Multifilamented fio, cordas e cordoagens, reinforcement element, medical device, composite artigo, product and painel
The development of UHMWPE multifilament yarns through a controlled gel spinning process addresses the issue of decreased tenacity in high-filament yarns, achieving enhanced strength and mechanical properties suitable for diverse applications, including heavy-duty operations and reinforcing elements.
Patent Information
- Application Number
- BR112014014313
- Authority / Receiving Office
- BR · BR
- Patent Type
- Patents
- Current Assignee / Owner
- Publication Date
- 2026-11-17
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing multifilament yarns with a large number of filaments exhibit suboptimal performance in terms of tenacity, particularly when the number of filaments increases, leading to decreased strength and potential issues in productivity and applicability across various applications.
A multifilament yarn is developed using ultra-high molecular weight polyethylene (UHMWPE) filaments, manufactured through a specific gel spinning process involving controlled UHMWPE solution concentration, spinning plate geometry, and multiple stretching steps, resulting in a tenacity formula of Ten (cN/dtex) = fx n-0.05x dpf-0.15, where n is the number of filaments and dpf is the dtex per filament, with optimized parameters for high yarn count and high dtex.
The yarns exhibit enhanced tenacity, strength, and improved mechanical properties, suitable for heavy-duty operations and reinforcing elements, with applications in ropes, cords, medical devices, and composite articles, demonstrating improved performance in ballistic resistance and bending properties.
Smart Images

Figure 00000031_0000
Abstract
Description
Multifilament yarn, ropes and cords, reinforcing element, medical device, composite article, product and panel.
[001] The invention relates to a multifilament yarn containing n filaments, which are obtained from ultra-high molecular weight polyethylene (UHMWPE), wherein n is at least 25. The invention also relates to various products containing said yarn.
[002] A multifilament yarn with high performance in terms of toughness, modulus of elasticity, deformation and other mechanical and physical properties, for example, is known from document WO 2005 / 066401. The yarn disclosed in the cited document contains a plurality of filaments manufactured from a UHMWPE polymer, the toughness of which depends on the number of filaments in the yarn. In particular, the multifilament yarn of document WO 2005 / 066401 exhibits surprisingly high or strong toughness, for example, of more than 5.5 GPa (about 56.4 cN / dtex), for a relatively large number of filaments. These yarns are highly suitable for use in various semi-finished and end-use articles, examples of which include cables, ropes, fishing nets, sporting equipment, medical implants and ballistic-resistant composites.
[003] An additional multifilament yarn is disclosed in US document 6,969,553, the yarn having a resistance of about 40 g / d (about 36 cN / dtex) and containing 120 filaments with a single filament titer of 4.34 denier (about 4.8 dtex). 2 / 27
[004] However, it is well known in the literature that the tenacity of multifilament yarns decreases as the number of filaments in the yarn increases and, although known multifilament yarns, such as those in WO 2005 / 066401 or US 6,969,553, exhibit good properties, it has been found that yarns with a large number of filaments may have suboptimal performance for some applications. Therefore, it has been observed that there is room to further improve the tenacity of a multifilament yarn with a high yarn count, i.e., a multifilament yarn with a large number of filaments, but also the tenacity of a multifilament yarn with a high yarn count exhibiting a high dtex or high linear density.
[005] The present invention therefore aims to provide advantages and / or alternatives with respect to known multifilament yarns. A specific objective is to provide a multifilament yarn that exhibits optimized performance when used in various applications across diverse technological fields. It is also an objective of the invention to provide a multifilament yarn with a tenacity that decreases less than the tenacity of known yarns when the number of filaments is increased.
[006] The invention provides a multifilament yarn containing n filaments, wherein the filaments are obtained by spinning an ultra-high molecular weight polyethylene, said yarn having a tenacity (Ten), as expressed in cN / dtex according to Formula 1: Ten (cN / dtex) = fx n-0.05x dpf-0.15Formula 1 3 / 27 where Ten represents at least 39 cN / dtex, n is at least 25, 1 is a factor of at least 58.0, and dpf is the dtex per filament.
[007] It has been observed that the multifilament yarn of the invention, hereinafter also referred to as the yarn of the invention, can have optimized performance when used in various applications. In particular, it has been observed that yarns of the invention with a high count can be obtained that can be provided exhibiting excellent tenacity, even when the number of their filaments is increased. More particularly, it has been observed that a high yarn count can be provided exhibiting excellent strength and filaments with a surprisingly high dpf.
[008] It has been observed that the aforementioned advantages can be obtained, in particular, for the yarns of the invention having a factor f of at least 60.0, preferably at least 62.0, more preferably at least 64.0, most preferably at least 67.0.
[009] It was also found that yarns of the invention with high tenacities were obtained with yarns having a large number n of filaments, that is, at least 25, preferably at least 50, more preferably at least 100, even more preferably at least 200, even more preferably at least 400, most preferably at least 700. Such yarns can also be manufactured with high productivity.
