Low-yield-ratio, easy-to-weld and weather-proof bridge steel and manufacturing method therefor

AU2022457248B2Pending Publication Date: 2026-11-19ANGANG STEEL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
AU2022457248
Authority / Receiving Office
AU · AU
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-05-06
Filing Date
2022-05-10
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing technologies cannot simultaneously meet the requirements for bridge steel with high strength and toughness, low yield strength ratio, good weldability and weather resistance, and also suffer from high production costs and smelting difficulties.

Method used

Specific chemical composition design and production process are adopted, including low C and low Mn design, combined with Nb, V and Ti elements to refine grains, and Ni, Cu, Cr and Mo elements to improve low temperature toughness and weather resistance. Through controlled rolling and cooling and high temperature tempering heat treatment, ferrite + pearlite or bainite composite structure is obtained, and the uniformity of the core structure of the steel plate is controlled.

Benefits of technology

Bridge steel with high strength, low yield strength ratio, excellent weldability and weather resistance has been developed, reducing production costs and improving the plasticity, toughness and low-temperature toughness of steel plates, thus meeting the weather resistance and welding requirements of bridge engineering.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000022_0000
    Figure 00000022_0000
  • Figure 00000022_0001
    Figure 00000022_0001
  • Figure 00000022_0002
    Figure 00000022_0002
Patent Text Reader

Abstract

A low-yield-ratio, easy-to-weld and weather-proof bridge steel and a manufacturing method therefor. The present invention comprises the following components in percentages by mass: C: 0.051-0.080%, Si: 0.20-0.50%, Mn: 1.20-1.50%, P≤0.010%, S≤0.003%, Cr: 0.30-0.60%, Ni: 0.20-0.50%, Cu: 0.20-0.50%, Mo: 0-0.20%, Nb: 0.02-0.06%, V: 0-0.070%, Ti: 0.005-0.025%, Al: 0.010-0.040%, CEV≤0.46%, Pcm≤0.20% and the balance of iron and inevitable impurities. The production method comprises the process steps of molten iron pretreatment, converter smelting, external refining, continuous casting, rolling, cooling, straightening and heat treatment, and the steel and the corresponding production process solve matching problems of technical indexes, such as high strength, low yield ratio, weather resistance and welding performance, of the bridge steel.
Need to check novelty before this filing date? Find Prior Art

Description

A low-yield-to-strength ratio, easily welded, weather-resistant bridge steel and its manufacturing method Technical Field

[0001] The present invention relates to the field of metal materials, and in particular to a low-yield-to-strength ratio, easily welded, weather-resistant bridge steel and a manufacturing method thereof. Background Art

[0002] Steel is widely used for long-span bridges spanning rivers, lakes, seas, and deep mountain valleys due to its advantages of high strength, light weight, and excellent plasticity and toughness. Since 1990, a series of studies have been conducted abroad on the practicality and reliability of high-performance steel in bridge engineering. These results have shown that high-performance steel offers significant improvements over conventional steel in low-temperature toughness, brittle fracture resistance, fatigue resistance, and endurance strength.

[0003] Ordinary steel bridges are prone to rust, seriously impacting their safety during service. Therefore, anti-corrosion coatings for steel bridges are crucial. However, the cost of repeated coatings during bridge construction and service is enormous. Data shows that over a 40-year service life, the cost of three re-coatings of ordinary steel exceeds twice the cost of bare weathering steel. This indicates that the use of uncoated weathering steel can significantly reduce the lifecycle cost of a bridge, offering significant economic benefits. Therefore, high-performance weathering steel is a trend in bridge development both domestically and internationally.

[0004] To ensure the safety and longevity of bridge structures, steel plates must not only possess a certain level of strength, plasticity, and toughness, but also a low yield ratio and excellent Z-axis properties. Bridge steel serving in special environments must also exhibit excellent weathering resistance. With the increasing number of steel bridge structures, improving the welding efficiency of bridge steel structure manufacturers is imperative, which requires bridge steel to possess excellent welding properties. Therefore, the development of bridge steel that combines high strength and toughness, a low yield ratio, weathering resistance, and excellent welding properties has become an urgent need for the development of new green bridges.

