α-olefin polymer, preparation method therefor and use thereof
Patent Information
- Application Number
- AU2023370362
- Authority / Receiving Office
- AU · AU
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-10-25
- Filing Date
- 2023-10-25
- Publication Date
- 2026-11-19
AI Technical Summary
While existing olefin copolymer viscosity index improvers improve high-temperature lubrication efficiency, it is difficult to balance system stability and thickening ability at low temperatures, and when α-olefin is used as the main polymerization monomer, the thickening efficiency is poor.
Using a late transition metal catalyst consisting of α-olefin monomers with diimine as the ligand to polymerize, an α-olefin polymer with 58-87% main chain carbon atoms is used as a viscosity index improver in lubricating oils. Achieve excellent thickening efficiency.
It overcomes the problem of low thickening efficiency of α-olefin polymers at high temperatures, provides higher thickening efficiency and a wider selection of viscosity index improvers, and significantly improves the viscosity performance of lubricating oils.
Abstract
Description
Alpha-olefin polymer and its preparation method and application
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of Chinese patent application 202211308644.8 filed on October 25, 2022, Chinese patent application 202211308376.X filed on October 25, 2022, and Chinese patent application 202211309110.7 filed on October 25, 2022, the contents of which are incorporated herein by reference. Technical Field
[0003] The present invention relates to the technical field of olefin polymerization, and in particular to an alpha-olefin polymer and a preparation method and application thereof. Background Art
[0004] Lubricating oils often require additives in actual use, such as detergents and dispersants, viscosity index improvers, and antioxidants, to improve their properties. Among these, viscosity index improvers are a very important type of additive.
[0005] The viscosity of lubricating oil varies significantly with temperature. At low temperatures, viscosity increases, while at higher temperatures, viscosity decreases, resulting in poor lubrication. The addition of a viscosity index improver can effectively enhance lubrication efficiency at high temperatures, thereby improving the viscosity-temperature performance of the lubricant. Among these, olefin copolymer viscosity index improvers (OCPs) are the most widely used, offering suitable thickening capacity and shear stability at a moderate price.
[0006] Olefin copolymer viscosity index improvers typically use ethylene as the primary monomer. However, these copolymers struggle to achieve good thickening performance, solubility, and low-temperature stability. To ensure solubility in base oils and maintain stability at low temperatures, α-olefins such as propylene are typically copolymerized with ethylene to increase the branch content of the polyolefin. However, while increasing the α-olefin copolymerization ratio, and therefore the branch content, significantly improves solubility and low-temperature stability, it also significantly reduces thickening performance. To ensure adequate thickening efficiency, the branch content must be kept to a minimum. For example, when preparing viscosity index improvers using ethylene-propylene copolymerization, the propylene unit content in the polymer typically does not exceed 50%. Therefore, in traditional production methods, the amount of α-olefin used as a comonomer is strictly limited. Furthermore, using α-olefins (especially long-chain α-olefins) as the primary monomer typically results in low viscosity and poor thickening efficiency due to excessive branch content.
[0007] Summary of the Invention
[0008] The present invention aims to overcome the problems of the prior art in which the amount of α-olefin used in preparing olefin copolymer viscosity index improvers is strictly limited, and the olefin polymers prepared using α-olefin as the main polymerization monomer have poor thickening efficiency. The present invention provides an α-olefin polymer, a preparation method, and applications thereof. The α-olefin polymer according to the present invention is obtained entirely from the polymerization of one α-olefin or two or more α-olefins, and the α-olefin polymer has excellent thickening efficiency when used as a viscosity index improver for lubricating oils.
[0009] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides an α-olefin polymer, which is formed by polymerizing at least one α-olefin monomer CH2=CHR. In the α-olefin polymer, the carbon atoms located in the main chain account for 58-87% of the total number of carbon atoms, wherein R is a linear or branched alkyl group with a carbon atom number ≥2; the weight-average molecular weight of the α-olefin polymer is 10,000-250,000, preferably 25,000-150,000, and more preferably 30,000-120,000; the molecular weight distribution PDI of the α-olefin polymer is <3, preferably ≤2.
[0010] The second aspect of the present invention provides a method for preparing the α-olefin polymer described above, which comprises: polymerizing an α-olefin monomer having a carbon number of not less than 4 in the presence of a main catalyst, a co-catalyst, an optional reversible chain transfer agent and an optional solvent, wherein the main catalyst is a late transition metal catalyst with a diimine as a ligand.
[0011] The third aspect of the present invention provides use of the aforementioned α-olefin polymer as a viscosity index improver.
[0012] A fourth aspect of the present invention provides a lubricating oil comprising a base oil and the α-olefin polymer described above.
[0013] According to the technical solution of the present invention, the α-olefin polymer has good thickening efficiency, overcoming the technical problem that the α-olefin polymer contains too many branched carbons, which makes the α-olefin polymer have poor performance as a viscosity index improver in the prior art.
[0014] Moreover, the present invention uses α-olefin polymer as a viscosity index improver, further broadening the optional types of viscosity index improvers. Whether from the practical aspect or the technical research direction, the polyα-olefin viscosity index improver of the present invention has extremely high value. DETAILED DESCRIPTION
[0015] The following is a detailed description of the specific embodiments of the present invention. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention and are not intended to limit the present invention.
[0016] The α-olefin polymer of the present invention is formed by polymerizing at least one α-olefin monomer (CH2=CHR), wherein R is a linear or branched alkyl group having ≥ 2 carbon atoms. In the α-olefin polymer, the carbon atoms in the backbone chain account for 58-87%, preferably 60-85%, and more preferably 63-82% of the total carbon atoms.
[0017] The α-olefin polymer comprises a first unit -(CH2)-, a second unit -CH(CH3)-, and a third unit -CH(R)-. The first unit accounts for 77% or more of the total number of carbon atoms in the main chain of the α-olefin polymer, and the third unit accounts for 18% or less of the total number of carbon atoms in the main chain of the α-olefin polymer. Preferably, the first unit accounts for 80-95% of the total number of carbon atoms in the main chain of the α-olefin polymer, the second unit accounts for 1-10% of the total number of carbon atoms in the main chain of the α-olefin polymer, and the third unit accounts for 2-12% of the total number of carbon atoms in the main chain of the α-olefin polymer. In the present invention, the third unit is a unit obtained by α-olefin monomers without undergoing chain walking.
[0018] In the present invention, the weight average molecular weight of the α-olefin polymer is 10,000-250,000, preferably 25,000-150,000, and more preferably 30,000-120,000.
[0019] In the present invention, the molecular weight distribution PDI of the α-olefin polymer is less than 3, preferably ≤2, and more preferably 1.01-2.
[0020] In the present invention, the weight average molecular weight M of the α-olefin polymer is w The molecular weight distribution (PDI) was determined by gel permeation chromatography-infrared detector (GPC-IR).
[0021] In some embodiments, the α-olefin polymer is obtained by homopolymerizing an α-olefin monomer once, and has a weight average molecular weight of 20,000-250,000 (preferably 30,000-150,000) and a molecular weight distribution PDI <3 (preferably ≤2).
[0022] In a preferred embodiment, the α-olefin polymer is a diblock polymer AB or a triblock polymer ABA, wherein the degree of branching of the A block is greater than that of the B block. α-olefin polymers according to this preferred embodiment have improved thickening efficiency. In the present invention, the degree of branching refers to the number of branches per 1000 carbon atoms, as measured by gel permeation chromatography-infrared detection (GPC-IR).
