Natural latex healing with nanotechnology and bioative compostes from bixa orellana for the treatment of chronic fevers
A natural latex biomembrane with a nanoemulsion of Bixa orellana bioactive compounds addresses the limitations of conventional dressings by enhancing healing and antimicrobial activity, reducing amputation and hospitalization rates.
Patent Information
- Application Number
- BR102025009002
- Authority / Receiving Office
- BR · BR
- Patent Type
- Applications
- Publication Date
- 2026-11-17
AI Technical Summary
Conventional dressings for chronic wounds, particularly diabetic foot ulcers, face limitations in promoting rapid and lasting healing, are costly, cause skin irritation, and fail to actively combat bacterial infections, leading to high amputation and hospitalization rates.
A dressing composed of a natural latex biomembrane combined with a nanoemulsion containing bioactive compounds from Bixa orellana, including bixin, geranylgeraniol, and tocopherols, which enhances tissue regeneration and antimicrobial activity.
The dressing accelerates wound healing, reduces the need for frequent changes, decreases secondary infections, and lowers treatment costs, providing a more effective and sustainable solution for chronic wounds.
Smart Images

Figure 00000000_0000_ABST
Description
Natural latex dressing with nanotechnology and bioactive compounds from Bixa orellana for the treatment of chronic wounds. FIELD OF THE INVENTION
[001] This patent application relates to a dressing based on nanotechnology and natural products for the treatment of chronic and infected wounds, especially diabetic foot ulcers. The dressing is composed of a biomembrane based on natural latex (Hevea brasiliensis) - previously described in process no. BR 10 2016 019963-8 - with the added benefit of being associated with a nanoemulsion formulation containing standardized Bixa orellana extract (Bioxina®). The improved dressing, referred to in this document as CuraTex, integrates the anti-inflammatory and healing properties of latex with the bioactive compounds of Bioxina® (bixin, geranylgeraniol, and tocopherols), aiming for therapeutic synergy to reduce infections and promote tissue regeneration. It is noteworthy that the innovation of CuraTex lies in its technology, which favors greater bioavailability of its bioactive compounds in the wound, promoting accelerated healing. STATE OF TECHNOLOGY
[002] In recent years, several technologies have been developed for the treatment of chronic wounds, such as diabetic foot ulcers (DFU). However, the healing of Petition 870250036431, dated 06 / 05 / 2025, page 9 / 111 2 / 37 Diabetes-related wounds remain a challenge, given the inherent difficulty in healing these wounds, the high risk of infection, and the high rates of associated amputations.
[003] The dressing of this invention - CuraTex - has the potential to reduce amputations and hospitalizations in the Unified Health System (SUS) resulting from chronic wounds.
[004] The prior art search identified several patents that, at first glance, appear similar to the invention described in this document. However, they differ significantly in terms of chemical composition and / or therapeutic purpose. The following paragraphs will describe the research problem and the gaps in which our technology fits, as well as the therapeutic proposals of similar inventions.
[005] Diabetes is a chronic disease that affects millions of people worldwide and can lead to several serious complications if not properly controlled. According to the World Health Organization (WHO), approximately 422 million people live with diabetes globally, most of whom reside in low- and middle-income countries (WORLD HEALTH ORGANIZATION. 2023.)
[006] The complications associated with diabetes are diverse and include blindness, kidney failure, heart attacks, strokes, and lower limb amputations. These consequences not only affect the quality of life of patients but also impose a large financial burden on them. Petition 870250036431, dated 06 / 05 / 2025, page 10 / 111 3 / 37 health systems around the world (WORLD HEALTH ORGANIZATION. 2023; PAN AMERICAN HEALTH ORGANIZATION, 2023).
[007] The healing process, in turn, is highly complex, involving a series of carefully coordinated molecular and cellular events. In diabetic patients, the presence of chronic hyperglycemia triggers the formation of reactive oxygen species (ROS) and inflammatory cytokines.
[008] All these factors impair collagen synthesis and cell proliferation, resulting in a significant delay in wound healing (DIEGELMANN; EVANS. Frontiers in Bioscience. v.9, p. 283-289. 2004; TSOURDI et al. BioMed Research International. p.1-6. 2013).
[009] Furthermore, chronic wounds in diabetics often become favorable environments for the development of bacterial infections. This further aggravates the clinical picture, increasing the risk of severe complications such as amputations. Proper management of these wounds is therefore crucial to minimize negative impacts and improve patient prognosis (NOUVONG et al. Physiol Genomics. v. 1;48, n. 12, p.889-896. 2016).
[010] Infections, ulcers, and gangrene in the feet are frequent causes of hospitalization in diabetic patients, leading to more than 100,000 amputations annually. The economic and social impact of this condition is significant, both in terms of individual disability and healthcare costs, estimated at more than $1 billion annually (DRIVER et al. J Vasc Surg. v. 52, n. 3 Suppl, p. 17S-22S. Petition 870250036431, dated 06 / 05 / 2025, page 11 / 111 4 / 37 2010).
[011] In 2021, approximately 3 million people in Brazil were diagnosed with diabetic ulcers. Conventional approaches to the treatment of diabetic ulcers and chronic wounds often face limitations regarding effectiveness and the ability to promote rapid and lasting healing (BRAZILIAN DIABETES SOCIETY, 2021).
[012] This scenario highlights the urgent need for investments in research aimed at developing more innovative and curative therapeutic strategies.
[013] Treatment of UPD involves a multidisciplinary approach, including podiatric care, infection control, proper glycemic management and, in some cases, the use of advanced therapies such as negative pressure therapy and skin grafts (GARCES et al. Rev Esc Enferm USP. v. 57:e20230218. 2023).
[014] Early interventions are crucial to prevent serious complications and amputations (ARMSTRONG et al. N Engl J Med. v. 376 n. 24, p. 2367-2375, 2017). Many of the dressings available are made of synthetic materials that, while offering physical barriers against infection, do not actively stimulate the tissue regeneration process.
[015] Moreover, these materials can, in certain cases, cause skin irritation or allergic reactions, limiting their prolonged use and requiring constant replacements, which increases Petition 870250036431, dated 06 / 05 / 2025, page 12 / 111 5 / 37 costs and hinders adherence to treatment, especially in patients with reduced mobility (TSOURDI et al. BioMed Research International. p.1-6.2013; FALANGA. Lancet. v. 366, n. 9498, p. 1736-1743. 2005).
[016] Another significant limitation is the inability of conventional dressings to actively combat bacterial infections that frequently affect chronic wounds, especially in diabetic patients (SACCO et al. Soci. Brasil. de Diabetes. 2023; STANCU et al. Intern. Jour. of Environmental Research and Public Health. v. 20, no. 1, p. 187. 2022).
[017] Although some newer technologies include antimicrobial agents, such as silver and antibiotics, the continuous use of these compounds can lead to the development of bacterial resistance, as well as causing adverse effects, such as an imbalance in the skin's natural microbiota (BRAZIL, Advances and challenges in the industrial complex of health products. Ministry of Health. p. 232. 2017). In addition, the high cost and complexity of some existing biomaterials, such as those based on collagen and living cells, limit access and their viability in health systems with limited human resources.
