Multi-layer cleaning artigo and manufacturing method of a multi-layer cleaning artigo
A multilayer cleaning article with polyurethane foam and a semi-abrasive pad addresses the limitations of conventional sponges by efficiently cleaning non-stick surfaces without damage, enhancing durability and safety.
Patent Information
- Application Number
- BR102025008979
- Authority / Receiving Office
- BR · BR
- Patent Type
- Applications
- Publication Date
- 2026-11-17
AI Technical Summary
Conventional cleaning sponges for non-stick surfaces damage the coating, release harmful particles, retain residues, and are inefficient in removing stubborn dirt, posing safety and durability issues.
A multilayer cleaning article composed of high-performance polyurethane foam and a semi-abrasive pad with bactericidal and antiviral nanoparticles, optimized for non-stick surfaces, ensuring effective residue removal without scratching.
The cleaning article effectively removes grease and carbonized particles while preserving non-stick surfaces, offering superior durability, antimicrobial properties, and safe sanitization.
Description
TECHNICAL DESCRIPTION REPORT: MULTILAYER CLEANING ARTICLE AND MANUFACTURING METHOD OF A MULTILAYER CLEANING ARTICLE.
[001] The present invention relates to a cleaning article, specially developed for utensils and equipment that have a non-stick surface, such as, for example, electric hot air circulation fryers, commonly known as air fryers. The article comprises a structure composed of high-performance polyurethane foam, a semi-abrasive layer and nanoparticles with bactericidal and antiviral properties. The invention aims at the efficient removal of residues and grease, without damaging surfaces with a non-stick coating. FUNDAMENTALS OF THE INVENTION
[002] Abrasive and non-abrasive sponges are commonly used for household cleaning, including on appliances. However, these products generally do not offer protection against scratches on sensitive surfaces such as the Teflon coatings found in air fryers. Some sponges may also shed fragments or not withstand continuous use, compromising the durability and safety of the appliance.
[003] Conventional household cleaning sponges, widely used in kitchens for cleaning utensils, pans and appliances, have several limitations when applied to surfaces with non-stick or sensitive coatings. These sponges are generally composed of an abrasive side, whose function is to remove adhered dirt. However, using this abrasive side on non-stick surfaces entails a series of functional and structural disadvantages.
[004] The abrasiveness of the rougher side of conventional sponges can damage the non-stick coating of cookware, causing scratches. Petition 870250036351, dated 06 / 05 / 2025, page 11 / 28 / 13 and premature wear. The deterioration of this protective layer compromises not only the non-stick function of the material, but also its safety, as it can release microscopic fragments of the coating during food preparation.
[005] Additionally, these sponges have a high retention of moisture and organic residues, which favors the proliferation of microorganisms and the formation of unpleasant odors. This aspect is especially problematic in the cleaning of frequently used appliances, such as electric fryers, sandwich makers and griddles, whose surfaces require specific care to avoid contamination.
[006] Another limiting factor concerns the difficulty of sanitizing and safely reusing conventional sponges. Even after home disinfection processes, such as boiling, sponges tend to retain residues, odors, and deformations that reduce their lifespan and effectiveness.
[007] In addition, it is common for low-quality sponges to release foam particles or synthetic fibers during use, which can lead to cross-contamination and accumulation of debris on cleaned surfaces.
[008] Finally, the efficiency of removing residue in specific situations, such as adhered crusts, carbonized residues or solidified grease, is limited, since greater abrasiveness cannot be applied without the risk of damaging sensitive surfaces.
[009] Given these limitations, there is a need to develop more effective and safe cleaning solutions for utensils and appliances with non-stick coating, capable of combining performance, durability, antimicrobial properties and compatibility with delicate surfaces.
[010] The main objective of the cleaning article is to offer a solution that combines efficiency in removing residues, especially Petition 870250036351, dated 06 / 05 / 2025, page 12 / 28 / 13 grease and carbonized particles, while preserving the internal surfaces of appliances. This is possible through a carefully developed composition that combines soft polyurethane foam, special semi-abrasive fillers, and nanoparticles with bactericidal and antiviral properties. The cleaning product also features a semi-abrasive pad that allows for the removal of more stubborn dirt without scratching or degrading the non-stick coating of utensils and equipment.
[011] The state of the art includes some solutions for cleaning delicate surfaces, however, they fail to achieve a cleaning product capable of combining performance, durability, antimicrobial properties and compatibility with delicate surfaces.
