylene and one or more C4-C8 alpha-olefins comprising 0.5-4.5 wt% ethylene and 2-6 wt% C4-C8 alpha-olefins, provided that the ratio of ethylene and C4-C8 alpha-olefins in the terpolymer is 0.5-4.5 wt%. (B) 0 to 80 wt.% of one or more propylene-based components selected from the group consisting of copolymers of propylene and one or more C4 to C8 alpha-olefins containing more than 8 wt.% to 30 wt.% of C4 to C8 alpha-olefins, and terpolymers of propylene and ethylene and one or more C4 to C8 alpha-olefins containing 1 to 7 wt.% of ethylene and 6 to 18 wt.% of C4 to C8 alpha-olefins.
[0023] A foamed polyolefin composition comprising a reactor-produced propylene-based RACO having a melt flow rate between 0.3 and 15 g / 10 min, the melt flow rate value being measured according to ASTM D 1238. The RACO may be a crystalline propylene / ethylene random copolymer having about 4.5 wt% to about 8 wt% ethylene and about 92 wt% to about 95.5 wt% propylene.
[0024] A foamed polyolefin composition comprising a reactor-produced propylene-based RACO having a melt flow rate between 0.3 and 15 g / 10 min (melt flow rate values are measured according to ASTM D 1238). The RACO may be a crystalline RACO having: (A) 20-60 wt% copolymer of propylene and ethylene, the ethylene content being about 1 wt% to about 5 wt% ethylene, and (B) 40-80 wt% terpolymer of propylene with ethylene and C4-C8 α-olefins, the ethylene content being about 1 wt% to about 5 wt% and the C4-C8 α-olefin content being about 7 wt% to 12 wt%. The total ethylene content in the RACO is between about 1 wt% to about 5 wt%, and the total C4-C8 α-olefin content in the RACO is between about 2.8 wt% to about 9.6 wt%.
[0025] Any of the above foam compositions were foamed using either a chemical foaming agent (CFA) or a physical foaming agent (PBA).
[0026] In any of the above foaming compositions, at least one masterbatch having at least one chemical foaming agent is added to a reactor-made propylene-based RACO or terpolymer resin having a high comonomer content prior to melting, and the carrier resin for the masterbatch is compatible with at least one polymer or monomer in the RACO or terpolymer resin.
[0027] In any of the above foam compositions, the chemical foaming agent may be an endothermic or foaming agent and / or may function as a nucleating agent.
[0028] In any of the above foam compositions, at least one masterbatch having at least one chemical foaming agent and optionally at least one nucleating agent is added to the RACO or terpolymer resin prior to melting.
[0029] In any of the above foam compositions, a masterbatch containing a physical blowing agent and a nucleating agent is used to generate the foam composition.
[0030] In any of the above foam compositions, the total amount of masterbatches combined in the foam composition is less than 5 wt% of the final composition, alternatively from 0.25 to 3 wt% of the final composition.
[0031] In either the reactor-produced propylene-based RACO or terpolymer resins described above, the C4 to C8 α-olefin may be 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene or 1-octene.
[0032] A method of producing any of the above foamable polyolefin compositions using a chemical foaming agent, comprising dry blending a reactor-produced propylene-based RACO or terpolymer resin with a masterbatch(s), melting the composition, and extruding the composition through a die, where the chemical foaming agent decomposes to release a gas, and the released gas is used to form one or more closed cells in the molten RACO or terpolymer. Multiple chemical foaming agents can be used in this method, including the use of a nucleating agent that also acts as a chemical foaming agent to release gas during the extrusion step. The extrusion step can produce a foamed sheet, strand, tube, container, or other extruded article.
[0033] A method of producing any of the above foamable polyolefin compositions using dry blending a reactor-made propylene-based RACO or terpolymer resin with a masterbatch(s), melting the composition, and extruding the composition through a die, wherein the chemical foaming agent decomposes, liberating a gas, and the liberated gas is used to form one or more closed cells in the molten reactor-made propylene-based RACO or terpolymer. The density of the foamed reactor-made propylene-based RACO or terpolymer can be up to 70% lower than a non-foamed reactor-made propylene-based RACO or terpolymer having the same composition, and the average cell size range in the foamed reactor-made propylene-based RACO or terpolymer is between 25-40 microns.
[0034] A method of producing any of the above foamable compositions comprising melting the foamable composition, injecting one or more physical blowing agents into the polymer melt in an extruder, and extruding the composition through a die. The extruding step can produce a foamed sheet, strand, tube, container, or other extruded article. The density of the foamed reactor-made propylene-based RACO or terpolymer can be up to 50% lower than a non-foamed reactor-made propylene-based RACO or terpolymer having the same composition, and the average cell size range in the foamed reactor-made propylene-based RACO or terpolymer is between 20-40 microns.
[0035] A method of producing any of the above foamable compositions comprising dry blending a reactor-made propylene-based RACO or terpolymer resin with a masterbatch containing at least one nucleating agent, melting the foamable composition, injecting one or more physical blowing agents into the polymer melt in an extruder, and extruding the composition through a die. The extrusion step can produce a foamed sheet, strand, tube, container, or other extruded article. The density of the foamed reactor-made propylene-based RACO or terpolymer can be up to 50% lower than a non-foamed reactor-made propylene-based RACO or terpolymer having the same composition, and the average cell size range in the foamed reactor-made propylene-based RACO or terpolymer is between 20-40 microns.