[018] These bio-dressings require specific production and storage conditions, hindering their availability for widespread use (BRAZIL, Advances and challenges in the industrial complex of health products. Ministry of Health. p. 232. 2017). Thus, there is a gap in the market for Petition 870250036431, dated 06 / 05 / 2025, page 13 / 111 6 / 37 a solution that, in addition to being effective, is accessible and has biocompatible and biodegradable characteristics, in order to promote natural healing without the limitations associated with current technologies.
[019] Biomaterials have shown promise for the treatment of various wounds, including diabetic wounds, stimulating cellular recovery and being biocompatible (PIRES; BIERHALZ; MORAES. Química Nova. v. 500, 13083-852. (2015). Natural latex, a biomaterial produced by the rubber tree Hevea brasiliensis, has anti-inflammatory and healing properties (ROSA et al. Ann Biomed Eng. v. 47, n. 4, p. 1153-1164, 2019; NUNES et al. Research on Biomedical Engineering, vol. 32, no. 1, p. 3 — 13. 2016).
[020] Our research group has developed the Rapha® tissue neoformation therapeutic system, which consists of a combination of a natural latex biomembrane (NLB) with a low-intensity phototherapy device. This invention is described in process No. BR 10 2016 019963 8 29 / 8 / 2016.
[021] BLN-based dressings have properties that promote angiogenesis, re-epithelialization, and granulation tissue formation, being highly effective in wound treatment (ROSA, SSRF et al. Ann Biomed Eng. v. 47, n. 4, p. 1153-1164, 2019; BRASILEIRO et al. J Vasc Br. v. 4(1), p. 1121. 2005; ZIMMERMANN et al. Glob Health Res Policy. v. 3, n.3, p. 25. 2018).
[022] LED phototherapy, used in the Rapha® system, Petition 870250036431, dated 06 / 05 / 2025, p. 14 / 111 7 / 37 has been shown to be an efficient tool for accelerating wound healing, due to its ability to modulate inflammation and promote tissue regeneration (LI; XIA; KHOONG et al. Biomater Res. v. 27, p. 87. 2023; KUFFLER. Regen Med v. 11, no. 1, p. 107-22. 2016).
[023] Preliminary clinical trials with patients with UPD demonstrated healing rates superior to the conventional treatment used in the SUS (NUNES et al. Research on Biomedical Engineering, v. 32, n. 1, p. 3 — 13. 2016; MOIZINHO, CS Dissertation. (Mes. in Eng. Biom.) Univ. de Bras. 2021).
[024] Furthermore, it was observed that the Rapha® system was able to reduce non-viable tissue, wound edge contraction and inflammation, favoring the healing process and increasing the speed of diabetic ulcer healing (REIS. Thesis (PhD in Electrical Engineering) Univ. of Bras., 2013; ROSA, SSRF, et al. Ann Biomed Eng. v. 47, n. 4, p. 1153-1164, 2019).
[025] The Rapha® system was improved by adding curcumin to BLN (BioCur), due to the high therapeutic potential of this compound. Preliminary clinical trials (n = 5) showed that this system promoted superior healing compared to conventional SUS treatment and treatment with conventional Rapha®, although it did not show a significant antimicrobial effect (SANTANA, Dissert. (Mes. in Biom. Eng.) Univ. de Bras. 2021). This invention is described in process No. BR1020160199638.
[026] Considering these limitations, the present invention consists of a natural latex biomembrane combined with Petition 870250036431, dated 06 / 05 / 2025, page 15 / 111 8 / 37 nanotechnology (nanoemulsion formulation containing three bioactive compounds from Bixa orellana, including bixin, geranylgeraniol and tocotrienols, which have medicinal properties favorable to tissue healing and antimicrobial activity).
[027] Bixa orellana (BixO), popularly known as annatto, has bioactive compounds that are favorable to tissue regeneration (KAR et al. Proc. Natl. Acad. Sci. v. 119 (28) e2202222119. 2022; SANTOS et al. Rev Bras Pl Med. v. 16:637-643. 2014). Bixin, one of the main compounds of Bixa orellana, has antioxidant, antimicrobial and anti-inflammatory effects, making it effective in combating infections and in tissue regeneration.
[028] Through tocotrienols extracted from the seeds, this plant demonstrated inhibitory properties in individuals infected with methicillin-resistant Staphylococcus aureus, i.e., the methicillin-resistant S. aureus bacterium, significantly reducing the bacterial load of wounds in mice.
[029] The inhibitory effect of BixO seed extract can also be attributed to the presence of flavonoids, which can form extracellular complexes with soluble proteins and with the bacterial cell wall (DA SILVA et al. Studies in Natural Products Chemistry, v. 77, p. 1-36, 2023).
[030] The use of nanoemulsions to encapsulate bioactive compounds allows for a sustained and prolonged release of the substances directly at the wound site, increasing the Petition 870250036431, dated 06 / 05 / 2025, page 16 / 111 9 / 37 treatment effectiveness and reducing the need for frequent dressing changes (SILVA et al. Revista da Escola de Enfermagem da USP, v. 51, n. 1, p. 1-10, 2017). Furthermore, natural latex serves as a support for the incorporation of nanoemulsion, offering biocompatibility, biodegradability, and healing properties. This combination of materials allows for a comprehensive and effective solution for tissue regeneration and combating infections in chronic wounds (REIS. Thesis (Doctorate in Electrical Engineering) University of Brazil, 2013; ROSA, SSRF, et al. Ann Biomed Eng. v. 47, no. 4, p. 1153-1164, 2019).
[031] Reducing frequent dressing changes, a common problem in previous treatments, lowers costs, minimizes wound manipulation, and reduces the risk of secondary infections, providing more effective and convenient treatment for patients with chronic wounds (SILVA et al. Revista da Escola de Enfermagem da USP, v. 51, n. 1, p. 1-10, 2017; Ozelim et al. Journal of Pharmaceutical Sciences, vol. 113, p. 2383-2393, 2024).
[032] Inventions related to BixO will be presented below, as well as the differences between existing inventions and the invention proposed in this document.
[033] Patent BR 102014000206-5 A2 presents a liquid solution composed of bixin, a carotenoid from annatto seeds, combined with Dimethyl Sulfoxide (DMSO). The formulation has anti-inflammatory, antioxidant, and healing properties. The solution is indicated for topical application with a swab and has no contraindications or side effects. Petition 870250036431, dated 06 / 05 / 2025, page 17 / 111 10 / 37 significant adverse effects and is adaptable to various types of lesions and patients. This product (bixin solution) is not focused on the treatment of diabetic foot ulcers, and is a liquid solution with an isolated molecule from annatto, unlike the present solution, which consists of a latex biomembrane containing a nanoemulsion containing Bioxin® for the treatment of chronic wounds.
