Equipment for perfuration, finishing, arrangement and transportation of oil e / ou oil gas e / ou gas

A highly structured composite coating with a cured binder and hydrophilic flakes addresses corrosion and abrasion issues in oil and gas equipment, offering enhanced protection against hydrogen sulfide, carbon dioxide, and high-salt water, ensuring equipment durability.

BR112014015121B1Inactive Publication Date: 2026-11-17TENARIS CONNECTIONS BV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
BR112014015121
Authority / Receiving Office
BR · BR
Patent Type
Patents
Current Assignee / Owner
Publication Date
2026-11-17
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing coatings for oil and gas equipment fail to provide effective protection against corrosion, abrasion, and diffusion of hydrogen sulfide, carbon dioxide, and high-salt water under hydrothermal conditions, leading to material degradation and costly replacements.

Method used

A highly structured composite coating comprising a cured binder with polar groups and hydrophilic flakes with an aspect ratio greater than 10, which enhances adhesion and barrier properties against corrosive substances.

Benefits of technology

The coating provides excellent corrosion resistance, abrasion resistance, and a high barrier function against hydrogen sulfide, carbon dioxide, and high-salt water, preventing material degradation and extending equipment lifespan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000053_0000
    Figure 00000053_0000
  • Figure 00000054_0000
    Figure 00000054_0000
  • Figure 00000055_0000
    Figure 00000055_0000
Patent Text Reader

Abstract

Abstract of invention patent: "Corrosion-resistant equipment for oil and / or gas applications". The present invention relates to equipment for drilling, finishing, storage and transportation of oil and / or gas, including pressure vessels, tools, piping, pipes, fittings and any other parts coated with a highly structured composite material. Due to its highly structured composition, it is a particularly effective barrier to protect metals against attack by corrosive substances such as hydrogen sulfide, carbon dioxide and seawater, if necessary under hydrothermal conditions. At the same time, it is also abrasion-stable, for example, against a grinding effect by sand, as well as resistant to impact from mechanical loads, for example, by tools.This is achieved by means of a coating comprising a binder comprising at least one cross-linked resin, wherein the resin comprises at least one polar group; at least one type of hydrophilic flakes with an aspect ratio of more than 10, wherein the surface of the flakes at least partially comprises a metal oxide.
Need to check novelty before this filing date? Find Prior Art

Description

Equipment for drilling, finishing, storing and transporting oil and / or gas. FIELD OF THE INVENTION

[001] The present invention relates to drilling, finishing, storage and transportation equipment for oil and / or gas, including pressure vessels, tools, piping, pipes, fittings and any other parts, coated with a highly structured composite material. Due to its highly structured coating, such equipment is protected against attack by corrosive substances such as hydrogen sulfide, carbon dioxide and seawater, if necessary under hydrothermal conditions. At the same time, the coating is also abrasion-resistant, for example, against a grinding effect by sand, as well as resistant to mechanical load, for example, by tools. INTRODUCTION

[002] Structures made of corrosion-resistant materials generally require adequate corrosion protection to ensure the overall structural stability of the design over a long period of time. In particular, surface coatings with good adhesion and a strong barrier effect are used in these applications. For durable and versatile use, suitable corrosion protection coatings should advantageously be resistant to abrasion and hydrolysis and have good mechanical stability. Especially in the oil and gas industries, steel is widely used as a material for casing pipes and feed pipes, which are placed in the wellbore. Steel is used because of its good temperature resistance and excellent mechanical properties with respect to stiffness and a certain resistance to abrasion. In various wells, not only oil containing sand, temperature Petition 870260066502, dated 06 / 07 / 2026, page 14 / 234 2 / 49 and pressure are factors that act on steel, but there is also a considerable amount of corrosive substances. This includes, in addition to formation and injection water with high salt content, which generally leads to corrosion (red rust), especially hydrogen sulfide and carbon dioxide, which act on steel under hydrothermal conditions in the borehole and cause sustained damage. Continued exposure to hydrogen sulfide leads to embrittlement (sulfide stress stress cracking) and / or acid corrosion of the steel. Carbon dioxide causes surface corrosion with the formation of iron carbonate, which can be easily scraped off by sand removes in the oil-seawater mixture (sweet corrosion). These mechanisms lead to brittle failure or loss of solid mass of the steel, respectively. This can cause the pipeline to become unusable and must be replaced. Replacement causes a complete production stoppage and leads to large financial losses and potential accidents.In practice, one encounters this problem through the use of steels containing high levels of chromium and other expensive alloys. The use of such materials is only truly economically viable in specific cases. Carbon steels with a suitable protective coating in this context could lead to a significant cost reduction. It is essential that the coating, in addition to corrosion protection, meets all other requirements for abrasion resistance, temperature resistance, and impact resistance. DESCRIPTION OF THE RELATED TECHNIQUE

[003] In order to protect metals from corrosion, for example, such as steel against the effects of hydrogen sulfide, carbon dioxide and the formation and injection of water with a high salt content under hydrothermal conditions, the application of a surface coating with a very good diffusion barrier for small gas molecules is required. For hydrogen sulfide, the damaging effect is already Petition 870260066502, dated 06 / 07 / 2026, page 15 / 234 3 / 49 starts at low concentrations. It may also be advisable to additionally provide an absorber in order to achieve maximum long-term effect. Inorganic materials such as ceramics or glass are structurally impermeable to gases.

[004] Coppe / UFRJ (WO 2004 / 022806 A1) claims niobium oxide layers applied by thermal spraying to protect steel against FhS attack. Due to their purely inorganic ceramic nature, these layers are brittle and may be prone to cracking if the coated steel components are mixed, losing the good intrinsic barrier effect again.

[005] To overcome the problem of fragility and open up the possibility of coating three-dimensional internal surfaces homogeneously, polymer-based coatings were used. Amorphous and semi-crystalline polymers are not, due to their structure, completely gas-tight, but can be applied by wet chemical processes to surfaces such as by painting. The matrices used are normally selected from the class of thermosetting materials because they adhere well to metals and are among the most gas-tight polymers. By forming composite materials with inorganic fillers, attempts are made to improve the barrier effect on the one hand and to provide additional absorbent properties on the other.

[006] Nippon Steel Corp. (JP S54-011938 A) describes a protective layer against FkS based on epoxy-polyurea resin and lead powder. Hydrogen sulfide is absorbed by reaction with lead during diffusion to the metal surface. The disadvantage here is the use of polluting heavy metals for protection of the patch. Furthermore, the lead powder is coarse microscale and interferes at high concentrations with the network structure of the epoxy resin matrix, resulting in loss of the barrier effect. Petition 870260066502, dated 06 / 07 / 2026, page 16 / 234 4 / 49

[007] BASF Company (WO 2006 / 079643 A1) claims protective layers with intrinsic inhibitory function in the context of FkS based on polymer matrices with nitrile and thioamide functions. Similar concepts were pursued by Universal Oil Products (US 3,705,109) using matrices containing carboxyl groups or Rossi- jskij KHIM (RU 2083621) using ketimines and 2,4,6-tris(dimethylaminopropyl)phenol as a sequestrant. The disadvantage here is the lack of abrasion resistance.

[008] Schlumberger Canada Ltd. (US 2009 / 0277625 A1) claims compositions of a thermoplastic resin, a thermosetting resin and at least one component that can interact with FkS. This component is a polymer containing an amine group which can interact and is applied to the surface of silica particles. Also, this composition does not show increased abrasion resistance.

[009] Alongside an active absorber function for hydrogen sulfide, the effect of corrosive gas molecules on the metal surface can be reduced by delaying the diffusion of these gas molecules through a tile-like arrangement of flake-shaped particles. This lengthens the diffusion path of the gas molecules and is called the geometric approach according to Nielsen's model.

[0010] In such layers, the filler content, as well as the aspect ratio, the ratio between the length and thickness of the platelet-shaped particles, is of crucial importance for the barrier effect. The thinner and longer the plates, the greater the barrier effect. To achieve a significant effect, the aspect ratio must be at least greater than 10. The aspect ratio of such a particle is defined as the ratio of the average length measurement value, which corresponds to the average diameter here, to the average thickness measurement value. Such values ​​can be measured Petition 870260066502, dated 06 / 07 / 2026, p. 17 / 234 5 / 49 by TEM.