[0036] Any of the above methods, wherein the density of the propylene-based RACO or terpolymer made in the foaming reactor is about 10 to about 50% lower than the density of the propylene-based RACO or terpolymer made in a non-foaming reactor having the same composition. Alternatively, the density of the propylene-based RACO or terpolymer made in the foaming reactor is about 10 to about 25% lower than the density of the propylene-based RACO or terpolymer made in a non-foaming reactor having the same composition.
[0037] Any of the above processes, wherein the average cell size range in the propylene-based RACO or terpolymer produced in the foaming reactor is from about 10 to about 60 microns, from about 10 to about 25 microns, or from about 25 to about 55 microns, or from about 45 to about 60 microns.
[0038] Any of the above methods, wherein the physical blowing agent added during the extrusion step is injected at about 100-3,000 mL / min, or about 400-1,500 mL / min, or about 500-800 mL / min, or about 600 mL / min, or about 1,300 mL / min.
[0039] An article comprising any of the foam compositions described above, or produced from any of the methods described above. [Brief description of the drawings]
[0040] [Figure 1] FIG. 1 shows a schematic of the Catalloy process. Image courtesy of LyondellBasell (Houston, TX). [Diagram 2] FIG. 1 shows exemplary extrusion process conditions for a monolayer foamed sheet formed from the presently disclosed novel composition of RACO or terpolymer and masterbatch having endothermic chemical nucleation and foaming agents. [Diagram 3] Figure 3A shows the cell size distribution for Adsyl 5C30F foam strands, and Figure 3B shows a histogram of the cell size distribution for Adsyl 5C30F foam strands. Adsyl 5C30F is a commercially available product from LyondellBasell (Houston, TX). [Figure 4] FIG. 1 shows the trend in cell count and cell size range for foam sheet samples K17218 and K17219 prepared using Adsyl 7416XCP, a commercially available product from LyondellBasell (Houston, TX). [Diagram 5]FIG. 1 shows cell size distribution for several RACO and terpolymer foam monolayer sheets. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0041] definition As used herein, the term "copolymer" refers to a polyolefin that contains two types of alpha-olefin monomer units. It does not refer to an alloy of two homopolymers.
[0042] As used herein, the term "comonomer" or "comonomers" refers to one or more types of monomers that are minor components in a polymer chain. As one example, ethylene is a comonomer in a random copolymer of propylene and ethylene, and ethylene and butene are comonomers in a terpolymer of propylene with ethylene and butene.
[0043] As used herein, the term "random copolymer" or "RACO" refers to a polymer that contains two types of monomer units such that the comonomer units are randomly distributed throughout the polymer chain.
[0044] As used herein, the term "terpolymer" refers to a polymer that contains three types of monomer units, such that the two types of comonomer units are randomly distributed throughout the polymer chain.
[0045] As used herein, the term "α-olefin" or "alpha-olefin" refers to an olefin of the general formula CH2=CH-R, where R is a linear or branched alkyl containing 1 to 10 carbon atoms. The α-olefin may be selected, for example, from 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, and the like.
[0046] The term "reactor made" is used to refer to polyolefins produced in a reactor system.
[0047] As used herein, the term "base resin" refers to a reactor-made propylene-based RACO or terpolymer resin that has been foamed with at least one chemical foaming agent or at least one physical foaming agent and has a high comonomer content. The phrase "high comonomer content" means that monomers other than propylene are present in an amount greater than about 5 wt%.
[0048] A "foam" is a continuous three-dimensional network or cellular structure of a solid or liquid phase that surrounds a gas phase dispersed therein. In polymer foams such as those disclosed herein, the solid phase is a polymer resin that forms the cell walls in a continuous "cell phase." The "cell fraction" of a foam is the amount of foam that is in the cell or gas phase.
[0049] The terms "chemical foaming agent" and "chemical blowing agent" are used interchangeably to refer to chemical compounds that undergo a decomposition reaction during polymer processing, resulting in the production and release of gas. These compounds may be inorganic or organic, and the decomposition may be endothermic (requires energy to cause the decomposition) or exothermic (releases energy during decomposition). The energy required to cause the decomposition may be supplied during the processing of the polymer.
[0050] In some embodiments, at least one chemical foaming agent may also act as a nucleating agent and may be referred to as a "nucleating chemical foaming agent."
[0051] "Physical blowing agents" are distinguishable from chemical foaming agents because they undergo a change of state during processing to produce a gas. Compressed liquefied gas can be utilized as a physical blowing agent, which is injected into a polymer melt under high pressure. When the pressure is released, the gas becomes less soluble in the melt, resulting in the formation of gas bubbles.
[0052] As used herein, the term "masterbatch" refers to a premixed composition having one or more solid or liquid additives used to impart other properties to the base resin. The masterbatch used in the present foaming composition can include at least one chemical foaming agent or at least one nucleating agent or both, as well as additives that do not interfere with the foaming ability of the base resin. Because the masterbatch is already a premixed composition, its use mitigates the problem of poor dispersion of the chemical foaming agent(s) and / or nucleating agent(s).
[0053] The terms "Melt Flow Rate" and "MFR" are used interchangeably to refer to a measure of the ability of a melt of a base resin to flow under pressure. Unless otherwise specified, melt flow rate is determined by ASTM D 1238L ("Standard Test Method for Melt Flow Rates of Thermoplastics by Extrusion Plastometer"). ASTM D 1238L measures melt flow rate at 230°C and a weight of 2.16 kg. "Melt flow range" is the range of melt flow rates.
[0054] All concentrations herein are in weight percent ("wt%") unless otherwise specified.