[012] Document US2023292977 describes an abrasive pad and a cleaning sponge that incorporate antiviral and / or antibacterial agents to combat microorganisms, including viruses and bacteria. However, this document fails to achieve a cleaning article that includes at least a proportion of short- and long-chain polyol, and foam density.
[013] In turn, document WO2023248201 describes a structured abrasive article that includes a substrate with a main surface and a plurality of molded abrasive composites. These abrasive composites are designed to provide high cleaning performance without causing significant damage to the underlying surfaces. The abrasive composite is formed by a phase of particulate grains dispersed in an organic binder phase. The geometry of the abrasive composites is optimized to improve cleaning performance and durability. However, this document fails to achieve a cleaning article that includes a ratio of short- and long-chain polyol, nanoparticles with bactericidal and antiviral action, and a specific ratio between foam and semi-abrasive mat. Petition 870250036351, dated 06 / 05 / 2025, page 13 / 28 / 13
[014] Thus, it is evident that the state of the art has solutions for delicate surfaces, however, none of them is capable of achieving the characteristics and advantages of the present invention. DESCRIPTION OF THE INVENTION
[015] The following detailed description refers to the invention in such a way as to allow a person skilled in the art to reproduce its results. Other embodiments are possible and can be carried out without departing from the concept and scope of the present invention. The following detailed description should therefore not be understood in a restrictive or limiting manner.
[016] The cleaning article of the present invention is of the multilayer type and, in a preferred embodiment, has two layers, one layer comprising foam and the other comprising a semi-abrasive pad. In this preferred embodiment, the proportion between the foam and the semi-abrasive pad can vary from 45% to 55% for the foam and from 45% to 55% for the semi-abrasive pad, allowing the product to achieve an effective balance between absorption capacity, softness to the touch and cleaning efficiency.
[017] The foam in the cleaning product has a unique formulation, comprising an ideal combination of two types of polyol, polyol 3000 and polyol 1000, which give the foam an optimized chemical structure for strength, flexibility and durability. More specifically, the foam comprises Polyol 1000, which has a molecular weight of 1000 g / mol, a Hydroxyl 110 KOH / mg used in 7 parts in its composition. The foam composition also includes a combination of polyols with molecular weights around 3000 g / mol, resulting in a combination of around 96 parts of Polyol 3000.
[018] This chemical mixture, associated with a controlled cylindrical expansion process and a density adjusted in the range of 18 to 24 g / mL, Petition 870250036351, dated 06 / 05 / 2025, page 14 / 28 / 13, preferably 20 to 22 g / mL, provides a material capable of accessing hard-to-reach areas inside equipment, while offering tear resistance and a longer lifespan compared to conventional sponges.
[019] The foam of the cleaning article preferably comprises the components according to table 1, in parts per hundred parts of polyol. Raw Materials Parts in ppm* POLYOL 3000 88.0 ~ 98.0 TDI 53.0 ~ 59.0 SILICONE 1.90 ~ 2.10 AMINE 0.076 ~ 0.084 TIN DYE 0.162 ~ 0.178 RED DYE 1.86 ~ 2.05 YELLOW DYE 0.105 ~ 0.116 WATER 3.9 ~ 4.4 POLYOL 1000 6.6 ~ 7.4
[020] One of the distinguishing features of the cleaning product, in addition to its specific application for non-stick surfaces, is the incorporation of nanoparticles with bactericidal and antiviral properties, which ensure more complete and safe sanitization.
[021] Nanoparticles with bactericidal and antiviral properties incorporated into the cleaning product are preferably zinc oxide (ZnO) nanoparticles, widely recognized for their antimicrobial efficacy. These nanoparticles act by releasing Petition 870250036351, dated 06 / 05 / 2025, page 15 / 28 / 13 controlled release of Zn2+ ions, which interfere with the metabolic processes of bacteria and viruses, promoting the rupture of cell membranes and the inactivation of microorganisms. Furthermore, zinc oxide exhibits good thermal stability and is compatible with polymeric matrices, making it suitable for applications in reusable cleaning products. Alternatively, the formulation may include other nanoparticles with similar properties, such as silver nanoparticles (Ag), provided they maintain the biocompatibility and stability necessary for safe household use. The choice of nanoparticle type can be adjusted according to the specific purpose of the cleaning product, the type of microorganisms to be combated, or applicable local regulations.
[022] The manufacturing method for the cleaning product involves a series of carefully controlled technical and chemical steps to ensure that a product with the desired characteristics is obtained.