[034] Document BR 10 2016 015777-3 A2 describes bixin-loaded polycaprolactone (PCL) nanofibers for the treatment of ulcerative wounds, especially in patients with Diabetes Mellitus. The nanofibers were obtained using the electrospinning technique. The nanofibers combine the antioxidant, anti-inflammatory, and hypoglycemic properties of bixin with the biocompatibility and biodegradability of PCL, promoting effective wound healing. The process involves adding bixin to the PCL solution, followed by electrospinning and heat treatment. Studies have shown that the application of nanofibers accelerates healing and improves cell proliferation in diabetic animal models. Despite their effectiveness, these materials have limitations, such as low biodegradability and complex production methods, which increase the cost of the process and limit access for more disadvantaged populations.Furthermore, although this product (nanofibers with bixin) has a similar application to ours (wound healing), our invention differs because it consists of a dressing based on different materials, since it is composed of latex containing a nanoemulsion with Bioxina®, which contains bixin, tocotrienols, and geranylgeraniol. Petition 870250036431, dated 06 / 05 / 2025, p. 18 / 111 11 / 37
[035] Document BR 102017018152-9 A2 describes the invention of a biodegradable film based on cassava starch and rice flour, incorporating lyophilized plant extracts, which confer antimicrobial, anti-inflammatory and healing properties. Developed by the Federal University of Maranhão, the film is intended for the treatment of skin lesions, inhibiting the adhesion and proliferation of microorganisms. The main applications include its use on wounds, promoting safe and effective healing. The invention presented in this document, unlike the one cited, comprises a natural biofilm based on other types of materials (natural latex from H. brasiliensis containing nanoemulsion with incorporated bioactive compounds of annatto extract).
[036] Document BR 102016010599-4 A2 describes lipid nanocarriers with annatto oil (Bixa orellana L.), developed by the Federal University of Rio Grande do Norte for topical treatment of cutaneous leishmaniasis. The formulation, obtained by fusion-emulsification and ultrasonication, contains an oily fraction of annatto, structural lipids and surfactants. This product aims to treat topical lesions caused by protozoa of the genus Leishmania, unlike the objective proposed by the invention described in this application, which focuses on the healing of chronic wounds, in addition to reducing the bacterial load. Furthermore, the product proposed here has a different composition and presentation, as it is a... Petition 870250036431, dated 06 / 05 / 2025, page 19 / 111 12 / 37 a nanocarrier formulation with BixO and our invention is a dressing. Although our technology is derived from BixO, the dressing consists of natural latex from H. brasiliensis containing a nanoemulsion with a standardized extract of the seeds containing incorporated bioactive compounds (bixin, geranylgeraniol and tocotrienols).
[037] Document BR 102018069700-5 A2 describes a veterinary formulation developed by the Federal University of Pelotas, composed of extracts of Triticum aestivum (wheat) and Bixa orellana (annatto). The technology is intended for veterinary use in the healing of open wounds and to repel ectoparasites. Our invention is aimed at the treatment of chronic human wounds, such as diabetic foot ulcers, focusing on accelerating healing and combating infections through the use of a natural latex biomembrane combined with a nanoemulsion containing bioactive compounds from Bixa orellana.
[038] Document BR 102020014685-8 A2 describes the invention of chitosan / norbixin and chitosan / PVA / norbixin films, developed by the Federal Institute of Education, Science and Technology of Piauí. The invention aims to create biomaterials in the form of polymeric films for application in tissue regeneration and drug delivery systems. These films, composed of chitosan, poly(vinyl alcohol) (PVA) and norbixin, retain moisture and serve as a support for the diffusion of cells, bioactive molecules and drugs, showing promise for the regeneration of cutaneous, bone, and other tissues. Petition 870250036431, dated 06 / 05 / 2025, page 20 / 111 13 / 37 cartilage lesions, among others. The films are produced using the solvent casting technique, involving the dissolution of the components, mixing, vacuum filtration, and controlled drying. This patent describes a biomaterial developed from 3 components (chitosan, PVA, and norbixin), none of which are present in the invention described in this application.
[039] Document BR 102020014685-8 A2 presents the development of a natural cluster containing standardized oil in tocotrienols and geranylgeraniol from Bixa orellana and standardized ethanolic extract in anthocyanins from Euterpe oleracea (acai), intended for the treatment of atherogenic dyslipidemia, osteoporosis, and oxidative stress. This product aims to combine the antioxidant and anti-inflammatory properties of tocotrienols and geranylgeraniol with anthocyanins to reduce abnormal blood lipids, promote bone health, and combat oxidative stress. The patent differs from the present application, which focuses on application for wound treatment. Furthermore, the dressing we developed uses entirely different materials (natural latex biomembrane with nanoemulsions containing bioactive compounds from BixO).
[040] Document BR1120210173396 describes an antimicrobial mixture intended for various cosmetic and pharmaceutical applications. The composition contains ingredients that confer antimicrobial properties (which may include components of Bixa orellana), making it suitable for use in personal care products, cleaning products, and other applications where the reduction or elimination of microorganisms is desired. Petition 870250036431, dated 06 / 05 / 2025, page 21 / 111 14 / 37 desirable. The objectives and benefits include efficacy against a wide range of microorganisms, safety for use in skin contact, and versatility for incorporation into various consumer product formulations.
[041] The product described refers to a formulation with biological activity restricted to antimicrobial action, which differs from the invention of the present application which consists of a dressing based on materials not previously described and which has application in wound healing.
[042] Patent BR1020160201900 A2 describes the use of an antimicrobial phytotherapeutic product obtained from the crude extract of Bixa orellana L. leaves, which can have various presentations from capsules to ointments, with antimicrobial action against bacteria and fungi, where the formulation inhibits the formation, as well as degrades the biofilm formed by these microorganisms. Unlike CuraTex, which uses standardized extract and Bixa orellana seed, this invention uses crude hydroalcoholic extract of Bixa orellana L. leaves, obtained from the fresh plant by cold maceration.
[043] Still regarding films with healing activity, invention BR 1020200146858 A2 refers to a chitosan and norbixin film for application in the regeneration of injured tissues. Our technology differs from this invention because it consists of a different composition, being natural latex from H. brasiliensis containing a nanoemulsion with incorporated bioactive compounds (bixin, geranylgeraniol and tocotrienols). Petition 870250036431, dated 06 / 05 / 2025, page 22 / 111 15 / 37
[044] Invention BR 1020170180808 A2 refers to the production of matrices for tissue engineering in the form of foams and / or membranes made of polymers, ceramics, polymeric and / or ceramic composites containing crude extract of Bixa orellana L., capable of inducing tissue regeneration in vivo, as well as tissue growth in vitro. Our technology differs from this invention because it is made up of other types of materials, namely, natural latex from H. brasilienses containing nanoemulsion with incorporated bioactive compounds (bixin, geranylgeraniol and tocotrienols).
