High-strength underwater non-segregating mortar composition for high-temperature environments and mortar using the same

A high-strength mortar composition with adjusted amorphous aluminosilicate and gypsum, along with a cellulose-based thickener, addresses the challenge of maintaining underwater inseparability and strength in high-temperature conditions, ensuring excellent fluidity and workability.

JP7574091B2Active Publication Date: 2024-10-28TAIHEIYO MATERIALS CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021012731
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-29
Publication Date
2024-10-28
Estimated Expiration
2041-01-29

AI Technical Summary

Technical Problem

Existing underwater non-separable mortars face challenges in maintaining high strength and underwater inseparability during high-temperature construction, particularly in summer conditions, due to decreased thickener performance and accelerated hydration reactions, leading to material separation and poor hardening.

Method used

A high-strength mortar composition is developed with a specific ratio of amorphous aluminosilicate and gypsum, combined with a cellulose-based thickener and fine aggregate, to maintain fluidity and underwater inseparability even in high-temperature environments.

Benefits of technology

The mortar composition ensures excellent fluidity for easy pumping, maintains workability, and achieves high strength development properties, even in temperatures up to 40°C, with improved shelf life and underwater inseparability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574091000001
    Figure 0007574091000001
  • Figure 0007574091000002
    Figure 0007574091000002
  • Figure 0007574091000003
    Figure 0007574091000003
Patent Text Reader

Abstract

To provide a high-strength underwater inseparable mortar composition for high-temperature environments, which is inseparable in water, ensures workability in high-temperature environments and has a high strength development.SOLUTION: A high-strength underwater inseparable mortar composition for high-temperature environments that includes a thickener, fine aggregate, and a binder containing cement, amorphous aluminosilicate and gypsum, wherein the total content of amorphous aluminosilicate and gypsum is 6 to 40 pts.mass relative to 100 pts.mass of binder. In the binder, the molar ratio of SO3 and Al2O3 as chemical components ([moles of SO3] / [moles of Al2O3]) is 0.25 to 0.8.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a high-strength underwater non-segregating mortar composition suitable for high-temperature environments and a mortar using the same. [Background technology]

[0002] Recently, due to climate change caused by an increase in greenhouse gases, the summer temperature has risen significantly, and the construction environment for cement concrete in hot weather has become more severe. The Standard Specifications for Concrete state that "if the pouring temperature exceeds 35°C, it must be confirmed that the concrete can maintain the specified quality," but the same rule can be applied to mortars such as various grouts.

[0003] Underwater non-separation mortar is generally composed of materials such as cement, water, aggregate, water reducing agent, and non-separation agent (thickener). However, the performance of thickeners tends to decrease as the temperature increases. Therefore, the underwater non-separation property of underwater non-separation mortar may decrease during construction in the summer when the temperature increases. When mortar is constructed underwater, including underwater, in civil engineering or construction work, it is filled underwater using a pressure pump, and if the underwater non-separation property decreases, material separation occurs, resulting in poor hardening and insufficient strength, resulting in construction failure. Underwater non-separation mortar compositions for high temperature environments that have excellent underwater non-separation property even in high temperature environments and can be mixed in a short time are known (for example, Patent Document 1).

[0004] Also, depending on the construction site, high-strength mortar is required. As an example of high-strength mortar, Patent Document 2 discloses a mortar composition containing cement, silica fume, water, a water reducing agent, an antifoaming agent, fine aggregate, and high tensile fibers, in which the cement contains 40.0 to 75.0 mass% of C3S and less than 2.7 mass% of C3A, and has a 45 μm sieve residue of less than 8.0 mass%, and the fine aggregate contains ferronickel slag. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2009-161387 A [Patent Document 2] JP 2012-144403 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in order to improve strength development, it is necessary to increase the unit amount of cement and binder and reduce the unit amount of water, but as a result, the hydration reaction of cement is accelerated in the high temperature environment of summer, making it difficult to ensure workable time (pot life). In addition, as mentioned above, there is also the problem that the performance of thickeners is easily reduced in high temperature environments. Therefore, it has been difficult to develop high strength while maintaining underwater non-separation properties in underwater construction in the recent summer.