[023] The process begins with the dosing of chemical components, including polyol, isocyanate, water, catalysts, dyes and various additives. The main reaction involved is the formation of polyurethane, which occurs from the combination of isocyanate with polyol. This reaction, exothermic in nature, releases heat and, in the presence of water, generates carbon dioxide, which acts as a blowing agent, forming the cellular structure of the foam.
[024] After the expansion and formation of the foamy cream, the mass is left to rest for at least 24 hours to complete its curing and structural stabilization.
[025] The semi-abrasive mat, in turn, is produced by polymerizing phenolic resins, which bind filler elements to a fibrous substrate, forming a rigid three-dimensional mesh. In a preferred embodiment of the invention, talc is the filler element used. Petition 870250036351, dated 06 / 05 / 2025, page 16 / 28 / 13 Talc, composed of hydrated magnesium silicate, has a lamellar structure and low-hardness particles, which gives it excellent mechanical removal capabilities without causing scratches or wear on sensitive surfaces, such as non-stick coatings. Furthermore, talc contributes to the pad's body and stability, enhancing its durability and flexibility during use. Alternatively, other fillers with similar characteristics can be used, such as calcium carbonate, precipitated silica, or kaolin, provided they are compatible with the pad matrix and do not compromise the integrity of the treated surfaces. The choice of filler may vary depending on the desired level of abrasiveness and the intended application of the cleaning product.
[026] The composition of the fibrous substrate comprises a mixture of at least two fibers: 45% to 55% white polyester fiber (manufacturer model 7.0 DTEX 50mm or equivalent) and 45% to 55% polyamide fiber (manufacturer model DTEX 17.0 / 40MM BR P-111 CT or equivalent).
[027] Additionally, the polymerization process of phenolic resins used in the formation of the semi-abrasive mat is based on the synthesis of resol-type resins, which occurs under alkaline conditions (pH between 8 and 10), with an excess of formaldehyde relative to phenol. This process is divided into the following stages: a) Hydroxymethylation step: in which phenol reacts with formaldehyde, producing intermediate compounds known as mono-, di-, or trimethylol-phenols, through the addition of hydroxymethyl groups (CH2OH) to the aromatic ring of phenol. This reaction is catalyzed by a base and depends on the ratio of reactants and the temperature of the reaction medium. The products formed in this step are the reactive precursors that will participate in the subsequent condensation reactions. Petition 870250036351, dated 06 / 05 / 2025, page 17 / 28 / 13 b) Condensation stage: in which the hydroxymethyl groups of the intermediates react with each other, promoting the formation of methylene (-CH2-) and ether (-CH2-O-CH2-) bonds, connecting the phenolic rings to each other. This stage leads to the formation of a three-dimensional polymeric structure. The extent of condensation determines the viscosity of the system, which can result in a liquid (resinous resol) or solid prepolymer, depending on the formulation parameters and subsequent curing conditions. c) Prepolymer formation: as condensation progresses, there is a gradual increase in viscosity, forming an intermediate material called resol. This prepolymer can be processed in liquid form or converted into a partially cross-linked solid, which will later be molded and cured to form the semi-abrasive mat. The resol exhibits thermal stability and good adhesion to fibrous substrates, making it ideal for impregnation and structuring of the cleaning mat.