[045] Invention BR 1020190040327 A2 also concerns a starch-melamine based polymeric matrix containing Bixa orellana L. extract with healing application in skin lesions. Although it has a similar application, our technology differs from this invention because it is constituted by natural latex of H. brasilienses with nanoemulsion containing incorporated bioactive compounds (bixin, geranylgeraniol and tocotrienols), unlike this invention.
[046] Invention number CN 109793914 describes a self-adhesive elastic latex bandage with antibacterial properties and a method for producing it. It is made of a natural latex adhesive and elastic fabric, with special components that help fight bacteria and prevent wound infections. The technology maintains the bandage's flexibility while including elements such as silver ions for antibacterial protection, helping to accelerate wound healing and improving its use in dressings. Our dressing integrates the anti-inflammatory and healing properties of latex with other bioactive compounds such as bixin, Petition 870250036431, dated 06 / 05 / 2025, p. 23 / 111 16 / 37 geranylgeraniol and tocopherols, from BixO. In the CN 109793914 technology there is no mention of the use of nanoemulsions with Bixa orellana compounds.
[047] Invention CN114605601A describes an active nano-latex and its production method. The nano-latex is formed by a polymeric particle with a core-shell structure, where the core and shell are made of different polymer segments. The outer part (shell) is composed of one type of polymer chain, while the core is formed by another type. In addition, there is an active cationic center at the end of one of the chains, which can facilitate chemical interactions. This type of latex can be used in various applications due to its advanced properties. In the cited technology, polymeric nanoparticles are used, and there is no mention of the use of nanoemulsions or Bixa orellana compounds.
[048] Invention CN101031281A refers to nanoemulsions and their production method. These nanoemulsions use vitamin E as an emulsifier, along with polyacrylic acid or its derivatives to aid in the emulsification process. The particles formed are very small, with a diameter between 43 and 96 nm, and are stable and safe. They are used in cosmetic compositions, providing benefits such as hydration, skin softening, improvement of dry or atopic skin, and helping to firm the skin. Nanoemulsions also have good spreading ability when applied to the skin. Petition 870250036431, dated 06 / 05 / 2025, page 24 / 111 17 / 37
[049] In technology CN101031281A, nanoemulsions using vitamin E (Bixa orellana oil) as an emulsifier are used. The nanoemulsions incorporated into CuraTex were produced with sunflower oil and other compounds. Furthermore, our technology refers to a dressing based on a natural latex biomembrane and nanoemulsions containing bioactive compounds from Bioxina® (bixin, geranylgeraniol and tocopherols) for cell regeneration, i.e., the presentation, application and composition are distinct from the technology referred to.
[050] The invention US 2009 / 0263468 A1 describes methods and compositions for wound healing. It uses modified molecules to attach and release active agents directly into the wound, helping to improve the healing process. Furthermore, the invention involves the use of oppositely charged polymers to form a protective layer called a polyelectrolyte on the wound surface, into which active agents can be incorporated, promoting more effective healing. In US patent 2009 / 0263468, it is unclear which molecules were used to promote healing. However, it is described that oppositely charged polymers (polyelectrolyte) are used in the wound.
[051] CuraTex, our technology, is based on a natural latex biomembrane and nanoemulsions containing bioactive compounds from Bioxina® (bixin, geranylgeraniol and tocopherols), meaning the composition is specific and not described in US patent 2009 / 0263468. Another technical difference is the use of natural latex as a support to incorporate the nanoemulsion. This material has properties that promote healing, in addition to exhibiting biocompatibility and biodegradability. Petition 870250036431, dated 06 / 05 / 2025, page 25 / 111 18 / 37 ensuring safe and environmentally sustainable treatment.
[052] The patents found in the prior art search address some level of similarity with our invention. However, none report the association of natural latex biomembrane, standardized annatto extract (Bioxina®) and / or nanoemulsions.
[053] The combination of latex biomembrane with nanoemulsion and bioactives solves technical problems that other technologies do not fully address. Thus, this invention stands out for its advanced technology, combining an innovative dressing containing nanoemulsion, biocompatible latex biomembrane and bioactive compounds that exhibit synergistic action for healing. This technology offers rapid healing, reduces the need for frequent dressing changes, and decreases the risk of secondary infections, thus providing a more effective and sustainable treatment compared to existing technologies. BRIEF DESCRIPTION OF THE FIGURES
[054] The invention may be better understood based on Figures 1 to 15, the description of which follows below:
[055] Figure 1 shows the visual aspect of the nanoemulsion containing Bioxina®. The homogeneity of the sample without phase separation is evident. Petition 870250036431, dated 06 / 05 / 2025, page 26 / 111 19 / 37
[056] Figure 2 shows a representation of a natural latex biomembrane containing Bioxina® (CuraTex).
[057] Figure 3 shows the scanning electron microscopy (SEM) of the biomembranes based on latex and annatto extract. LBM: biomembrane with only latex. LBM - A: Latex biomembrane with standardized annatto extract. LBM - Nano A: latex biomembrane with nanostructured standardized annatto extract.
[058] Figure 4 shows optical microscopy in reflection and transmission modes of biomembranes based on latex and annatto extract. LBM: biomembrane with only latex. LBM A: latex biomembrane with standardized annatto extract. LBM - Nano A: latex biomembrane with nanostructured standardized annatto extract. Long arrows indicate the presence of pores. Short arrows indicate the presence of striations.
[059] Figure 5 shows the infrared spectra of the natural latex samples (A), Bioxina® (B) and the superimposed spectra of the latex, Bioxina® and LBM-A samples (C).
[060] Figure 6 shows the Raman spectra of the latex samples, Bioxina®, latex biomembrane containing Bioxina® and physical mixture between latex and Bioxina®.
[061] Figure 7 represents the analyses obtained by the first derivative of TG (DrTG) of pure latex biomembranes or Petition 870250036431, dated 06 / 05 / 2025, page 27 / 111 20 / 37 containing nanoemulsion or Bioxina®. Each mass loss event is indicated in the figures as a percentage (%). LBMNano A: biomembrane containing nanostructured Bioxina®; LBM- A: Biomembrane containing Bioxina® with latex; LBM: Latex biomembrane.
[062] Figure 8 shows photomicrographs of the rupture of latex-based biomembranes and annatto extract after tensile strength testing. LBM: biomembrane with latex only. LBM - A: latex biomembrane with standardized annatto extract. LBM - Nano A: latex biomembrane with nanostructured standardized annatto extract. The arrows indicate the location where the samples ruptured.
[063] Figure 9 presents the evaluation of the tensile strength of biomembranes based on latex and annatto extract. A) Percentage of tensile strength. Values are expressed as mean ± SD. B) Relationship between tensile strength and elongation. LBM: biomembrane with only latex. LBM - A: Latex biomembrane with standardized annatto extract. LBM - Nano A: latex biomembrane with nanostructured standardized annatto extract.