[0010] Furthermore, it was observed that the yarns of the invention with high tenacities were also obtained by 4 / 27 yarns exhibiting a dpi of at least 0.8, preferably at least 1, more preferably at least 1.1. In a preferred embodiment, high-tenacity yarns were obtained even with a dpi of at least 1.2 and even at least 1.3. This advantage was surprising, since it is known that when the dpi of the individual filaments of a yarn is increased, the yarn's tenacity decreases. On the other hand, when yarns have filaments with high dpi, several yarn properties, for example, filament rupture, yarn productivity, and ballistics, can also be optimized. Consequently, it is desirable from the point of view of yarn productivity and applicability to have yarns exhibiting high tenacity and containing filaments with high dpi. For the first time, to the inventors' knowledge, the present invention provides such yarns.
[0011] According to the invention, the filaments that constitute the yarn of the invention are obtained by spinning an ultra-high molecular weight polyethylene polymer as previously mentioned and hereinafter referred to as UHMWPE. Preferably, said filaments are obtained by gel spinning of UHMWPE with a process containing the following steps: a) provision of a UHMWPE solution in a suitable solvent; b) spinning a multifilament yarn by passing the solution from step a) through a spinning plate containing a plurality of spinning holes to form the strands of said yarn; 5 / 27 c) dragging of the filaments in at least one stretching step before, during, or after solvent removal.
[0012] It was observed that the yarns of the invention were obtained when the UHMWPE solution contained a carefully controlled amount of UHMWPE polymer. Surprisingly, to manufacture the yarns of the invention, the UHMWPE solution needs to contain between 3% by weight and 12% by weight of UHMWPE polymer, preferably between 4% by weight and 10% by weight of UHMWPE polymer, more preferably between 5% by weight and 9% by weight of UHMWPE polymer, most preferably between 6% by weight and 8% by weight of UHMWPE polymer.
[0013] An additional parameter is the tensile strength (ES) of the UHMWPE polymer. Only after an understanding of the skill did the present inventors determine that the UHMWPE polymer preferably has an ES of at least 0.4 N / mm2, more preferably at least 0.45 N / mm2, even more preferably at least 0.5 N / mm2, most preferably at least 0.55 N / mm2. Preferably, said ES is at most 0.90 N / mm2, more preferably at most 0.85 N / mm2, even more preferably at most 0.80 N / mm2, most preferably at most 0.75 N / mm2. It is important to note that the ES of UHMWPE can be altered during its transformation into fiber, for example, due to chain scission. Consequently, the ES of UHMWPE in the fiber will generally be lower than the ES of UHMWPE in solution. These UHMWPEs are commercially available and can be purchased from DSM NV or Ticona. Also, someone versed in 6 / 27 technique can manufacture UHMWPEs with various ES following the methodology disclosed in documents WO 2009 / 060044 and WO 2012 / 139934 (pg.18).
[0014] Preferably, UHMWPE is a homopolymer, that is, a linear polyethylene with less than one rod per 100 carbon atoms, and preferably less than one branch per 300 carbon atoms. In one embodiment, UHMWPE is a linear polyethylene further containing up to 5 mol% of one or more comonomers, such as alkenes like propylene, 1-butene, 1-pentene, 4-methyl-1-pentene or 1-octene. UHMWPE may also contain small amounts, generally less than 5% by weight, preferably less than 3% by weight of common additives, for example, antioxidants, thermal stabilizers, colorants, flow promoters, etc.
[0015] Suitable examples of solvents include aliphatic and alicyclic hydrocarbons, for example, octane, nonane, decane and paraffins, including their isomers; petroleum fractions; mineral oil; kerosene; aromatic hydrocarbons, for example, toluene, xylene and naphthalene, including their hydrogenated derivatives, for example, decalin and tetralin; halogenated hydrocarbons, for example, monochlorobenzene; and cycloalkanes or cycloalkenes, for example, careen, fluorine, camphene, menthane, dipentene, naphthalene, acenaphthalene, methylcyclopentandiene, tricyclodecane, 1,2,4,5-tetramethyl-1,4-hexadiene, fluorenone, naphtindane, tetramethyl-p-benzodiquinone, ethylfluorene, fluoranthene and naphthenone. The combinations of solvents and spinning methods listed above can also be used for spinning with gel. 7 / 27 UHMWPE, the solvent combination also being referred to for simplicity as spinning solvent. In a preferred embodiment, the spinning solvent of choice is non-volatile at room temperature, for example, paraffin oil. It has also been found that the process of the invention is especially advantageous for solvents that are relatively volatile at room temperature, such as, for example, decalin, tetralin and kerosene grades. In the most preferred embodiment, the solvent of choice is decalin.
[0016] According to the invention, the UHMWPE solution is formed into individual filaments by spinning said solution through a spinning plate containing a plurality of spinning holes.
[0017] Preferably, the spinning plate contains at least 25 spinning holes. In a preferred embodiment, the yarn of the invention is a yarn thus spun, that is, a yarn of the invention is obtained at the end of the spinning process with gel. Therefore, since for a yarn of the invention such as is spun the number of spinning holes contained in said spinning plate determines the number of filaments in the yarn, it is needless to say that the preferred number of spinning holes is in accordance with that defined by the number of filaments contained in the yarn of the invention.