[0007] Therefore, an object of the present invention is to provide a high-strength, underwater non-separation mortar composition suitable for high-temperature environments, which has excellent fluidity when mixed with mortar and can be easily pumped with a grout pump, has non-separation properties under water, ensures workability in high-temperature environments, and has high strength development, and a mortar using the same. [Means for solving the problem]

[0008] As a result of intensive research into the above-mentioned problems, the inventors have found that by adjusting the total amount of amorphous aluminosilicate and gypsum to be mixed in the binder within a specific range, and by adjusting the molar ratio of SO3 to Al2O3 contained in the binder within a specific range, it is possible to achieve excellent workability and high strength expression even in high temperature environments.

[0009] That is, the present invention is represented by the following [1] to [7]. [1] A high-strength, underwater, non-separating mortar composition suitable for use in high-temperature environments, comprising a binder containing cement, amorphous aluminosilicate, and gypsum, a thickener, and fine aggregate, in which the total content of the amorphous aluminosilicate and gypsum is 6 to 40 parts by mass per 100 parts by mass of the binder, and the molar ratio of SO3 and Al2O3 ([moles of SO3] / [moles of Al2O3]) as chemical components in the binder is 0.25 to 0.8. [2] The high-strength, underwater non-separating mortar composition for use in high-temperature environments according to [1], wherein the thickener is a cellulose-based thickener having a viscosity of 30,000 to 60,000 mPa s at 20°C when made into a 2% by mass aqueous solution. [3] The high-strength underwater non-segregating mortar composition for high-temperature environments according to [2], wherein the lower critical solution temperature of the cellulose-based thickener is 45°C or higher. [4] The high-strength, underwater non-segregating mortar composition suitable for high-temperature environments according to any one of [1] to [3], wherein the binder further contains an expansive agent. [5] The underwater non-segregating mortar composition suitable for high temperature environments according to any one of [1] to [4], further comprising a polycarboxylic acid-based water-reducing agent. [6] [1] - [5] ] A high-strength, underwater, non-separating mortar capable of withstanding high temperatures, comprising the high-strength, underwater, non-separating mortar composition capable of withstanding high temperatures according to any one of the above, and water, wherein the water content is 15 to 40 parts by mass per 100 parts by mass of the binder. [7] The high-strength, underwater non-separating mortar for use in high-temperature environments according to [6], wherein the mass ratio of the thickener to water ([mass of thickener] / [mass of water]) is 0.0005 to 0.02. Effect of the Invention

[0010] According to the present invention, it is possible to provide a high-strength, underwater non-separation mortar composition suitable for high-temperature environments, in which the mixed mortar has excellent fluidity and can be easily pumped with a grout pump, has non-separation properties in water, and ensures workability in high-temperature environments, and has high strength development, and a mortar using the same can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] A preferred embodiment of the present invention will be described below. In this specification, "high temperature environment compatible" means that the mixed mortar has good fresh properties, excellent fluidity, and sufficient workability time in a high temperature environment of 30°C or higher. More specifically, when 120 minutes have passed since mixing, the mortar is filled into a cement paste container (flow cone) of JIS R 5201:1997 "Physical Testing Methods for Cement", and the table flow value after the container is pulled out (3 minutes after the flow cone is pulled out) is 200 mm or more.

[0012] The high-strength underwater non-separation mortar composition of this embodiment suitable for high-temperature environments comprises a binder containing cement, amorphous aluminosilicate, and gypsum, a thickener, and fine aggregate, in which the total content of the amorphous aluminosilicate and gypsum is 6 to 40 parts by mass relative to 100 parts by mass of the binder, and the molar ratio of SO3 and Al2O3 ([moles of SO3] / [moles of Al2O3]) as chemical components in the binder is 0.25 to 0.8.

[0013] The binder according to the present embodiment includes cement, amorphous aluminosilicate, and gypsum. The binder may include, in addition to the above components, an expansion agent, ground granulated blast furnace slag, silica fume, fly ash, and the like.