[0055] When used in the claims or this specification in conjunction with the term "comprising," the use of the word "a" or "an" means one or more than one, unless the context indicates otherwise.
[0056] The term "about" means the stated value plus or minus a margin of measurement error, or, if the method of measurement is not given, plus or minus 10%.
[0057] Use of the term "or" in the claims is used to mean "and / or" unless expressly indicated to refer to alternatives only or where the alternatives are mutually exclusive.
[0058] The terms "comprise," "have," "include," and "contain" (and variations thereof) are open-ended linking verbs which, when used in the claims, permit the addition of other elements.
[0059] The phrase "consisting of" is closed and excludes all additional elements.
[0060] The phrase "consisting essentially of" excludes additional material elements, but permits the inclusion of non-material elements that do not materially alter the nature of the compositions and methods disclosed herein.
[0061] The following abbreviations are used herein: [Table 1] Description of the embodiments of the present disclosure
[0062] The present disclosure provides novel foamable compositions of reactor-made random polypropylene copolymers (RACOs) or terpolymer polyolefins with improved physical properties compared to currently available foamed polyolefins. The RACOs and terpolymers used herein have a high comonomer content of more than about 5 wt%, which allows these polyolefins to have a wide range of stiffness, melting temperature and other physical properties, which allows the resulting foams to be used for a wide variety of applications. For example, a particular foaming composition with a stiffer copolymer or terpolymer can be used in the automotive industry for wrapping spare tires, while a softer, less stiff copolymer or terpolymer can be foamed for use as a transport material or food packaging. Furthermore, foaming agents can be selected as needed to create voids in the foam to induce certain cell characteristics in the copolymer or terpolymer and further expand the range of applications. Articles produced from the foamable compositions are also described.
[0063] Any reactor-made random copolymer or terpolymer polyolefin having propylene monomer as a base, having a high comonomer content (greater than about 5 wt%), and having a final melt flow rate (MFR) between 0.1 and about 15 g / 10 min (per ASTM D 1238L) can be used with the methods described herein.
[0064] In one embodiment, the reactor-made propylene-based polyolefin may be a crystalline copolymer having: (A) a propylene / ethylene copolymer comprising 1-7% ethylene; a copolymer of propylene and one or more C4-C8 alpha-olefins comprising 2-10% C4-C8 alpha-olefins; a terpolymer of propylene and ethylene and one or more C4-C8 alpha-olefins comprising 0.5-4.5% ethylene and 2-6% C4-C8 alpha-olefins, provided that the ethylene and C4-C8 alpha-olefins in the terpolymer are not crystalline; (A) 20-80% by weight of one or more propylene-based components selected from the group consisting of copolymers of propylene and one or more C4-C8 alpha-olefins, containing more than 10% to 30% of C4-C8 alpha-olefins, terpolymers of propylene and one or more C4-C8 alpha-olefins, containing 1-7% of ethylene and 6-15% of C4-C8 alpha-olefins. The MFR value (MFR(1)) of a precursor composition containing the same components (A) and (B) in the above proportions is 0.3-5 g / 10 min, and the MFR value (MFR(2)) obtained by subjecting the precursor composition to precursor composition decomposition is 2-15 g / 10 min, the ratio of MFR(2) to MFR(1) being 2 to 20.
[0065] Alternatively, the reactor-made propylene-based polyolefin may be a crystalline copolymer having: (A) a propylene / ethylene copolymer containing 1-7% ethylene, a copolymer of propylene and one or more C4-C8 alpha-olefins containing 2-14% C4-C8 alpha-olefins, or a terpolymer of propylene and ethylene and one or more C4-C8 alpha-olefins containing 0.5-4.5% ethylene and 2-6% C4-C8 alpha-olefins, provided that the ethylene and C4-C8 alpha-olefins in the terpolymer are not crystalline. (B) 0-80% by weight of one or more propylene-based components selected from the group consisting of copolymers of propylene and one or more C4-C8 alpha-olefins containing more than 8% to 30% of C4-C8 alpha-olefins, or terpolymers of propylene and one or more C4-C8 alpha-olefins containing 1-7% of ethylene and 6-18% of C4-C8 alpha-olefins. The melt flow rate of the copolymers may be between 2.0 and 15.0 g / 10 min.
[0066] Alternatively, the reactor-produced propylene-based polyolefin may be a RACO having a crystalline propylene / ethylene random copolymer having about 4.5 wt% to about 8 wt% ethylene and about 92 wt% to about 95.5 wt% propylene. The melt flow rate of this copolymer may be between 0.3 and 15.0 g / 10 min.
[0067] In yet another alternative, the reactor-made propylene-based polyolefin may be a reactor-made propylene-based RACO having: (A) 20-60% copolymer of propylene and ethylene, with the ethylene content being about 1 wt% to about 5 wt% ethylene, and (B) 40-80% terpolymer of propylene with ethylene and C4-C8 α-olefins, with the ethylene content being about 1 wt% to about 5 wt% and the C4-C8 α-olefin content being about 7 wt% to 12 wt%. The total ethylene content in the RACO is between about 1 wt% to about 5 wt%, and the total C4-C8 α-olefin content in the RACO is between about 2.8 wt% to about 9.6 wt%. The melt flow rate of the copolymer may be between 0.3 and 15.0 g / 10 min.
[0068] All the random copolymers and terpolymers mentioned above are exemplary and show a wide variety of formulations that allow the wide use of reactor-made RACO and terpolymer polyolefin resins and foam extrudates in the present disclosure.In addition to the random copolymer and terpolymer formulations mentioned above, the polyolefins for the present composition can also include any of the formulations described in EP0674991, EP1025162, and US6395831, each of which is incorporated herein in its entirety for all purposes.Similarly, the polyolefins can also be prepared by any of the reactor processes described in EP0674991, EP1025162, and US6395831.