[0023] When the α-olefin polymer is a diblock polymer or triblock polymer, in some embodiments, the α-olefin polymer is obtained from a single α-olefin monomer through at least two stages of continuous homopolymerization. During the at least two stages of continuous homopolymerization, the reaction temperature and / or α-olefin monomer concentration are controlled in different reaction stages to form a diblock polymer or triblock polymer having two or more blocks with different degrees of branching. In this embodiment, the α-olefin polymer has a weight-average molecular weight of 22,000-180,000 (preferably 32,000-160,000) and a molecular weight distribution (PDI) of <3 (preferably ≤2).
[0024] When the α-olefin polymer is a diblock polymer, in other embodiments, the α-olefin polymer is obtained by continuous homopolymerization of two α-olefin monomers in two stages, wherein each stage uses a different α-olefin monomer. In this embodiment, the α-olefin polymer has a weight-average molecular weight of 10,000-250,000 (preferably 25,000-150,000) and a molecular weight distribution (PDI) of less than 3 (preferably ≤2).
[0025] In the present invention, when the α-olefin polymer is a diblock polymer AB or a triblock polymer ABA, preferably, the degree of polymerization during the reaction stage is controlled so that the A block is amorphous (i.e., non-crystalline) and the B block has a certain degree of crystallinity. In this case, the B block in the block polymer has a melting point, while the A block does not. More preferably, the melting point of the block polymer is between -50°C and 80°C.
[0026] In the present invention, the α-olefin monomer is a linear or branched α-olefin having 4 to 20 carbon atoms (preferably 4 to 12, specifically, for example, 4, 5, 6, 7, 8, 9, 10, 11 or 12). Preferably, the α-olefin monomer is at least one selected from 1-butene, 2-methyl-1-butene, 3,3-dimethyl-1-butene, 1-pentene, 1-pentene substituted with one or more methyl, ethyl or propyl groups, 1-hexene, 1-hexene substituted with one or more methyl, ethyl or propyl groups, 1-heptene, 1-heptene substituted with one or more methyl, ethyl or propyl groups, 1-octene substituted with one or more methyl, ethyl or propyl groups, 1-nonene, 1-decene and 1-dodecene. More preferably, the α-olefin monomer is selected from at least one of 1-butene, 2-methyl-1-butene, 3,3-dimethyl-1-butene, 1-pentene, 1-pentene substituted with one or more methyl, ethyl, or propyl groups, 1-hexene, 1-hexene substituted with one or more methyl, ethyl, or propyl groups, 1-heptene, and 1-heptene substituted with one or more methyl, ethyl, or propyl groups, that is, preferably an α-olefin monomer having less than 8 carbon atoms.
[0027] The preparation method of the α-olefin polymer described in the present invention comprises: polymerizing an α-olefin monomer having a carbon number of not less than 4 in the presence of a main catalyst, a co-catalyst, an optional reversible chain transfer agent and an optional solvent, wherein the main catalyst is a late transition metal catalyst with a diimine as a ligand.
[0028] According to the preparation method of the α-olefin polymer described in the present invention, by using a late transition metal catalyst with a diimine as a ligand, the branching degree of the α-olefin polymer can be greatly reduced, so that the prepared α-olefin polymer exhibits good thickening efficiency when used as a viscosity index improver for lubricating oil. Its thickening efficiency is significantly improved compared with conventional α-olefin polymers, breaking the ratio limit of traditional α-olefins when used as viscosity index improvers.
[0029] In the method of the present invention, the polymerization reaction process may include only one reaction stage, or may include at least two reaction stages.
[0030] In some embodiments, the polymerization process includes only one reaction stage, and only one α-olefin monomer is used in the polymerization process.
[0031] In other embodiments, the polymerization process comprises at least two reaction stages, and the same α-olefin monomer is used in each reaction stage. In this embodiment, by controlling the reaction temperature and / or the concentration of the α-olefin monomer in the different reaction stages, a diblock polymer AB or a triblock polymer ABA is formed, wherein the degree of branching of the A block is greater than that of the B block.
[0032] In the above embodiment, controlling the reaction temperature in different reaction stages includes: making the absolute value of the difference between the polymerization reaction temperatures of two adjacent reaction stages not less than 10°C, preferably not less than 20°C.
[0033] In the above embodiment, controlling the concentration of the α-olefin monomer in different reaction stages includes: making the ratio of the concentrations of the α-olefin monomer in two adjacent reaction stages greater than 3.
[0034] In other embodiments, the polymerization process includes at least two reaction stages, and the α-olefin monomers used in each reaction stage are different. That is, by controlling the type of α-olefin monomers in different reaction stages, a diblock polymer AB or a triblock polymer ABA is formed, wherein the degree of branching of block A is greater than that of block B. In this embodiment, preferably, in two adjacent reaction stages, the number of carbon atoms in the α-olefin monomer added in the latter reaction stage is less than the number of carbon atoms in the α-olefin monomer added in the previous reaction stage.
[0035] In the method of the present invention, the reaction temperature of the polymerization reaction may be -40°C to 100°C, preferably 0°C to 70°C.
[0036] In the method of the present invention, the reaction time of the polymerization reaction can be 5 min-48 h, preferably 10 min-24 h.
[0037] In the method of the present invention, the concentration of the α-olefin monomer can be greater than 0.05 mol / L. The concentration range of the α-olefin monomer varies depending on the type of α-olefin monomer. For example, the concentration of an α-olefin monomer having 6 carbon atoms can be less than 8.15 mol / L, and the concentration of an α-olefin monomer having 14 carbon atoms can be less than 3.9 mol / L.
[0038] In some embodiments, the polymerization reaction process includes two reaction stages, and a diblock polymer is formed by controlling the reaction temperature of different reaction stages. Specifically, the reaction temperature of one reaction stage is -20°C to 30°C, preferably 0°C to 30°C, and the corresponding reaction time is 5 min-48 h, preferably 10 min-18 h; the reaction temperature of the other reaction stage is 0°C to 80°C, preferably 25°C to 55°C, and the corresponding reaction time is 5 min-24 h, preferably 5 min-4 h, and more preferably 5 min-2 h.
[0039] In other embodiments, the polymerization process includes at least two reaction stages, and the diblock polymer is formed by controlling the α-olefin monomer concentration in different reaction stages. Specifically, the ratio of the α-olefin monomer concentrations in two adjacent reaction stages is greater than 3, preferably greater than 8, and the α-olefin monomer concentration in the reaction stage with the lower monomer concentration is 0.1-2 mol / L, preferably 0.2-1 mol / L. Further preferably, the reaction time of the reaction stage with the lower monomer concentration in the adjacent reaction stages is 30 minutes to 18 hours, and the reaction time of the reaction stage with the higher monomer concentration is 3 minutes to 40 minutes.
[0040] In the present invention, the main catalyst can be selected from conventional late transition metal catalysts. In a preferred embodiment, the main catalyst is a metal complex represented by formula (I),
[0041] In formula (I), M is a Group VIII metal. Preferably, M is selected from nickel and palladium.
[0042] In formula (I), R1 and R4 may be the same or different and are each independently selected from a C1-C30 hydrocarbon group or a heterohydrocarbon group, and R1 and R4 may optionally form a ring with each other. Here, the C1-C30 hydrocarbon group may be selected from a substituted or unsubstituted C1-C30 alkyl group, a substituted or unsubstituted C2-C30 alkenyl group, a substituted or unsubstituted C2-C30 alkynyl group, a substituted or unsubstituted C6-C30 aryl group, a substituted or unsubstituted C7-C30 aralkyl group, and a substituted or unsubstituted C7-C30 alkaryl group; the C1-C30 heterohydrocarbon group may be selected from a substituted or unsubstituted C1-C30 alkoxy group, a substituted or unsubstituted C2-C30 alkenyloxy group, and a substituted or unsubstituted C2-C30 alkynyloxy group.