[0005] The complexity and diversity of technical features and indicators significantly increase the difficulty of research and development of high-strength, low-yield ratio, easily welded, weather-resistant bridge steel. First, the increase in steel plate strength increases the resistance to rolling deformation, limits the deformation rate per pass, and doubles the difficulty of grain refinement and control. The increase in steel plate thickness will lead to an increase in the temperature gradient of the thickness section, worsening the cooling and structural uniformity in the thickness direction. Secondly, the low yield ratio requirement of the steel plate will also intensify the strength-toughness contradiction, further increasing the difficulty of performance control. At the same time, bridge steel needs to have good corrosion resistance and welding performance, and the composition needs to be further optimized. Therefore, how to make high-strength bridge steel have comprehensive technical characteristics such as low yield ratio, good weather resistance and welding performance is the key problem to be solved by the present invention.

[0006] At present, there are some studies on high-strength, toughness, weather-resistant bridge steel plates at home and abroad. After searching, some patents and literature were found, but the contents recorded therein are obviously different from the composition, production method, performance, product category and other aspects described in the technical solution of the present invention.

[0007] Chinese invention patent application CN 107385358 A discloses a TMCP-type 420MPa yield strength bridge steel plate and its production method. The chemical composition and weight percentages of the steel plate are as follows: C: 0.07-0.09%, Si: 0.25-0.50%, Mn: 1.40-1.60%, P < 0.015%, S < 0.005%, Ni: 0.15-0.25%, Cr: 0.10-0.20%, Nb: 0.020-0.030%, Al: 0.030-0.050%, V: 0.030-0.040%, with the balance being Fe and unavoidable impurities. The production method includes smelting, continuous casting, heating, rolling, and cooling. The steel plate adopts a low-C, Nb, and V microalloying design, supplemented by alloying elements such as Ni and Cr to ensure balanced strength and toughness. The maximum thickness of the steel plate can reach 70mm. However, the disadvantage of this invention patent application is that the steel plate does not have weather resistance and cannot meet the requirements of exposed use of bridge steel.

[0008] Chinese invention patent application number CN 109797342 A discloses a high-strength, high-toughness, atmospheric corrosion-resistant steel plate for steel structure production and its manufacturing method, element composition wt%: C: 0.03-0.10%, Si: 0.30-0.50%, Mn: 1.10-1.50%, P < 0.010%, S < 0.003%, Cr: 0.45-0.70%, Cu: 0.25-0.40%, Ni: 0.30-0.40%, Alt: ≥ 0.030%, Ti: 0.006-0.030%, V: 0.040-0.080%, Mo: 0.02-0.08%, Ca: 0.0010-0.0030%, N: 0.0020-0.0080%, B: 0.0002-0.0030%, Ce: 0.001-0.010%, atmospheric corrosion resistance index I>6.5, CEV<0.54, Pcm<0.27, the balance being Fe and unavoidable impurities. This invention utilizes a specific chemical composition design and steel plate conditioning process to produce high-performance steel plates with a bainitic structure, suitable for use in steel structures such as bridges and high-rise buildings. However, the invention patent application has the following drawbacks: the steel plates do not have a low yield strength ratio, resulting in poor safety performance. The addition of rare elements such as Ca, B, and Ce makes smelting difficult, increasing production costs. Furthermore, the carbon equivalent is too high, resulting in poor weldability.

[0009] Chinese invention patent application CN 102534384 A discloses a Cr-free, high-performance, weather-resistant bridge steel and its preparation method. The chemical composition of this Cr-free, high-performance, weather-resistant bridge steel, by mass percentage, is as follows: C: 0.02-0.05%, Si: 0.20-0.30%, Mn: 0.6-1.00%, P ≤ 0.02%, S ≤ 0.010%, Cu: 0.20-0.40%, Ni: 0.30-0.80%, Nb: 0.04-0.07%, Ti: 0.005-0.015%, Al ≤ 0.02%, with the balance being Fe and impurities. This Cr-free, high-performance, corrosion-resistant bridge steel exhibits excellent comprehensive mechanical properties and weldability, is free of the toxic element Cr, and exhibits excellent resistance to atmospheric and marine corrosion. However, this steel, due to the addition of a relatively high amount of Ni alloy, is expensive and has a high yield strength ratio, failing to meet bridge safety requirements.

[0010] Japanese invention patent application No. JP1992173920(A) discloses a low yield ratio thick high tension plate, which contains relatively high Ni and B elements, has high cost, and has poor weather resistance, and cannot meet the requirements of relevant bridge engineering.