[028] The manufacturing method of the semi-abrasive pad, used in the cleaning article of the present invention, comprises a continuous industrial line process, which integrates material preparation steps, pad formation, resin impregnation, mineral filler application, thermal curing and final finishing. The steps of this process are described in detail below: a) Materials requisition: the process begins with the release of the necessary supplies from the warehouse, which include synthetic fibers (such as polyester or nylon), resol-type phenolic resin, pigments, functional additives, and a mineral filler element, such as talc. Petition 870250036351, dated 06 / 05 / 2025, page 18 / 28 / 13 b) Fiber opening: the synthetic fibers are unwound and subjected to a mechanical opening process, using openers equipped with oscillating cylinders or combs. This step aims to defibrate the bundles, promoting a more homogeneous and loose distribution, ideal for the subsequent formation of the fibrous web. c) Formation of the fibrous web: the open fibers are deposited onto a conveyor belt using a Random Machine, forming a continuous web with controlled thickness and basis weight. This web does not yet have structural cohesion, being held together solely by the random overlapping of the fibers. d) Resin impregnation and pre-drying: the formed veil is then conveyed to a foulard-type system, where it is uniformly impregnated with liquid phenolic resin (pre-polymerized in a separate process). After impregnation, the veil goes to a first oven, where pre-drying and the beginning of resin cross-linking occur, giving initial cohesion to the mat. e) Application of filler and partial drying: In the next step, the filler, such as talc, is applied to the surface of the impregnated blanket using a spray booth. Immediately afterwards, the blanket is directed to a second oven, where partial curing of the resin and fixation of the filler to the blanket structure occurs. f) Layer reinforcement and final curing: a second application of the filler element can be carried out, if desired, in a second spray booth, in order to reinforce the surface distribution. The sheet then sequentially passes through a third and a fourth oven, where the thermal curing of the phenolic resin is completed, ensuring dimensional stability, adhesion of the components and mechanical resistance. Petition 870250036351, dated 06 / 05 / 2025, page 19 / 28 / 13 g) Cutting and winding: after cooling, the finished sheet is cut to standard or custom widths, and then wound onto rolls. This product can be used directly or sent to additional stages, such as lamination with polyurethane foams. h) Product inspection and release: the finished membrane undergoes quality control, which includes verification of thickness, structural cohesion, mineral filler adhesion, and visual parameters. Once approved, the membranes are released as finished products. i) Parallel stage - preparation of formulations: running parallel to the main flow, the preparation of the formulations used in impregnation and spraying takes place. This stage involves weighing and mixing the components (resins, pigments, additives), as well as adjusting the viscosity and controlling the reactivity of the mixtures, according to process specifications.
[029] The residence time of the blanket in each oven is calculated to ensure complete curing of the resin, guaranteeing the desired physicochemical performance in the final product. The entire process is continuous, optimizing production yield and standardization of the semi-abrasive blanket.
[030] Thus, the manufacturing method for the cleaning article comprises the following steps: 1. Measure and mix the foam components; 2. To form the cream, the mixture becomes saturated with CO2, producing a creamy appearance (5-10 seconds after mixing); 3. Growth: the heat generated and the continuous formation of CO2 expand the mass (60-120 seconds); Petition 870250036351, dated 06 / 05 / 2025, page 20 / 28 / 13 4. Curing: the foam is left to rest for at least 24 hours to complete the reactions and stabilize the structure; 5. Cutting and finishing: the foam is cut to the desired dimensions; 6. Application of the semi-abrasive mat by fixing the abrasive grains to the foam substrate with resins. 7. Joining the blanket to the foam by applying controlled pressure, varying between 4 and 5 bar, ensuring efficient adhesion and product durability.
[031] In a preferred embodiment, the length of the cut foam ranges from 100mm to 105mm, more preferably between 102mm and 103mm. In addition, the width of the foam ranges from 26mm to 31mm, more preferably from 28mm to 29mm.
[032] For technical validation of the cleaning product, comparative tests were carried out. The tests were conducted by professionals in the areas of development and chemical engineering, based on national and international technical standards, including NBR 8515 (tensile strength), NBR 8516 (elongation strength), ASTM C373 (water absorption), and ISO 20567-1 (surface abrasiveness).
[033] The first set of tests evaluated the water absorption capacity of the cleaning article through controlled immersion in distilled water. After initial weighing of the dry sample, the cleaning article was immersed for 180 seconds, compressed for 1 minute to simulate manual drainage, and then weighed again. The cleaning article showed water absorption equivalent to 1029.18% of its dry mass, that is, it was able to absorb 10.29 times its own weight. This result classifies it as highly hydrophilic and places it above the average of conventional household sponges (which have absorption between 400% and Petition 870250036351, dated 06 / 05 / 2025, page 21 / 28 / 13 800%), making it comparable to advanced performance materials such as superabsorbent polymers.
[034] In tests carried out with a standard market sponge, under the same test conditions, an aqueous absorption of 731.65% was observed, showing that the cleaning article of the invention has superior performance in liquid retention, a desirable characteristic for cleaning tasks involving grease and adhered residues.
[035] Mechanical tensile strength and elongation tests were also conducted, in accordance with ABNT NBR 8515 and 8516 standards. The cleaning article obtained a peak tear strength of 29.3 Newtons and an elongation of 2057%. Comparatively, the conventional sponge tested showed a peak strength of 51.3 Newtons with an elongation of 1765%, demonstrating that, although it has lower maximum strength, the cleaning article of the invention has a greater capacity for deformation before rupture, a characteristic related to its elasticity and suitability for irregular surfaces.