[0043] In a preferred embodiment, R1 and R4 are each independently selected from a substituted or unsubstituted C1-C20 alkyl group and a substituted or unsubstituted C6-C20 aryl group. Further preferably, R1 and R4 are each independently selected from a substituted or unsubstituted C1-C10 alkyl group and a substituted or unsubstituted C6-C15 aryl group.
[0044] In the most preferred embodiment, R1 and R4 are each a group represented by formula II,
[0045] In formula (II), R 1 -R 5 may be the same or different, and are independently selected from hydrogen, halogen, hydroxyl, and substituted or unsubstituted C1-C30 hydrocarbon or heterohydrocarbon groups, and R 1 -R 5They may optionally form a ring with each other. Here, the C1-C30 hydrocarbon group may be selected from substituted or unsubstituted C1-C30 alkyl groups, substituted or unsubstituted C2-C30 alkenyl groups, substituted or unsubstituted C2-C30 alkynyl groups, substituted or unsubstituted C6-C30 aryl groups, substituted or unsubstituted C7-C30 aralkyl groups, and substituted or unsubstituted C7-C30 alkaryl groups; the C1-C30 heterohydrocarbon group may be selected from substituted or unsubstituted C1-C30 alkoxy groups, substituted or unsubstituted C2-C30 alkenyloxy groups, and substituted or unsubstituted C2-C30 alkynyloxy groups.
[0046] In the preferred case, R 1 and R 3 Each is independently selected from a substituted or unsubstituted C3-C10 alkyl or heteroalkyl group. Here, the C3-C10 alkyl group can be n-propyl, isopropyl, n-butyl, isobutyl, pentyl, heptyl, octyl, etc.; the C3-C10 heteroalkyl group can be selected from a substituted or unsubstituted C3-C10 alkoxy group, a substituted or unsubstituted C3-C10 alkenyloxy group, and a substituted or unsubstituted C3-C10 alkynyloxy group.
[0047] In formula (I), R2 and R3 may be the same or different and are each independently selected from hydrogen, a halogen (particularly a chlorine atom), and a C1-C20 hydrocarbon group or heterohydrocarbon group, and R2 and R3 may optionally form a ring with each other. Here, the C1-C20 hydrocarbon group may be selected from a substituted or unsubstituted C1-C20 alkyl group, a substituted or unsubstituted C2-C20 alkenyl group, a substituted or unsubstituted C2-C20 alkynyl group, a substituted or unsubstituted C6-C20 aryl group, a substituted or unsubstituted C7-C20 aralkyl group, and a substituted or unsubstituted C7-C20 alkaryl group; the C1-C20 heterohydrocarbon group may be selected from a substituted or unsubstituted C1-C20 alkoxy group, a substituted or unsubstituted C2-C20 alkenyloxy group, and a substituted or unsubstituted C2-C20 alkynyloxy group.
[0048] Preferably, R2 and R3 are each independently selected from substituted or unsubstituted C6-C20 aryl, substituted or unsubstituted C7-C20 aralkyl and substituted or unsubstituted C7-C20 alkylaryl, or R2 and R3 are cyclized to form an aralkylene group.
[0049] In formula (I), -L nrepresents n L groups connected to the metal M. The n L groups may be the same or different and each may be selected from a halogen, a C1-C10 hydrocarbon group, and a C1-C10 hydrocarbonoxy group; n is an integer satisfying the valence of M. Here, the C1-C10 hydrocarbon group may be selected from a substituted or unsubstituted C1-C10 alkyl group, a substituted or unsubstituted C2-C10 alkenyl group, a substituted or unsubstituted C2-C10 alkynyl group, a substituted or unsubstituted C6-C10 aryl group, a substituted or unsubstituted C7-C10 aralkyl group, and a substituted or unsubstituted C7-C10 alkaryl group; the C1-C10 hydrocarbonoxy group may be selected from a substituted or unsubstituted C1-C10 alkoxy group, a substituted or unsubstituted C2-C10 alkenyloxy group, and a substituted or unsubstituted C2-C10 alkynyloxy group. The halogen here may be selected from fluorine, chlorine, bromine, and iodine, with bromine being most preferred.
[0050] In the present invention, the alkyl group may be a linear alkyl group, a branched alkyl group or a cycloalkyl group. The alkoxy group may be a linear alkoxy group, a branched alkoxy group or a cycloalkoxy group.
[0051] In the present invention, the "substituted" in "substituted or unsubstituted" refers to containing substituents, and the substituents here can be selected from, for example, halogen, hydroxyl, C1-C6 alkyl, halogenated C1-C6 alkyl, C1-C6 alkoxy and halogenated C1-C6 alkoxy.
[0052] In the present invention, the alkyl group (such as C1-16 alkyl, C1-C20 alkyl or C1-C30 alkyl) can be selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, n-pentyl, isopentyl, n-hexyl, isohexyl and 3,3-dimethylbutyl.
[0053] In the present invention, the alkoxy group (such as C1-C10 alkoxy, C1-C20 alkoxy, C1-C30 alkoxy) can be selected from, for example, methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, n-pentoxy, isopentoxy, n-hexoxy, isohexoxy and 3,3-dimethylbutoxy.
[0054] In the present invention, the aryl group (eg, C6-C10 aryl group, C6-C20 aryl group, C6-C30 aryl group) can be selected from, for example, phenyl group, 4-methylphenyl group, 4-ethylphenyl group, dimethylphenyl group, and vinylphenyl group.
[0055] In the present invention, the halogen is selected from fluorine, chlorine, bromine and iodine.
[0056] The above-mentioned late transition metal catalysts can be commercially obtained or prepared according to conventional methods in the art. The specific preparation methods can refer to the methods disclosed in patent applications CN111116787A, CN112745362A, CN114478868A and documents such as Polymers 2018, 10, 2073-4360, Macromolecules 2014, 47, 3325-3331, Angew. Chem., Int. Ed. 2004, 43, 1821-1825, and J. Am. Chem. Soc. 2014, 136, 7213-7216. The relevant contents disclosed in the above-mentioned documents are fully incorporated into the present invention as a reference and will not be repeated here.
[0057] In the present invention, the co-catalyst can be selected from a wide range. In a preferred embodiment of the present invention, the co-catalyst is selected from at least one of an organoaluminum compound and an organoboron compound.
[0058] In the present invention, the organoaluminum compound may be selected from one or more of alkylaluminoxanes, alkylaluminums, and alkylaluminum halides. Specific examples of the organoaluminum compound may be selected from, but are not limited to, at least one of trimethylaluminum, triethylaluminum, triisobutylaluminum, tri-n-hexylaluminum, trioctylaluminum, diethylaluminum monohydrogen, diisobutylaluminum monohydrogen, diethylaluminum monochloride, diisobutylaluminum monochloride, ethylaluminum sesquichloride, ethylaluminum dichloride, methylaluminoxane (MAO), and modified methylaluminoxane (MMAO). In a preferred embodiment, the organoaluminum compound is at least one of MAO, MMAO, diethylaluminum monochloride, ethylaluminum dichloride, and ethylaluminum sesquichloride.
[0059] In the present invention, the organoboron compound may be selected from at least one of an aromatic boron and a borate. Specific examples of the organoboron compound may be selected from, but are not limited to, at least one of trispentafluorophenylboron, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, and triphenylmethyl tetrakis(pentafluorophenyl)borate.
[0060] In the present invention, the reversible chain transfer agent may be a dialkyl zinc. Specific examples of the dialkyl zinc include, but are not limited to, at least one of diethyl zinc, di(n-propyl) zinc, and di(n-octyl) zinc. When a dialkyl zinc (particularly diethyl zinc) is added as a reversible chain transfer agent during the reaction, the thickening efficiency of the prepared α-olefin polymer can be further improved.