[0011] Nippon Paint Co. Ltd. (JP S62-050368 A) uses a composite based on epoxy-phenolic resins in combination with metallic nickel platelets. These approaches utilize, firstly, the barrier effect of the cross-linked resin matrix and secondly, the active H2S immobilization function of metallic nickel.

[0012] Similar systems are claimed by Henkel (DE 10 (2006 062 500 A1) for coating metal surfaces. However, these systems are based on the use of aluminum flakes and are not intended to be used against H2S. The aluminum flakes are used instead to generate electrical conductivity and solderability of the coatings. They are randomly oriented in the resin matrix. The application refers to the coil coating process and the replacement of a zinc coating. An influence on the barrier effect is not described.

[0013] Nanosolar Inc. (WO 2005 / 044551 A1) claims a hybrid organic-inorganic nanolaminated barrier layer. The nanoscale phases contained in the coating are formed in situ by the sol-gel process of molecular precursors. The result is a semi-interpenetrating network system. A special effect on H2S is not described.

[0014] Eckart GmbH claims an inkjet coating containing aluminum and pearlescent effect pigments in a polymer matrix (DE 10 2009 037 323 A1) and an inkjet coating containing pearlescent pigments based on fine and fine substrates in a radiation-cured matrix (DE 102 009 031 266 A1), each using a polymer wax antisettling agent for plaque. This is necessary because inkjet printing ink is highly diluted with solvent, and the polymer binder is used in significantly smaller than stoichiometric quantities compared to effect pigments. Such compositions are not relevant for anti-corrosion applications. Petition 870260066502, dated 06 / 07 / 2026, p. 18 / 234 6 / 49

[0015] Plastlac (DE 603 ​​​​19 674 T2) has a similar approach to generating a UV-curing acrylic paint containing lamellar pearlescent pigments, in particular, for coating plastics. Here too, polymer-based wax dispersions to orient the platelet fillers are claimed to enhance the desired optical effects.

[0016] All three of the last approaches describe a visual and decorative effect and its improvement through plate alignment. None of the three describes an application in the field of corrosion protection.

[0017] Siemens Power Generation (WO 2006 / 007385 A1) claims highly structured resin system composites with high thermal conductivity fillers, wherein the highly structured resin systems include liquid crystal polymers, interpenetrating networks, dendrimers, star polymers, ladder polymers, expansion polymers or structured organic-inorganic hybrids. The high structure of the resulting composite and the high orientation of the fillers with high thermal conductivity and high aspect ratio are determined by the mesostructure of the polymer matrix and lead to composites with high thermal conductivity. Due to the matrix mesostructure, a close sequence between the polymer structures and the thermally conductive particles is achieved, which leads to good contact between the two phases and thus leads to thermal conductivity at an ideal level. A barrier effect against small molecule diffusion and corrosion protection are not described.

[0018] EP 1 718 690 A1 describes low-energy abrasion-resistant coatings with increased alkali resistance. The material composition comprises a curable organic binder system; at least one fluorine-containing polymer or oligomer. Petition 870260066502, dated 06 / 07 / 2026, page 19 / 234 7 / 49 functionalized, which is reactive with the binder, and inorganic particles. From the matrix, no crosslinking is formed for the particles used. The inorganic particles are mixed with the polymer matrix only physically. There is no phase connection, so the particles are not included as additional network points in the resulting composite, which weakens the material, particularly with respect to its barrier properties against water vapor and gas molecules. Furthermore, the functionalized fluorine component cannot be effectively integrated into the matrix if binder systems with low reactivity are used. The consequence is the occurrence of microphase separation of the fluorine component, resulting in poor adhesion to the substrate and extension function with respect to the matrix. A corrosion protection effect and a diffusion barrier effect are not described in the patent application. PROBLEM

[0019] The object of the present invention is to provide equipment for drilling, finishing, storage and transportation of oil and / or gas, including pressure vessels, tools, piping, tubes, connections and any other parts, coated with a coating that can protect the metal substrates of the equipment from corrosion (substrates that are prone to corrosion) and shows excellent adhesion to the substrates with excellent abrasion, wear resistance, flexible and impact resistance combined with a high barrier function against the diffusion of water vapor and corrosive gases, and optionally a repellent effect against hydrophilic and oleophilic substances. SOLUTION

[0020] The invention solves the task by means of equipment for drilling, finishing, storing and transporting oil and / or gas, including pressure vessels, tools, piping, tubes, Petition 870260066502, dated 06 / 07 / 2026, page 20 / 234 8 / 49 connections and any other parts, coated with a coating comprising a highly structured composite material, which protects the metal substrates from corrosion by excellent adhesion to the substrate and an effective barrier against particularly corrosive attack by hydrogen sulfide, carbon dioxide and the formation and injection of water with a high salt content under hydrothermal conditions (high pressure and temperature).

[0021] This objective is achieved by the inventions as claimed in the independent claims. The advantageous embodiments are described in the dependent claims.

[0022] Even if multiple back-referenced claims are not made, all reasonable combinations of aspects in the claims must be disclosed.

[0023] The problem is solved by equipment for drilling, finishing, storing and transporting oil and / or gas, including pressure vessels, tools, piping, tubes and parts, coated with a coating as a barrier against corrosive gaseous or liquid environments comprising

[0024] a cured binder comprising at least one cured crosslinkable resin, wherein the resin comprises at least one polar group;

[0025] at least one type of hydrophilic flakes with at least one type of hydrophilic flakes having an aspect ratio of more than 10, wherein the surface of the flakes at least partially comprises a metal oxide.

[0026] The main aspect of the equipment for oil and / or gas drilling, finishing, storage and transport, including pressure vessels, tools, piping, tubes, connections and any other parts of the invention is its coating with a highly structured composite structure, which is proposed to be Petition 870260066502, dated 06 / 07 / 2026, page 21 / 234 9 / 49 responsible for the excellent barrier properties and good adhesion to the substrate of the corrosion-resistant material combined with resistance to abrasion and hydrolysis. DETAILED DESCRIPTION OF THE INVENTION

[0027] The interaction of the polar group of the binder and the flocs (hydrophilic due to the metal oxide coating) leads to a uniform distribution of the flocs in the coating. The distribution function of the flocs within the coating is better, the smoother and more even the substrates of the flake carrier for the metal oxides are, because such entanglement between the particles during application and drying process is minimized.

[0028] Cured binder comprises at least one crosslinked resin, wherein the resin comprises at least one polar group. A resin may be a monomer, oligomer or polymer prior to crosslinking.

[0029] A polar group can be any group comprising a dipole moment. Preferably, polar groups that can form complexes with the metal oxide surface, preferably the transition metal oxide surfaces. Examples of such groups are groups containing heteroatoms, for example, an atom of an element in group 15 or 16 in periods 2 to 4 of the periodic table, typically nitrogen, oxygen, sulfur, phosphorus, and similar atoms.

[0030] A polar group having such a heteroatom may be, for example, hydroxyl, alkoxysilyl, epoxy, carboxyl, ester, carbonyl, oxycarbonyl, sulfide, disulfide, sulfonyl, sulfinyl, thiol, thiocarbonyl, imino, amino, nitrile, ammonium, imide, amide, hydrazo, azo, diazo, cyanide, guanidine, oxygen-containing heterocyclic groups, nitrogen-containing heterocyclic groups, sulfur-containing heterocyclic groups, and the like.

[0031] Among those polar groups, hydroxyl, alkoxysyl, epoxy, Petition 870260066502, dated 06 / 07 / 2026, page 22 / 234 10 / 49 Carboxyl, sulfide, sulfonyl, thiol, amino, cyanide, nitrogen-containing heterocyclic groups and the like are preferred.

[0032] Those most preferred are hydroxyl, alkoxysilyl, epoxy, carboxyl, amino, nitrogen-containing heterocyclic groups, and the like, with those particularly preferred being hydroxyl and amino groups.

[0033] A polar group may be the functional group of the resin, through which the resin was cured. It may also be an additional or separate group.

