Anti-Reflective Film for BIPV Modules
Patent Information
- Application Number
- KR1020250023662
- Authority / Receiving Office
- KR · KR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-02-24
- Publication Date
- 2026-09-02
Smart Images

Figure PAT00002_ABST
Abstract
Description
Technology Field
[0001] The present invention relates to an anti-reflective film for double-sided / color BIPV solar cells that secures an anti-reflective function together with a weather-resistant top coating. Background Technology
[0002] Solar power generation technology is gaining worldwide attention as a sustainable energy source, and Building Integrated Photovoltaics (BIPV) technology, in particular, is becoming increasingly widespread. BIPV modules are designed to be installed directly on building exterior walls or windows, enabling them to simultaneously perform power generation functions and serve as building materials. Consequently, various factors—such as harmony with the building, aesthetic appeal, and reflectivity control—become critical design requirements, in addition to the efficiency of the BIPV modules.
[0003] Generally, Anti-Reflection Coating (ARC) technology is applied to reduce the reflectivity of solar modules. One conventional ARC method involves forming a coating layer containing micro-sized beads to scatter light through fine pores on the surface and reduce reflectivity. This method can contribute to increasing the power generation efficiency of solar modules by reducing reflected light. However, bead-based anti-reflection coating methods have limitations in providing uniform anti-reflection performance. Reflectivity can vary depending on the viewing angle, and there are difficulties in precisely controlling the size and depth of the fine pores. Furthermore, due to the structural characteristics of the bead-containing coating layer, there is a possibility that solar transmittance may decrease, which could impede power generation efficiency.
[0004] Unlike conventional solar modules, BIPV modules require consideration of harmony with architectural design, so various colored glasses and films are applied. However, due to their high reflectivity, these colored glasses and films can cause glare issues for adjacent buildings. Consequently, there is an increasing need for anti-reflective films that can provide a uniform visual effect while reducing reflectivity. Conventional anti-reflective film technology primarily utilizes the Anti-Glare (AG) method, which induces light scattering by forming protrusions and patterns on the surface. However, this method is also only effective at specific angles, and there is a possibility that the appearance or physical properties may change if exposed to outdoor environments for a long period.
[0005] Therefore, for anti-reflective films to be applied to BIPV solar cell modules, a technical solution is required that can overcome the limitations of existing ARC or AG methods and provide a uniform anti-reflective effect from various angles. In addition, durability must be ensured so that the physical properties and appearance of the film are maintained even when exposed outdoors for a long period. To this end, the application of a new pattern coating method is required that can optimize anti-reflective performance while maintaining visual uniformity. The problem to be solved
[0006] The objective of the present invention is to provide an anti-reflective film for BIPV color solar cells that can exhibit nearly the same anti-reflective effect at various angles without a decrease in transmittance, together with a weather-resistant hard coating. means of solving the problem
[0007] As a technical means for achieving the above-mentioned technical problem, an anti-reflective film according to one embodiment of the present invention comprises a substrate layer, a weather-resistant top coating layer formed on one side of the substrate layer, and an adhesive layer formed on the other side of the substrate layer, wherein the top coating layer is configured such that a pattern is transferred by laminating a pattern paper in a partially cured state and then fully cured to transfer an uneven pattern including pores, and the pores are configured to scatter light proceeding toward the top coating layer to reduce surface reflectivity.
[0008] In addition, according to one embodiment of the present invention, the top coating layer comprises a urethane acrylate-based resin and can be partially cured at a temperature of 80°C or lower and then maintained in an environment of 50°C to 70°C for 24 hours or more to be fully cured. Effects of the invention
[0009] According to the means for solving the problem of the present invention described above, the present invention can achieve uniform anti-reflection performance even at various angles and can obtain a reflectance reduction effect of 2.5% or more when attached to a color film using a weather-resistant top coating double-sided / color BIPV solar cell anti-reflection film of a pattern coating method that does not change the appearance and physical properties of the window even when exposed outdoors for a long period of time.