[0061] In some preferred embodiments, when the polymerization reaction process includes two reaction stages, and the reaction temperatures and / or α-olefin monomer concentrations in the two reaction stages differ, the polymerization reaction time for each reaction stage can be appropriately adjusted based on the catalyst system employed. For example, when the cocatalyst is methylaluminoxane (MAO), modified methylaluminoxane (MMAO), sesquiethylaluminum chloride, arylborone, etc., the reaction time is preferably 5 minutes to 2 hours, more preferably 10 minutes to 1 hour, in the low-concentration or low-temperature reaction stage; and preferably 3 minutes to 1 hour, more preferably 5 minutes to 30 minutes, in the high-concentration or high-temperature reaction stage. When the co-catalyst is trimethylaluminum, triethylaluminum, triisobutylaluminum, tri-n-hexylaluminum, trioctylaluminum, diethylaluminum monohydrogen, diisobutylaluminum monohydrogen, diethylaluminum monochloride, diisobutylaluminum monochloride, ethylaluminum dichloride, etc., in the low concentration or low temperature reaction stage, the reaction time is preferably 10 min-48 h, more preferably 30 min-18 h; in the high concentration or high temperature reaction stage, the reaction time is preferably 10 min-24 h, more preferably 20 min-2 h.
[0062] In the present invention, when the co-catalyst is an organoaluminum compound, the molar ratio of aluminum in the co-catalyst to M in the main catalyst can be (10-10 7 ):1, (for example, 10:1, 20:1, 50:1, 100:1, 200:1, 300:1, 500:1, 700:1, 800:1, 1000:1, 2000:1, 3000:1, 5000:1, 10000:1, 1000000:1, 10000000:1 and any value therebetween), preferably (10-100000):1, more preferably (100-10000):1.
[0063] In the present invention, when the co-catalyst is an organic boron compound and an organic aluminum compound, the molar ratio of boron in the co-catalyst to M in the main catalyst can be (0.1-1000):1, (for example, 0.1:1, 0.2:1, 0.5:1, 1:1, 2:1, 3:1, 5:1, 8:1, 10:1, 20:1, 50:1, 100:1, 200:1, 300:1, 500:1, 700:1, 800:1, 1000:1 and any value therebetween, preferably (0.1-500):1. The molar ratio of organoaluminum to M in the main catalyst can be (10-10 5):1, for example, 10:1, 20:1, 50:1, 100:1, 200:1, 300:1, 400:1, 500:1, 600:1, 700:1, 800:1, 1000:1, 2000:1, 3000:1, 5000:1, 100000:1 and any value therebetween), preferably (10-5000):1, more preferably (10-1000):1.
[0064] In the present invention, the molar amount of α-olefin monomer relative to 1 mole of the main catalyst has a wide selection range. In a preferred embodiment, the molar amount of α-olefin monomer relative to 1 mole of the main catalyst can be 100-30,000 moles, and specifically can be 100, 500, 1,000, 5,000, 10,000, 20,000 or 30,000 moles.
[0065] In the present invention, the polymerization reaction can be carried out in an inert solvent, or bulk polymerization can be carried out directly in an olefin without using an inert solvent. When a solvent is used, the solvent is preferably at least one of unsubstituted or halogen-substituted aromatic hydrocarbons (e.g., toluene, xylene, chlorobenzene) and unsubstituted or halogen-substituted C5-C20 saturated hydrocarbons (e.g., n-butane, isobutane, n-pentane, n-hexane, cyclohexane, n-heptane, octane, decane, heptane, dichloromethane, 1,2-dichloroethane, and 1,1,2,2-tetrachloroethane). More preferably, the solvent comprises an unsubstituted or halogen-substituted aromatic hydrocarbon, and most preferably comprises at least one of toluene, xylene, and chlorobenzene.
[0066] In the present invention, additional solvent may or may not be added (i.e., the amount of solvent is 0). When no additional solvent is added, the added α-olefin monomer itself can serve as the solvent. In the present invention, the volumetric amount of the solvent used relative to 1 volume of the α-olefin monomer has a wide range of selectable amounts. In a preferred embodiment, the volumetric amount of the solvent used relative to 1 volume of the α-olefin monomer is 0-200 volumes, preferably 0-100 volumes, and more preferably 0.5-50 volumes.
[0067] In the present invention, the number of carbon atoms of the α-olefin monomer may be 4-20, preferably 4-12. The α-olefin monomer may be a linear or branched α-olefin. Preferably, the α-olefin monomer is selected from at least one of 1-butene, 2-methyl-1-butene, 3,3-dimethyl-1-butene, 1-pentene, 1-pentene substituted with one or more methyl, ethyl, or propyl groups, 1-hexene, 1-hexene substituted with one or more methyl, ethyl, or propyl groups, 1-heptene, 1-heptene substituted with one or more methyl, ethyl, or propyl groups, 1-octene substituted with one or more methyl, ethyl, or propyl groups, 1-nonene, 1-decene, and 1-dodecene. More preferably, the α-olefin monomer is selected from at least one of 1-butene, 2-methyl-1-butene, 3,3-dimethyl-1-butene, 1-pentene, 1-pentene substituted with one or more methyl, ethyl, or propyl groups, 1-hexene, 1-hexene substituted with one or more methyl, ethyl, or propyl groups, 1-heptene, and 1-heptene substituted with one or more methyl, ethyl, or propyl groups, that is, preferably an α-olefin monomer having less than 8 carbon atoms.
[0068] In the method for preparing an α-olefin polymer described herein, the polymer solution obtained after the polymerization reaction may be post-treated. The post-treatment may be performed by conventional means in the art. In some embodiments, the post-treatment comprises adding an ethanol-hydrochloric acid solution to the polymer solution to deactivate the active centers.
[0069] The present invention also provides the use of the aforementioned α-olefin polymer as a viscosity index improver, particularly as a viscosity index improver for lubricating oils. When used as a viscosity index improver, the α-olefin polymer of the present invention exhibits significantly higher thickening efficiency compared to existing olefin polymers. Specifically, as measured according to the method in Appendix A of SH / T 0622-2007, the thickening efficiency of the α-olefin polymer of the present invention is 2-15 mm / s. 2 / s, preferably 3-10mm 2 / s.
[0070] The present invention provides a lubricating oil comprising a base oil and the aforementioned α-olefin polymer, wherein the α-olefin polymer is used as a viscosity index improver in the lubricating oil.
[0071] The content of the α-olefin polymer in the lubricating oil can be determined based on the content of the viscosity index improver in conventional lubricating oils. Preferably, the content of the α-olefin polymer is 0.01-20 wt.%, preferably 0.5-10 wt.%, based on the total weight of the lubricating oil.
[0072] The α-olefin polymer can be applied to lubricating oils using conventional methods in the art. Typically, a certain proportion of the α-olefin polymer is mixed with a lubricating base oil. The mixing temperature and heating time can be adjusted based on the specific mixing conditions, but are generally set at 110-130°C and stirred for 3-4 hours.
[0073] In the present invention, the base oil may be a conventional lubricating base oil in the art, and may generally be one or more of Group I, II, III, IV and V base oils in the American Petroleum Institute (API) classification.
[0074] The following examples further illustrate the α-olefin polymers of the present invention, their preparation methods, and applications. The examples are based on the technical solutions of the present invention and provide detailed implementation methods and specific operating procedures. However, the scope of protection of the present invention is not limited to the following examples.
[0075] The experimental methods in the following examples, unless otherwise specified, are all conventional methods in the art. The experimental materials used in the following examples, unless otherwise specified, are all commercially available.