[064] Figure 10 presents the results of the evaluation of cell viability in keratinocyte cells (HaCat) for 24h in 5 different concentrations of Bioxina®, nanoemulsion containing Bioxina® and the blank nanoemulsion. DMEM medium was used as a control, as was DMSO, used to solubilize the extract. The data represent the Mean ± Standard Deviation. (*) Two-way ANOVA: significant difference between the negative control and DMSO groups compared to the others. Petition 870250036431, dated 06 / 05 / 2025, page 28 / 111 21 / 37 groups p<0.05 (Tukey post-test).
[065] Figure 11 presents the results of the evaluation of cell viability in keratinocyte cells (HaCat) for 24h in 3 different concentrations of latex, latex mixed with Bioxina® and latex mixed with nanoemulsion containing Bioxina®. DMEM medium was used as a control, as was DMSO, used to solubilize the extract. The data represent the Mean ± Standard Deviation. Two-way ANOVA: significant difference between the negative control and DMSO groups compared to the other groups p<0.05 (Tukey post-test).
[066] Figure 12 presents the results of the evaluation of cell viability in fibroblast cells (FGH) for 24h in 5 different concentrations of Bioxin®, nanoemulsion containing Bioxin® and the blank nanoemulsion. DMEM medium was used as a control, as was DMSO, used to solubilize the extract. The data represent the Mean ± Standard Deviation. (*) Two-way ANOVA: significant difference between the negative control and DMSO groups compared to the other groups p<0.05 (Tukey post-test).
[067] Figure 13 shows photographic records of the wells with keratinocyte cells in the cell migration assay with treatments with Bioxina®, nanoemulsion containing Bioxina® (NBIX) or not (NB), DMSO and the control.
[068] Figure 14 represents the rate of cell migration in keratinocyte cells (HaCat). Data represent Mean ± Standard Deviation. (*) Two-way ANOVA: significant difference between the negative control and DMSO groups in Petition 870250036431, dated 06 / 05 / 2025, page 29 / 111 22 / 37 comparison with the other groups p<0.05 (Tukey post-test).
[069] Figure 15 presents the MTT bacterial viability assay in methicillin-resistant Staphylococcus aureus (MRSA) bacteria, subjected to treatments with isolated Bioxin extract diluted in Andiroba oil and negative controls (culture medium) and DMSO (culture medium and 0.6% Dimethyl sulfoxide-DMSO) at concentrations of 31.25 to 250 μg / mL over a 24-hour period. Two-way ANOVA: significant difference between the negative control and DMSO groups compared to the other groups p<0.0001 (Tukey post-test). The different letters indicated in the graph show statistical differences between the groups. DETAILED DESCRIPTION OF THE INVENTION
[070] This invention addresses the development of a dressing based on a natural latex biomembrane (Hevea brasiliensis) with a nanoemulsion containing a standardized extract of bixin, geranylgeraniol and tocopherols from Bixa orellana L. (Bioxina®), for the treatment of chronic wounds, especially pressure ulcers.
[071] Natural latex biomembranes are produced by incorporating a suspension of nanoemulsions containing Bioxina® into liquid natural latex mixed in a ratio of 1:1 to 1:3 (v / v). The incorporation of the Bioxina® extract into nanostructures involves the development of a nanoemulsion system, consisting of an aqueous and an oily phase, stabilized by a mixture of non-ionic surfactants. The procedure for obtaining this dressing comprises the following steps: Petition 870250036431, dated 06 / 05 / 2025, page 30 / 111 23 / 37 a. Incorporation of bioxin extract at concentrations of 5 to 100 mg / mL into an oily matrix formed by sunflower oil (Helianthus annuus) at concentrations of 1 to 30% (w / v). b. Mixture of the surfactants Span® 80 and Tween® 20 at concentrations of 1 to 25% (w / v). c. Dispersion of all components in ultrapure water obtained by reverse osmosis. d. Sonication under ice bath with an energy input of 1,000,000 to 5,000,000 J and an amplitude of 10 to 50% in alternating pulse (on / off) for a period of 1 to 100 minutes. e. Centrifugation at a speed of 1,000 to 10,000 rpm to remove insoluble bioxin extract residues. f. Mixing the nanoemulsion solution with liquid natural latex in a ratio of 1:1 to 1:3 (v / v) in a glass beaker. g. After homogenization for 10 minutes under magnetic stirring at 900 to 1200 rpm, 10 mL of this mixture were dispersed in 10 cm diameter Petri dishes using an automatic pipette. The dish served as a mold for the vulcanization process, and the material deposited in it was left to stand for 48 hours at room temperature. h. After this time has elapsed, the plates are stored in a Petition 870250036431, dated 06 / 05 / 2025, page 31 / 111 24 / 37 oven at 35°C for 1 hour to complete the vulcanization process. Subsequently, the biomembranes were left to rest for another hour at room temperature for complete cooling. Demolding was performed using Adson forceps, and the edges were removed with the aid of a disposable scalpel blade #22. Finally, the samples were stored wrapped in parchment paper inside surgical grade paper, awaiting analysis.
[072] The material produced was characterized in terms of chemical, physical, biological and mechanical aspects, as described below. a) Morphology: Morphology was evaluated by high-resolution SEM (Tabletop SEM, TM4000 PLUS II series with Oxford Aztec EDS detector, Hitachi), at a 90° angle, 5.00 kV, and 300X magnification. Before obtaining the images, the sample was fixed with carbon-coated double-sided tape. It was also evaluated by Transmission and Reflection Optical Microscopy using an optical microscope (Hirox-KH1300 model, MX(G) 5040Z), in transmission and reflection mode, at 100X magnification. b) Attenuated total reflectance infrared spectroscopy (ATR-FTIR): This was applied to identify functional groups of latex and Bioxin®, as well as their interactions when combined. A spectrophotometer (Bruker, model Vertex 70) was used. Measurements were averaged over 96 scans, performed with a resolution of 4 cm⁻¹ from 400 to 4000 cm⁻¹. Petition 870250036431, dated 06 / 05 / 2025, p. 32 / 111 25 / 37 c) Raman Spectroscopy: The determination of the vibrational energy levels of atoms or molecules present in samples and the chemical bonds present were evaluated using Raman microspectroscopy (LabRam HR Evolution, Horiba). The analysis was performed with a resolution of 0.7 cm⁻¹ in the range of 500 to 3800 cm⁻¹, with equipment equipped with an 1800 lines / mm grating and a charge-coupled device (CCD). Measurements were taken with a semiconductor laser source tuned to the 532 nm line, focused on the samples using an Olympus microscope with a 50X objective and numerical aperture (NA) = 0.55. The biomembranes were placed directly in the microscope, with no alteration in their physical characteristics. d) Thermal analysis: Thermogravimetric analysis (TGA) was performed using a thermogravimetric module (model DTG-60, Shimadzu). For this, 6 mg of sample was placed in an aluminum crucible with a temperature range of 30 to 600°C and a heating rate of 10°C / min, in a nitrogen atmosphere with a flow rate of 50 mL min-1. e) Tensile strength: Biomechanical tests were performed to determine the degree of deformation and resistance of the biomaterials. The biomembranes were subjected to a mechanical tensile strength test using a universal testing machine, model 3366, Instron, USA. For the evaluation, 5 (five) test specimens were cut from the sample in a hydraulic press using a type 3 mold and prepared according to ABNT NBR ISO 37:2014. The equipment Petition 870250036431, dated 06 / 05 / 2025, page 33 / 111 26 / 37 was operated with a 10 kN load cell and the nominal displacement speed of the gripper movement was determined to be 200 mm.min-1.