[0011] In summary, the existing technology is still insufficient in the research of low yield ratio, easy-to-weld weather-resistant bridge steel. Most bridge steels do not have low yield ratio and weather resistance and cannot meet the requirements of relevant engineering applications.

[0012] Summary of the Invention

[0013] The present invention aims to overcome the shortcomings of the prior art by providing a low-yield-to-strength ratio, easily weldable, weather-resistant bridge steel and a method for manufacturing the same. The product produced according to the chemical composition and production process requirements of the present steel exhibits high strength and toughness, high plasticity, a low yield ratio, excellent weather resistance, weldability, and lamellar tear resistance. The technical means employed by the present invention are as follows:

[0014] A low-yield ratio, easily welded, weather-resistant bridge steel, comprising the following components and mass percentages: C: 0.051%-0.080%, Si: 0.20%-0.50%, Mn: 1.20%-1.50%, P≤0.010%, S≤0.003%, Cr: 0.30%-0.60%, Ni: 0.20%-0.50%, Cu: 0.20%-0.50%, Mo: 0%-0.20%, Nb: 0.02%-0.06%, V: 0%-0.070%, Ti: 0.005%-0.025%, Al: 0.010%-0.040%, with the remainder being iron and unavoidable impurities. The steel has a carbon equivalent CEV≤0.46%, a welding sensitivity Pcm≤0.20%, and an atmospheric corrosion resistance index I≥6.2.

[0015] Furthermore, the maximum thickness of the steel plate is 100 mm, the yield strength is ≥345 MPa, the tensile strength is ≥500 MPa, the elongation after fracture is ≥22%, the yield strength ratio is ≤0.80, the Z-direction cross-sectional shrinkage in the thickness direction is ≥60%, and the -40°C impact energy of the steel plate base material is ≥200 J.

[0016] Furthermore, the thickness corrosion rate of the 168h immersion corrosion test under the preset atmospheric environment corrosion is 0.74~1.20g / m 2 .h.

[0017] Furthermore, the weather resistance is more than twice that of 345MPa grade ordinary bridge steel.

[0018] Furthermore, the impact energy of the welding heat affected zone at -40°C is ≥100J.

[0019] To achieve the purpose of the present invention, the present invention further discloses a technical solution, namely, a method for producing low-yield-ratio, easily welded, weather-resistant bridge steel, comprising the steps of molten iron pretreatment, converter smelting, refining outside the furnace, continuous casting, rolling, cooling, straightening, and heat treatment, wherein the steps of molten iron pretreatment, converter smelting, and refining outside the furnace can adopt existing technologies. The main specific process steps of the present invention are as follows:

[0020] 1) Continuous casting process: The continuous casting slab casting superheat is 10-25℃, and the continuous casting slab thickness is greater than 6 times the thickness of the finished steel plate; the control of casting superheat and continuous casting slab casting speed can effectively reduce the quality defects of the slab.

[0021] 2) Rolling process:

[0022] Continuous casting billet heating process: The temperature of the continuous casting billet heating section is 1210-1250℃, the temperature of the soaking section is 1190-1230℃, and the soaking section time is not less than 60 minutes; the heating process can meet the solid solution of the alloy, especially Nb and V elements, while preventing excessive growth of austenite grains; the heating time can ensure the temperature uniformity of the billet.

[0023] Rolling includes rough rolling process and finishing rolling process;

[0024] Among them, the starting rolling temperature of the rough rolling process is 1070~1120℃, and the final rolling temperature of the rough rolling is 1020~1070℃. The rolling temperature and deformation process in the rough rolling stage cause the austenite grains to recrystallize and inhibit grain growth. The rough rolling stage ensures that the deformation rate of each of at least the last two passes is greater than 15% and the pass interval does not exceed 15s. The cumulative deformation rate in the rough rolling stage is ≥50%. The large reduction and short interval process is used in the last stage of rough rolling to reduce the equipment load for producing bridge steel. The superposition effect of multiple passes of large reduction rate deformation is utilized to promote the recrystallization of austenite and achieve the goal of grain refinement, which is suitable for the production of weather-resistant bridge steel plates of the present invention; increasing the compression ratio from the continuous casting billet to the finished steel plate can effectively control the grain size, and the total compression ratio is ≥6, and the total compression ratio is the ratio of the thickness of the continuous casting billet to the thickness of the finished steel plate.