[0034] Possible resins are cured polyepoxides. Polyepoxides can be saturated or unsaturated, and can be aliphatic, cycloaliphatic, aromatic, or heterocyclic. They may also contain 30 substituents that do not cause any secondary interference reactions under the reaction conditions, for example, alkyl or aryl substituents, ether groups, and the like.

[0035] These epoxide compounds are preferably polyglycidyl ethers based on polyhydric compounds, alcohols, phenols, hydrogenation products of these phenols and / or novolacs (reaction products of mono- or polyhydric phenols with aldehydes, in particular formaldehydes, in the presence of acid catalysts). The epoxide equivalent weights of these epoxide compounds (epoxy resins) are between 100 and 5000, preferably between 160 and 4000.Examples of polyhydric phenols are: resorcinol, hydroquinone, 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), mixtures of dihydroxydiphenylmethane isomers (bisphenol-F), tetrabromobisphenol A, 4,4'-dihydroxydiphenylcyclohexane, 4,4'-dihydroxy-3,3'-dimethyldiphenylpropane, 4,4'-dihydroxybiphenyl, 4,4'-dihydroxybenzophenone, 1,1-bis(4-hydroxyphenyl)ethane, 1,1-bis(4-hydroxyphenyl)isobutane, 2,2-bis(4-hydroxy-tert-butylphenyl)propane, bis(2-hydroxynaphthyl)methane, 1,5-dihydroxynaphthalene, tris(4-hydroxyphenyl)methane, bis(4-hydroxyphenyl) ether, bis(4-hydroxyphenyl) sulfone, etc., and the chlorination and bromination products of the compounds. Petition 870260066502, dated 06 / 07 / 2026, page 23 / 234 11 / 49 mentioned above. Bisphenol A and bisphenol F are particularly preferred in this respect.

[0036] Also suitable are polyglycidyl ethers of polyhydric alcohols. Examples of such polyhydric alcohols are ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, polyoxypropylene glycols (n=1-10), 1,3-propylene glycol, 1,4-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, 1,2,6-hexanotriol, glycerol and 2,2-bis(4-hydroxycyclohexyl)propane.

[0037] Polyglycidyl esters of polycarboxylic acids can also be used, which are obtained by reacting epichlorohydrin or similar epoxy compounds with an aliphatic, cycloaliphatic or aromatic polycarboxylic acid, such as oxalic acid, succinic acid, adipic acid, glutaric acid, phthalic acid, terephthalic acid, hexahydrophthalic acid, 2,6-naphthalenedicarboxylic acid and dimerized linolenic acid. Examples are diglycidyl adipate, diglycidyl phthalate and diglycidyl hexahydrophthalate.

[0038] These polyepoxide compounds may also be present in mixtures with each other and, if appropriate, in mixtures with monoepoxides. Examples of suitable monoepoxides are: epoxidized monounsaturated hydrocarbons (butylene oxide, cyclohexene oxide, styrene oxide), epoxide ethers of monohydric phenols (phenol, cresol and other o- or p-substituted phenols), and glycidyl esters of saturated and unsaturated carboxylic acids.

[0039] Also suitable epoxides for the reaction are those containing amide or urethane groups, for example, triglycidyl isocyanurate or glycidyl-blocked hexamethylene diisocyanate.

[0040] Also, suitable epoxide compounds for the resin are derived from unsaturated fatty acids, for example, linoleic acids or linolenic acids. Examples of suitable epoxidized fatty acid derivatives are those from linseed oil, soybean oil, Petition 870260066502, dated 06 / 07 / 2026, page 24 / 234 12 / 49 Alkyl esters of ricinene fatty acid, soybean oil or linoleic, oleic or arachidonic fatty acid, and oligomeric fatty acids and their esters, and epoxidized alkyl esters having two or more ester groups are also suitable. Epoxidized linseed oil and soybean oil are preferred.

[0041] Mixtures of the established epoxides may also be employed. A precondition for all epoxides that may be employed within the scope of the present invention, where they have not been completely or partially reacted with monocarboxylic acids, is that they contain polar groups.

[0042] Provided they contain a sufficient number of polar groups, polyepoxide compounds can be employed as such; however, it is often advantageous to react some of the reactive epoxide groups with a modifying material in order to obtain free polar hydroxyl groups.

[0043] Plasticized epoxy resins with terminal epoxy groups are particularly preferred, which are prepared by partial reaction of the epoxy groups of epoxy resins containing at least two epoxy groups with substances containing OH and COOH, such as polyhydric alcohols, for example, the diols or phenols mentioned above, polycarboxylic acids or polyesters containing carboxyl or OH groups, or by reaction with polyamines.

[0044] Possible epoxides containing hydroxyl groups are also reaction products of compounds having at least two 1,2-epoxide groups by equivalent molecular weights and epoxides from 160 to 600, and aromatic dicarboxylic acids or mixtures thereof with compounds of the group comprising (cyclo)aliphatic dicarboxylic acids, monocarboxylic acids and / or monohydric phenols, and optionally cyclic anhydrides. Products of this type are described in EP 0 387 692 A2, to which reference is made herein. For the preparation Petition 870260066502, dated 06 / 07 / 2026, page 25 / 234 13 / 49 of these reaction products, it is possible to use all the epoxy compounds mentioned in the introduction.

[0045] binder may also comprise a cured phenolic resin. Suitable phenolic resins are, for example, reaction products of monohydric or polyhydric phenols with an aldehyde. Typical examples are resins prepared from phenol, resorcinol, o-, m- or p-cresol, xylenol, para-tertiarybutylphenol, nitrophenol or 2,2-bis(4-hydroxyphenol)propane condensed with formaldehyde, acetaldehyde or propionaldehyde.

[0046] Preferred phenolic resins are polyalkylol phenols in which the phenolic functionality has been at least partially etherified with, for example, ethyl or butyl groups.

[0047] binder may also comprise a phenoxy resin. Phenoxy resins, sometimes referred to herein as thermoplastic polyhydroxy ethers, are known in the art as components of corrosion-resistant coatings. Phenoxy resins is the generic term used to describe amorphous high molecular weight poly(hydroxy ethers) derived from diphenols and epichlorohydrin. The phenoxy resins useful in this invention are the high molecular weight reaction products of Bisphenol A and epichlorohydrin. Such poly(hydroxy ether) reaction products have molecular weights ranging from about 6000 to about 85000.

[0048] Phenoxy resin provides a high molecular weight thermoplastic copolymer having good adhesive properties, dimensional stability, and good resistance to many acids, alkalis, and aliphatic hydrocarbons. Phenoxy resins are usually derived from the same materials as epoxy resins, but phenoxy resins do not have epoxy groups in their molecular chains.Phenoxy resins have hydroxyl groups in their molecular chains; these hydroxyl groups allow crosslinking (curing) with isocyanates, anhydrides, triazines, and melamines. Phenoxy resins are copolymers that are usually derived from... Petition 870260066502, dated 06 / 07 / 2026, p. 26 / 234 14 / 49 bisphenol A and epichlorohydrin and have the repeating structural formula - [OC6H4C (CH3) 2C6H4OCH2CH (OH) CH2 ] n- ( I )

[0049] In preferred embodiments of phenoxy resin, n in the above structural formula (Formula I) is from about 35 to about 120. Phenoxy consequently has a molecular weight of about 10000 to about 35000.

[0050] Preferred resins are epichlorohydrin-bisphenol A type resins, for example, available under the trademark Beckopox from Cytec. Preferred resins show an equivalent epoxide weight between 1500 and 2500.

[0051] The aminoplast resins useful in this invention are the well-known reaction products of urea and triazine compounds with aldehydes further etherified with alcohols. Such resins include those derived from urea, thiourea, ethylene urea, melamine, benzoguanamine, and acetoguanamine. The aldehydes used in the reaction with urea and triazine are aldehydes of 1 to 8 carbons, for example, formaldehyde and the formaldehyde-forming compounds, trioxane and paraformaldehyde, acetaldehyde, propionaldehyde, and butyraldehyde. Alcohols that are used to alkylate or etherify the urea and triazine reaction products are monohydric alcohols of 1 to 8 carbons, for example, methyl alcohol, isopropyl alcohol, butyl alcohol, and 2-ethylhexyl alcohol. Examples of aminoplast resins for use in this invention are butylated urea-formaldehyde resins, methylated and butylated melamine-formaldehyde resins, and benzoguanamine-formaldehyde.