[073] Assays were performed to evaluate the cytotoxicity characteristics of the biomembranes in vitro. For this, the MTT assay (3-[4,5-dimethylthiazol-2-yl]-2,5-diphenyltetrazolium bromide) was used. For the assay, the biomembranes were weighed, added to an extraction solution (PBS) in a 1:1 (w / v) ratio and incubated at 37°C for 24 hours. Subsequently, the extraction solution was immediately incubated with the cells as described below. f) Cells were seeded in a 96-well culture plate at a density of 5 x 10³ cells per well in culture medium overnight at 37°C, 5% CO₂ in a humid atmosphere. The medium was then changed, and various proportions of biomembrane extracts (6.25 to 25%) were added. For the nanostructures, blank nanoemulsion (without annatto extract), annatto-free extract, and annatto extract nanoemulsion (6.25 to 200 μg / mL, considering the annatto extract concentration) were added to the cells. The annatto-free extract was previously diluted in ethanol with a final ethanol concentration of less than 1% per well, which is non-toxic to the cells. The plates were incubated for 24 hours at 37°C, 5% CO₂ in a humid atmosphere. g) After 24 hours of incubation, the treatments were removed, and 150 pL of MTT solution (0.5 mg / mL in DMEM) Petition 870250036431, dated 06 / 05 / 2025, page 34 / 111 27 / 37 were added to each well. The plates were incubated for 2 hours at 37°C and 5% CO2 in a humid atmosphere. The culture medium was discarded and 150 μL of dimethyl sulfoxide (DMSO) were added to each well. Absorbance was measured using a spectrophotometer with a microplate reader at 595 nm. The control group was considered to have 100% cell viability. Each concentration was performed in triplicate. Mean cell viability values were calculated relative to the control mean (PBS and DMSO).
[074] To assess the potential for tissue regeneration, a cell migration assay was performed on keratinocyte cell lines over a period of 6 h and 24 h. After trypsinization, 3 x 10⁴ cells / well were seeded in 24-well plates to grow as a monolayer for 48 hours in DMEM medium supplemented with 1% (v / v) fetal bovine serum (v / v), incubated overnight at 37°C, 5% CO₂ in a humid atmosphere. For the cell migration assay (scratch), a straight scratch was made in the central region of each well using the tip of a 200 μL pipette, simulating a wound. After the risk assessment, the cells were exposed to the biomaterials (Bioxina®, nanoemulsion with and without Bioxina®, biomembrane with Bioxina® nanoemulsion) at a concentration of 31.25 μL / ml and controls (DMSO and DMEM) for a period of 24 hours in culture medium containing 1% fetal bovine serum. For image recording, the EVOS microscope was used at 0 h, 6 h and 24 h.
[075] In order to verify the antimicrobial potential of Bioxina®, the MTT method was used with methicillin-resistant Staphylococcus aureus (MRSA) bacterial strains. In this Petition 870250036431, dated 06 / 05 / 2025, page 35 / 111 In the 28 / 37 experiment, Bioxina® extract was diluted in Andiroba oil (Carapa guianensis), a vegetable oil rich in bioactive compounds that exhibits various healing, anti-inflammatory, and antioxidant activities (HENRIQUES; PENIDO. Current Pharmaceutical Design. v. 20, n. 6, p. 850 — 856. 2014).
[076] The isolated extract diluted in DMSO and in Andiroba oil was tested at concentrations of 31.25, 62.5, 125 and 250 μg / mL. The bacteria were incubated with the extracts at these concentrations for 24 h. After this period, 10 μL of 5 mg / mL MTT solution were added and the plate was incubated again in an oven. After a 1 h incubation period, 100 μL of DMSO were added to each of the wells. Absorbance was determined using a spectrophotometer with a microplate reader (Thermo Fisher Scientific, USA) at a wavelength of 595 nm. EXAMPLES OF CONCRETIZATIONS OF THE INVENTION
[077] Cell viability, mechanical resistance, and antimicrobial assays were performed, demonstrating that the dressing can reduce bacterial load and promote rapid and efficient healing. Application examples are presented to illustrate certain embodiments of the invention in more detail. It is important to note that the present invention is not limited to the examples cited and can be used in all the applications described or in any other equivalent variations. Unlike other technologies mentioned, such as PCL (polycaprolactone) nanofibers, CuraTex uses a latex biomembrane with bioactive compounds from annatto (Bioxin orellana), Petition 870250036431, dated 06 / 05 / 2025, page 36 / 111 29 / 37 demonstrating to be an advanced therapeutic solution for healing chronic wounds. EXAMPLE 1: Production of nanoemulsions
[078] In order to evaluate the effectiveness of the development of nanostructures, the nanoemulsions produced (Figure 1) were characterized in terms of their physicochemical characteristics of hydrodynamic diameter, polydispersity index and zeta potential by means of the dynamic light scattering technique in the Zetasizer equipment (Malvern, UK).
[079] The nanoemulsions produced presented a hydrodynamic diameter of 132.26 ± 13.10 nm, a polydispersity index of 0.362 ± 0.081, and a zeta potential of -36.13 ± 1.08 mV. All these characteristics described are in accordance with the literature description of nanoemulsion systems for therapeutic use, which consist of homogeneous nanodroplets smaller than 200 nm, exhibiting a polydispersity index less than or equal to 0.3 and a zeta potential of ±30 mV, which guarantees the electrostatic repulsion necessary to prevent coalescence between the nanodroplets and ensure greater stability of the formulation (CHAVDA et al. Nanomedicine. v. 19, n. 6, p.519-536, 2024). EXAMPLE 2: Physicochemical characterization - Morphology
[080] With the purpose of analyzing the morphology of the biomaterial For CuraTex (Figure 2), an electron microscope was used. Petition 870250036431, dated 06 / 05 / 2025, page 37 / 111 30 / 37 scan (SEM). SEM allowed visualization of the sample surface, showing that the LBM biomembrane exhibits a surface roughness similar to the arrangement of latex fibers, which apparently promotes its elasticity. In LBM A, the presence of fibers is reduced, and the surface roughness is less pronounced compared to LBM. In the LBM Nano A sample, the presence of fibers is not observed. Some dark spots in the image are perceptible, potentially associated with the presence of oil in the sample (one of the components of this formulation) (Figure 3).
[081] Using optical microscopy in reflection mode, it was possible to observe the presence of whitish spots indicative of pores in the samples (Figure 4). LBM exhibits a denser topography with fewer pores. LBM - A shows the presence of pores distributed heterogeneously along the surface. Interestingly, LBM - Nano A presents numerous pores uniformly distributed across the surface of the biomembrane.