[0018] In a preferred embodiment, each wiring hole of the wiring plate has a geometry comprising at least one shrinkage zone. A shrinkage zone is understood, in this document, to be a zone with a gradual reduction in diameter with a cone angle preferably below 60°, more preferably below 8 / 27 50°, or even more preferably below 40°, from an initial diameter D0 to a final diameter Dntal, such that a stretching ratio of DRSP is obtained in the spinning hole. Preferably, the spinning hole further comprises, upstream and / or downstream of the shrinkage zone, a zone of constant diameter, such zone preferably having a length / diameter ratio Ln / Dn between 1 and 50.
[0019] Preferably, the multifilament yarn is emitted from the spinning holes into an air slot and between a quenching zone, said air slot having a length preferably between 1 mm and 20 mm, more preferably between 2 mm and 15 mm, even more preferably between 2 mm and 10 mm, most preferably between 2 mm and 5 mm. Although called an air slot, said slot may be filled with any gas or gaseous mixture, for example, air, nitrogen or other inert gases. Air slot is understood in this document as the distance between the spinning plate and the quenching zone. The quenching zone may be a liquid, for example, water, containing a bath at a temperature below the spinning temperature, for example, around room temperature.Preferably, the multifilament yarn is dragged in the air gap with a drag ratio, DRag, typically referred to in the art as downstream drag, between 2 and 30, more preferably between 3 and 10, most preferably between 4 and 8.
[0020] Preferably, the spinning step b) is carried out at a spinning temperature below the boiling point of the solvent, preferably between 150°C and 250°C. 9 / 27 If, for example, decalin is used as a solvent, the spinning temperature will preferably be a maximum of 210°C, more preferably a maximum of 190°C, even more preferably a maximum of 180°C, more preferably a maximum of 170°C, and preferably at least 115°C, more preferably at least 120°C, most preferably at least 125°C. In the case of paraffin as a solvent, the spinning temperature is preferably below 220°C, more preferably between 130°C and 200°C, most preferably between 130°C and 195°C.
[0021] It is essential for obtaining the yarns of the invention that a reduced yield of UHMWPE solution per spinning hole of the spinning plate be used. Determining the correct yield for manufacturing the multifilament yarns of the present invention required lengthy and intensive inventive work; one reason being that high yields per spinning hole did not appear to produce the desired results and another reason being that by reducing said yield, the productivity of the entire process may decrease to commercially unacceptable levels. Preferably, said yield is between 1.0 and 3.0 g of solution / minute / hole, more preferably between 1.2 and 2.6 g of solution / minute / hole, most preferably between 1.4 g of solution / minute / hole and 2.4 g of solution / minute / hole. Said yield can be easily adjusted by using a spinning pump or a gear pump.In a preferred embodiment, a UHMWPE solution is rotated with a yield between 1.0 and 3.0 g of solution / minute / orifice, said UHMWPE exhibiting. 10 / 27 ES of at least 0.60 N / mm2, more preferably ES of at least 0.65 N / mm2. For the aforementioned yields and for ES above that of UHMWPE, preferably a wiring hole having a diameter Dn between 0.5 mm and 2 mm is used, preferably between 0.8 mm and 1.2 mm.
[0022] The process according to the invention further comprises stretching the filaments before, during and / or after said solvent removal. Preferably, the filament dragging after solvent removal is carried out in at least one stretching step, with a stretching ratio of at least 3, more preferably at least 4, most preferably at least 5. More preferably, the filament dragging is carried out in at least two steps, or even in at least three steps. Preferably, each stretching step is carried out at a different temperature, which is preferably chosen to obtain the desired drag ratio without filament breakage occurring. Preferably, the dragging is carried out in more than two steps, and if UHMWPE is used, preferably the dragging will be carried out at different temperatures, with an increasing profile between about 120 and 155°C.If the dragging of solid filaments is carried out in more than one step, the solid drag ratio (DRS) will be calculated by multiplying the drag ratios obtained for each individual solid dragging step. Preferably, the total drag ratio applied to the filaments during and / or after solvent removal, hereinafter referred to as DRtotal, is at least 10, more preferably at least 20, even more. 11 / 27 preferably at least 30, even more preferably at least 40, most preferably at least 50.
[0023] Preferably, the total draw ratio, that is, the total draw ratio to which the filaments are subjected during their entire manufacturing process, is at least 20, more preferably at least 25, even more preferably at least 30, most preferably at least 40. It has been observed that, by increasing the total draw ratio, the mechanical properties of the yarns of the invention were improved. Specifically, the tensile strength and modulus of elasticity increased.