[0052] binder may also comprise a cured polyurethane resin derived from polyisocyanates. The polyisocyanate may have two or more isocyanate groups. It may be, for example, aliphatic, alicyclic, aromatic or heterocyclic, monocyclic or polycyclic. It is possible to use conventional polyisocyanates, for example, monomeric polyisocyanates, polyisocyanate adducts, called polyisocyanates Petition 870260066502, dated 06 / 07 / 2026, page 27 / 234 15 / 49 modified or mixtures thereof. These are known to those skilled in the art and are commercially available. The adducts may have, for example, an average NCO functionality of 2 to 6, preferably 2.4 to 4. Polyisocyanate adducts are, for example, those that typically find use as hardeners for two-component urene coating systems.Examples of suitable poly-isocyanates are di-isocyanates known from polyurethane chemistry, e.g., 1,3-diisocyanatobenzene, di-isocyanate of 2,4- and 2,6-tolylene (TDI), di-isocyanate of 1,4,4HMD4-hexame and 2,4'diphenylmethane (MDI), naphthylene di-isocyanate, xylene di-isocyanate, isophorone di-isocyanate, paraphenyl di-isocyanate, dicyclo-hexylmethane di-isocyanate, cyclo-hexyl di-isocyanate, poly-isocyanate dimethyl-polycyanate 1,6-dodecamethylene, 1,4-bis(isocyanatocyclo-hexyl)methane, pentamethylene di-isocyanate, trimethylene di-isocyanate, triphenylmethane di-isocyanate, and higher molecular weight polyisocyanates derivatives, exocyanate bases, and diisocyanate bases allophanate and biuret. Isocyanates were obtained, for example, under the trade names Desmodur and Baymidur (from Bayer), CARADATE (from Shell), TEDIMON (from Enichem) and LUPRANAT (from BASF).Examples of monomeric polyisocyanates that have more than two isocyanate groups are, for example, 4-isocyanatomethyl1,8-octane diisocyanate and aromatic polyisocyanates such as 4,4',4-triphenylmethane triisocyanate or polyphenolpolymethylene polyisocyanates.

[0053] Polyisocyanate can be used in blocked form in order to prevent a rapid, uncontrolled reaction from the creation, and become active only after unblocking, for example, by heating. Blocking isocyanates is a process known to those skilled in the art to reversibly reduce the reactivity of Petition 870260066502, dated 06 / 07 / 2026, page 28 / 234 16 / 49 Isocyanates. To block isocyanates, all common blocking agents are useful, for example, acetone oxime, cyclohexanone oxime, methyl ethyl ketoxime, acetophenone oxime, benzophenone oxime, 3,5-dimethylpyrazole, 1,2,4-triazole, ethyl malonate, ethyl acetate, scarprolactam, phenol or ethanol.

[0054] The polyol component used for curing may be di-, tri-, or polyalcohols, for example, ethylene glycol, trimethylolpropane, or partially hydrolyzed fatty acid glycerides. However, these are commonly used only as the initial base for higher molecular weight polyhydroxyl compounds. These may be, for example, more or less highly branched polyester polyols (Desmophen(R) types) formed with dicarboxylic acids or polyether polyols formed by the addition of epoxides (Desmophen U(R) types). Other examples are hydroxy-functional acrylic resins (Desmophen A(R) types).

[0055] Polyurethane resin coating materials can be formed from polyisocyanates and polyols. Of course, particularly in the case of unblocked polyisocyanates, it may be necessary to mix the components together just before use. Polyisocyanates can also be reacted with compounds that have other functional groups containing active hydrogen. Examples of such groups are thiol groups (-SH), primary or secondary amino groups (-NHR' where R' can be, for example, H, alkyl, cycloalkyl, aryl and corresponding aralkyl and alkyl groups) or carboxyl groups (-COOH). The reaction products formed in the reaction with isocyanates are urethanes (in the case of hydroxyl and carboxyl), thiourethanes (in the case of thiol) or ureas (in the case of amine).

[0056] binder may also comprise cured acrylic resins comprising at least one polar group. Such resins may also comprise monomers comprising at least one group Petition 870260066502, dated 06 / 07 / 2026, p. 29 / 234 17 / 49 polar or may comprise copolymers of (meth)acrylic monomers with one or more ethylenic monomers comprising at least one polar group. Examples for (meth)acrylic monomers hydroxymethyl(meth)acrylate, hydroxyl-ethyl(meth)acrylate (HEA, HEMA), Hydroxypropyl(meth)acrylate (HPA, HPMA), hydroxybutyl(meth)acrylate (HBA, HBMA), 2(2-Ethoxy-ethoxy)ethyl(meth)acrylate, 2-Phenoxyethyl(meth)acrylate, Caprolactone (meth)acrylate (HO- (CH2) 5COO- (CH2) 5COOCH2CH2CH=CH2), methoxypolyethyleneglocolmono(meth)acrylate, polypropyleneglycolmono(meth)acrylate, polyethyleneglycolmono(meth)acrylate, tetrahydrofurfuryl(meth)acrylate, furfuryl(meth)-acrylate, 1,3-butyleneglycoldi (meth)acrylate, 1,4-butandioldi(meth)acrylate, diethyleneglycoldi(meth)acrylate, dipropyleneglycoldi(meth)acrylate, ethoxylated Bisphenol-A-di(meth)acrylate, trimethylolpropanetri(meth)acrylate, ethyleneglycolmonoacetoacetatomono(meth)acrylate, dimethylamino-(2-)-ethyl(meth)acrylate, tetraethylene glycol(meth)acrylate.

[0057] As ethylenic monomers, allylic alcohol or propoxylated allylic alcohol may be present.

[0058] In a preferred embodiment, the cured binder comprises a mixture of epoxy resins and phenolic resins and / or phenoxy resins.

[0059] For a typical coating, 40 to 98% by weight of binder is present, preferably 40 to 95% by weight, more preferably 50 to 95% by weight.

[0060] All % by weight of the coating in this descriptive report is calculated with respect to all coating components excluding the organic solvent.

[0061] If a mixture of epoxy resins and phenolic resins and / or phenoxy resins (the phenolic resin and phenoxy added) is present, the preferred ratio is between 10:1 and 1:1, preferably 8:1 and 2:1 (in % by weight). Petition 870260066502, dated 06 / 07 / 2026, page 30 / 234 18 / 49

[0062] coating further comprises at least one type of hydrophilic flakes with an aspect ratio of more than 10.

[0063] The average aspect ratio of the flakes, that is, the ratio of the average length measurement value, which corresponds to the average diameter for such flakes, to the average thickness measurement value, is usually 10 to 200, preferably 10 to 150 and particularly preferably 10 to 100. The aspect ratio can be measured with TEM.

[0064] The surface of the flakes at least partially comprises a metal oxide, which makes the flakes hydrophilic. Therefore, either the particle itself may be composed of metal oxide (e.g., TiC>2 flakes) or a carrier substrate is at least partially covered by at least one layer of metal oxide. Such layered coatings may comprise more than one layer of different compositions. For the invention, only the surface layer is important.

[0065] The metal oxide on the surface is a metal oxide capable of complex formation, primarily an oxide in which organic compounds with polar groups can be absorbed. In a preferred embodiment of the invention, the metal oxide is a transition metal oxide, more preferably TiCh, Fe2C>3 or ZrC>2 or mixtures thereof.

[0066] The metal oxide surface of the flakes is very important. It is possible to use glass flakes with the same size distribution, but without a metal oxide coating, without a highly structured composite coating. Such a coating does not exhibit the desired barrier properties and corrosion protection. Therefore, the interface between the metal oxide and the binder is very important.