[0076] In the following examples and comparative examples, the weight average molecular weight M of the olefin polymer is w and molecular weight distribution PDI were determined by gel permeation chromatography-infrared detector (GPC-IR);
[0077] The degree of branching of olefin polymers was determined by gel permeation chromatography-infrared detector (GPC-IR);
[0078] The amount of each unit (molar percentage) and the main chain carbon ratio are detected and calculated based on the nuclear magnetic resonance spectroscopy;
[0079] The melting point of the olefin polymer is measured by differential scanning calorimetry (DSC).
[0080] The thickening efficiency of olefin polymers when used as viscosity index improvers for lubricating oils was determined according to the method in Appendix A of SH / T 0622-2007, where the polymer concentration was 1% and the kinematic viscosity of the base oil at 100°C was 5.8912 mm 2 / s, and the kinematic viscosity at 40℃ is 29.6238mm 2 / s.
[0081] The viscosity index of olefin polymers used as viscosity index improvers for lubricating oils is calculated in accordance with GB / T 1995-1998.
[0082] Preparation Example 1
[0083] The complex shown in formula A is prepared by the following process:
[0084] Using p-toluenesulfonic acid as a catalyst, 0.87 g of acenaphthenequinone and 1.9 mL of 2,6-diisopropylaniline were refluxed in 100 mL of toluene for 24 hours, cooled to room temperature, and the solvent was removed in vacuo. The product was separated by column chromatography to obtain ligand L A .
[0085] A dichloromethane solution containing 0.23 g of (DME)NiBr2 was slowly added dropwise to a solution containing 0.50 g of ligand L A The product was added to a dichloromethane solution and stirred at room temperature for 6 hours, and then anhydrous ether was added to precipitate the product. After filtration, the filter cake was washed with anhydrous ether and dried in vacuo to obtain the complex shown in Formula A.
[0086] Preparation Example 2
[0087] The complex shown in formula B is prepared by the following process:
[0088] Using p-toluenesulfonic acid as a catalyst, 1.14 g of 9,10-dihydro-9,10-ethyleneanthracene-11,12-dione and 1.9 mL of 2,6-diisopropylaniline were refluxed in 100 mL of toluene for 24 hours, cooled to room temperature, and the solvent was removed in vacuo. The product was separated by column chromatography to obtain ligand L B .
[0089] A dichloromethane solution containing 0.23 g of (DME)NiBr2 was slowly added dropwise to a solution containing 0.45 g of ligand L B The product was added to a dichloromethane solution and stirred at room temperature for 6 hours, and then anhydrous ether was added to precipitate the product. After filtration, the filter cake was washed with anhydrous ether and dried in vacuo to obtain the complex shown in Formula B.
[0090] Preparation Example 3
[0091] The complex shown in formula C is prepared by the following process:
[0092] The ethanol solution containing 0.23 g of (DME)NiBr2 was slowly added dropwise to the ethanol solution containing 0.50 g of ligand L A The product was added to a dichloromethane solution and stirred at room temperature for 6 hours, and then anhydrous ether was added to precipitate the product. After filtration, the filter cake was washed with anhydrous ether and dried in vacuo to obtain the complex shown in Formula C.
[0093] Preparation Example 4
[0094] The complex shown in formula D is prepared by the following process:
[0095] 3.0 g of compound D (shown below) and 4 mL of 2,6-diisopropylaniline were refluxed in 100 mL of toluene with p-toluenesulfonic acid as catalyst for 24 hours. The solvent was removed after filtration. The residue was dissolved in dichloromethane and passed through an alkaline alumina column. The column was eluted with petroleum ether / ethyl acetate (20:1). The second fraction was the product. The solvent was removed to obtain ligand L. D .
[0096] A dichloromethane solution containing 0.50 g of (DME)NiBr2 was added dropwise to a 10 ml solution containing 1.05 g of ligand L D The mixture was added to a dichloromethane solution and stirred at room temperature for 6 hours to precipitate a precipitate, which was filtered, washed with ether and dried to obtain a complex shown in formula D.
[0097] Example 1
[0098] A 250 mL reaction flask was heated and dried at 100 ° C for 2 hours, evacuated while hot, and replaced with nitrogen three times, 7 mg of the complex represented by formula A was added, and then 30 mL of toluene was added with a syringe, stirred and dissolved, 10 mL of 1-hexene was added, and then 1.8 mL of 1.53 mol / L methylaluminoxane toluene solution was added, followed by 2 mL of 1.0 mol / L diethylzinc hexane solution. The reaction temperature was maintained at 30 ° C and the polymerization reaction was carried out for 60 minutes. The reaction was quenched with a 10% volume concentration of hydrochloric acid ethanol solution, precipitated and washed with ethanol, and vacuum dried and washed, and then vacuum dried to obtain a polymer product.
[0099] Example 2
[0100] A 250 mL reaction flask was heated and dried at 100 ° C for 2 hours, evacuated while hot, and replaced with nitrogen three times, 7 mg of the complex represented by formula A was added, and then 20 mL of toluene was added with a syringe, stirred and dissolved, 20 mL of 1-hexene was added, and then 3 mL of 0.4 mol / L sesquiethylaluminum chloride hexane solution was added, followed by 0.5 mL of 1.0 mol / L diethylzinc hexane solution. The reaction temperature was maintained at 30 ° C and the polymerization reaction was carried out for 20 minutes. The reaction was quenched with a 10% volume concentration of hydrochloric acid ethanol solution, precipitated and washed with ethanol, and vacuum dried and washed, and then vacuum dried to obtain a polymer product.
[0101] Example 3
[0102] A 250 mL reaction flask was heated and dried at 100° C. for 2 hours, evacuated while hot, and replaced with nitrogen three times. 7 mg of the complex represented by formula A was added, and then 20 mL of toluene was added with a syringe and stirred thoroughly to dissolve. 7 mL of 1-hexene was added, and then 3 mL of a 0.4 mol / L sesquiethylaluminum chloride hexane solution was added. The reaction temperature was maintained at 30° C. and the polymerization reaction was carried out for 10 minutes. The reaction was quenched with a 10% volume concentration of hydrochloric acid ethanol solution, precipitated with ethanol and washed, and vacuum dried to obtain a polymer product.
[0103] Example 4
[0104] A 250 mL reaction flask was heated and dried at 100 ° C for 2 hours, evacuated while hot, and replaced with nitrogen three times, 7 mg of the complex represented by formula A was added, and then 30 mL of dichloromethane was added with a syringe, stirred and dissolved, 20 mL of 1-hexene was added, and then 2 mL of 0.4 mol / L sesquiethylaluminum chloride hexane solution and 25 mg of tris(pentafluorophenyl)borane were added, followed by 0.2 mL of 1.0 mol / L diethylzinc hexane solution. The reaction temperature was maintained at 30 ° C and the polymerization reaction was carried out for 10 minutes. The reaction was quenched with a 10% volume concentration of hydrochloric acid ethanol solution, precipitated and washed with ethanol, and vacuum dried to obtain a polymer product.
[0105] Example 5
[0106] 24 mg of the complex represented by Formula B and 39 mL of chlorobenzene were used as material A; 30 mL of 1-hexene, 6 mL of a 1.53 mol / L methylaluminoxane solution in toluene, and 3 mL of chlorobenzene were used as material B; 0.8 mL of a 1.0 mol / L diethylzinc solution in hexane, 30 mL of 1-hexene, and 47.2 mL of chlorobenzene were used as material C. Materials A and B were separately injected into two nitrogen-purged pipelines at a flow rate of 0.25 mL / min, then mixed through T-type mixer 1 placed in a 0°C oil bath. The mixed materials A and B were immediately mixed with material C through T-type mixer 2 placed in a 0°C oil bath. Material C was injected into the pipeline at a flow rate of 0.5 mL / min. The mixed solution of materials A, B, and C then entered a 28.7 m pipeline placed in a 0°C oil bath. The reactants at the outlet of the pipelines were dropwise added to a 10% by volume hydrochloric acid-ethanol solution, precipitated and washed with ethanol, and vacuum dried to obtain the polymer product. The pipelines used are all polytetrafluoroethylene (PTFE) pipelines with an inner diameter of 2 mm.