[0024] The solvent removal process can be carried out by known methods, for example by evaporation, when a relatively volatile solvent, for example decalin, is used to prepare the UHMWPE solution, or using an extraction liquid, for example, when paraffin is employed, or by a combination of both methods. Suitable extraction liquids are liquids that do not cause significant changes in the UHMWPE filament network structure, for example, ethanol, ether, acetone, cyclohexanone, 2-methylpentanone, n-hexane, dichloromethane, trichlorotrifluoroethane, diethyl ether and dioxane, or mixtures thereof. Preferably, the extraction liquid is chosen in such a way that the solvent can be separated from the extraction liquid for recycling.
[0025] The yarns of the invention, the inventive yarns, have properties that make them an interesting material for use in ropes, cords and the like, preferably ropes designed for heavy-duty operations such as, for example, 12 / 27 marine, industrial and offshore operations. In particular, it has been observed that the wires of the invention are particularly useful for heavy-duty, long-term and very long-term operations.
[0026] Heavy operations may also include, but are not limited to, handling anchors, mooring support platforms for renewable energy generation in offshore operations, mooring offshore oil drilling platforms and production platforms and the like.
[0027] The yarns of the invention are also very suitable for use as a reinforcing element for reinforced products, such as hoses, pipes, electrical and optical cables, especially when said reinforced products are used in deep water environments, where reinforcement is necessary to support the load of the reinforced products when in free suspension. Consequently, the invention also relates to a reinforced product containing reinforcing elements, wherein the reinforcing elements contain the yarns of the invention.
[0028] The invention also relates to medical devices comprising the threads of the invention. In a preferred embodiment, the medical device is a cable or a suture thread. Other examples include knitted products, endless loop products, similar products, or bags or balloons, but also other woven fabrics and / or knitted products. Good examples of cables include a trauma fixation cable, a sternal closure cable, and a prosthetic or prophylactic cable, a long bone fracture fixation cable, and a small bone fracture fixation cable. Also, 13 / 27 tube-like products, for example, for ligament replacement, are suitably manufactured using the inventive wires.
[0029] The invention also relates to ropes and, in particular, to mooring cables, with or without a covering, containing the inventive yarns. Preferably, the ropes of the invention are braided cables. It has been observed that the ropes of the invention exhibit good bending properties. Preferably, at least 50% by weight, more preferably at least 75% by weight, even more preferably at least 90% by weight of the total weight of the yarns used to manufacture the rope and / or the covering consists of the yarns of the invention. More preferably, the weight of the yarns used to manufacture the rope and / or covering consists of the yarns of the invention. The remaining percentage by weight of the yarns in the cable according to the invention may contain yarns or combinations of yarns obtained from other materials suitable for obtaining yarns such as, for example, metal, glass, carbon, nylon, polyester, aramid, other types of polyolefins and the like.
[0030] The invention also relates to composite articles containing the yarns of the invention. Preferably, the composite articles comprise networks of inventive yarns. By network it is understood that the filaments of said yarns are arranged in configurations of various types, for example, a knitted or woven fabric, a non-woven fabric with a random or ordered orientation of the yarns, an arrangement of parallel rows, also known as a unidirectional UD arrangement, in layers or formed in a 14 / 27 woven by any one of a variety of conventional techniques. Preferably, said articles comprise at least one network of one of said yarns. More preferably, said articles comprise a plurality of networks of inventive yarns. Such networks of inventive yarns may be included in cut-resistant clothing, for example, gloves, and also in anti-ballistic products, for example, bulletproof panels, vests and helmets. Therefore, the invention also relates to such articles.
[0031] In a preferred embodiment, the composite article contains at least one monolayer comprising the yarns of the invention. The term monolayer refers to a layer of yarns, i.e., yarns in a plane. In another preferred embodiment, the monolayer is a unidirectional monolayer. The term unidirectional monolayer refers to a layer of unidirectionally oriented yarns, i.e., yarns in a plane that are essentially oriented in parallel. In yet another preferred embodiment, the composite article is a multilayer composite article containing a plurality of unidirectional monolayers, the direction of the yarns in each monolayer preferably being rotated by a certain angle relative to the direction of the yarns in an adjacent monolayer. Preferably, the angle is at least 30°, more preferably at least 45°, even more preferably at least 75°, most preferably the angle is about 90°.Multilayer composite articles have proven to be very useful in ballistic applications, for example vests, helmets, shields, rigid and flexible panels, panels for... 15 / 27 vehicle armoring and the like. Therefore, the invention also refers to bulletproof articles such as those listed above containing the inventive wires.
[0032] It has also been observed that the yarns of the invention are also suitable for use in other applications, such as, for example, fishing lines and fishing nets, land nets, cargo nets and curtains, kite strings, dental floss, tennis racket strings, canvas (e.g., tent canvas), nonwoven fabrics and other types of fabrics, belts, battery separators, capacitors, pressure vessels, hoses, (offshore) umbilical cables, electrical, optical and signaling cables, automotive equipment, power transmission belts, assembly of building materials, cut-resistant and blade-resistant articles and incision-resistant articles, protective gloves, composite sports equipment such as skis, helmets, kayaks, canoes, bicycles and boat hulls and masts, loudspeaker cones, high-performance electrical insulation, protective domes, sails, geotextiles and the like.Therefore, the invention also relates to the applications listed above, containing the inventive threads.