[0014] Various types of cement can be used, including, for example, various types of Portland cement such as ordinary, early strength, super early strength, low heat and moderate heat, ecocement, rapid hardening cement, etc. As the cement, ordinary Portland cement and early strength Portland cement are preferred from the viewpoint of ensuring fluidity and pot life even in a high temperature environment. One type of cement may be used alone, or two or more types may be used in combination.

[0015] The content of cement is preferably 60 to 85 parts by mass, more preferably 65 to 82 parts by mass, and further preferably 68 to 80 parts by mass, relative to 100 parts by mass of the binder.

[0016] The amorphous aluminosilicate is not particularly limited as long as it is derived from a clay mineral and contains an amorphous portion, and any of them can be used. Examples of the clay mineral as the raw material include kaolin minerals, mica clay minerals, smectite minerals, and mixed layer minerals formed by mixing these. The amorphous aluminosilicate can be obtained by, for example, calcining and dehydrating these crystalline aluminosilicates to make them amorphous. From the viewpoint of further excellent reactivity, the amorphous aluminosilicate is preferably derived from kaolin minerals such as kaolinite, halloysite, and dickite, and metakaolin obtained by calcining kaolinite. but The amorphous aluminosilicate may be used alone or in combination of two or more kinds.

[0017] In this specification, "amorphous" means that the peaks derived from the raw clay mineral are almost not observed in the measurement by a powder X-ray diffractometer. The amorphous aluminosilicate according to this embodiment may have an amorphous ratio of 70% by mass or more, preferably 90% by mass or more, more preferably 100% by mass, that is, most preferably has no peaks observed in the measurement by a powder X-ray diffractometer. The amorphous ratio is a value obtained by the standard addition method. Aluminosilicates with a high amorphous ratio, i.e., aluminosilicates with a low crystalline ratio, tend to have better strength development at the same mixing amount than aluminosilicates with a low amorphous ratio. Examples of heating for amorphizing aluminosilicate include firing in an externally heated kiln, an internally heated kiln, an electric furnace, etc., and melting using a melting furnace.

[0018] The content of the amorphous aluminosilicate is preferably 5 to 25 parts by mass, more preferably 10 to 22 parts by mass, and even more preferably 12 to 20 parts by mass, relative to 100 parts by mass of the binder. If the content of the amorphous aluminosilicate is within the above range, it is easy to ensure higher strength development while maintaining good workability.

[0019] Examples of gypsum include anhydrous gypsum, hemihydrate gypsum, and dihydrate gypsum. As the gypsum, anhydrous gypsum is preferable from the viewpoint of further improving the strength development. One type of gypsum may be used alone, or two or more types may be used in combination. The fineness of the gypsum is 2500 cm2 in terms of Blaine specific surface area from the viewpoint of further improving the short-term strength development due to the reaction activity. 2 The fineness of the gypsum is preferably 12,000 cm2 / g or more in terms of Blaine specific surface area. 2 It is preferable that the molecular weight is not more than 1 / g.

[0020] The content of the gypsum is preferably 1 to 15 parts by mass, more preferably 2 to 12 parts by mass, and even more preferably 3 to 10 parts by mass, relative to 100 parts by mass of the binder. If the content of the gypsum is within the above range, it is easy to ensure higher strength development.

[0021] In addition, in the binder of the mortar composition of this embodiment, the total content of the amorphous aluminosilicate and gypsum is 6 to 40 parts by mass relative to 100 parts by mass of the binder. If the total content of the amorphous aluminosilicate and gypsum is outside the above range, there is a risk of a decrease in strength development, difficulty in obtaining fluidity, and a decrease in usable time at high temperatures. From the viewpoint of further improving workability and strength development at high temperatures, the total content of the amorphous aluminosilicate and gypsum is preferably 10 to 30 parts by mass, more preferably 15 to 28 parts by mass, relative to 100 parts by mass of the binder.

[0022] The expansive agent may be any JIS-compliant expansive agent (JIS A 6202:2008) that is generally used as an expansive agent for concrete. Examples of the expansive agent include expansive agents mainly composed of free quicklime (quicklime-based expansive agents), expansive agents mainly composed of auin (ettringite-based expansive agents), and composite expansive agents of free quicklime and ettringite-forming substances. One type of expansive agent may be used alone, or two or more types may be used in combination. The expansive agent has a Blaine specific surface area of ​​2000 to 6000 cm. 2 It is preferable to use one having a molecular weight of 1 / g.