[0107] Example 6
[0108] A 250 mL reaction flask was heated and dried at 100 ° C for 2 hours, evacuated while hot, and replaced with nitrogen three times. 7 mg of the complex represented by formula A was added, and then 15 mL of toluene and 5 mL of hexane were added with a syringe. After thorough stirring and dissolution, 11 mL of 1-pentene was added, and then 3 mL of 0.4 mol / L sesquiethylaluminum chloride hexane solution was added. Subsequently, 0.5 mL of 1.0 mol / L diethylzinc hexane solution was added. The reaction temperature was maintained at 20 ° C. After the polymerization reaction for 30 minutes, the reaction was quenched with a 10% volume concentration of hydrochloric acid ethanol solution, precipitated with ethanol and washed, and vacuum dried to obtain a polymer product.
[0109] Example 7
[0110] A 250 mL reaction flask was heated and dried at 100° C. for 2 hours, evacuated while hot, and replaced with nitrogen three times. 7 mg of the complex represented by formula A was added, and then 20 mL of toluene was added with a syringe and stirred thoroughly to dissolve. 13.5 mL of 1-hexene was added, and then 3 mL of a 0.4 mol / L sesquiethylaluminum chloride hexane solution was added, followed by 0.25 mL of a 1.0 mol / L diethylzinc hexane solution. The reaction temperature was maintained at 50° C. and the polymerization reaction was carried out for 20 minutes. The reaction was then quenched with a 10% volume concentration of hydrochloric acid ethanol solution, precipitated with ethanol and washed, and vacuum dried to obtain a polymer product.
[0111] Example 8
[0112] A 250 mL reaction flask was heated and dried at 100° C. for 2 hours, evacuated while hot, and replaced with nitrogen three times. 7 mg of the complex represented by formula A was added, and then 10 mL of toluene was added with a syringe and stirred thoroughly to dissolve. 30 mL of 1-octene was added, and then 5 mL of a 0.4 mol / L sesquiethylaluminum chloride hexane solution was added, followed by 0.5 mL of a 1.0 mol / L diethylzinc hexane solution. The reaction temperature was maintained at 50° C. and the polymerization reaction was carried out for 10 minutes. The reaction was then quenched with a 10% volume concentration of hydrochloric acid ethanol solution, precipitated with ethanol and washed, and vacuum dried to obtain a polymer product.
[0113] Example 9
[0114] A 250 mL reaction flask was heated and dried at 100° C. for 2 hours, evacuated while hot, and replaced with nitrogen three times. 7 mg of the complex represented by formula A was added, and then 30 mL of toluene was added with a syringe and stirred thoroughly to dissolve. 14 mL of 1-decene was added, and then 2 mL of a 1.53 mol / L methylaluminoxane toluene solution was added. Subsequently, 0.2 mL of a 1.0 mol / L diethylzinc hexane solution was added. The reaction temperature was maintained at 55° C. After the polymerization reaction for 10 minutes, the reaction was quenched with a 10% volume concentration of hydrochloric acid ethanol solution, precipitated with ethanol and washed, and vacuum dried to obtain a polymer product.
[0115] Example 10
[0116] 22.5 mL of 1-octene and 7.5 mL of a 0.4 mol / L sesquiethylaluminum chloride hexane solution were used as material A; 50 mg of the complex represented by Formula C, 22.5 mL of toluene, and 7.5 mL of 1-octene were used as material B; and 0.5 mL of a 1.0 mol / L diethylzinc hexane solution, 26.5 mL of 1-octene, and 32 mL of toluene were used as material C. Materials A and B were each injected into two nitrogen-purged pipelines at a flow rate of 0.666 mL / min, then mixed in T-type mixer 1 placed in a 30°C oil bath. The mixed materials A and B were then immediately mixed with material C in T-type mixer 2 placed in a 30°C oil bath. Material C was injected into the pipelines at a flow rate of 1.333 mL / min. The mixed solution of materials A, B, and C then enters pipeline T1 (30 meters long) placed in a 30°C oil bath. It then flows into pipeline T2 (20 meters long) placed in a 55°C oil bath. The reactants at the T2 outlet are dripped into a 10% volume concentration hydrochloric acid-ethanol solution, precipitated and washed with ethanol, and vacuum-dried to obtain the polymer product. The pipelines used are all PTFE tubing with an inner diameter of 1 mm. The polymer has a branching degree of 72 and is a diblock polymer with a melting point of 55.4°C.
[0117] Example 11
[0118] 7 mg of the complex represented by formula A and 15 mL of toluene were used as material A; 6.3 mL of 1-decene, 3 mL of a 0.4 mol / L sesquiethylaluminum chloride hexane solution, and 5.7 mL of toluene were used as material B; and 20 mL of 1-decene was used as material C. Materials A and B were respectively injected into two nitrogen-purged pipelines at a flow rate of 0.268 mL / min, and then mixed in T-type mixer 1 placed in a 15°C oil bath. The mixed solution of materials A and B then entered pipeline T1, which was also placed in a 15°C oil bath. The length of T1 was 20.5 m. Subsequently, the solution was mixed with material C via T-type mixer 2 placed in a 15°C oil bath. Material C was injected into the pipelines at a flow rate of 0.358 mL / min. The mixed solution of materials A, B, and C then enters pipeline T2, which is 5.7 meters long and placed in a 15°C oil bath. The reactants at the T2 outlet are then dripped into a 10% volume concentration hydrochloric acid-ethanol solution. Ethanol precipitation and washing are performed, followed by vacuum drying to obtain the polymer product. The pipelines used are all PTFE tubing with an inner diameter of 1 mm. The polymer has a branching degree of 61 and is a diblock polymer.
[0119] Example 12
[0120] 9 mg of the complex represented by Formula D and 30 mL of toluene were used as material A; 12.6 mL of 1-decene, 6 mL of a 0.4 mol / L sesquiethylaluminum chloride hexane solution, and 11.4 mL of toluene were used as material B; and 40 mL of 1-hexene was used as material C. Materials A and B were respectively injected into two nitrogen-purged pipelines at a flow rate of 0.287 mL / min. The mixed solution of materials A and B then entered pipeline T1, which was also placed in a 15°C oil bath. The mixed solution then entered pipeline T1, which was 21.9 m long and filled with an SK-type spiral mixing core and also placed in a 15°C oil bath. The solution was then mixed with material C via T-mixer 2, also placed in a 15°C oil bath. Material C was injected into the pipelines at a flow rate of 0.383 mL / min. The mixed solution of materials A, B, and C then enters pipeline T2, which is placed in a 15°C oil bath. T2 is 6.1 meters long and filled with an SK-type spiral mixing core. The reactants at the T2 outlet are dripped into a 10% volume concentration hydrochloric acid-ethanol solution, precipitated and washed with ethanol, and vacuum-dried to obtain the polymer product. The pipelines used are all stainless steel with an inner diameter of 1 mm. The polymer has a branching degree of 71 and is a diblock polymer with a melting point of 45.3°C.