[0069] In further embodiments, the random copolymer or terpolymer is prepared using a multi-stage gas phase polymerization process. In some embodiments, the multi-stage gas phase polymerization process is the Catalloy process of LyondellBasell (Houston, TX). The Catalloy process, shown in FIG. 1, utilizes a unique combination of catalyst, two or three independent fluidized bed reactors, and multiple monomer capabilities to expand the performance of the resulting polyolefin by adding new functionality. The Catalloy process can produce random copolymers or terpolymers in each gas phase reactor, creating an alloy of copolymers and / or terpolymers in the reactor. This process allows for the incorporation of a higher amount of comonomer into a polyolefin containing two different comonomers in the same reactor compared to conventional polypropylene production processes. The high comonomer content and the presence of multiple comonomers leads to a new combination of thermal, physical, and optical properties for the resulting RACO or terpolymer. Advantages of using Catalloy produced copolymers and terpolymers include ease of processing, the ability to produce resins in a wide range of polymer compositions, and unique thermal properties, including, but not limited to, low seal initiation temperatures. Thus, Catalloy polymers commercially available from LyondellBasell (Houston, TX), including Adsyl products, can be used in the present compositions as base resins for foams.
[0070] To create a foamed cellular structure using either the reactor-produced propylene-based RACO or terpolymers, each base resin can be mixed with a chemical or physical foaming agent and an optional nucleating agent.
[0071] The reactor-made RACO or terpolymer-based resin can be combined with at least one chemical foaming agent (CFA). Chemical foaming agents acceptable for use in this disclosure generate gas in the resin via thermal decomposition or chemical reaction. In some embodiments, the CFA decomposes during the extrusion process to generate and release gas in the extruded polymer, causing the resin to foam. To ensure proper dispersion of the CFA, the CFA is in a masterbatch using a carrier resin that is compatible with at least one polymer or monomer in the polyolefin-based resin, such as ethylene or propylene. This allows the CFA to create a consistent bubble morphology with controlled size distribution throughout the extruded and foamed reactor-made propylene-based RACO or terpolymer resin.
[0072] Many CFAs are known in the art and / or commercially available. Exemplary organic CFAs include azo and diazo compounds (e.g., azodiacarbonamide), hexahydrophthalic acid and hydrazines, including their salts and anhydrides (e.g., sulfonylhydrazides or triazines), N-nitroso compounds, azides, sulfonylsemicarbazides, triazoles and tetrazoles, urea derivatives, guanidine derivatives, and esters. Exemplary inorganic CFAs include ammonium carbonate and alkali metal carbonates, such as sodium bicarbonate, and citric acid. CFAs can also include mixtures of acids and metals, mixtures of organic acids and inorganic carbonates, and mixtures of nitrites and ammonium salts.
[0073] At least one optional nucleating agent can also be combined with the CFA(s). In some embodiments, at least one CFA is present in the same masterbatch with the optional nucleating agent, or at least one CFA is present in a separate masterbatch, or at least one CFA acts as a nucleating agent. Nucleating CFAs are useful for enhancing properties, improving molding or extrusion productivity, and increasing clarity for many polyolefins. In a masterbatch having a nucleating agent and multiple CFAs, at least one CFA may be a nucleating agent. Alternatively, any or all CFAs used in the composition may be nucleating. Additionally, one or more of the CFAs in the masterbatch may be endothermic so that they do not decompose in the reactor-made propylene-based RACO or terpolymer resin until the extrusion process. This is because endothermic CFAs require heat to activate, and heat is provided by the extrusion process.
[0074] In another embodiment of the present disclosure, multiple masterbatches can be mixed with reactor-made propylene-based RACO or terpolymer resins to achieve the desired cell morphology of the resulting foam. The final concentration of the masterbatches in the foamed resin can be limited to 5% by weight of the foamed resin. Alternatively, the final concentration of the masterbatches in the foamed resin can be between 0.25-3 wt%.
[0075] The reactor-made propylene-based RACO or terpolymer resins have a wide range of physical properties, which when mixed with CFAs selected to achieve specific cell sizes, cell distributions and cell stability, lead to flexible formulations. This combination allows the composition to be fine-tuned to form foam structures with enhanced stability and performance properties. Thus, the resulting foams can then have a wide range of physical properties, density reduction, cell sizes, cell patterns and / or cell stability. This allows the foams to be used for a variety of applications, for example, in the automotive, transportation, and food packaging industries.
[0076] CFAs can be chosen to produce large cell sizes (above 150 microns in diameter) or small cell sizes (below 120-150 microns in diameter) and a wide or narrow distribution of cell sizes. In some applications, a narrow distribution of cell sizes is desirable. In some embodiments, the desired cell size is in the range of 25-55 microns, since these foams can be classified as fine-cell foams. However, the desired cell density will depend on the application of the foam. For example, low cell density foams are the most flexible and better for many applications such as thermal insulation and comfort (e.g., furniture and car seats), while high cell densities can be used for more rigid foams such as energy absorption applications, pipes, appliances, food and beverage containers, etc. The mechanical strength of polymeric foams can be proportional to the foam density, so the application of the foam will dictate the range of foam densities that will be refined.
[0077] In addition to cell size and density, the CFA may be selected to achieve a certain flexibility in the resulting foamed extrudate.