[0025] The thickness of the intermediate warm billet is 2.5 to 3.5 t, where t is the thickness of the finished steel plate. The starting rolling temperature of the finishing rolling process is 830 to 900 ° C, and the finishing rolling temperature is 770 to 830 ° C. The appropriate intermediate warm billet thickness and pass deformation rate can not only meet the deformation and deformation energy accumulation of austenite in the non-recrystallization zone, but also ensure that a sufficient deformation rate is obtained in the rough rolling stage under the condition of a certain thickness of the original casting billet, thereby achieving the purpose of grain refinement. The low finishing rolling temperature promotes the accumulation of austenite deformation energy and the induced precipitation of fine precipitates of Nb, V, and Ti, thereby increasing the nucleation position. Sufficient deformation near the phase transformation point temperature at the end of finishing rolling is conducive to the formation of fine ferrite, which can reduce the effective grain size and significantly improve the low-temperature toughness.

[0026] 3) Cooling process: After rolling, the steel plate is accelerated water cooling. After rolling, the steel plate is kept warm and the water cooling temperature is 680-740℃, the red-return temperature is 400-600℃, and the cooling rate is 10-25℃ / s. Subsequently, hot straightening and air cooling are carried out. Controlling the starting water cooling temperature of the steel plate can improve the excessive stress of the steel plate during cooling, ensure the plate shape of the steel plate, and form fine proeutectoid ferrite, making the grain size of the steel plate more uniform and further reducing the yield strength ratio of the steel plate. The appropriate final cooling temperature can promote the formation of bainite, refine the M / A island, and improve the strength of the steel plate.

[0027] To further ensure uniform grain size and improve the steel's plasticity and toughness, the process also includes a 4) heat treatment process: the rolled steel plate undergoes high-temperature tempering heat treatment at a temperature of 580-690°C for a total holding time of 2.5-4.5 min / mm, followed by air cooling to room temperature after exiting the furnace. The purpose of high-temperature tempering is to eliminate residual stress in the steel plate, making its properties more uniform and facilitating subsequent processing and manufacturing; to generate a portion of ferrite through two-phase tempering, thereby reducing the yield strength ratio; and to further refine the grain size, improving the steel's plasticity and low-temperature impact resistance.

[0028] Furthermore, during the finishing rolling process, the deformation rate of a single pass is not less than 10%.

[0029] Furthermore, after the finish rolling process, the rolled steel plates are stacked and slowly cooled, the stacking slow cooling temperature is ≥300° C., and the stacking time is ≥24 hours.

[0030] Furthermore, the final microstructure of the steel plate is one of the composite structures of ferrite + pearlite, ferrite + pearlite + bainite, and ferrite + bainite, wherein the volume percentage of ferrite is 20% to 70%.

[0031] The selection principles and content design reasons of the chemical components of the present invention are as follows:

[0032] In the present invention, carbon can exert a strengthening effect through interstitial solid solution and can also react with alloying elements such as Nb to form fine carbide precipitation. These precipitations occur before rolling deformation or austenite transformation, hindering grain growth, increasing the nucleation rate, and refining the structure. Furthermore, they can also hinder dislocation movement, effectively increasing tensile strength and reducing the yield ratio. Therefore, the carbon content should not be too low. However, increasing carbon has a negative impact on toughness, especially low-temperature toughness. Furthermore, increasing carbon can deteriorate the weldability of the steel plate. Therefore, the carbon content should not be too high either. The present invention believes that a carbon content of 0.051% to 0.080% is more suitable.

[0033] Si is a deoxidizing element in steel. It improves the steel's corrosion resistance and has a strong solid-solution strengthening effect. Si increases the amount of retained austenite in steel and reduces the yield ratio of the steel plate. However, excessive Si increases the size of bainite grains, impairing the steel's toughness and weldability. Therefore, in the present invention, the Si content is preferably controlled within a range of 0.20% to 0.50%.

[0034] Mn can effectively improve strength and hardenability; reduce the austenite phase transformation temperature, inhibit the growth of phase transformation grains before accelerated cooling of the steel plate, play a role in refining grains, and improve the strength of the steel plate; however, too high a Mn content can easily inhibit ferrite transformation, affect the yield strength of the steel, and is not conducive to reducing the yield strength ratio. Too high a Mn content can induce segregation, deteriorate the uniformity of the steel plate's structure and lamellar tearing performance, and be detrimental to welding. The present invention believes that it is more appropriate to control the Mn content within 1.20% to 1.50%.