[0023] The content of the expansive material is preferably 0.1 to 5 parts by mass, more preferably 0.5 to 4 parts by mass, and even more preferably 1 to 3 parts by mass, relative to 100 parts by mass of the binder. If the content of the expansive material is within the above range, the compressive strength, dimensional change rate, etc. will be further improved.

[0024] In the binder of the mortar composition of this embodiment, the molar ratio of SO3 and Al2O3 ([moles of SO3] / [moles of Al2O3]) as chemical components is 0.25 to 0.8. If the molar ratio of SO3 and Al2O3 is outside the above range, good fluidity is not obtained and strength development in water is also reduced. From the viewpoint of obtaining higher strength development while maintaining good fluidity, the molar ratio of SO3 and Al2O3 is preferably 0.28 to 0.76, more preferably 0.3 to 0.65.

[0025] The molar ratio of SO3 and Al2O3 as chemical components in the binder can be adjusted by increasing or decreasing the content of gypsum containing SO3 as a main component and amorphous aluminosilicate containing Al2O3 as a main component.

[0026] One method for determining the molar ratio of SO3 and Al2O3 as chemical components in the binder is to analyze the various raw materials in the binder using an X-ray fluorescence analyzer and convert the total component values ​​of SO3 and Al2O3 shown as oxides into a molar ratio.

[0027] The thickener is not particularly limited, and examples thereof include cellulose-based thickeners, acrylic thickeners, and guar gum thickeners. Among these thickeners, cellulose-based thickeners are preferred. Examples of cellulose-based thickeners include carboxymethylcellulose, methylcellulose, hydroxypropylmethylcellulose, hydroxyethylcellulose, and hydroxypropylcellulose. As cellulose-based thickeners, methylcellulose and hydroxypropylmethylcellulose are preferred, and hydroxypropylmethylcellulose is more preferred, from the viewpoint that they have a high lower critical solution temperature (LCST) and are likely to exhibit excellent functions even in a high temperature environment.

[0028] The lower critical solution temperature of the cellulose-based thickener is preferably 45° C. or higher, more preferably 50° C. or higher, and even more preferably 55° C. or higher. If the lower critical solution temperature of the cellulose-based thickener is 45° C. or higher, the thickener is less likely to undergo phase transition and is likely to exhibit excellent functions even in high-temperature environments. The lower critical solution temperature can be measured, for example, by observing the change in the aqueous solution due to temperature using an absorbance meter or a dynamic light scattering measuring device.

[0029] The viscosity of the thickener is preferably 30000 to 60000 mPa·s, more preferably 30000 to 55000 mPa·s, and even more preferably 35000 to 50000 mPa·s. If the viscosity of the thickener is within the above range, the underwater non-separation property of the mortar can be improved and good fluidity can be maintained. In this specification, the viscosity of the thickener is a value measured by using a rotational viscometer in an environment of 20°C for an aqueous solution of the thickener prepared to have a concentration of 2% by mass. The rotational viscometer may be one that is commonly used, and for example, an inner cylinder rotational viscometer or an outer cylinder rotational viscometer may be used.

[0030] The content of the thickener is preferably 0.005 to 0.5 parts by mass, more preferably 0.01 to 0.4 parts by mass, and even more preferably 0.02 to 0.3 parts by mass, relative to 100 parts by mass of the binder. If the content of the thickener is within the above range, good fluidity can be easily ensured, and even better anti-separation properties in water can be ensured.

[0031] Examples of fine aggregate include river sand, silica sand, crushed sand, kansui stone, limestone sand, slag aggregate, etc. Of these, it is preferable to use silica sand, limestone sand, etc., adjusted to a particle size that does not contain fine powder or coarse aggregate, as the fine aggregate. One type of fine aggregate may be used alone, or two or more types may be used in combination. It is preferable to use fine aggregate with a particle size of 5 mm or less (passing a 5 mm sieve), which is commonly used.