[0010] However, the effects obtainable from the present invention are not limited to those described above, and other effects may exist. Brief explanation of the drawing
[0011] FIG. 1 is a schematic diagram illustrating an anti-reflective film (9) with a conventional bead coating layer applied. FIG. 2 is a schematic diagram illustrating an anti-reflective film (1) according to one embodiment of the present invention. FIG. 3 is a diagram comparing the physical properties of a conventional anti-reflection film (9) with a bead coating layer and the anti-reflection film (1) of the present invention. Figure 4 is a diagram showing the change in surface reflectance when an anti-reflective film is attached to a color film for BIPV. Specific details for implementing the invention
[0012] Embodiments of the present invention are described below with reference to the attached drawings so that those skilled in the art can easily implement the invention. However, the present invention may be embodied in various different forms and is not limited to the embodiments described herein. Furthermore, in order to clearly explain the present invention in the drawings, parts unrelated to the explanation have been omitted, and similar parts throughout the specification are denoted by similar reference numerals.
[0013] Throughout the specification of this invention, when a part is described as being "connected" to another part, this includes not only cases where they are "directly connected," but also cases where they are "electrically connected" or "indirectly connected" with other elements interposed between them.
[0014] Throughout the entire specification of the present invention, when a member is described as being located "on," "on the upper," "on the top," "under," "on the lower," or "on the bottom" of another member, this includes not only cases where the member is in contact with the other member, but also cases where another member exists between the two members.
[0015] Throughout the specification of the present invention, when a part is described as "comprising" a certain component, this means that, unless specifically stated otherwise, it does not exclude other components but may include additional components.
[0016] Referring to FIG. 1, a conventional anti-reflection film (9) with a bead coating layer applied comprises a substrate layer (91), a bead coating layer (92) formed as a coating layer on one side of the substrate layer, an adhesive layer (93) formed on the other side of the substrate layer, and a release film (94) formed to protect the adhesive layer. Such a conventional anti-reflection film (9) employs a method in which light is scattered by micro-pores formed by mixing micro-sized beads on the surface of the coating layer and the beads are exposed on the surface of the coating layer, thereby reducing the reflectivity. For uniform surface reflection, very uniform beads must be used, and the film can be combined with a binder layer so that the beads can be safely attached inside the coating layer.
[0017] Referring to FIG. 2, an anti-reflection film (1) according to one embodiment of the present invention may include a substrate layer (10), a weather-resistant top coating layer (20) formed on one side of the substrate layer, an adhesive layer (30) formed on the other side of the substrate layer, and a release film (40). The anti-reflection film may be formed in a type with an additional adhesive layer so as to be attached to a front sheet for a BIPV module, a module with a color film attached, or a general glass module, but the adhesive layer (30) and the release film (40) may not be provided. The adhesive layer (30) and the release film (40) may be understood as known conventional adhesive layers and release films.
[0018] The substrate layer (10) is a film layer serving as a base substrate, and the first substrate film layer (11) may be formed as a transparent film with a thickness of 50 to 200 μm. The substrate layer (10) may be a film layer comprising one or more selected from polyester resin, polycarbonate resin, polyvinyl resin, polyimide resin, and polyurethane resin, and preferably may be a PET film.
[0019] A weather-resistant top coating layer (20) may be provided to be coated on a substrate layer (10) to protect the substrate layer, thereby protecting the substrate layer from external foreign substances such as moisture or dust. Additionally, a pattern paper may be laminated onto the top coating layer (20) in a partially cured state to transfer a pattern, and then fully cured to transfer an uneven pattern containing pores. The pores may scatter light traveling toward the top coating layer, thereby reducing the surface reflectivity.
[0020] In the case of a pattern coating method in which a pattern paper is laminated onto the surface of a coating layer after the top coating layer is partially cured so that the protrusions and pore patterns of the pattern paper are transferred to the surface of the coating layer, the uniformity is superior compared to the conventional method of incorporating beads because the fine pattern is transferred from a roll processed with the fine pattern, and wider and deeper pore surfaces can also be produced.
[0021] Furthermore, since the weather-resistant top coating layer, which is an organic binder, is processed into a patterned shape, changes in appearance and physical properties do not occur even with repeated temperature fluctuations. The anti-reflective effect of the surface is determined by the width and depth of the pores, and when comparing the bead coating method and the pattern coating method, films produced using the pattern coating method exhibit superior anti-reflective effects.
[0022] As can be seen in FIG. 3, when referring to the anti-reflection film of the comparative example and embodiment described later, in the case of the bead coating type anti-reflection film (9), the glossiness in the 20° direction is 1.5, the glossiness in the 60° direction is 18.2, and the glossiness in the 85° direction is 82.6, which is very high at Haze 74.85%. When observed from the side, there is a surface reflection reduction effect, but when observed from the front, the effect is minimal, and the transmittance is reduced to the extent that the light source on the back is hardly visible when observed with the naked eye.