[0078] Alternatively, reactor made RACO or terpolymer based resins in molten form can be combined with a physical blowing agent such as CO2, N2, isobutane or CFC derivatives and foamed. The process conditions for the blowing agent are controlled to tailor the cell phase, cell size and other cell features of the resulting foam.
[0079] When using PBA, reactor-made RACO or terpolymer-based resins can be optionally combined with a masterbatch having at least one nucleating agent. The PBA and nucleating agent work synergistically to achieve desirable cell morphology, including both large cell sizes (above 150 microns in diameter) or small cell sizes (below 120-150 microns in diameter), and wide or narrow distribution of cell sizes. As mentioned above, the final concentration of the masterbatch in the foamed resin can be limited to 5% of the weight of the foamed resin. Alternatively, the final concentration of the masterbatch in the foamed resin can be between 0.25-3 wt%.
[0080] The foam compositions containing either the reactor made RACO or terpolymer-based resins disclosed herein can be used to form articles of various shapes and sizes.
[0081] The base resin compositions disclosed herein are exemplified with respect to the disclosure below, however, they are exemplary and the methods are broadly applicable to any reactor-made propylene-based RACO and terpolymer base resins with high comonomer content and chemical or physical blowing agents.
[0082] The following description illustrates various embodiments, is illustrative, and is intended not to unduly limit the scope of the appended claims. Those skilled in the art should recognize that many changes can be made in the specific embodiments disclosed without departing from the spirit and scope of the present disclosure and still obtain the same or similar results. In no way should the following be read to limit or define the scope of the appended claims.
[0083] Base Polymer: A series of commercially available Catalloy random copolymer and terpolymer resins with high comonomer content from LyondellBasell (Houston, TX) were extruded with foaming agents, foamed, and analyzed by the methods described below. The examples utilized resins from the Adsyl product line. These base polymer resins were chosen because they have a wide range of comonomer types and contents, which leads to a large number of potential applications. In addition, these resins have moderate melt elasticity and melt strength, which is desirable for foam production.
[0084] The Adsyl product line includes propylene-based terpolymers formed by polymerizing propylene with high ethylene and butene comonomer content. These polymers have excellent sealing properties, good optics, a wide operating window, and are suitable for metallization. They are also compatible with PE and PP. In addition, the Adsyl product line also has RACO copolymers with either high ethylene or high butene content.
[0085] Together, this selection of commercially available resins offers a wide range of thermal, physical and optical properties to study the applicability of the proposed method.
[0086] Chemical Foaming Agents: A series of commercially available masterbatches containing at least one chemical foaming agent were obtained in combination with propylene-based polymers. Masterbatch A (MB-A) contains an endothermic chemical nucleating and foaming agent used at a concentration of 1.5-2.25 wt%. The CFA in MB-A is also used to create bubbles in the medium density extrudate to reduce density and improve throughput. Masterbatch B (MB-B) contains an olefinic nucleating agent used at a concentration of 0.75-1.0 wt%. The CFA in MB-B is used to improve bubble distribution, size and uniformity in the extrusion process to produce chemical foams. Masterbatch C (MB-C) contains an endothermic / exothermic blended chemical foaming agent at a concentration of 1 wt%. The CFA in MB-C is used in both injection molding and extrusion applications to create bubbles in the medium density extrudate. Masterbatch D (MB-D) contains a chemical foaming agent at a concentration of 2.5 wt%. Masterbatch E (MB-E) contains a nucleating agent used at a concentration of 1 wt% and was combined with one of the other above masterbatches with CFA.
[0087] A masterbatch having at least one CFA was mixed with the resin prior to extrusion and foaming. While the use of one nucleating chemical foaming agent is sufficient to foam the selected base polymer, a mixture of chemical foaming agents may be desirable to fine-tune the properties of the foamed extrudate.
[0088] Unless otherwise noted, the selected masterbatch was dry blended with the base resin prior to the melt step.
[0089] CFA Foam Extrusion: Various sample compositions with CFA were prepared and extruded as foam strands for initial analysis. Without modification of the extrusion equipment or resin grade, the base polymer and masterbatch were dry blended and extruded. The foam strand samples were then analyzed for cell phase, cell size, and other cell features.
[0090] From the results of the foam strand characterization, certain sample compositions with CFA were extruded as sheets. For sheets, the base polymer and masterbatch were dry blended and extruded as a multi-layer sheet (mode 2) to produce a foam sheet that was approximately 40 mm thick. Certain foam sheet samples were subjected to further analysis for density, density reduction compared to the base polymer alone, cell size, and other cell features.
[0091] No modifications to the extrusion equipment or resin grade were required to produce the sample foam sheets. Figure 2 illustrates exemplary process conditions for the extrusion of foam sheets (in this case, a monolayer foam sheet sample using Masterbatch A). These conditions did not vary significantly for the different foam sheets. The dashed box in Figure 2 highlights barrel zone 2, which uses a higher temperature than barrel zones 1 and 3 to activate the chemical foaming agent.
[0092] Foam characterization: Morphological characterization of the cell structure of foamed Catalloy extrudates was determined by optical and scanning electron microscopy (SEM). Foam samples were cryomicrotomed in the direction perpendicular to the extrudate using a Leica MZ6 ultramicrotome with a diamond knife at -40°C. Thin cross sections were examined by optical microscopy (Olympus BX51 compound microscope) using both transmitted and cross-polarized light. Bulk cross sections were examined using a SEM (Hitachi S-3500N or SU8230) in high vacuum mode at an accelerating voltage of 5 kV. SEM images were acquired at the same low magnification (25x) to allow the entire extrudate cross section of each sample to be included in a single image. Prior to SEM imaging, bulk cross section specimens were coated with PT using a sputter coater (Emitech K550X) to eliminate charging from the SEM electron beam.