[036] Field tests were also carried out under real-world conditions using anodized aluminum plates with a non-stick coating, simulating the internal surfaces of electric fryers. Using neutral detergent and scrubbing carbonized residues of oxidized vegetable oil (at 180°C for 2 hours), it was found that the cleaning article of the invention provided effective cleaning without causing visible abrasion to the protective film. The results confirm that the article meets the Class A abrasiveness criteria according to ISO 20567-1:2024, guaranteeing the preservation of non-stick surfaces.
[037] Thus, laboratory and usage tests confirm that the cleaning article, the subject of the present invention, has a high capacity to Petition 870250036351, dated 06 / 05 / 2025, page 22 / 28 / 13 absorption, excellent mechanical performance, and safe cleaning efficiency for sensitive surfaces, fully achieving its technical objective.
Claims
1. Multilayer cleaning article characterized in that it comprises a first layer comprising polyurethane foam obtained from the combination of long-chain polyol and short-chain polyol, and a second layer of semi-abrasive mat adhered to the foam; wherein the volumetric ratio between the foam and the mat varies from 45% to 55% for the foam and from 45% to 55% for the mat; wherein the foam has a density between 18 and 24 g / mL and incorporates nanoparticles with bactericidal and antiviral properties.
2. Cleaning article, according to claim 1, characterized in that it comprises the following components in parts per hundred parts of polyol: Polyol 3000: 88.0 ~ 98.0; TDI: 53.0 ~ 59.0; silicone: 1.90 ~ 2.10; amine: 0.076 ~ 0.084; tin dye: 0.162 ~ 0.178; red dye: 1.86 ~ 2.05; yellow dye: 0.105 ~ 0.116; water: 3.9 ~ 4.4; Polyol 1000: 6.6 ~ 7.
4.
3. Cleaning article, according to claim 1, characterized in that the foam preferably has a density between 20 and 22 g / mL. Petition 870250036351, dated 06 / 05 / 2025, page 24 / 28 2 / 4 4. Cleaning article, according to claim 1, characterized in that the nanoparticles with bactericidal and antiviral properties are zinc oxide; wherein, alternatively, silver, titanium dioxide, copper or functionalized graphene nanoparticles may be used.
5. Cleaning article, according to claim 1, characterized in that the semi-abrasive pad comprises a fibrous substrate and talc as a filler element.
6. Cleaning article, according to claim 1, characterized in that the fibrous substrate comprises a mixture of two fibers: 50% to 50% white polyester fiber and 50% to 50% polyamide fiber.
7. Method for manufacturing a multilayer cleaning article, characterized by comprising the steps of: polymerizing phenolic resins; producing a semi-abrasive mat by polymerizing phenolic resins with the incorporation of fillers on a fibrous substrate; dosing and mixing the chemical components of the foam; forming a foamy cream by exothermic reaction, with the release of carbon dioxide as an expanding agent; allowing the mixture to expand and letting it rest for complete curing and stabilization of the foam's cellular structure; cutting the foam; applying the mat over the foam by controlled pressure to ensure efficient adhesion and durability of the cleaning article. Petition 870250036351, dated 06 / 05 / 2025, page 25 / 28 3 / 4 8. Method according to claim 7, characterized in that the step of polymerizing phenolic resins comprises: a) hydroxymethylation step: in which phenol reacts with formaldehyde, originating intermediate compounds through the addition of hydroxymethyl groups (-CH2OH) to the aromatic ring of phenol; b) condensation step: in which the hydroxymethyl groups of the intermediates react with each other, promoting the formation of methylene and ether type linkages, connecting the phenolic rings to each other; c) prepolymer formation: as condensation progresses, there is a gradual increase in viscosity, forming the resol.
9. Method, according to claim 7, characterized in that the production step of the semi-abrasive blanket comprises: opening of synthetic fibers, in which these are unwound and subjected to a mechanical opening process; formation of the fibrous veil from the opened fibers, which are deposited on a conveyor belt, forming a continuous veil with controlled thickness and basis weight; impregnation with resin and pre-drying, in which the formed veil is uniformly impregnated with liquid phenolic resin and proceeds to a first oven, where pre-drying and the beginning of resin cross-linking occur; application of the filler element on the surface of the impregnated blanket and subsequent direction to a second oven, where partial curing of the resin and fixation of the filler to the blanket structure occurs; final curing of the phenolic resin by passing through a third and a fourth oven. Petition 870250036351, dated 06 / 05 / 2025, page 26 / 28 4 / 4 10. Method, according to claim 7, characterized in that the adhesion of the semi-abrasive pad to the foam is achieved by applying controlled pressure between 4 and 5 bar.