[0067] In a preferred embodiment of the invention, the coated flakes used are generated by the use of transport substrates, Petition 870260066502, dated 06 / 07 / 2026, page 31 / 234 19 / 49 which are available through a warp coating process. The resulting carrier flakes are then crushed and subsequently fractionated. These flakes are then coated with metal oxide with thickness controlled by wet chemical precipitation (G. Buxbaum and G. Pfaff Industrial Inorganic Pigments, 3rd ed. Wiley-VCH pages 243-248 FJ Maile et al. Progress in Organic Coating 2005, 54, 150-163).

[0068] After filtration and drying, the coated flakes are then calcined. This leads to metal oxide layers with a closed grain structure, which is well suited for a good interface between the binder and the flakes.

[0069] The metal oxide layer typically has a thickness between 10 nm and 1000 nm.

[0070] In a preferred embodiment, at least one of the broad surfaces of the flakes is coated with the metal oxide coating, preferably both broad surfaces, more preferably the entire surface of the particles is coated with the metal oxide coating.

[0071] As a transport substrate, any substrate can be chosen, which can be coated with a corresponding metal oxide coating. This can therefore be a metal, metal oxide or other inorganic material. Depending on their resistance to the temperature required by the coating process, organic substrates are also possible. It is very important that the flakes used have a very low variation in thickness.

[0072] Initially, the connection mechanism works even with mica platelets coated with metal oxide, but the distribution of these types of particles on the polymer matrix prevents the formation of the structure in some aspect, since the mica flakes in their longitudinal direction considered a more pronounced variation in Petition 870260066502, dated 06 / 07 / 2026, p. 32 / 234 20 / 49 thickness compared to boards obtained by the warp coating process. This can lead to the interlocking mentioned above.

[0073] In a preferred embodiment, the flakes are chosen from glass flakes coated with metal oxide, silicon dioxide coated with metal oxide (or mica) or alumina flakes coated with metal oxide.

[0074] The average diameter of the flakes is usually between 1 and 500 µm, preferably between 5 and 200 µm and in particular 10 and 150 µm. The smaller flake sizes preferred are, in addition, those in the range of 1 to 100 µm, in particular 5 to 60 µm and 1 to 15 µm. The average thickness is between 0.1 and 5 µm and preferably 0.1 and 1 µm.

[0075] Flakes are typically present between 2% by weight and 60% by weight, preferably 2% by weight and 50% by weight, more preferably 5% by weight to 40% by weight, more preferably 5% by weight to 25% by weight.

[0076] The conventional additives that may possibly be present in the coating according to the invention are dependent on the particular intended use or production process. Conventional coating additives such as pigments, pigment pastes, antioxidants, leveling and thickening agents, flow aids, antifoaming and / or wetting agents, fillers, catalysts, additional curing agents and additional curable compounds, solvents, etc. These additives are usually present at up to 5% by weight.

[0077] The coating may also comprise inorganic particles. Suitable particles are virtually ceramic and glass systems, but also in some cases metals, semiconductors and conventional fillers. They are preferably ceramic particles. Frequently, oxides, nitrides, carbides, carbonitrides, silicides or borides are used. It is also possible to use Petition 870260066502, dated 06 / 07 / 2026, page 33 / 234 21 / 49 mixtures of different particles. Preference is given to using abrasive particles or hard substances. The particles may be modified or unmodified on the surface.

[0078] The particles are, for example, metal particles including metal alloys, semimetals (e.g., B, Si and Ge) or metal compounds, in particular metal chalcogenides, more preferably oxides and sulfides, nitrides, carbides, silicides and borides. It is possible to use one type of particle or a mixture.

[0079] Examples are (optionally hydrated) oxides such as ZnO, SiO2, GeO2, TO2, ZrO2, CeO2, SnO2, AbO3 (e.g., Amperite, Boehmite, AlO(OH), also in the form of aluminum hydroxide), B2O3, La2O3, Fe2O3 (e.g., Hematite), Fe3O4, Ta2O5, Nb2O5, V2O5, MoO3 or WO3; also chalcogenides, e.g., sulfides (e.g., ZnS and Ag2S), selenides (e.g., GaSe and ZnSe) and tellurides (e.g., ZnTe); halides such as AgCl, AgBr, AgI; carbides such as SiC; nitrides such as BN, AlN, Si3N4 and Ti3N4; Phosphides such as GaP, Zn3P2, phosphates, silicates including relatively complex silicates, for example, phyllosilicates, talc, zirconates, aluminates, stannates and the corresponding mixed oxides (for example, indium tin oxide (ITO), fluorinated tin oxide (FTO).Usual fillers are also useful, for example, graphite, sulfates such as barite and gypsum, carbonates such as calcite, dolomite and chalk, sulfides such as zinc sulfide or lithopones, glass, and also oxides and silicates such as silica, cristobalite, talc, kaolin and mica, provided they are insoluble in the selected medium.

[0080] Preference is given to using abrasive powders for the particles. Examples of abrasive or hard powders which are also referred to as abrasives are diamond powder, granite, pumice, tripel, silicon carbide, emery, aluminas, for example, amperite and corundum, silica such as Kieselguhr, quartz or abrasive sands. Petition 870260066502, dated 06 / 07 / 2026, page 34 / 234 22 / 49 gypsum, boron carbide and other oxides, borides, silicides, carbides, carbonitrides and nitrides.

[0081] In one embodiment, the Mohs hardness value of the particles is greater than 5. In certain embodiments, the Mohs hardness value of the particles, such as silica, is greater than 6.

[0082] The particles are preferably selected from particles consisting of at least one of boron carbide, silicon carbide and / or silicon nitride.

[0083] The particle size of the particles is not particularly restricted. Suitablely, the average particle diameter is, for example, in the range of at least 0.1 pm, preferably at least 0.5 pm and more preferably at least 1 pm up to no more than 100 pm, more preferably no more than 50 pm and particularly preferably no more than 20 or 10 pm. It is also possible to use mixtures of particles of different particle sizes. For example, SiC UF-10 with coarse UF-05 and even finer UF-15 can be used in combination. Furthermore, it is also possible to add finer particle fractions to the nm range, as is usual, for example, in nanocomposites which are described, for example, in DE 42 12 633 A1. It is also possible to use very fine particles of such nanoscale solid particles with an average particle diameter below 0.1 pm alone.

[0084] Also as in the most recent data, the average particle diameter is based on the determined volume average, the distributions being determined through the use of laser diffraction processes (evaluation according to Mie) in the particle size range of 1 to 2000 pm and UPA (ultrafine particle analyzer, Leeds Northrup (optical laser)) in the range of 3.5 nm to 3 pm. In the intersection range of 1 to 3 pm, reference is made here to the measurement with UPA.

[0085] The particles used can also be modified in Petition 870260066502, dated 06 / 07 / 2026, page 35 / 234 23 / 49 surface. For example, SiO2 particles, especially quartz particles, can be surface-modified with epoxy or amino groups or other functional groups.

[0086] The modification of particle surfaces is a known process, as described for nanoscale solid particles, for example, in WO 93 / 21127 A1 or WO 96 / 31572 A1. The preparation of surface-modified particles can, in principle, be carried out in two different ways, especially firstly by modifying already prepared particles, and secondly by preparing particles using one or more compounds that have appropriate functional moieties.

[0087] Inorganic particles are usually present between 5% by weight to 30% by weight, preferably 10 to 25% by weight.

[0088] In a preferred embodiment, the coating comprises no more than 40% by weight of inorganic flakes and particles, more preferably between 15% by weight and 40% by weight or between 20% by weight and 40% by weight.

[0089] In another embodiment of the invention, the coating comprises a fluorine-containing polymer or oligomer. Such polymers are reactive perfluoropolyethers. The fluorine content improves the barrier properties of the cured coating against water penetration due to the hydrophobic character of the fluorine-containing compound. In one embodiment, the perfluoropolyether is chemically connected to the binder, forming a plurality of covalent bonds between the perfluoropolyether and the polymer (oligomer or active fluorine-containing polymer). Furthermore, the perfluoropolyether may be condensed with the binder. In one embodiment, the perfluoropolyether comprises Fluorolink® D10H (Solvay Solexis). This compound may alternatively be referred to as D10H herein. In certain embodiments, about 0.01 to 2% by weight of the fluorine-containing polymer, based on the total weight of the coating, may be Petition 870260066502, dated 06 / 07 / 2026, page 36 / 234 24 / 49 present, preferably 0.28 to 0.5% by weight. In other embodiments, non-reactive fluorine compounds may be present to accomplish this purpose.