[0035] P and S are harmful impurity elements in the present invention, and the lower the content, the better. Among them, too high P will cause structural segregation and have a significant adverse effect on low-temperature toughness. In the present invention, P is controlled to ≤0.010%. An increase in S content will promote the formation and growth of inclusions, deteriorate low-temperature performance and thickness direction performance. Therefore, S is ≤0.003%.

[0036] Cr is the main element for improving weather resistance in the present invention. The increase of Cr content is beneficial to the refinement of α-FeOOH, and Cr can replace Fe3+ Amorphous α-(Fe1-XCrX)OOH is formed. A dense rust film of α-FeOOH and δ-FeOOH is formed on the surface of the steel plate, which can protect the steel from further corrosion. The combined addition of Cr and Cu can form a denser rust layer, significantly improving weather resistance. Cr also has good hardenability. During the accelerated cooling process of steel plate rolling, it can increase the cooling rate of the steel plate core, refine the steel plate core structure, and improve the low-temperature toughness and Z-direction performance of the steel plate. However, too high a Cr content will lead to deterioration of the hot workability of the steel plate, so the Cr content is limited to 0.30% to 0.60%.

[0037] The effect of Ni on improving the strength of steel is not obvious, but it can maintain good plasticity, low-temperature toughness and corrosion resistance, and at the same time has rust resistance and heat resistance at high temperatures. When Ni is added in combination with Cr and Cu, it can not only significantly improve the low-temperature toughness, but also improve the stability of the rust layer and significantly improve the corrosion resistance. Through austenite stabilizing elements such as Ni and Mn, an appropriate amount of fine and stable reverse transformation austenite can be obtained during the two-phase zone heat treatment process, which is beneficial to the improvement of the plasticity of steel and the reduction of the yield strength ratio. However, if the Ni content is too high, a large amount of iron oxide scale that is difficult to fall off will easily form on the surface of the steel plate, and the cost will also increase. The present invention believes that it is more appropriate to control the Ni content to 0.20% to 0.50%.

[0038] Cu improves the hardenability of steel and significantly increases the core strength of thick steel plates. It is also an important element for improving weather resistance. During the slow cooling process of thick steel plates, an appropriate amount of Cu can precipitate ε-Cu through auto-tempering, thereby improving the strength of the steel plates. Excessive Cu content can reduce the surface quality and plasticity of the steel plates. The present invention considers that a Cu content of 0.20% to 0.50% is more suitable.

[0039] Mo stabilizes the rust layer and effectively improves the corrosion resistance of steel plates, particularly in chloride-containing environments, where it significantly enhances resistance to pitting and crevice corrosion. Mo also contributes to the refinement of austenite grains during rolling and improves the steel's high-temperature tempering stability. However, excessive Mo content can reduce weldability. Furthermore, Mo is a precious element, significantly increasing steel costs. Therefore, the Mo content in this steel is limited to 0% to 0.20%.

[0040] The effects of Nb in the present invention include (1) solid solution strengthening; (2) precipitation during rolling and before accelerated cooling, pinning grain boundaries, promoting nucleation, and effectively refining grains, thereby increasing strength and improving toughness; (3) lowering the austenite transformation temperature, which can refine grains; and NbC particles precipitated during high-temperature processes or combined with V and Mo to form a second phase, which can improve the high-temperature strength of the steel. However, excessive Nb content can deteriorate the toughness of the weld and heat-affected zone and increase costs. The present invention believes that controlling the Nb content to 0.02% to 0.06% is more appropriate.

[0041] Because V has a low total solution temperature and is essentially fully dissolved during soaking, the dissolved V during rolling effectively improves hardenability and recrystallization temperature. During rapid water cooling, V forms fine carbonitrides that precipitate, significantly increasing the strength of the steel plate. During high-temperature tempering, the dissolved V carbonitrides also precipitate, ensuring the high-temperature tempering strength of the steel plate. V also has both solid solution strengthening and yield strength reduction effects. Excessive V content significantly improves strength but degrades low-temperature toughness and weldability. The present invention considers controlling the V content to between 0.0% and 0.070% to be more suitable.