[0032] The particle size of the fine aggregate is not particularly limited, and can be adjusted within the required particle size range of the fine aggregate. The particle size of the fine aggregate can be considered from the coarse aggregate ratio defined by JIS A 1102:2014 "Sieving test method for aggregates". From the viewpoint of obtaining better fluidity when made into mortar and suppressing bleeding, the coarse aggregate ratio of the fine aggregate is preferably 1 to 4, more preferably 1.5 to 3.8, and most preferably 1.8 to 3.7.

[0033] The content of the fine aggregate is preferably 40 to 75 parts by mass, more preferably 45 to 70 parts by mass, and even more preferably 50 to 68 parts by mass, relative to 100 parts by mass of the binder. If the content of the fine aggregate is within the above range, good fluidity is easily obtained, and strength development is further improved.

[0034] The water reducing agent includes a high-performance water reducing agent, a high-performance AE water reducing agent, an AE water reducing agent, and a superplasticizer. Examples of such water reducing agents include those specified in JIS A 6204:2011 "Chemical admixtures for concrete". Examples of water reducing agents include polycarboxylic acid water reducing agents, naphthalene sulfonic acid water reducing agents, lignin sulfonic acid water reducing agents, and melamine water reducing agents. Among these water reducing agents, polycarboxylic acid water reducing agents are preferred from the viewpoint that the fluidity retention time can be easily ensured even with a small amount of addition. The water reducing agents may be used alone or in combination of two or more types.

[0035] The content of the water reducing agent is preferably 0.3 to 5 parts by mass, more preferably 0.5 to 4 parts by mass, and even more preferably 0.8 to 3 parts by mass, relative to 100 parts by mass of the binder. If the content of the water reducing agent is within the above range, the pot life is easily ensured and the fluidity is further improved.

[0036] The mortar composition of this embodiment may contain various admixtures within the range in which the effects of the present invention are not impaired. Examples of admixtures include foaming agents, antifoaming agents, polymers for cement, waterproofing agents, rust inhibitors, shrinkage reducing agents, water retention agents, pigments, fibers, water repellents, efflorescence inhibitors, quick-setting agents (materials), quick-hardening agents (materials), setting retarders, ground granulated blast furnace slag, stone powder, silica fume, volcanic ash, air entraining agents, and surface hardeners.

[0037] The method for producing the mortar composition of the present embodiment is not particularly limited, and the mortar composition can be produced by mixing, for example, with a gravity mixer such as a V-type mixer or a tilting concrete mixer, a Henschel mixer, a jet mixer, a ribbon mixer, or a paddle mixer.

[0038] The mortar composition of the present embodiment can be prepared as a mortar by mixing with water, and the water content may be appropriately adjusted depending on the application. The water content is preferably 15 to 40 parts by mass, more preferably 18 to 35 parts by mass, and even more preferably 20 to 30 parts by mass, relative to 100 parts by mass of the binder. If the water content is within the above range, the strength development is further improved while maintaining good underwater non-separation properties.

[0039] In the mortar of this embodiment, the mass ratio of the thickener to water ([mass of thickener] / [mass of water]) is preferably 0.0005 to 0.02, more preferably 0.0008 to 0.018, and even more preferably 0.001 to 0.015. If the mass ratio of the thickener to water is within the above range, the underwater non-separation property will be further improved.

[0040] The preparation of the mortar of this embodiment can be carried out using a kneading tool similar to that used for ordinary mortar compositions, and is not particularly limited. Examples of the kneading tool include a mortar mixer, a grout mixer, a hand mixer, a tilting mixer, and a twin-shaft mixer.