[0090] In a preferred embodiment of the invention, the coating further comprises a crosslinked comonomer or oligomer or polymer for crosslinking the binder. This comonomer may comprise at least one functional group, which is reactive with the binder curing reaction. It may also be a different crosslinking reaction. Such crosslinking may improve the barrier properties of the cured coating. These comonomers may carry independent functional groups, such as polar or nonpolar groups, or may be used to introduce halogens such as fluorine groups into the coating. In a preferred embodiment of the invention, the comonomer is a reactive fluorine-containing oligomer or polymer as described above.

[0091] In another embodiment of the invention, the binder further comprises a comonomer comprising at least one cyano group. This reactive group is beneficial insofar as it can react with hydrogen sulfide. The comonomer may be a monomer, oligomer, or polymer based on a cyano-containing compound. Such a compound comprises functional groups compatible with functional groups in the resin. The compound may be polymerized with the resin curing reaction. It may also react only with other functional groups present in the resin. Preferably, the compounds act as crosslinkers, and may contain more than two functional groups to react with the resin.

[0092] For epoxy resins or polyurethane resins, such a compound may be cyanoguanidine derivatives. Such compounds may be oligomeric cyanoguanidines such as dicyandiamide or monomeric cyanoguanidine. Petition 870260066502, dated 06 / 07 / 2026, page 37 / 234 25 / 49

[0093] comonomer, in its cured form, is typically present at 0.01% by weight to 20% by weight, preferably 2% by weight to 15% by weight.

[0094] A comonomer comprising a cyano group (in its uncured form) is especially beneficial for barriers against corrosive gaseous media, preferably in combination with a fluorine-containing comonomer.

[0095] It is also possible to use a mixture of comonomers.

[0096] In another embodiment of the invention, the coating further comprises at least one rheology additive.

[0097] Such rheological additives are, for example, waxes capable of providing anti-settling, abrasion resistance, and floc orientation aspects that may be present in the coating.

[0098] Such rheology additives may be synthetic waxes, polyethylene waxes, polytetrafluoroethylene (PTFE) waxes, high-density polyethylene waxes, polypropylene waxes, ethylene copolymers, ethylene acrylic acid (EAA) copolymers, and ethylene vinyl acetate (EVA) copolymers.

[0099] In yet another embodiment of the invention, the rheology additive is chosen from the group containing an ethylene copolymer and / or an ethylene acrylic acid copolymer, preferably ethylene vinyl acetate (EVA) copolymers and / or ethylene acrylic acid (EAA) copolymers.

[00100] Rheology additives are, for example, ethylene vinyl acetate (EVA) copolymers.

[00101] Rheology additives may be present from 0.05% by weight to 5% by weight, preferably 1% to 3% by weight.

[00102] Equipment for drilling, finishing, storing and transporting oil and / or gas, including pressure vessels, tools, piping, tubes, fittings and any other parts thereof. Petition 870260066502, dated 06 / 07 / 2026, page 38 / 234 26 / 49 invention, coated with a coating as a barrier against corrosive gaseous or liquid environments, can be made of any suitable material. The equipment also includes piping for the production and transport of oil and gas, a container for transporting gas, and high-pressure gas cylinders.

[00103] In another embodiment of the invention, the equipment for drilling, finishing, storing and transporting oil and / or gas comprises at least one of the following: casing pipes, piping, connectors and connecting pipes or pipes used as pipeline, coiled pipe, artificial lifting parts and gas containers.

[00104] Examples of suitable equipment are substrates made of metal or glass, ceramic coatings including coatings of porous ceramic composite materials, glass ceramics or inorganic-organic materials. The substrates can be penetrated, for example, by sandblasting or glass bead blasting or by a preliminary coating such as a varnish coating (varnished surfaces), an enamel coating, a paint coating or a metallized surface, or by impregnation.

[00105] Examples of metal substrates include, for example, iron, steel, and some alloys. Glass used as liners can be any type of conventional glass, for example, silica glass, borosilicate glass, or soda ash glass. Examples of plastic substrates used as liners are polycarbonate, polymethyl methacrylate, polyacrylates, polyethylene terephthalate, and cellulose acetate (TAC).

[00106] The coating on the substrate typically has a thickness of 5 µm to 500 µm, preferably between 8 µm and 200 µm, more preferably between 8 µm and 100 µm or 8 µm and 50 µm. In a Petition 870260066502, dated 06 / 07 / 2026, page 39 / 234 27 / 49 preferred modality, the coating has a thickness between 8 pm and 40 pm.

[00107] For coating the equipment, any suitable process may be used. Preferably, a composition consisting of the uncured coating as described is mixed with a solvent and applied to the substrate by spray coating. Suitable solvents are, for example, aliphatic and / or aromatic solvents with a boiling point or range of about 120°C to 180°C, such as butyl acetate or methoxypropyl acetate. The solvent may be used in any suitable quantity, provided that good mixing of the compounds is possible. Typically, the solvent is used in a ratio of 2:1 to 1:5 of uncured binder and solvent by weight. The applied coating composition may be cured as known to a person skilled in the art.

[00108] The invention also relates to the use of a substrate coated with a coating as described above for drilling, finishing, storage and transportation of oil and / or gas, including pressure vessels, tools, piping, tubes, fittings and any other parts. This may include coating casing pipes, tubing, connectors and fittings or pipes used as pipeline, coiled pipe, artificial lifting parts and gas container.

[00109] Such substrates also include well tools, devices or components adapted to comprise at least part of a well finishing assembly or well drilling assembly. For example, such substrates may be centralizers, casing pipes, casings, production screens, production tubing, artificial lift parts and the like in oil or gas wells and gas storage containers. Petition 870260066502, dated 06 / 07 / 2026, page 40 / 234 28 / 49

[00110] Due to its special properties, the coating is particularly suitable for corrosive environments, for example, in hydrothermal conditions (high pressure and temperature, for example, >5 bar and < 200°C). DETAILED SPECIFICATION FOR CORROSIVE LIQUID AND GASEOUS ENVIRONMENTS

[00111] Depending on the desired properties of the coating, the coating composition can be optimized. For corrosive liquid environments, the addition of hard particles is preferred in order to increase the abrasion resistance of the cured coating.

[00112] For such environments, the coating may comprise 50% to 98% by weight of binder; 2 to 25% by weight of flakes, 0 to 25% by weight of hard particles, 0 to 0.5% by weight of a fluorine-containing comonomer and 0 to 3% by weight of a rheology additive, preferably 50% to 93% by weight of binder; 2 to 25% by weight of flakes, 5 to 25% by weight of hard particles, 0 to 0.5% by weight of a fluorine-containing comonomer and 0 to 3% by weight of a rheology additive. Cured coatings typically have a thickness between 7.5 µm and 100 µm.

[00113] In the case of corrosive gaseous environments, the addition of crosslinking comonomers such as cyanoguanidine is preferred. Such compositions may not comprise any hard particles.

[00114] For such environments, the coating may comprise 50% to 98% by weight of the binder; 2 to 25% by weight of flakes, 0 to 25% by weight of hard particles, 0 to 0.5% by weight of a fluorine-containing comonomer, 0 to 20% by weight of a crosslinked comonomer and 0 to 3% by weight of a rheology additive, preferably 50% to 96% by weight of the binder; 2 to 25% by weight of flakes, 0 to 25% by weight of hard particles, 0 to 0.5% by weight of a fluorine-containing comonomer, 2 to 20% by weight of a Petition 870260066502, dated 06 / 07 / 2026, page 41 / 234 29 / 49 crosslinking comonomer and 0 to 3% by weight of a rheology additive. Cured coatings typically have a thickness between 15 µm and 100 µm.

[00115] Tables 1 and 2 show different results for different coating compositions with the following abbreviations: CS = Crystal Silver Flakes (Merck); LS = Pencil Sunlight Flakes (Merck); CTX = Ceratix 8461 (Byk); CF = Cerafak 100 (Byk); PS = P 104 S 30 (Byk); FL = Fluorolink D10H (Solvay). Samples labeled H (Table 1) are compositions specifically for liquid environments, while samples labeled G (Table 2) are preferred for gaseous environments. Some of the specific compositions will be present in the example section. Samples H193, H139 are comparative examples in Table 1. Samples G046, G014, G099 are comparative examples in Table 2.