[0042] Ti can exert its nitrogen-binding effect, forming a precipitate primarily composed of TiN. This can inhibit austenite grain growth under high-temperature conditions and improve the toughness of the heat-affected zone (HAZ) after welding. During welding, TiN particles prevent grain growth in the heat-affected coarse-grained zone, enhancing the low-temperature toughness of the welded joint. Furthermore, due to its low solid solubility, Ti readily forms interphase precipitations during the austenite-to-ferrite transformation, improving high-temperature strength. However, excessive Ti content can reduce the toughness of the steel. The present invention proposes that a Ti content of 0.005% to 0.0025% is more suitable.

[0043] Al is a strong deoxidizing element and can also combine with nitrogen to form AlN, which can refine grains, improve low-temperature impact toughness, and lower the brittle transition temperature of steel. Al also has antioxidant and corrosion resistance. When used in combination with Cr and Si, Al can significantly improve the high-temperature non-scaling performance and high-temperature corrosion resistance of steel. However, excessive Al content is detrimental to weldability. The present invention believes that the Al content should be controlled between 0.010% and 0.040%.

[0044] The carbon equivalent value (CEV) and weld crack sensitivity index (Pcrn) can predict the steel's tendency to cold crack. Lower values ​​indicate a lower tendency to crack during welding and better weldability. The calculation formulas are: Carbon equivalent (CEV%) = C + Mn / 6 + (Cr + Mo + V) / 5 + (Ni + Cu) / 15; Weld crack sensitivity index (Pcm%) = C + Si / 30 + Mn / 20 + Cu / 20 + Ni / 60 + Cr / 20 + Mo / 15 + V / 10 + 5B. The present invention has a CEV of ≤0.46% and a Pcm of ≤0.20, demonstrating excellent weldability.

[0045] The I value is the atmospheric corrosion resistance index, and its calculation formula is:

[0046] I=26.01(%Cu)+3.88(%Ni)+1.20(%Cr)+1.49(%Si)+17.28(%P)-7.29(%Cu)(%Ni)-9.10(%Ni)(%P)-33.39(%Cu) 2 When the I value is ≥6.0, the steel is considered corrosion-resistant steel and can be used bare steel (unpainted) when normally exposed to air. The steel plate of the present invention has an I value of ≥6.20 and has good atmospheric corrosion resistance.

[0047] The present invention has the following advantages:

[0048] 1. The composition of the present invention improves material toughness through low C and low Mn design, utilizes Nb, V, and Ti elements to inhibit austenite grain growth and promote nucleation during austenite transformation to refine grains, control the core structure of the steel plate thickness, and improve structural uniformity; increases the solid solution strengthening effect of Ni, Cu, Cr, and Mo elements to improve the low-temperature toughness and weather resistance of the steel plate; and, combined with the corresponding production process, solves the difficult problem of matching technical indicators such as high strength, low yield ratio, weather resistance, and weldability for bridge steel.

[0049] 2. The present invention does not add rare earth elements, which reduces the cost of some alloys and further improves the plasticity and toughness of the steel plate.

[0050] 3. The present invention has low CEV and Pcm, high I value, and excellent welding performance and weather resistance.

[0051] 4. The smelting and continuous casting process scheme of the present invention improves the quality of the ingot, thereby improving the low-temperature toughness and Z-direction performance of the steel plate.

[0052] 5. The present invention utilizes a high-temperature tempering heat treatment process to ultimately achieve a composite microstructure composed of one of ferrite + pearlite, ferrite + bainite, or ferrite + pearlite + bainite. Proper control of the ratio of the soft and hard phases optimizes strength, plasticity, and toughness, achieving increased strength while reducing the yield strength ratio, thereby achieving excellent seismic performance.

[0053] 6. The present invention is a manufacturing method of controlled rolling, controlled cooling and one-time heat treatment, and the process is simple.

[0054] 7. The low-yield-ratio, easily weldable, weather-resistant bridge steel plate described in this invention has a maximum thickness of 100 mm, a yield strength ≥345 MPa, a tensile strength ≥500 MPa, an elongation ≥22%, a yield ratio ≤0.80, a through-thickness Z-axis performance ≥60%, an impact energy at -40°C ≥200 J, and weather resistance more than twice that of ordinary 345 MPa-grade bridge steel. The impact energy at -40°C in the weld heat-affected zone is ≥100 J. This plate meets the seismic, weathering, and weldability requirements for bridge steel under low-temperature conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.

[0056] FIG1 is a metallographic structure diagram of Example 1 of the present invention.

[0057] FIG2 is a metallographic structure diagram of Example 4 of the present invention.