[0121] Example 13
[0122] A 250 mL reaction flask was heated and dried at 100°C for 2 hours. The flask was then evacuated while hot and replaced with nitrogen three times. Seven mg of the complex represented by Formula A was added, followed by 20 mL of toluene added via syringe and thoroughly stirred to dissolve. Seven thousand and five mL of 1-hexene was added, followed by 3 mL of a 0.4 mol / L sesquiethylaluminum chloride hexane solution and 0.3 mL of a 1.0 mol / L diethylzinc hexane solution. The polymerization reaction was maintained at 30°C for 30 minutes. A small amount of the sample was withdrawn with a syringe and precipitated into ethanol to obtain a polymer sample for characterization. The polymer sample had a branching degree of 110. The reaction flask was transferred to 55°C and the reaction continued for 20 minutes. The reaction was quenched with 10% (volume) hydrochloric acid in ethanol, precipitated with ethanol, washed, and dried under vacuum to obtain the polymer product. The polymer product had a branching degree of 95 and was a diblock polymer with a melting point of -22°C.
[0123] Example 14
[0124] A 250 mL reaction flask was heated and dried at 100°C for 2 hours. While hot, the flask was evacuated and replaced with nitrogen three times. 7 mg of the complex represented by Formula A was added, followed by 15 mL of toluene added via syringe and thoroughly stirred to dissolve. 6 mL of 1-hexene was added, followed by 3 mL of a 1.53 mol / L methylaluminoxane toluene solution, followed by 0.3 mL of a 1 mol / L diethylzinc hexane solution. The reaction temperature was maintained at 35°C. After polymerization for 20 minutes, a small amount of sample was withdrawn via syringe and precipitated in ethanol to obtain a polymer sample for characterization. This sample had a branching degree of 111. 40 mL of toluene was then added and the reaction continued for 60 minutes. The reaction was quenched with a 10% volume concentration of hydrochloric acid in ethanol, precipitated with ethanol, washed, and dried under vacuum to obtain a polymer product with a branching degree of 86. This polymer is a diblock polymer.
[0125] Example 15
[0126] A 250 mL reaction flask was heated and dried at 100°C for 2 hours. While still hot, the flask was evacuated and replaced with nitrogen three times. 7 mg of the complex represented by Formula A was added, followed by 10 mL of toluene added via syringe and thoroughly stirred to dissolve. 10 mL of 1-octene was added, followed by 1 mL of a 2 mol / L solution of diethylaluminum chloride in hexane. The reaction temperature was maintained at 25°C and the polymerization reaction continued for 10 minutes. A small amount of sample was withdrawn via syringe and precipitated into ethanol to obtain a polymer sample for characterization. The polymer sample had a branching degree of 74. The reaction flask was transferred to a 50°C environment and the reaction continued for 10 minutes. The reaction was quenched with a 10% volume concentration of hydrochloric acid in ethanol, precipitated with ethanol, washed, and dried under vacuum to obtain a polymer product with a branching degree of 64. This polymer is a diblock polymer with a melting point of 54.4°C.
[0127] Example 16
[0128] A 250 mL reaction flask was heated and dried at 100°C for 2 hours. While still hot, the flask was evacuated and replaced with nitrogen three times. 7 mg of the complex represented by Formula A was added, followed by 15 mL of toluene added via syringe and thoroughly stirred to dissolve. 6 mL of 1-hexene was added, followed by 3 mL of a 1.53 mol / L methylaluminoxane solution in toluene, followed by 0.3 mL of a 1 mol / L diethylzinc in hexane solution. The polymerization reaction was maintained at 35°C for 15 minutes. 40 mL of toluene was then added and the reaction continued for 60 minutes. 18 mL of 1-hexene was then added and the reaction continued for 15 minutes. The reaction was quenched with 10% (volume) hydrochloric acid in ethanol, precipitated with ethanol, washed, and dried under vacuum to obtain the polymer product. This polymer is a triblock polymer.
[0129] Comparative Example 1
[0130] A 100 mL reaction bottle was heated and dried at 100 ° C for 2 hours, evacuated while hot, and replaced with nitrogen three times. 10 mg of metallocene catalyst Ph2C (Cp) (Flu) ZrCl2 (purchased from APAC Pharmaceutical) was added, and then 15 mL of 1-hexene and 2 mL of 1.53 mol / L methylaluminoxane toluene solution were added with a syringe. The reaction was carried out at 25 ° C for 1 hour. The reaction was quenched with a 10% volume concentration of hydrochloric acid ethanol solution, precipitated and washed with ethanol, and the polymer product was obtained after vacuum drying.
[0131] Comparative Example 2
[0132] A 100 mL reaction bottle was heated and dried at 100 ° C for 2 hours, evacuated while hot, and replaced with nitrogen three times, 10 mg of metallocene catalyst Ph2C (Cp) (Flu) ZrCl2 was added, and then 15 mL of 1-hexene and 2 mL of 1.53 mol / L methylaluminoxane toluene solution were added with a syringe. The reaction was carried out at 25 ° C for 2 hours, and the reaction was quenched with a 10% volume concentration of hydrochloric acid ethanol solution. The product was precipitated and washed with ethanol, and the polymer product was obtained after vacuum drying.
[0133] Comparative Example 3
[0134] A 100 mL reaction bottle was heated and dried at 100 ° C for 2 hours, evacuated while hot, and replaced with nitrogen three times, 10 mg of metallocene catalyst Ph2C (Cp) (Flu) ZrCl2 was added, and then 15 mL of 1-hexene and 2 mL of 1.53 mol / L methylaluminoxane toluene solution were added with a syringe. The reaction was carried out at 25 ° C for 1 hour, the temperature was raised to 55 ° C, and the reaction was continued for 1 hour. The reaction was quenched with a 10% volume concentration of hydrochloric acid ethanol solution, precipitated and washed with ethanol, and the polymer product was obtained after vacuum drying.
[0135] Comparative Example 4
[0136] A 100 mL reaction flask was heated and dried at 100°C for 2 hours. The flask was then evacuated while hot and replaced with nitrogen three times. 10 mg of the metallocene catalyst Ph2C(Cp)(Flu)ZrCl2 was added. Then, 15 mL of 1-hexene and 2 mL of a 1.53 mol / L methylaluminoxane toluene solution were added via syringe. The reaction was continued at 25°C for 1 hour. 5 mL of 1-decene was added and the reaction continued for another hour. The reaction was quenched with 10% ethanolic hydrochloric acid solution, precipitated with ethanol, washed, and dried under vacuum to obtain the polymer product.
[0137] Comparative Example 5
[0138] A 250 mL reaction flask was heated and dried at 100° C. for 2 hours, evacuated while hot, and replaced with nitrogen three times. 7 mg of the complex represented by formula A was added, and then 30 mL of toluene was added with a syringe, stirred thoroughly to dissolve, 10 mL of 1-hexene was added, and then 2.8 mL of a 1.53 mol / L methylaluminoxane toluene solution was added. The reaction temperature was maintained at −10° C. After the polymerization reaction for 40 minutes, the reaction was quenched with a 10% volume concentration of hydrochloric acid ethanol solution, precipitated and washed with ethanol, and vacuum dried to obtain a polymer product.
[0139] Application Examples 1-16 and Application Comparative Examples 1-5
[0140] The olefin polymers prepared in the above examples and comparative examples were added to lubricating base oil 150SN and stirred at 120° C. for about 2 hours until completely dissolved. The thickening efficiency was then tested. The results are shown in Table 1 below.
[0141] Table 1
[0142] The results in Table 1 show that the α-olefin polymer of the present invention has excellent thickening efficiency when used as a viscosity index improver for lubricating oil.
[0143] The preferred embodiments of the present invention have been described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, various simple variations of the technical solution of the present invention may be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as disclosed in the present invention and fall within the scope of protection of the present invention.