[0033] The invention also relates to a round elastic comprising the yarn of the invention.
[0034] The invention also relates to sporting equipment comprising inventive yarn, including a fishing line, a kite string and a yacht line. The invention also relates to a cargo container having walls comprising the inventive yarn. 16 / 27
[0035] The invention will be better explained through the following examples and comparative experiment, but first the methods used to determine the various parameters used above are presented. Measurement Methods - Fiber tenacity (dtex) was measured by weighing 100 meters of fiber. The decitex of the fiber was calculated by dividing the weight in milligrams by 10; - Tensile properties of fibers: tensile strength (or resistance), tensile modulus (or modulus), and elongation at break (EAB) are defined and determined in multifilament yarns, as specified in ASTM D885M, using a nominal fiber gauge length of 500 mm at a crosshead speed of 50 mm / min and Instron 2714 staples, Fibre Grip type D5618C. Based on the measured stress-strain curve, the modulus is determined as the gradient between 0.3 and 1% strain. For the calculation of modulus and resistance, the measured tensile forces are divided by the titer; the values in GPa are calculated assuming a density of 0.97 g / cm3. - Tensile properties of fibers exhibiting a ribbon-like form: Tensile strength, modulus of elasticity, and elongation at break are defined and determined at 25°C in ribbons with a width of 2 mm as specified in ASTM D882, using a nominal ribbon gauge length of 440 mm and a crosshead speed of 50 mm / min. - Number of branches, especially ethyl branches, per thousand carbon atoms: It was 17 / 27 determined by FTIR on a 2 mm thick compression-molded film by quantifying the absorption at 1,375 cm⁻¹ using a calibration curve based on NMR measurements as, for example, in document EP 0 2 69 151 (in particular page 4 thereof). - The tensile strength (ES) of a UHMWPE is measured according to ISO 1542-1 2A. - Back face deformation (BFD) of a sample can be tested according to NIJ 0101.04 level IIIA using, for example, a FSP of 1.1 mm and an FSP of 20 mm in an internal firing jig. In particular for this invention, flexible panels were subjected to these BFD tests by placing them in a Roma Plastilina No. 1 support. Before testing, the consistency of the support material was validated according to NIJ Standard-1.001.06 (ball drop test). The support material was preconditioned at 35°C. BFD was quantified by measuring the penetration depth in the support material resulting from the impact of a .44 Magnum Semi Jacketed Hollow Point (SJHP) bullet impacting at 400 m / s a flexible panel with a total area density of 5.2 kg / m2. The BFD is determined as the average penetration depth of 4 shots in the same flexible panel. - The ballistic performance of a sample was measured by subjecting the sample to firing tests conducted with various projectiles, such as AK47 MSC bullets (hereinafter AK47), 0.357 Magnum 10.2 g bullets (hereinafter Magnum), 9 mm Full Metal Jacket 8.0 g bullets (hereinafter 9 mm), and standard (STANAG) 20 g FSP (hereinafter FSP20) and 1.1 g FSP (hereinafter FSP1 1.1) bullets. The first shot was fired at a velocity The projectile velocity (V50) of 18 / 27 was predicted to be 50% stopped. The actual bullet velocity was measured at a short distance before impact. If a stop occurred, the next shot would be fired at a predicted velocity 10% higher than the previous velocity. If a puncture occurred, the next shot would be fired at a velocity 10% lower than the previous velocity. The experimentally obtained V50 value was the average of the two highest stops and the two lowest punctures. The bullet's kinetic energy at V50 was divided by the total area density of the sample to obtain a so-called Eabs value. Eabs reflects the stopping power of the sample relative to its weight / thickness. The higher the Eabs, the better the ballistic properties of the sample. EXAMPLES 1 and 2
[0035] A 6% by weight suspension of a UHMWPE homopolymer powder having a tensile strength (ES) of approximately 0.68 N / mm2 was prepared in decalin and fed into a 42 mm co-rotating twin-screw extruder heated to a temperature of 180°C. The extruder was also equipped with a gear pump. In the extruder, the mixture was transformed into a solution, and the solution was emitted through a spinning plate with 50 spinning holes at a speed of approximately 2.1 g / min per hole.
[0036] The spinning holes had an initial cylindrical channel of 2 mm diameter (D0), followed by a conical contraction with a cone angle of 15°C into a cylindrical channel of 0.8 mm diameter (Dn) and Ln / Dnde 10. The fluid filaments emitted from the channel 19 / 27 cylindrical filaments entered the air slot with a length of 15 mm, and were drawn in at such a speed that a downstream drag of about 4 was applied to the air slot. Subsequently, they were cooled to room temperature in a water bath to form gel filaments, i.e., cooled filaments containing a large amount of solvent.