[0058] FIG3 is a metallographic structure diagram of Example 7 of the present invention. DETAILED DESCRIPTION

[0059] To make the objectives, technical solutions, and advantages of the embodiments of the present invention more clear, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts shall fall within the scope of protection of the present invention.

[0060] The chemical composition of the embodiments of the present invention is shown in Table 1; the smelting continuous casting and slab heating processes of the corresponding embodiments are shown in Table 2; the roughing process of the corresponding embodiments is shown in Table 3; the finishing process of the corresponding embodiments is shown in Table 4; the cooling and heat treatment system of the corresponding embodiments is shown in Table 5; the performance and microstructure ratio of the corresponding embodiments are shown in Table 6; the corrosion rate of the corresponding embodiments is shown in Table 7, wherein the metallographic diagrams of Examples 1, 4, and 7 are shown in Figures 1 to 3, respectively.

[0061] Table 1 Chemical composition (wt%) of the examples of the present invention

[0062] Example CSiMnSPCrNiCuMoNbVTiAlCEVPcmI10.0510.311.210.0030.0090.420.280.2600.02200.0080.0230.370.166.220.0630.421.400.0020.0080.440.340.380.040.0450.0550.0120.030.450.206.730.0710.351.350. 0030.0100.390.460.360.030.0580.0620.0180.0340.450.206.740.0520.431.370.0020.0090.360.450.280.040.0240.0480.0150.0330.420.186.750.060.351.260.0020.0100.530.270.3500.0320.0220.0170.0350 .420.196.760.0550.381.230.0020.0080.480.420.450.030.0550.0450.0140.0320.430.196.470.0580.321.420.0030.0070.460.330.270.120.0340.0580.0210.0250.460.206.380.0750.461.330.0020.0100.420.2 50.250.050.0470.0660.0110.0280.440.206.390.0710.361.400.0020.0090.420.350.320.040.0420.0520.0140.0230.450.206.6100.0650.411.350.0030.0100.450.320.430.050.0410.0470.0120.0320.450.206.5

[0063] Table 2 Continuous casting and slab heating process of the embodiment of the present invention

[0064] Example Pouring superheat, °C Heating section temperature / °C Soaking temperature / °C Soaking section time / min 118 1220 119769 2211228 1207783 20123 112098 24221230 1217765 191245 12107862 11240 121273 723 1229 121675 820 123 31211809 211238 11989 210 221243 122895

[0065] Table 3 Rough rolling process of the embodiment of the present invention

[0066]

[0067] Table 4 Finishing rolling process of the embodiment of the present invention

[0068]

[0069] Table 5 Cooling and heat treatment process of the embodiment of the present invention

[0070]

[0071] The present invention smelted and rolled 10 embodiments according to the chemical composition of Table 1 and the production process of Tables 2 to 5. The properties of the 10 smelted and rolled embodiments of the present invention are shown in Table 6.

[0072] Table 6 Performance and microstructure ratio of the embodiments of the present invention

[0073]

[0074] The weather resistance of the present invention was evaluated by mass loss after a 168-hour cyclic immersion corrosion test. Specifically, the corrosion test solution was 0.01 mol / L NaHSO3; the replenishing solution was 0.02 mol / L NaHSO3; the test temperature was 45±2°C; the relative humidity was 70±5%; and the cyclic immersion wheel speed was 1 revolution / 60 minutes. The results are shown in Table 7.

[0075] Table 7 Corrosion rate of the embodiment of the present invention

[0076]

[0077]

[0078] The present invention discloses a low-yield ratio, easily welded, weather-resistant bridge steel and a manufacturing method thereof. The composition design improves the toughness and welding performance of the material through low C and low Mn, utilizes Nb, Ti, and V elements to inhibit the growth of austenite grains and promote nucleation during the austenite transformation to refine the grains, control the thickness core structure of the steel plate, and improve the uniformity of the structure; at the same time, based on the high strength characteristic, the effect of Nb on suppressing austenite recrystallization is utilized to increase the rolling temperature, effectively reduce the rolling resistance, and also facilitate the increase of the deformation rate of the rolling pass; the solid solution strengthening effect is increased by the Ni element, and the low-temperature toughness is improved by the Ni element; the hardenability of the steel plate is improved by using Cr, Cu, and Mo, the solid solution strengthening effect is enhanced, and the weather resistance of the steel plate can be improved; and corresponding smelting, heating, rolling, cooling, heat treatment and other production processes are used to obtain comprehensive properties such as high strength, low yield ratio, good weather resistance, and weldability, as well as an ideal microstructure.