[00116] Figures 2A and 2B show light microscope and scanning electron microscopy (SEM) images of the surface of a sample from different points of the coated substrate (arrows). Figure 3 shows the effect of the additive orientation on the orientation of the flakes in the cured layers. MATERIALS AND METHODS Autoclave Test

[00117] Experiments for the H2S tests were conducted in a laboratory-scale H2S test facility. The autoclave (Model LaS-4-13-MCS-J, Laborautoklav 13 1, 4 bars) with stainless steel fittings (discharge tap, safety valve, pressure gauge and connections) was provided by Adolf Wolf SANOclav, Bad ÜberkingenHausen. The gas mixture for the tests was supplied by LINDE GAS Deutschland, Düsseldorf. It contains 10% H2S and 90% CO2. For safety reasons, the test facility components were constructed in a locked, skeletonized container. Petition 870260066502, dated 06 / 07 / 2026, page 42 / 234 30 / 49

[00118] The H2S test was performed as follows: Water containing 5% by weight of sodium chloride is placed in the flask to form vapor during the H2S test procedure. 5x5 cm samples are mounted on a base frame and placed in the flask so that they do not come into contact with the saltwater (samples indicated G) or are immersed with 50% of their size in the saltwater (samples indicated H) at the bottom of the flask. The lid is closed and the autoclave is now flooded with the gas mixture from the external gas cylinder to 1.0 bar internal pressure. The flask is now heated to 85°C, thus increasing the pressure in the flask to 1.4 bar. The corrosion time is counted from the point at which the test parameters are reached.

[00119] After the time has elapsed (usually after every 14 days) the flask is cooled to room temperature and the gas mixture is allowed to discharge. Then, the cap is opened and a certain amount of samples is removed. The rest remains in the flask and the process is started again as described previously.

[00120] The removed samples are cleaned only with water and a brush, using no other cleaning agents, and dried with a towel. They are now ready for examination via cross-sectional / tape test (CC / TT). A successful sample will have to reach 720 h in this test and complete the CC / TT test. The results are shown in Table 1 and Table 2. Cross-sectional Test - Tape (CC / TT) according to DIN ISO 2409

[00121] Cross-sectional tape test, performed after the H2S test, provides information on the adhesion of the coating material to the sample surface after the corrosion test. It is performed on the back of 5x5 cm samples. A knife with 6 parallel blades (1 mm apart) is passed across the coating surface. Petition 870260066502, dated 06 / 07 / 2026, page 43 / 234 31 / 49 so that the coating layer is completely cut. The same is done perpendicularly, thus giving a cross-section. The sample is brushed after cutting to remove separated coating material. The remaining amount of coating on the surface is examined and judged according to a classification (see Figure 1). After that, a tape is placed on the surface and pulled down. Also, the remaining coating is examined. All samples that showed values ​​greater than CC / TT 1 / 1 do not meet the requirements for good adhesion. Liquid CC / TT means the part of the sample immersed in brine, gas CC / TT means the part of the sample in the gas phase. The results are shown in Table 1 and Table 2. Vibrational Traction Test (Fatigue Test)

[00122] Tests were performed on both sides of the coated flat tensile specimens using an Instron testing machine which has a chamber that is cooled with liquid N2 to -40°C. Sample elongation was performed within a loading range of 1 to 10 kN. The frequency used was 1.0 Hz. Thus, the required 15000 cycles were performed in approximately 4 hours. Crack formation was investigated visually, by light microscopy and by scanning electron microscopy (SEM) as can be seen in the sample photos in Figure 2A and Figure 2B.

[00123] The requirement for a sample to pass the test is no cracks after 15,000 cycles. The results are given as a fatigue test in Table 2 and as can be seen in Figures 2A and 2B, there are no visible cracks. Taber abrasion according to DIN 53754

[00124] For this test, 2 x 500 g CS-17 rollers were used for 400 cycles. Weight loss is given in mg. Samples showing a weight loss of <5 mg meet the requirements. The results are shown in Table 1. Petition 870260066502, dated 06 / 07 / 2026, page 44 / 234 32 / 49 Neutral salt spray test (SST)

[00125] This test was performed in accordance with DIN 50021. Samples were investigated for blistering, delamination, and subsurface migration. Sample duration is given in hours. All samples that pass the 300 h SST requirement meet the test. The 300 h is based on the corrosion stability required by the US standard for submarine vessels. The results are shown in Table 1. Impact test (ball drop test)

[00126] Impact behavior was tested by the ball drop test using a 10 mm diameter steel ball loaded to 1500 g. The drop height was chosen to be 1 m. The impact area was visually inspected with the naked eye and with a magnifying glass for delamination and cracking. The classification was made as follows:

[00127] I1: no damage

[00128] I2: small scratch, sharp edge

[00129] I3: scratching with the wall

[00130] I4: scratching with the wall and cracks

[00131] - I5: 50% fragmentation

[00132] A successful sample must obtain a minimum of 12. Tests in environments with the presence of H2S

[00133] A low-alloy Cr-Mo steel with different tensile strength (TS) was tested with and without a coating developed in the present invention. Tubular pieces were cut as rolled tubes and subjected to quenching and tempering at different temperatures in order to achieve the desired mechanical properties. Samples were used to evaluate resistance to Sulfide Stress Cracking in environments with H2S (using NACE TM0177 tensile test method) and performance in a gaseous environment with the presence of H2S. Petition 870260066502, dated 06 / 07 / 2026, page 45 / 234 33 / 49 (through slow deformation rate tests). NACE Method A Test in GO55

[00134] The longitudinal samples for NACE testing were machined from heat-treated tubular parts.

[00135] The tests were performed according to NACE TM 0177-2005 Method A. Test solution A, as reported in NACE TM0177-2005, was used in all tests. The initial pH was 2.7 and the solution was saturated with 100% H2S.

[00136] The samples with and without a coating developed in the present invention were evaluated. The coating used was a mixture called G055 with a thickness of 33 + / - 2 µm. Samples 1 and 2 were coated and passed the required number of hours (720 h), all other uncoated samples failed. Table 3 shows the results of the NACE tests performed. Cyclic slow deformation rate tests on G055

[00137] The longitudinal samples were then machined from tubular parts. A transverse electro-erosion machining (EDM) groove was placed in the intermediate section of the sample (see Figure 4).

[00138] The samples were fatigue tested in an autoclave with CH4 gas at a pressure of 200 bar, 4% CO2 and 330 ppm H2S with a controlled dew point to allow condensation of water vapor. Before testing, the samples were air-cracked to develop a sharp crack in the pre-existing groove. Samples 11, 12, and 13 were coated with a G055 combination and a thickness of + / - 3 µm.

[00139] The samples were fatigue tested in different numbers of cycles and, at the end of the test, fatigue crack propagation was observed and measured by metallographically polished sections or by opening the sample at liquid nitrogen temperature.

[00140] All samples coated with delta-stress applied Petition 870260066502, dated 06 / 07 / 2026, page 46 / 234 Samples 34 / 49, with a different number of cycles, show crack propagation of less than 0.1 mm, while all other uncoated samples show crack propagation of 0.2 mm until sample failure. Table 4 shows the results of the cyclic creep rate tests.

[00141] In the following sections, examples are given to illustrate the invention. EXAMPLES Example 1: Composition for corrosive liquid media H 247

[00142] 10.40 g of bisphenol A type epichlorohydrin epoxy resin (Cytec Beckopox EP307) are dissolved in 20.80 g of methoxypropyl acetate (CAS 108-65-6). To this, 4.90 g of Cytec Phenodur PR722 / 53BG / B phenolic resin solution (PR722), 0.07 g of Fluorolink D10H (Comonomer 2 FL), 3.58 g of BYK Ceratix 8461 (CTX) and 2.70 g of Borcarbid HD20 (HC Starck) are added. The mixture is milled in a ball mill (VMA Getzmann Dispermat CA with APS milling system, 1.2 to 1.4 mm zirconium oxide balls). The balls are then removed and the yield is determined. In a yield, 75% of 1.34 g (= 1.79 g * 75%) Merck Colorstream Lapis Sunlight T20-04 WNT (Pigment 1) are stirred with a dissolving disc. Application is done with a SATA minijet spray gun onto sandblasted steel plates (wet film thickness of 80 to 100 µm), curing occurs for 30 minutes at 200°C.This gives a glossy, homogeneous, highly adhesive green-gray coating with excellent stability in the ball drop test after curing. The impact test rating was 12.