[082] In transmission mode, LBM-A reveals the presence of regular striations along the surface, in addition to pores indicated by the dark spots in the image. Some whitish spots are also visible, possibly related to the presence of annatto extract. Notably, the LBM and LBM-Nano A samples do not show striations. LBM presents a limited number of pores heterogeneously distributed along the surface. LBM-Nano A exhibits numerous pores (dark spots) uniformly distributed along the surface and the presence of whitish spots, possibly associated with the organization of the annatto extract. Petition 870250036431, dated 06 / 05 / 2025, p. 38 / 111 31 / 37 after vulcanization. EXAMPLE 3: Physicochemical characterization - Attenuated total reflectance infrared spectroscopy (ATR-FTIR)
[083] Infrared spectroscopy is performed to analyze the structural chemical characteristics of latex and Bioxina®, as well as their interactions when associated in LBM-A. The organic components of the latex were identified by absorbance peaks, such as poly(cis-1,4-polyisoprene) between 2926-2852 cm-1, 1446 cm-1, 1375 cm-1 (CH2 and CH3 deformation), and 833 cm-1 (out-of-plane bending of =CH), consistent with the literature and related to the non-rubber fraction (AGOSTINI. Dissert. (Mes. in Science and Technology of Materials) Univ. Est. Paul. 2009). The peak at 1647 cm-1 indicates the symmetrical stretching of the carboxylate anion, linked to the protein part of the latex, and the peak at 833 cm-1 is essential to identify natural latex (Figure 5). The region between 1700 and 1000 cm-1 highlights the protein component, which is relevant for angiogenesis and tissue regeneration.
[084] The FTIR of Bioxina® reveals a peak at 1150 cm-1, characterizing the CO bond of bixin, a carotenoid present in the standardized annatto extract (Bioxina®), caused by the stretching vibration of the carboxylic acid. Another peak between 1100 cm-1 and 1000 cm-1, at 1018 cm-1, indicates the ether vibration (YUSÁ-MARCO et al. Arché. n. 3, p. 153—158. 2008). Bixin appears in three peaks due to vibrational transitions (BRITTON; LIAAEN-JENSEN; PFANDER. Scientific Research Publishing. v. 1B. 1995), and the signals at 1635 cm-1, Petition 870250036431, dated 06 / 05 / 2025, p. 39 / 111 32 / 37 2916 cm⁻¹, 2920 cm⁻¹ and 1375 cm⁻¹ indicate C=C and CH bonds, present in geranylgeraniol. (ZEFERINO. Thesis (Doctorate in Chemical Engineering) Federal University of San Cat. 2021. The main characteristic absorption bands of natural latex (A) and bioxin (B) are presented in Table 1: Table 1. Main absorption bands of Latex and Bioxin in infrared spectra (FTIR). AB Main Absorption Bands of Latas Legend Frequency Experimental Literature Chemical Group 1 3387 3200-2400 Free NH OH (Hydrogen bonding) 2 292b 2852 2960-2852 Cis-1,4-polyisopropene (symmetrical CH2 and asymmetrical CH3 stretching) 3 1647 1659 C=C elongation 4 1446-1375 1446-1375 CH=C deformation 5 833 835 Out-of-plane bending of CH 6 732-493 800-100 Presence of aldehydes, ketones, carboxylic acids and amino acids 7 1123-1012 1100-1000 Rubber molecules Source: Adapted from Agostini (2009) Main Absorption Bands of Bioxin Legend Experimental Frequency Literature Chemical Group 1 2916-2920 1375 2968-2856 1376 Bonds present in Geraniol 2 1635 1667 C=C 3 1375-1635 1465-1380 CH3 present in Tocotrienols 4 1150 1100-1000 C-O present in Bixin 5 1018 1018 Ether stretching Source: Adapted from Marquardt (2022)
[085] These results are aligned with the literature, which also associates the peaks at 1375 cm⁻¹ and 1635 cm⁻¹ with the presence of flavonoids in Bioxina® (MARQUARDT. TCC (Gradu. in Textile Engineering) Univ. Fed. de Santa Cat. 2022) (Figure 5)
[086] The results of the overlapping spectra of the latex, Bioxina®, and LBM-A samples show that the peaks at 2916 cm⁻¹ and 2920 cm⁻¹ of Bioxina® intensified the peak of the poly(cis-1,4-polyisoprene) chain in the latex, evidencing an interaction between the biomaterials. The region between 1700 and 1000 cm⁻¹ highlights the protein part of the latex, which remains in the biomembrane and acts as an inducer of angiogenesis, essential for tissue regeneration (AGOSTINI. Dissert. (Mes. in Cien. e Tec. de Mater.) Univ. Est. Paul. 2009). It is concluded that there was an interaction between latex and Bioxina® in LBM-A, preserving important peaks for Petition 870250036431, dated 06 / 05 / 2025, page 40 / 111 33 / 37 regeneration and therapeutic activity, reinforcing its potential as a bioactive curative (Figure 5). EXAMPLE 4: Physicochemical characterization - Spectroscopy Raman
[087] Raman spectra were obtained from samples of raw latex, Bioxina®, a physical mixture of raw latex with Bioxina® (prepared at the time of analysis), and a latex biomembrane containing Bioxina®. The Bioxina®, LBM-A, and physical mixture samples exhibited fluorescence, which masked the signal of the peaks (AGOSTINI. Dissert. (Mes. in Cien. e Tec. de Mater.) Univ. Est. Paul. 2009). Even so, the latex, LBM-A, and physical mixture samples showed characteristic isoprene peaks, with emphasis on the 998 cm-1 peak, linked to =CH vibrations, which did not persist in LBM-A and the physical mixture (Figure 6).
[088] Furthermore, peaks were observed at 1371 cm⁻¹, representing the deformation of the CH₃ groups in the latex, and at 1440 cm⁻¹, linked to HC=O bonds. The peak at 1668 cm⁻¹ indicated cis vibrations of C=C, while the vibration at 2930 cm⁻¹ corresponded to the CH stretching of the CH₂ and CH₃ groups (NALLASAMY; MOHAN. The Arabian Journal for Science and Engineering, v. 29, n. 1a. 2004). Despite the fluorescence, characteristic carotenoid bands from Bioxina® were identified between 1500-1550 cm⁻¹, attributed to the C=C mode (OLIVEIRA; SIQUEIRA; OLIVEIRA. 31st Annual Meeting of the Brazilian Chemical Society, 2008) (Figure 6). Petition 870250036431, dated 06 / 05 / 2025, page 41 / 111 34 / 37 EXAMPLE 5: Physicochemical characterization - Analysis (TGA)
[089] To evaluate thermal stability, in order to verify variations in the behavior of samples during thermal decomposition, thermogravimetric analysis (TGA) was performed in a thermogravimetric module (model DTG-60, Shimadzu). The biomembrane containing nanostructured Bioxina® (LBM - Nano A) showed 93.3% loss, while the biomembrane with Bioxina® and latex (LBM - A) had 94.4% and the latex biomembrane (LBM) showed 88.7% (Figure 7).