Claims
1. An a-olefin polymer formed by polymerizing at least one a-olefin monomer CH2=CHR, characterized in that in the a-olefin polymer, carbon atoms located in a main chain account for 63-82% of the number of all carbon atoms, wherein R is a linear or branched alkyl group having the number of carbon atoms more than or equal to 2, wherein the a-olefin monomer is a linear or branched a-olefin having 4-20 carbon atoms;the a-olefin polymer has a weight average molecular weight within the range of 10,000-250,000, 25,000-150,000 or 30,000-120,000;the a-olefin polymer has a molecular weight distribution PDI less than 3, or less than or equal to 2;the a-olefin polymer is a diblock polymer A-B or a triblock polymer A-B-A, wherein the branching degree of the block A is greater than that of the block B; the a-olefin polymer comprises a first unit -(CH2)-, a second unit -CH(CH3)-, and a third unit -CH(R)-, the first unit is present in a number of 80-95%, the second unit is present in a number of 1-10%, and the third unit is present in a number of 2-12%, based on the total number of carbon atoms in main chain of the a-olefin polymer.
2. The a-olefin polymer according to claim 1, wherein the a-olefin monomer is at least one selected from the group consisting of 1-butene, 2-methyl-1-butene, 3,3-dimethyl-1-butene, 1-pentene, 1-pentene substituted with one or more methyl, ethyl, and propyl, 1-hexene, 1-hexene substituted with one or more methyl, ethyl, and2023370362 26 Oct 2026propyl, 1-heptene, 1-heptene substituted with one or more methyl, ethyl, and propyl, 1-octene substituted with one or more methyl, ethyl, and propyl, 1-nonene, 1-decene, and 1-dodecene.
3. A method for preparing the a-olefin polymer according to claim 1, the method comprisinges the following steps: carrying out a polymerization reaction of linear or branched a-olefin monomers having 4-20 carbon atoms in the presence of a main catalyst, a cocatalyst, an optional reversible chain transfer agent, and an optional solvent, wherein the main catalyst is a post-transition metal catalyst with diimine as a ligand;the polymerization reaction process comprises at least two reaction stages, the diblock polymer A-B or the triblock polymer A-B-A is formed by controlling the reaction temperatures and / or the a-olefin monomer concentrations of the different reaction stages, or the diblock polymer A-B or the triblock polymer A-B-A is formed by controlling the a-olefin monomer species of the different reaction stages.
4. The method according to claim 3, wherein controlling the reaction temperatures of the different reaction stages comprises: arranging that the absolute value of the difference in polymerization reaction temperatures of two adjacent reaction stages is not less than 10°C, optionally not less than 20°C.2023370362 26 Oct 20265. The method according to claim 3, wherein controlling the a-olefin monomer concentrations of the different reaction stages comprises: arranging the ratio of the a-olefin monomer concentrations of two adjacent reaction stages to be greater than 3.
6. The method according to claim 3, wherein controlling the a-olefin monomer species of the different reaction stages comprises: in the two adjacent reaction stages, the number of carbon atoms of the a-olefin monomer added in the next reaction stage is less than the number of carbon atoms of the a-olefin monomer added in the previous reaction stage.
7. The method according to any one of claims 3-6, wherein the reaction temperature of the polymerization reaction is within the range from -40°C to 100°C, or within the range from 0°C to 70°C, and the a-olefin monomer concentration is 0.05mol / L or more.
8. The method according to any one of claims 3-7, wherein the main catalyst is a metalcomplex represented by formula (I),Formula (I)Wherein M is a group VIII metal; R1 and R4, which are the same or different, eachindependently selected from C1-C30 hydrocarbyl or heterohydrocarbyl, R1 and R42023370362 26 Oct 2026optionally bonded together to form a ring structure; R2 and R3, which are the same ordifferent, each independently selected from hydrogen, halogen, and C1-C20hydrocarbyl or heterohydrocarbyl, R2 and R3 optionally bonded together to form a ringstructure; there are number n of the group L, which are the same or different, eachselected from halogen, C1-C10 hydrocarbyl, and C1-C10 Hydrocarbon oxygen group;n is an integer satisfying the M valence state;optionally M is selected from nickel and palladium;optionally R1 and R4 are each independently selected from substituted or unsubstitutedC1-C20 alkyl, and substituted or unsubstituted C6-C20 aryl; orR1 and R4 are each agroup represented by formula (II),Formula (II)R1, R2, R3, R4, and R5 in formula (II) are the same or different, each independentlyselected from hydrogen, halogen, hydroxyl, and substituted or unsubstituted C1-C30 hydrocarbyl or heterohydrocarbyl, R1, R2, R3, R4, and R5 optionally bonded together to form a ring structure; more preferably, R1 and R3 in formula (II) are each independently selected from substituted or unsubstituted C3-C10 alkyl or heterohydrocarbyl.
9. The method according to any one of claims 3-8, wherein the cocatalyst is at least one selected from the group consisting of organoaluminum compounds and2023370362 26 Oct 2026organoboron compounds;optionally the organoaluminum compound is one or more selected from the group consisting of alkylalumoxane, alkylaluminum, and alkylaluminum halide;optionally the organoboron compound is at least one selected from the group consisting of an aryl hydrocarbyl boron and a borate.
10. The method according to claim 3, wherein the polymerization reaction is carried out in the presence of the reversible chain transfer agent, and the reversible chain transfer agent is dialkylzinc;optionally the dialkylzinc is at least one selected from the group consisting of diethylzinc, di(n-propyl)zinc, and di(n-octyl)zinc.
11. The method according to any of claims 3-10, wherein when the cocatalyst is an organoaluminum compound, the molar ratio of aluminum in the cocatalyst to M in the main catalyst is (10-107): 1, (10-100,000): 1, or (100-10,000): 1;when the cocatalyst is an organoboron compound and an organoaluminum compound, the molar ratio of boron in the cocatalyst to M in the main catalyst is (0.1-1,000): 1, or (0.1-500): 1; and the molar ratio of organoaluminum to M in the main catalyst is (10-105): 1, (10-5,000): 1, or (10-1,000): 1;optionally the molar dosage of the a-olefin monomer is 100-30,000 moles with respect to the 1 molar dosage of the main catalyst;optionally the volume dosage of the solvent is 0-200 volume, 0-100 volume or 0.5-502023370362 26 Oct 2026volume, relative to 1 volume dosage of the a-olefin monomer.
12. The method according to any one of claims 3-11, wherein the solvent is at least one selected from the group consisting of unsubstituted or halogen-substituted aromatic hydrocarbons and unsubstituted or halogen-substituted C5-C20 saturated hydrocarbons, optionally containing unsubstituted or halogen-substituted aromatic hydrocarbons, optionally containing at least one of toluene, xylene, and chlorobenzene.
13. The method according to any one of claims 3-12, wherein the number of carbon atoms in the a-olefin monomer is within the range of 4-12;optionally the a-olefin monomer is selected from the group consisting of 1-butene, 2-methyl-1-butene, 3,3-dimethyl-1-butene, 1-pentene, 1-pentene substituted with one or more methyl, ethyl, and propyl, 1-hexene, 1-hexene substituted with one or more methyl, ethyl, and propyl, 1-heptene, 1-heptene substituted with one or more methyl, ethyl, and propyl, 1-octene substituted with one or more methyl, ethyl, and propyl, 1-nonene, 1-decene, and 1-dodecene.
14. A use of the a-olefin polymer according to claim 1 or 2 as a viscosity index improver.2023370362 26 Oct 202615. A lubricating oil comprising a base oil and the a-olefin polymer according to claim 1 or 2;optionally the a-olefin polymer is contained in an amount of 0.01-20wt.% or 0.5-10wt.%, based on the total weight of the lubricating oil.
Citation Information
Patent Citations
Olefin block copolymer, viscosity index improver for lubricating oils and lubricating oil composition
EP1262498A2
Regioregular polymerization of alpha-olefins to produce polyethylene with a predominance of methyl substituents
WO2007070342A2