[0079] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the above embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A low-yield-ratio, easy-to-weld and weather-resistant bridge steel, comprising the following components in percentages by mass: C: 0.051%-0.080%, Si: 0.20%-0.50%, Mn: 1.20%-1.50%, P < 0.010%, S < 0.003%, Cr: 0.30%-0.60%, Ni: 0.20%-0.50%, Cu: 0.20%-0.50%, Mo: 0%-0.20%, Nb: 0.02%-0.06%, V: 0%-0.070%, Ti: 0.005%-0.025%, Al: 0.010%-0.040%, and a balance of iron and inevitable impurities,CEV < 0.46%, Pcm < 0.20%, and an atmospheric corrosion resistance index I > 6.2, Wherein the steel further hasCEV%=C+Mn / 6+(Cr+Mo+V) / 5+(Ni+Cu) / 15;Pcm%= C + Si / 30 + Mn / 20 + Cu / 20 + Ni / 60 + Cr / 20 + Mo / 15 + V / 10 + 5B; andI=26.01(%Cu)+3.88(%Ni)+1.20(%Cr)+1.49(%Si)+17.28(%P)-7.29(%Cu)(%Ni)-9.10(%Ni)(%P)-33.39(%Cu)2; anda yield ratio of <0.80, a Z-direction area reduction in a thickness direction of >60%, and an impact energy of a base material at -40 °C of >200 J; wherein the steel is in the form of a steel plate having a thickness of not more than 100 mm, a yield strength of >345 MPa, a tensile strength of >500 MPa, and an elongation after fracture of >22%; and wherein the final microstructure of the steel plate is a composite structure selected from ferrite + pearlite, ferrite + bainite, and ferrite + pearlite + bainite, wherein the volume percentage of ferrite is 20%-70%.

2. The low-yield-ratio, easy-to-weld and weather-resistant bridge steel according to claim 1, wherein in a preset atmospheric corrosion environment, a thickness corrosion rate in a 168 h alternate immersion corrosion test is 0.74-1.20 g / m2^h.

3. The low-yield-ratio, easy-to-weld and weather-resistant bridge steel according to claim 1, wherein an impact energy of a heat affected zone in welding of the steel plate at -40°C is >100 J.

4. A method for preparing the low-yield-ratio, easy-to-weld and weather-resistant bridge steel according to any one of claims 1 to 3, comprising process steps of continuous casting, rolling, cooling, straightening and heat treatment, wherein the process steps are as follows:1) the continuous casting process: a casting superheat temperature of a continuous casting billet is 10-25C;2) the rolling process:heating of the continuous casting billet: a heating zone temperature of the continuous casting billet is 1210-1250C, a soaking zone temperature is 1190-1230C, and a soaking time is not less than 60 min;2022457248   21 Oct 2026the rolling process comprises rough rolling and finish rolling;wherein,an initial rolling temperature of the rough rolling is 1070-1120C, a finishing rolling temperature of the rough rolling is 1020-1070C, it should be ensured that each deformation rate of at least the last two passes is greater than 15% and a pass interval does not exceed 15 s in the rough rolling, and a cumulative deformation rate in the rough rolling is >50%;a thickness of an intermediate billet at holding temperature is 2.5t - 3.5t, wherein t is a thickness of the finished steel plate;an initial rolling temperature of the finish rolling is 830-900C, and a finishing rolling temperature of the finish rolling is 770-830C, and a deformation rate of each pass is not less than 10% in the finish rolling;3) the cooling process: a rolled steel plate is subjected to accelerated water cooling, wherein the steel plate is subjected to temperature holding after completion of the rolling, an initial temperature of water cooling is 680-740C, a self-tempering temperature is 400-600C, and a water cooling rate is 10-25C / s; subsequently, the water-cooled steel plate is subjected to thermal straightening and air cooling, followed by stacking for slow cooling, with a stacking temperature of >300°C and a stacking time of >24 h; and4) the heat treatment: the rolled steel plate is subjected to high-temperature tempering, wherein a heating temperature is 580-690C, a total holding time is 2.5-4.5 min / mm, and the steel plate is air-cooled to room temperature after taken out of a furnace.

Citation Information

Patent Citations

  • Weather-resistance bridge high-strength steel plate and production method thereof

    CN101876032A