[0041] The mortar composition and mortar of the present embodiment have excellent fluidity and pot life even in a high temperature environment of 30°C or higher, good underwater non-separation properties, and excellent compressive strength when hardened. Therefore, even under harsh environmental conditions such as summer, it can be used for casting normal underwater structures, and can also be suitably used for construction of offshore facilities that require strong strength characteristics. The construction method is not particularly limited, and a method of making a formwork and filling it can be selected. EXAMPLES

[0042] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0043] The materials used in the examples are as follows: High early strength Portland cement (HC) Ordinary Portland Cement (NC) Amorphous aluminosilicate (AS): Amorphous aluminosilicate compound (commercially available product; no peaks derived from the clay minerals used as raw materials are observed when measured using a powder X-ray diffraction device (amorphous)) Gypsum (G): Anhydrous gypsum (powderness: 7100cm 2 / g) Expansion material (EX): Lime-based expansion material (Blaine specific surface area: 3105 cm 2 / g) Thickener 1 (MC1): Water-soluble cellulose ether (hydroxypropyl methylcellulose, viscosity at 20°C when made into a 2% by mass aqueous solution: 45,500 mPa s, lower critical solution temperature: 55°C or higher) Thickener 2 (MC2): Water-soluble cellulose ether (hydroxypropyl methylcellulose, viscosity at 20°C when made into a 2% by mass aqueous solution: 30,800 mPa s, lower critical solution temperature: 55°C or higher) Water reducing agent (AD): Polycarboxylate-based high-performance water reducing agent Fine aggregate (S): Silica sand (with grain size adjusted to 2.6 to 3.6) Mixing water (W): Tap water

[0044] [Experimental Example 1] <Production of mortar composition> The materials used were blended in the proportions shown in Table 1, charged into a Henschel mixer, and mixed to produce mortar compositions (Invention Products 1 to 6, Reference Products 1 to 4).

[0045] <Mortar manufacturing> The mortar composition (6 kg) and water were mixed for 6 minutes using a high-speed hand mixer to prepare a mortar. The proportion of water is shown in Table 1.

[0046] [Table 1]

[0047] <Evaluation of fresh properties of mortar> The fresh properties (fluidity and workability retention time) of the prepared mortars (Products 1 to 6 of the present invention, Reference Products 2 to 4) were measured and evaluated in a high temperature environment of 30°C (test room temperature and material temperature, water temperature 30°C ± 1°C). The evaluation test methods are as follows. [Liquidity] Mortar was filled into a cement paste container (flow cone) according to JIS R 5201:1997 "Physical Testing Methods for Cement," and the table flow value after the container was removed (3 minutes after the flow cone was removed) was measured. [Workability retention time] The workability retention time was determined based on the table flow value of the above test, and was determined from the fluidity 120 minutes after mixing. Table flow values ​​of 200 mm or more were judged as good, and those less than 200 mm were judged as unacceptable. Before measuring the table flow value after aging, the mixture was mixed again with a hand mixer for 30 seconds.

[0048] Table 2 shows the evaluation results of fresh properties in a 30°C environment. It was confirmed that the products of the present invention all had a high fluidity with a flow value of 250 mm or more immediately after mixing at a mixing temperature of around 40°C (37.1 to 40.4°C), and maintained a flow value of 200 mm or more 120 minutes after mixing. No mortar lumps, aggregate separation, or bleeding were visually observed in the products of the present invention.

[0049] [Table 2]

[0050] [Experimental Example 2] <Evaluation of hardening properties of mortar> The compressive strength and anti-segregation property in water during hardening of the prepared mortars (Products 1 to 6 of the present invention and Reference Product 1) were measured and evaluated. The evaluation test methods are shown below. [Compressive strength] The compressive strength was measured at 28 days of age according to JIS A 1108:2006 "Testing method for compressive strength of concrete". The dimensions of the specimen were 50mm in diameter and 100mm in height. The specimens were molded underwater according to JSCE-504, and the specimens in air were molded in exactly the same way as the specimens molded underwater, except that they were molded in air. [Inseparability in water] In accordance with JSCE-D-104-2007 "Quality Standard for Underwater Anti-Segregation Admixtures for Concrete," the underwater and air compressive strength ratio of the compressive strength obtained in the above test was calculated, and a compressive strength ratio of 80% or more in the underwater and air condition at 28 days was rated as good, and less than 80% as poor.

[0051] Table 3 shows the evaluation results of the hardening properties of mortar in a 30°C environment. The products of the present invention all had a compressive strength of 100 N / mm 2 The products of the present invention exhibited ultra-high strength as described above. The underwater and air compressive strength ratios of the products of the present invention were all 80% or more, confirming their excellent anti-segregation properties underwater.