[0093] Image analysis was performed using Olympus Stream Essentials image software on SEM images in which air bubbles, shown as dark holes, were dispersed in a bright polymer matrix. For this type of air bubble morphology, the particle analysis function of the software was the most suitable means to measure the size and number of air bubbles in each foam cross section. To ensure accurate results, each SEM image was inspected and manually corrected using Adobe Photoshop software to enhance the contrast between the air bubbles and the solid phase prior to image analysis. The gray value threshold that distinguishes air bubbles from the solid phase in the image analysis was adjusted for each individual image to ensure the greatest number of air bubbles were counted. To ensure consistency, no further manual editing of image detection was performed after the automated image analysis by Stream Essentials software. The average air bubble size or radius, cumulative air bubble area distribution, and air bubble morphology (continuous or isolated) were determined from the images.
[0094] Density measurements were performed according to standard method tests established in ASTM D792-13 using water or alcohol displacement. Density reduction was calculated based on the density of the base polymer for each example without the addition of any foaming agent. CFA Foam Strand
[0095] Foamed strands of Adsyl 5C30F were prepared using CFA and analyzed for maximum density reduction and minimum cell size compared to non-foamed resin. Compositions and results for preliminary samples are shown in Table 1. [Table 2]
[0096] The Adsyl 5C30F samples with 1.5% MB-A combined with 1% MB-B or MB-E from Table 1 were selected for further characterization, including image analysis. The results of the additional analysis are shown in Table 2. [Table 3]
[0097] From image analysis, selected extruded strands in Table 2 were found to have circular cross-sections with diameter measurements ranging from 2.75 mm. These foam compositions exhibited slight variations in stiffness and size, reflecting different foaming agent compositions and levels of foam expansion.
[0098] All of the optical images were obtained from a microscope at the lowest magnification possible, so that the largest area of the foam cross-section could be included. The bubble morphology differed among the strand samples. In general, the bubble size was smaller near the strand surface, where the polymer melt was subjected to higher shear forces during processing. The bubble size gradually increased with distance from the surface. Near the center, many small bubbles appeared to aggregate to form larger bubbles of irregular shape, either because of the low shear forces of the polymer melt that made it impossible to disperse the individual bubbles during the initial bubble formation, or because of the high extensional forces of the melt that caused the bubbles to burst during bubble growth. In some samples, the larger bubbles observed could be the result of the disappearance of the bubble walls that separate the individual bubbles. However, the bubble walls tend to collapse because they are too thin to withstand the low temperature microtoming used to prepare the samples for analysis.
[0099] SEM was used to confirm the variation of bubble size with distance from the strand surface and to observe bubble aggregation. Some of the aggregates formed clusters of bubbles with solid walls between adjacent bubbles. Others formed larger bubble aggregates of irregular shapes. Many of the bubbles in the foam strand samples were non-spherical. Foamed polymer melts tend to be stable when the gas bubbles are strictly spherical in shape to minimize interfacial area and capillary pressure, but the bubbles elongate in the extrusion direction, resulting in a non-uniform distribution of mechanical stress during foaming. It appears that the gas bubbles tend to expand along the direction of minimum local stress resulting in anisotropic shape of the bubbles. Furthermore, there is more freedom in the extrusion direction during foaming since there are fewer geometric constraints.
[0100] SEM images did not show enclosures for these hemispherical cells, and although SEM images can show individual cells within larger interconnected cell aggregates, there is no morphological evidence in the full field of view to characterize any of these foam samples as open-cell foams.
[0101] The bubbles were not uniformly distributed in the solid polymer. For this type of foam, the bubble size analysis provides a comprehensive and useful characterization of the foam structure to distinguish between various foam samples. Some morphological parameters, such as wall thickness and cell packing geometry, were not measurable or meaningful.
[0102] Table 2 lists the results of bubble count, average bubble size and relative standard deviation obtained by Stream Essentials image software via particle analysis. The bubble phase size and bubble phase area fraction were calculated based on these results and the measured strand diameter. The bubble phase area fraction for these samples is less than 42%.
[0103] Use of Masterbatch C appeared to achieve the greatest reduction in resin density, with a reduction of over 52%, while Masterbatch A was in the range of 39-44%.
[0104] However, when Masterbatch A was combined with the second Masterbatch, the bubble size was smallest, exhibiting a small bubble size of 130 microns in diameter. These results illustrate the fine tuning of the foaming agent in the masterbatch to elicit the desired properties from each base polymer. As shown in Table 2, the average bubble size fell within the range of approximately 97-100 μm equivalent diameter, therefore, these are classified as small cell foams.
[0105] The results of the bubble size measurements were further analyzed for size distribution. As shown in Figure 3A (cumulative bubble count vs. bubble radius) and Figure 3B (histogram of bubble size), and also shown in Table 2, these foam strand samples are not symmetrical. The curves in Figure 3A indicate that foaming agent composition is the main source of differences in bubble formation. The range of variation within each pair of foams produced from the same resin was relatively wide. The bubble dimensions most frequently detected in each foam sample are in the smallest particle size range. This type of particle size distribution results in a relatively high standard deviation in the bubble size measurements.