[090] All biomembranes showed a single mass loss stage between 301-470 °C, related to the decomposition of substances. This result suggests that biomembranes undergo a similar decomposition process, occurring at similar temperatures and with similar mass loss percentages. EXAMPLE 6: Physicochemical characterization - Resistance Mechanics
[091] Tensile tests revealed that the composition of the biomembranes influences their deformation and resistance (Figure 8). The addition of Bioxin extract to natural latex resulted in a slight decrease in mechanical resistance. The latex biomembrane (LBM) ruptured at approximately 10.23 mm of deformation, while the biomembrane containing Bioxin (LBM-A) ruptured at 11.36 mm of deformation. The rupture forces were 10.95 MPa for LBM and 10.93 MPa for CuraTex, indicating that, despite the Petition 870250036431, dated 06 / 05 / 2025, page 42 / 111 35 / 37 Although CuraTex underwent greater deformation, the difference between the biomaterials was not significant (Figure 9).
[092] These variations in mechanical properties are probably related to the number and type of cross-links, which increase with the addition of compounds to the latex (HERCULANO. Thesis (PhD in Applied Physics to Medicine and Biology) Univ. of São Paulo. 2009). Natural latex has sufficient resistance for biological applications, and the small changes observed with the addition of Bioxin do not compromise its effectiveness. Both biomaterials have adequate resistance for use as a primary dressing for diabetic foot ulcers. EXAMPLE 7: Cell viability assay - in vitro
[093] The evaluation of cell viability of treatments with free Bioxina®, Nanoemulsion with and without Bioxina®, was performed with keratinocyte (HaCat) and fibroblast (FGH) cell lines at concentrations of (C1 = 500 pL / mL, C2 = 250 pL / mL, C3 = 125 pL / mL, C4 = 62.5 pL / mL and C5 = 31.25 pL / mL) over a period of hours. In HaCat cells, the dry extract and the blank nanoemulsion caused marked toxicity at a concentration of 500 pL / mL, and moderate toxicity at 250 pL / mL. Cell viability with the nanoemulsion treatment containing Bioxina® averaged 75% at concentrations greater than 125 pL / mL, but 100% at lower concentrations (Figure 10). In FGH cells, all three treatments were toxic at the highest concentration (500 pL / mL). At other concentrations, Bioxina® demonstrated a proliferative effect, with cell viability above 100%. The treatment with the nanoemulsion containing Bioxina® showed 100% viability at concentrations below 125 pL / mL (Figure Petition 870250036431, dated 06 / 05 / 2025, page 43 / 111 36 / 37 11).
[094] Cell viability assays were also performed with the HaCat cell line under treatment with extracts of natural latex biomembrane, latex biomembrane with dry Bioxina® extract, and biomembrane with nanoemulsion containing Bioxina® at 3 concentrations (25% = 50 pL / mL, 12.5% = 25 pL / mL and 6.25% = 12.5 pL / mL) using PBS as a diluent. The concentration of the extracts with latex and the latex with nanoemulsion at 25% showed a significant difference compared to the control group (DMEM); the other treatments and concentrations demonstrated high cell viability (Figure 12). EXAMPLE 8: Cell migration assay
[095] The cell migration assay allows evaluating the ability of cells to move from one location to another, a fundamental process in various biological conditions, such as wound healing (Figure 13). In 24 hours, the nanoemulsion with Bioxina® demonstrated a cell migration potential of approximately 80%, while the free extract resulted in a closure of less than 50% (Figure 14). EXAMPLE 9 - Antimicrobial activity
[096] Diluting the dry annatto extract in vegetable oil can promote the dispersion of the extract molecules, by Petition 870250036431, dated 06 / 05 / 2025, page 44 / 111 37 / 37 exhibit lipophilic characteristics. After a 24-hour incubation period, both Bioxina® extracts, isolated and diluted in Andiroba oil, at concentrations of 31.25 to 250 μg / mL, showed antimicrobial activity, reducing the viability of MRSA bacteria by approximately 51.2% (± 3.6%) (Figure 15). However, no significant difference was observed at the different concentrations (31.25 to 250 μg / mL) of these two groups. The control group using isolated Andiroba oil showed the highest antimicrobial activity, reducing bacterial viability by approximately 83% (± 5.16%), however, this result did not show a statistically significant difference compared to the groups containing Bioxina® extract. It can be concluded that the Bioxina® extract is biocompatible at concentrations of 31.25 to 250 μρ / mL and exhibits antimicrobial activity at the same concentrations; however, this effect was not potentiated after association with Andiroba oil.
Claims
1. PROCESS FOR PRODUCING A LATEX DRESSING characterized by comprising a natural latex biomembrane (Hevea brasiliensis) associated with a nanoemulsion containing a standardized extract of Bixa orellana (Bioxina®), consisting of the compounds bixin, geranylgeraniol and tocopherols, through the following steps: A. Mixing the Bioxina® extract in concentrations between 5 and 100 mg / mL in an oily base of sunflower oil (Helianthus annuus), varying from 1 to 30% (w / v); B. Addition of the surfactants Span® 80 and Tween® 20 in proportions of 1 to 25% (w / v); C. Dispersion of the components in ultrapure water obtained by reverse osmosis; D. Sonication in an ice bath, with energy application between 1,000,000 and 5,000,000 J, amplitude of 10 to 50%, in alternating pulses (on / off), for 1 to 100 minutes; E. Centrifugation at speeds of 1,000 to 10,000 rpm, removing insoluble residues from the Bioxina® extract; F.Mixture of a nanoemulsion suspension containing Bioxina® in natural liquid latex in proportions of 1:1 to 1:3 (v / v), under magnetic stirring at 900 to 1200 rpm for 10 minutes; G. Dispersion of 10 mL of the mixture in Petri dishes (10 cm in diameter), with rest for up to 48 hours at room temperature; Petition 870250036431, dated 06 / 05 / 2025, page 54 / 111 2 / 2 H. Vulcanization in an oven at 35°C for 1 to 3 hours, followed by cooling and demolding; I. Refinement of the edges with a disposable scalpel and storage in surgical paper; 2. USE OF LATEX DRESSING, according to claim 1, characterized by being for the treatment of chronic or infected wounds, such as diabetic foot ulcers.
3. USE OF LATEX DRESSING, according to claim 1, characterized by being for the prevention of bacterial infections, including resistant strains such as methicillin-resistant Staphylococcus aureus (MRSA); 4. USE OF LATEX DRESSING, according to claim 1, characterized by being for the promotion of angiogenesis, granulation tissue formation and re-epithelialization, accelerating healing and reducing frequent dressing changes.
5. USE OF LATEX DRESSING, according to claim 1, characterized by being used to reduce complications associated with chronic wounds in diabetic patients.
6. USE OF LATEX DRESSING, according to claim 1, characterized by being used as a method that combines encapsulation of bioactive compounds in nanoemulsions incorporated into natural latex biomembranes.