[0052] [Table 3]

[0053] [Experimental Example 3] The fresh properties (fluidity and workability retention time) of the present invention products 1 and 4 in a high temperature environment of 40°C (test room temperature and material temperature, water temperature 40°C ± 1°C) were measured and evaluated in the same manner as in Experimental Example 1. The mortar was produced in consideration of the heat storage property of the mass effect as described below, and the mixing amount of the mortar composition was set to 100 kg. <Mortar manufacturing> The mortar composition (100 kg) and water were mixed for 2 minutes in a high-speed grout mixer to prepare a mortar. The proportion of water is shown in Table 1.

[0054] Table 4 shows the evaluation results of fresh properties in a high-temperature environment of 40°C. Although the mixing temperature of all the products of the present invention exceeded 45°C, it was confirmed that the flow value immediately after mixing was 250 mm or more, and the flow value 120 minutes after mixing was also maintained at 200 mm or more. The products of the present invention did not visually show any mortar lumps, aggregate separation, or bleeding.

[0055] [Table 4]

[0056] [Experimental Example 4] For the present invention products 1 and 4, the hardening properties (compressive strength and anti-separation property in water) in a high temperature environment of 40° C. were measured and evaluated in the same manner as in Experimental Example 2. The mortar was produced in the same manner as in Experimental Example 3.

[0057] Table 5 shows the evaluation results of the hardening properties of mortar in a high-temperature environment of 40°C. The compressive strength of the mortar of the present invention was 100 N / mm2 at 28 days. 2 The products of the present invention also exhibited underwater and air compressive strength ratios of 90% or more, confirming their excellent anti-segregation properties in water.

[0058] [Table 5]

Claims

1. The present invention includes a binder including cement, amorphous aluminosilicate, and gypsum, a thickener, and a fine aggregate, The total content of the amorphous aluminosilicate and the gypsum is 6 to 40 parts by mass relative to 100 parts by mass of the binder, In the binder, SO is used as a chemical component. 3 and Al 2 O 3 Molar ratio of ([SO 3 moles of Al 2 O 3 [number of moles] is 0.25 to 0.8, The thickener is a cellulose-based thickener having a viscosity of 30,000 to 60,000 mPa·s at 20°C when made into a 2% by mass aqueous solution and a lower critical solution temperature of 45°C or higher.

2. The high-temperature environment-compatible, high-strength, underwater non-segregating mortar composition according to claim 1, wherein the binder further comprises a lime-based expansive material.

3. A high-strength, underwater non-separating mortar composition suitable for high-temperature environments as described in claim 2, wherein the content of the lime-based expansive agent is 1 to 3 parts by mass per 100 parts by mass of the binder.

4. The high-temperature environment-compatible underwater non-segregating mortar composition according to any one of claims 1 to 3, further comprising a polycarboxylic acid-based water reducing agent.

5. A mortar composition according to any one of claims 1 to 4, which is suitable for high-temperature environments, and which does not separate underwater and has high strength, and which contains water, The water content is 15 to 40 parts by mass per 100 parts by mass of the binder, and the high-strength underwater non-separating mortar is suitable for high-temperature environments.

6. The high-temperature environment-compatible high-strength underwater non-separating mortar according to claim 5, wherein the mass ratio of the thickener to the water ([mass of thickener] / [mass of water]) is 0.0005 to 0.

02.

7. A high-strength underwater non-segregating mortar suitable for high temperature environments as described in claim 5 or 6, having an underwater and air compressive strength ratio of 80% or more at 28 days of age in accordance with JSCE-D-104-2007 "Quality Standard for Underwater Non-Segregating Admixtures for Concrete".

Citation Information

Patent Citations

  • Antiwashout underwater mortar composition for high temperature environment, and antiwashout underwater grout mortar composition for high temperature environment

    JP2009161387A

  • High-strength mortar composition

    JP2012144403A

  • Thickener for hydraulic composition, one-component type water-reducing agent, and hydraulic composition including thereof

    JP2016056081A

  • Quick-hardening ultrahigh-strength grout composition

    JP2018193280A

  • Cement composition

    JP2019099439A