[0037] The filaments were subsequently placed in an oven. In the oven, the filaments were further stretched 10 times at approximately 147°C and the decalin was evaporated. The yarn was then dragged in a second stage with various drag ratios, as shown in Table 1 below. The wire had the following properties: TABLE 1 Example 1 Example 2 Drag ratio 3.5 3.9 Yarn dtex 78 68 Yarn tenacity 49 52.4 cN / dtex Yarn modulus 1,798.7 1,981.6 cN / dtex Yarn EAB 3.4 3.2 Dpf 1.56 1.36 dtex EXAMPLE 3
[0038] A 7% by weight suspension of a UHMWPE homopolymer powder having a tensile strength (ES) of approximately 0.68 N / mm2 was prepared and fed into a 133 mm co-rotating twin-screw extruder heated to a temperature of 180°C; the extruder is also equipped with a gear pump. In the extruder, the mixture was transformed into a solution and the solution was emitted through 20 / 27 of a wiring board with 780 wiring holes and a speed of approximately 2.4 g / min per hole.
[0039] The spinning holes had an initial cylindrical channel of 2 mm diameter (D0), followed by a conical contraction with a cone angle of 15°C into a cylindrical channel of 0.8 mm diameter (Dn) and Ln / Dnde 10. The fluid filaments emitted from the cylindrical channel entered the air slot with a length of 15 mm. The fluid filaments were absorbed at such a speed that a downstream drag of about 5 was applied to the fluid filaments in the air slot, and were then cooled to ambient temperature in a water bath.
[0040] The filaments were subsequently placed in an oven. In the oven, the filaments were further stretched 9 times at approximately 147°C and the decalin was evaporated. The thread was dragged in a second stage at a temperature of 152°C with a drag ratio of 4.7.
[0041] The wire had the following properties: TABLE 2 Drag ratio 4.7, Yarn dtex 1,024.0, Yarn tenacity 41.6 cN / dtex, Yarn modulus 1,613 cN / dtex, Yarn EAB 3.14, Dpf 1.3 dtex EXAMPLES 4 and 5
[0042] A 7% by weight suspension of a UHMWPE homopolymer powder exhibiting a tensile strength (ES) of approximately 0.61 N / mm2 was prepared and fed to a The 21 / 27 twin-screw extruder, 133 mm in diameter, is heated to a temperature of 180°C and is also equipped with a gear pump. In the extruder, the mixture is transformed into a solution, which is then emitted through a spinning plate with 780 spinning holes at a speed of approximately 1.4 g / min per hole.
[0043] The spinning holes had an initial cylindrical channel of 2 mm diameter (D0), followed by a conical contraction with a cone angle of 15°C into a cylindrical channel of 0.8 mm diameter (Dn) and Ln / Dnde 10. The fluid filaments emitted from the cylindrical channel entered the air slot with a length of 15 mm. The fluid filaments were absorbed at such a speed that a downstream drag of about 6.2 was applied to the fluid filaments in the air slot, and then cooled to ambient temperature in a water bath.
[0044] The filaments were subsequently placed in an oven. In the oven, the filaments were further stretched 10 times at approximately 147°C and the decalin was evaporated. The yarn was dragged in a second stage at a temperature of 153°C at various drag ratios.
[0045] The wire had the following properties: TABLE 3 Example 4 Example 5 Drag ratio 4 5 Yarn dtex 869 687 dtex Yarn tenacity 41.6 45.4 cN / dtex Yarn modulus 1.568 1.772 cN / dtex Yarn EAB 3.14 3.07 22 / 27 DPF 1.1 0.9 dtex
[0046] The invention is further explained with the aid of the figure. The figure shows the tenacity of the yarns versus fxn ~0.05x dp f-0.15. The figure clearly shows that the yarns of the invention (represented by o), as manufactured according to Examples 1-5, exhibit a higher tensile strength than known commercial yarns or the best yarns reported in WO 2005 / 066401 (all represented by ·) and in US 6,969,553 B1 (represented by ▲) at a given filament count and dpf. Therefore, the inventors were able to manufacture for the first time yarns that exhibit a large number of high dtex filaments while also surprisingly increasing the yarn tenacity. In the figure, the dashed lines represent Formula 1 Ten (cN / dtex) = fxn~0'05x dp f-0,15 where f was 68.6, 62.5, 64.0, 67.0 respectively. EXAMPLE 6
[0047] A unidirectional monolayer was formed from a plurality of yarns aligned to operate in parallel. The yarns had a dtex of approximately 1,220.0; a tenacity of approximately 39.7 cN / dtex; a modulus of approximately 1,450 cN / dtex and a dtex per filament of approximately 1.5. The yarns were held together by approximately 17% by weight (relative to the total weight of the monolayer) of a Kraton® rubber-based elastomeric matrix material. A sheet was formed with 4 unidirectional monolayers stacked in a 0-90° orientation. [degrees]. The area density of the resulting sheet was 212 g / m2. 23 / 27
[0048] The wires were manufactured according to Example 3, with the difference that the solution was emitted at a rate of 1.7 g / min. / orifice; a downstream drag of about 6.5 was used; the wire was dragged 8 times at about 147°C in the first stage and 3.8 times in a second stage at a temperature of about 152.5°C.