[0106] In conclusion, the base resins used in the strand examples were able to form foams. This foamability was unexpected for two reasons. First, reactor-made propylene-based RACOs and terpolymers, such as Adsyl-based resins, are not heterophasic copolymers with a semi-crystalline matrix component and a partially amorphous bipolymer component. These two components are thought to be necessary to form foams. However, this example shows that both components are not necessary. Second, the reactor-made propylene-based RACOs and terpolymer-based resins used in the compositions have lower melt strengths compared to polyolefins with high molecular weight bipolymer components. Since high melt strengths are required to foam polyolefins, these polymers become poor foaming candidates. However, the compositions were able to produce foamed strands. Additionally, the foamed strand compositions selected were small cell foams with smaller cells found near the surface, but larger irregularly shaped cells located near the center. It is generally known in the art that small cell structures tend to have less negative impact on mechanical properties than large cell structures. The density reduction was up to 70% when compared to the base resin.
[0107] These results indicate that Catalloy reactor produced RACO and terpolymer polyolefins with high comonomer content can not only be foamed, but that the foam characteristics (e.g., cell size, density reduction, etc.) can be tailored by the choice of chemical foaming agent(s) and / or the addition of one or more nucleating agents. Furthermore, due to the breadth of possible applications for foamed polyolefins, any "drawbacks" observed for one particular application, such as foamed strands with inconsistent cell size, have many more uses. CFA foam sheet
[0108] Based on the results of the foam strand testing, additional Adsyl grades were used to prepare CFA foam sheets. The compositions were foamed either as a single layer sheet (mode 1) or as a multi-layer sheet (mode 2). Similar to the foam strands, Masterbatch A and Masterbatch B were utilized for the CFA foam sheets. The foam sheets were produced by dry blending a combination of Masterbatch A and Masterbatch B with selected base Adsyl resin and extruding through an 8 inch flat die to prepare foam sheets with a target thickness of 40 mils (approximately 1 mm).
[0109] The compositions of each CFA foam sheet for the different Adsyl grades and the results of density testing according to ASTM D792 are shown in Tables 3 and 4. Table 3 shows the results for the multi-layer samples (mode 2) and Figure 4 shows the cumulative cell area distribution for each composition, labeled with density. The results for the single layer samples (mode 1) are shown in Table 4 and Figure 5. [Table 4]
[0110] The chemical foaming agent was able to reduce density for each of the base polymer resins tested. With these foam sheet samples, there was a good range of reduction up to about 25%.
[0111] Table 3 shows the results using Adsyl 7416XCP extruded as a multi-layer sheet. Sample No. K17218 produced a foam with a density of 44.7 lb / ft3, a reduction of 21%. Sample No. K17219 used the same concentration of Masterbatch A but added 0.75 wt% of Masterbatch B. This composition also provided a comparable density reduction of 21%. Example No. K17218 had an average cell radius of 15 microns, while Example No. K17219 achieved a cell radius of 18 microns.
[0112] Further examples using Adsyl 7416XCP were foamed as monolayer sheets. The results in Table 4 show how changes in the composition and / or concentration of the masterbatch can affect the foam characteristics. Example No. K19011 has the same masterbatch composition as No. K17219, and similar results were seen between modes 1 and 2. However, increasing the content of masterbatch A for Example No. K19012 increased the density reduction to about 6%. Thus, the concentration of masterbatch A appears to have a greater effect on the density reduction of Adsyl 7416XCP foam. Similar results were seen with Adsyl 5C30F foam, where the addition of masterbatch B did not increase the density reduction. [Table 5]
[0113] As explained above, Adsyl resins are not heterophasic copolymers with a semi-crystalline matrix component and a partially amorphous bipolymer component. Second, the reactor-made RACOs and terpolymers do not have long chain or high molecular weight components. Thus, these polyolefins have lower melt strength compared to polyolefins that have these features. Thus, these resins were considered to be poor choices for foaming. However, based on the foaming results obtained from earlier examples, different grades of this reactor-made random copolymer and terpolymer were mixed with various combinations of masterbatches and foamed as monolayer sheets. The results in Table 4 illustrate how different grades of these reactor-made random copolymers and terpolymers foamed unexpectedly with changes in masterbatches.
[0114] The foamed compositions produced using Adsyl 6C30F as the base resin showed an increase in cell size radius with increasing amounts of Masterbatch A, similar to Adsyl 7416XCP, whereas Adsyl 3C30F-HP showed a decrease in cell radius with increasing amounts of Masterbatch A. The Adsyl grades showed density reduction with increasing amounts of Masterbatch A and when Masterbatch B was added.
[0115] As before, SEM was used to see the variation in cell size with distance from the monolayer surface of the exemplary sheets in Table 4 and to observe cell agglomerations. Some of the agglomerations formed clusters of cells with solid walls between adjacent cells. Others formed larger cell agglomerates of irregular shapes. Many of the cells in the foam monolayer samples were non-spherical as they were elongated during the extrusion process.
[0116] The cell diameters were reduced to about 25-55 microns, and therefore these foams can be classified as small cell foams. Furthermore, each sample was predominantly a closed cell foam, as the foam cells were separated from one another and the cells were surrounded by complete cell walls. This desirable feature is useful in selecting applications for the foam composition. The foam samples also showed variation in cell size and shape with distance from the foam surface. Smaller cells were found near the surface, while larger cells with irregular shapes were located near the center, suggesting that the foam structure is strongly dependent on the rheological behavior of the base resin and the equipment used for foaming.