[0023] On the other hand, in the case of the anti-reflection film (1) to which the hardened top coating layer (20) is applied after laminating the pattern paper according to the present invention, the glossiness in the 20° direction is 1.4, the glossiness in the 60° direction is 5.1, and the glossiness in the 85° direction is 26.3 at Haze 74.72%, which is very low compared to the bead method, so excellent reflection reduction effect can be expected when observed from the side and when observed from the front, and in particular, it can be seen that the transmittance is maintained to the extent that the light source on the rear can be observed even at the same Haze, so it does not have a significant effect on power generation efficiency.
[0024] Referring to Figure 4, the visible light reflectance of a module with a BLUE color film attached for BIPV modules was measured to be 8.5%, and it was confirmed that the reflectance decreased to 6.0% when an anti-reflective film was attached to the surface of the BLUE color film.
[0026] Comparative example
[0027] As a comparative example, an anti-reflective film comprising a top coating layer containing beads was used, and a PET film (ASTROLL, Kolon Industries) with a thickness of 100 μm was used as the base film layer. For the adhesive layer, a composition was prepared by mixing an acrylic binder (AT-377, Samwon) at 35 parts by weight per 100 parts by weight of the adhesive layer, an epoxy curing agent (CAT-EX, Samwon) at 1 part by weight per 100 parts by weight of the adhesive layer, and a MEK solvent at 64 parts by weight per 100 parts by weight of the adhesive layer, and curing the composition at 120°C for 2 minutes to achieve a thickness of 10 μm.
[0028] As a top coating layer, 30 parts by weight of 3-5㎛ monodisperse beads (600-SOL, Daeha Mentec) were mixed based on 100 parts by weight of a urethane acrylate top coating layer (sju-1002, Samyoung Ink), and then the solvent was removed and the top coating layer was cured in a ventilated oven at 120℃ for 1 minute.
[0030] Examples
[0031] As an example, as an anti-reflective film with a pattern formed on the top coating layer (20), a PET film (ASTROLL, Kolon Industries) with a thickness of 100 μm was used as the base film layer, and for the adhesive layer, an acrylic binder (AT-377, Samwon) was mixed in 35 parts by weight based on 100 parts by weight of the adhesive layer, an epoxy curing agent (CAT-EX, Samwon) was mixed in 1 part by weight based on 100 parts by weight of the adhesive layer, and a MEK solvent was mixed in 64 parts by weight based on 100 parts by weight of the adhesive layer, and the composition was cured in an environment of 120°C for 2 minutes to obtain a thickness of 10 μm.
[0032] As for the top coating layer, a urethane acrylate top coating layer (SJU-1002, Samyoung Ink) was partially cured by removing the solvent for 1 minute in an environment inside a ventilated oven at 80°C, and a pattern paper was laminated onto the partially cured coating layer and cured by leaving it in a 60°C oven for 24 hours to allow for pattern transfer and complete curing.
[0034] The foregoing description of the present invention is for illustrative purposes only, and those skilled in the art will understand that other specific forms can be easily modified without altering the technical spirit or essential features of the present invention. Therefore, the embodiments described above should be understood as illustrative in all respects and not restrictive. For example, each component described as a single unit may be implemented in a distributed manner, and components described as distributed may likewise be implemented in a combined form.
[0035] The scope of the present invention is defined by the claims set forth below rather than by the detailed description above, and all modifications or variations derived from the meaning and scope of the claims and equivalent concepts thereof should be interpreted as being included within the scope of the present invention. Explanation of the symbols
[0036] 1: Anti-reflective film 10: Base layer 20: Top coating layer 30: Adhesive layer 40: Release film
Claims
Claim 1 An anti-reflective film comprising a substrate layer, a weather-resistant top coating layer formed on one side of the substrate layer, and an adhesive layer formed on the other side of the substrate layer, wherein the top coating layer is configured such that a pattern is transferred by laminating a pattern paper in a partially cured state and then fully cured to transfer an uneven pattern including voids, and the voids are configured to scatter light proceeding to the top coating layer to reduce surface reflectivity. Claim 2 An anti-reflective film according to claim 1, wherein the top coating layer comprises a urethane acrylate-based resin and is partially cured at a temperature of 80°C or lower, and then maintained in an environment of 50°C to 70°C for 24 hours or more to be fully cured.