[0049] Several such sheets were pressed together to form a rigid panel with an area density of 15.5 kg / m2. The V50 of the panel for an AK47 FMJ MSC bullet was determined to be approximately 891 m / s, which corresponds to an Eabs of approximately 242 J.m2 / kg. The data are included in Table 4. Comparative Experiment 1 (CE1)
[0050] Example 6 was repeated with the difference that commercial UHMWPE yarns sold by DSM Dyneema® BV, Netherlands, and known as SK76 (1,500 dtex; toughness of 36.5 cN / dtex; modulus of 134 N / tex) were used instead of the yarns of Example 3. A monolayer contained approximately 16% by weight of matrix. The area density of the sheet was approximately 233 g / m2 and the area density of the pressed panel was approximately 16.0 kg / m2. The V50 of the panel for an AK47 FMJ MSC bullet was determined to be approximately 814 m / s, which corresponds to an Eabs of approximately 166 J.m2 / kg. The data are included in Table 4. EXAMPLE 7
[0051] A certain number of sheets, as in Example 6, were obtained, with the difference that each sheet also contained two 7 µm thick LDPE films interleaved between the stack of four monolayers. The area density of such a sheet was approximately 157 g / m2. Three 24 / 27 flexible panels, two having an overall density of approximately 3.1 kg / m² and one having an overall density of approximately 4.9 kg / m², were formed by assembling a number of flexible sheets. The sheets were not pressed. The panels with 3.1 kg / m² were shot with a .357 Magnum JSP bullet and with a 9 mm FMJ Parabellum bullet. The panel with 4.9 kg / m² was shot with a 17 grain FSP bullet. The data are included in Table 4. Comparative Experiment 1 (CE2)
[0052] Example 7 was repeated with the difference that commercial UHMWPE yarns sold by DSM Dyneema® BV, Netherlands, and known as SK76 were used instead of the yarns of Example 3 and the sheet contained only two monolayers. The area density of such a sheet was about 132 g / m2. The data are reported in Table 4. Table 4 Example ADsheet ADpanel Matrix BFD Arma V50 Eabs g / m2 kg / m2 % mm m / s J / [kg / mL] 6 212 15, 5 16,7 ^^^B AK4 7 891,3 242 CE1 233 16, 0 16 ^^^B AK4 7 814 166 7 157 3.1 17 34 Magnum 522.8 453 3.1 9 mm 534.4 373 4.9 FSP1.1 611.6 41 CE2 132 3.0 17 40 Magnum 457 358 3.0 9 mm 400 218 4.9 FSP1.1 535 33
[0053] It can be easily observed from the Table 4 shows that the panels based on the yarns of the invention exhibit a notable improvement in their properties. 25 / 27 ballistics. Therefore, the invention relates to a panel comprising a multiplicity of sheets containing the yarn of the invention. Preferably, each sheet has a plurality of monolayers, preferably at least 2 monolayers, more preferably at least 4 monolayers. Preferably, each sheet has a maximum of 8 monolayers, more preferably a maximum of 6 monolayers. Preferably, the yarns in the sheets or monolayers are arranged unidirectionally, i.e., they run along a common direction. Preferably, the sheets or monolayers also contain a matrix material, generally used to stabilize their handling, in an amount of at most 25% by weight based on the total weight of the panel, more preferably at most 21% by weight, preferably up to at most 19% by weight, more preferably at most 17% by weight.Preferably, the quantity of said matrix material is at least 5% by weight, more preferably at least 10% by weight, most preferably at least 15% by weight. In a preferred embodiment, the panel comprises a number of sheets, each sheet comprising a stack of single layers which further comprises two polymer films, preferably polyethylene films, more preferably LDPE films, which are interleaved within said stack of single layers.
[0054] In a preferred embodiment, the panel of the invention is a rigid panel, preferably having an Eabs (J / [kg / m2]) of at least 170 against an AK47 FMJ MSC projectile, more preferably of at least 190, even more preferably of at least 210, most preferably 26 / 27 at least 230, said Eabssendo determined by a panel area density of about 15.5 kg / m2. Preferably, the article of the invention is a rigid article. Rigid panel is understood in the present document as an article having a flexural strength preferably of at least 10 mPa, more preferably of at least 20 mPa, most preferably of at least 40 mPa, as measured before impacts. Flexural strength can be measured using a methodology as described on page 14 of document WO 2012 / 032082. A rigid panel can be obtained by treating a stack of sheets comprising fibers, preferably unidirectional alignment yarns containing fibers, at a pressure of at least 5,000 kPa, more preferably at least 7.000 kPa, more preferably at least 9000 kPa; and at a temperature preferably below the melting temperature of said fibers, more preferably within a range of 20 degrees below said melting temperature. The melting temperature of the fibers can be determined by DSC using a method such as described on page 13 of document WO 2009 / 056286.