[0117] Results from each foam sample indicate that multiple Adsyl grades can be successfully foamed as sheets or strands using chemical foaming agents. Similarly, foaming capabilities using PBAs, both with and without nucleating agents, are expected to be similarly successful. The foam extrudates exhibit a wide range of properties, allowing for a wide range of applications. Furthermore, the choice of chemical foaming agents or combinations thereof, and nucleating agents can be utilized to tailor the characteristics of the foam extrudate for selected applications. Additionally, it was observed that foaming of random copolymers and terpolymers from different reactors does not require modifications to the system hardware, thereby reducing downtime and capital costs.
[0118] The following references are incorporated herein by reference in their entireties:
[0119] ASTM D792-13, Standard Test Methods for Density and Specific Gravity(Relative Density) of Plastics by Displacement
[0120] ASTM D 1238L, Standard Test Method for Melt Flow Rates of Thermoplastics by Extrusion Plastometer
[0121] EP0674991
[0122] EP1025162
[0123] US6395831
Claims
1. A foam composition comprising: A reactor-made polyolefin composition comprising a crystalline random copolymer having the following a) and / or b): said crystalline random copolymer having a melt flow rate (ASTM D 1238) between 2 and 15 g / 10 min: a) a first propylene-based copolymer or terpolymer selected from the group including: i) copolymers of propylene and ethylene, the ethylene content being between 1 and 7 wt %; ii) Copolymers of propylene and at least one C4-C8 alpha-olefin, the alpha-olefin content being between 2-14 wt %; iii) a terpolymer of propylene, ethylene and at least one C4 to C8 alpha-olefin, the content of ethylene being between 0.5 and 4.5 wt % and the content of alpha-olefin being between 2 and 6 wt %, the total content of said ethylene and said at least one alpha-olefin being less than or equal to 6.5 wt %; and / or b) a second propylene-based copolymer or terpolymer selected from the group including: i) copolymers of propylene and at least one C4-C8 alpha-olefin, the content of the alpha-olefin being between 8-30 wt %; ii) a copolymer of propylene, ethylene and at least one C olefin, the content of ethylene being between 1 and 7 wt % and the content of alpha-olefin being between 6 and 8 wt %; 4 ~C 8 Alpha-olefin terpolymers (wherein said first propylene-based copolymer is present at 0-80 wt % and said second propylene-based copolymer is present at 20-100 wt %).
2. 10. The foam composition of claim 1, wherein the reactor-made polyolefin composition is foamed using at least one physical blowing agent (PBA) or at least one chemical foaming agent (CFA).
3. 3. The foam composition of claim 2, wherein the reactor made polyolefin composition is combined with a masterbatch comprising at least one nucleating agent.
4. The physical blowing agent is high pressure CO 2 , N 2 4. The foam composition of claim 3, wherein the gas is selected from the group consisting of air, propane, isobutane, butane, a CFC derivative, argon, or combinations thereof.
5. 4. The foam composition of claim 3, wherein the chemical foaming agent is in the same masterbatch as the at least one nucleating agent or in a different masterbatch as the at least one nucleating agent.
6. 6. The foam composition of claim 5, wherein the total amount of masterbatches in the foam composition is 5 wt% or less of said reactor made polyolefin composition.
7. 3. The foam composition of claim 2, wherein the chemical foaming agent is endothermic or exothermic.
8. 3. The foam composition of claim 2, wherein the chemical foaming agent acts as a nucleating agent.
9. 10. An article comprising the reactor-made polyolefin composition of claim 1.
10. 10. The article of claim 9 which is a sheet, strand, tube or container.
11. 1. A foam composition comprising: The foam composition comprises a reactor-made polyolefin composition comprising a crystalline propylene / ethylene random copolymer; The reactor-made polyolefin composition containing the crystalline propylene / ethylene random copolymer comprises the following a) and b) a) about 4.5 wt % to about 8 wt % ethylene, and; b) about 92 wt % to about 95.5 wt % propylene A reactor-made polyolefin composition comprising a crystalline propylene / ethylene random copolymer having The crystalline propylene / ethylene random copolymer has a melt flow rate (ASTM D 1238) between 0.3 and 15 g / 10 min; and The reactor-made polyolefin composition is foamed using at least one physical foaming agent (PBA) or at least one chemical foaming agent (CFA); and A foam composition, wherein the reactor-made polyolefin composition is combined with a masterbatch comprising at least one nucleating agent.
12. The physical blowing agent is high pressure CO 2 , N 2 12. The foam composition of claim 11, wherein the gas is selected from the group comprising: air, propane, isobutane, butane, a CFC derivative, argon, or a combination thereof.
13. 12. The foam composition of claim 11, wherein the chemical foaming agent is in the same masterbatch as the at least one nucleating agent or in a different masterbatch as the at least one nucleating agent.
14. 14. The foam composition of claim 13, wherein the total amount of masterbatches in the foam composition is 5 wt% or less of said reactor made polyolefin composition.
15. 12. The foam composition of claim 11, wherein the chemical foaming agent is endothermic or exothermic.
16. 12. The foam composition of claim 11, wherein the chemical foaming agent acts as a nucleating agent.
17. 12. An article comprising the reactor-made polyolefin composition of claim 11.
Citation Information
Patent Citations
Core material for automobile bumper
JP1990158441A
Manufacture of foamed product having good low-temperature toughness from high-melt strength propylene polymer material
JP1999246716A
Propylenic copolymer material, film made therefrom, and method for producing propylenic copolymer material
JP2008208362A
Resin composition for extrusion foam molding and foam using the same
JP2009275120A
Polypropylene resin foamed particles, in-mold foam molded body of polypropylene resin, and method for manufacturing same
US20170218158A1