[0055] In another preferred embodiment, the panel of the invention is a flexible panel that preferably has an Eabs (J / [kg / m2]) of at least 370 against a .357 Magnum JSP projectile, more preferably at least 390, even more preferably at least 410, even more preferably at least 430, most preferably at least 450; said Eabs being determined by a flexible panel having an area density of about 3.1 kg / m2. Flexible panel is understood in this document as a 27 / 27 panel manufactured by assembling together a plurality of sheets without compression. Spot joining or gluing of the sheets together can be used to provide the panel with improved handling capacity. Alternatively, the sheets can be joined by a bag. Preferably, the flexible panel has an Eabs (J / [kg / m2]) against a 9 mm FMJ Parabellum projectile of at least 220, preferably at least 250, even more preferably at least 280, even more preferably at least 310, even more preferably at least 340, most preferably at least 370; said Eabs being determined by a flexible panel having an area density of about 3.1 kg / m2.Preferably, the flexible panel has an Eabs (J / [kg / m2]) against a 17-grain FSP projectile of at least 35, more preferably at least 38, most preferably at least 41; said Eabs being determined by a flexible panel having an area density of about 3.1 kg / m2. EXAMPLE 8
[0056] The rope was braided with yarns of the present invention. It was observed that, when subjected to bending, the bending performance of such rope improved by 38% compared to a similar rope braided with known SK75 Dyneema® fiber yarns. The bending performance of the braided rope from the yarns of the invention was also improved by approximately 10% compared to the braided rope with yarns as reported in document WO 2005 / 066401.
Claims
1. Multifilament yarn characterized by containing n filaments, wherein the filaments are obtained by spinning an ultra-high molecular weight polyethylene (UHMWPE), said yarn having a tenacity (Ten) as expressed in cN / dtex according to Formula 1: Ten (cN / dtex) = 1 x n-0.05 x dp f-0.15 Formula 1 where Ten is at least 39 cN / dtex, n is at least 25, f is a factor of at least 58.0 and dpf is the dtex per filament.
2. Wire, according to claim 1, characterized in that the factor f is at least 60.
0.
3. Wire, according to claim 1, characterized in that the factor f is at least 64.
0.
4. Yarn, according to any one of claims 1 to 3, characterized in that the dpf index is at least 0.
8.
5. Ropes and cordages characterized in that they comprise any of the yarns as defined in any one of claims 1 to 4.
6. Reinforcing element suitable for reinforcing products characterized in that the element comprises any of the wires as defined in any of claims 1 to 4.
7. Medical device characterized by comprising any of the wires as defined in any of claims 1 to 4.
8. Composite article characterized by comprising any of the wires as defined in any of claims 1 to 4. Petition 870210081708, dated 03 / 09 / 2021, page 14 / 16 2 / 3 9. Composite article according to claim 8, characterized by containing at least one unidirectional monolayer comprising the yarns, as defined in any one of claims 1 to 4.
10. A multilayer composite article containing a plurality of unidirectional monolayers, said monolayers being characterized in that they comprise any of the yarns as defined in any of claims 1 to 4, wherein the yarn direction in each unidirectional monolayer is rotated by an angle relative to the yarn direction of an adjacent monolayer.
11. Product characterized by comprising any of the yarns, as defined in any of claims 1 to 4, wherein the product is chosen from the group consisting of fishing lines and fishing nets, land nets, cargo curtain nets and kite lines, dental floss, tennis racket strings, cargo tarpaulins, tent tarpaulins, nonwoven fabrics, belts, battery separators, capacitors, pressure vessels, hoses, umbilical cables, electrical fiber, optical fiber and signaling cables, automotive equipment, power transmission belts, construction materials, cut and stab resistant articles, and incision resistant articles, protective gloves, composite sports equipment, skis, helmets, kayaks, canoes, bicycles and boat hulls and masts, loudspeaker cones, high-performance electrical insulation, protective domes, sails and geotextiles. Petition 870210081708, dated 03 / 09 / 2021, p. 15 / 16 3 / 3 12. Panel characterized by comprising a plurality of sheets containing the wires, as defined in any one of claims 1 to 4.
13. Panel, according to claim 12, characterized in that each sheet comprises at least 2 monolayers.
14. Panel, according to claim 12 or 13, characterized by being a rigid panel and having Eabs (J / [kg / m2]) of at least 170 against an AK47 FMJ MSC projectile, said Eabs being determined by a panel area density of 15.5 kg / m2.
15. Panel, according to claim 14, characterized by having an Eabs of at least 210 J / [kg / m2].
16. Panel, according to claim 12 or 13, characterized by being a flexible panel and having an Eabs (J / [kg / m2]) of at least 370 against a .357 Magnum JSP projectile; said Eabs being determined by a panel area density of 3.1 kg / m2.
17. Panel, according to claim 16, characterized by having Eabs of at least 410 J / [kg / m2].
18. Panel, according to claim 16 or 17, characterized in that said panel exhibits an Eabs (J / [kg / m2]) against a grain 17 FSP projectile of at least 35; said Eabs being determined by a panel area density of 3.1 kg / m2.