[00143] After the complete set of tests (autoclave, SST, CC / TT, Taber Abrasion) has been carried out, it can be observed that this example meets the requirements, as can be derived from Table 1. Example 2: Composition for corrosive liquid media H 253

[00144] 9.60 g of bisphenol A type epichlorohydrin epoxy resin (Cytec Petition 870260066502, dated 06 / 07 / 2026, page 47 / 234 35 / 49 Beckopox EP307) are dissolved in 19.20 g of methoxypropyl acetate (CAS 108-65-6). To this, 4.50 g of Cytec Phenodur PR722 / 53BG / B phenolic resin solution, 0.06 g of Fluorolink D10H, 3.30 g of BYK Ceratix 8461 and 2.48 g of Borcarbid HD20 (HC Starck) are added. The mixture is milled in a ball mill (VMA Getzmann Dispermat CA with APS grinding system, 1.2-1.4 mm zirconium oxide balls). The balls are then removed and the yield is determined. At a 75% yield, 1.24 g (= 1.65 g * 75%) Merck Xirallic Crystal Silver T60-10 SW (Pigment 2) is stirred with a dissolving disc. The application is done with a SATA minijet spray gun on sandblasted steel plates (wet film thickness of 80 to 100 µm), curing occurs for 30 minutes at 200°C. This gives a bright, homogeneous, well-adherent green-gray layer with excellent stability in the drop ball test after curing. The impact test rating was 12.

[00145] After the complete set of tests (autoclave, SST, CC / TT, Abrasion taber) has been carried out, it can be observed that this example meets the requirements, as can be derived from Table 1. Example 3: Composition for corrosive liquid media H 226

[00146] 11.30 g of bisphenol A type epichlorohydrin epoxy resin (Cytec Beckopox EP307) are dissolved in 22.60 g of methoxypropyl acetate (CAS 108-65-6). To this, 5.30 g of Cytec Phenodur PR722 / 53BG / B phenolic resin solution, 0.07 g of Fluorolink D10H and 2.64 g of Borcarbid HD20 (HC Starck) are added. The mixture is milled in a ball mill (VMA Getzmann Dispermat CA with APS grinding system, 1.2 to 1.4 mm zirconium oxide balls). The balls are then removed and the yield is determined. At a 75% yield, 0.66 g (=0.88 g * 75%) of Merck Colorstream Lapis Sunlight T20-04 WNT is stirred with a dissolving disc. Application is done with a SATA minijet spray gun onto blasted steel plates. Petition 870260066502, dated 06 / 07 / 2026, page 48 / 234 36 / 49 sand (Wet film thickness of 80 to 100 µm), curing occurs for 30 minutes at 200°C. This gives a bright, homogeneous, well-adherent green-grey layer with excellent stability in the ball drop test after curing. The impact test rating was 12.

[00147] After the complete set of tests (autoclave, SST, CC / TT, Abrasion taber) has been carried out, it can be observed that this example meets the requirements as can be derived from table 1. Example 4: Composition for corrosive liquid media H 232

[00148] 10.40 g of bisphenol A type epichlorohydrin epoxy resin (Cytec Beckopox EP307) are dissolved in 20.80 g of methoxypropyl acetate (CAS 108-65-6). To this, 4.90 g of Cytec Phenodur PR722 / 53BG / B phenolic resin solution, 0.07 g of Fluorolink D10H and 3.02 g of Borcarbid HD20 (HC Starck) are added. The mixture is milled in a ball mill (VMA Getzmann Dispermat CA with APS grinding system, 1.2 to 1.4 mm zirconium oxide balls). The balls are then removed and the yield is determined. At a 75% yield, 3.02 g (= 4.02 g * 75%) of Merck Colorstream Lapis Sunlight T20-04 WNT is stirred with a dissolving disc. Application is made with a SATA minijet spray gun onto sandblasted steel plates (wet film thickness of 80 to 100 µm), curing occurs for 30 minutes at 200°C. This gives a bright, homogeneous, well-adherent green-grey layer with excellent stability in the drop ball test after curing. The impact test rating was 12.

[00149] After the complete set of tests (autoclave, SST, CC / TT, Abrasion taber) has been carried out, it can be observed that this example meets the requirements as can be derived from table 1. Comparative example 1 (without flakes) for corrosive liquid media: H 139

[00150] 12.80 g of bisphenol A type epichlorohydrin epoxy resin (Cytec Beckopox EP307) are dissolved in 25.60 g of acetate Petition 870260066502, dated 06 / 07 / 2026, page 49 / 234 37 / 49 methoxypropyl (CAS 108-65-6). To this end, 6.00 g of Cytec Phenodur PR722 / 53BG / B phenolic resin solution, 0.08 g of Fluorolink D10H and 5.36 g of Borcarbid HD20 (HC Starck) are added. The mixture is ground in a ball mill (VMA Getzmann Dispermat CA with APS grinding system, 1.2 to 1.4 mm zirconium oxide balls). The balls are then removed. Application is done with a SATA minijet gun on sandblasted steel sheets (wet film thickness of 80 to 100 µm), curing occurs for 30 minutes at 200°C. This gives a glossy, homogeneous, well-adherent green-grey layer with excellent stability in the drop ball test after curing. The impact test score was 12.

[00151] After the complete set of tests (autoclave, SST, CC / TT, Abrasion taber) was performed, it can be observed that this sample did not meet the requirements as can be derived from table 1. Due to SST failure. Example 5: Composition for corrosive gaseous media G 089

[00152] 12.40 g of bisphenol A type epichlorohydrin epoxy resin (Cytec Beckopox EP307) are dissolved in 24.80 g of methoxypropyl acetate (CAS 108-65-6). To this, 5.85 g of Cytec Phenodur PR722 / 53BG / B phenolic resin solution, 0.08 g of Fluorolink D10H, 8.85 g of BYK Ceratix 8461 and 2.00 g of cyanoguanidine (CAS 461-58-5) are added. The mixture is milled in a ball mill (VMA Getzmann Dispermat CA with APS grinding system, 1.2 to 1.4 mm zirconium oxide balls). The balls are then removed and the yield is determined. At a 75% yield, 1.50 g (= 2.00 g * 75%) of Merck Colorstream Lapis Sunlight T20-04 WNT is stirred with a dissolving disc. Application is done with a SATA minijet spray gun onto sandblasted steel plates (wet film thickness of 80 to 100 µm), curing occurs for 30 minutes at 200°C.

[00153] This gives a bright, homogeneous, golden-green layer, Petition 870260066502, dated 06 / 07 / 2026, page 50 / 234 38 / 49 very adherent.

[00154] After the complete test set (autoclave, SST, CC / TT) was performed, it can be observed that this example meets the requirements as can be derived from table 2. Also for this example, the fatigue test was successfully performed (figure 2b). Example 6: Composition for corrosive gaseous media G 055

[00155] 16.00 g of bisphenol A type epichlorohydrin epoxy resin (Cytec Beckopox EP307) are dissolved in 32.50 g of methoxypropyl acetate (CAS 108-65-6). To this, 7.50 g of Cytec Phenodur PR722 / 53BG / B phenolic resin solution, 0.10 g of Fluorolink D10H, 11.00 g of BYK Ceratix 8461 and 3.00 g of cyanoguanidine (CAS 461-58-5) are added. The mixture is milled in a ball mill (VMA Getzmann Dispermat CA with APS grinding system, 1.2 to 1.4 mm zirconium oxide balls). The balls are then removed and the yield is determined. At an 80% yield, 4.72 g (= 5.90 g * 80%) of Merck Colorstream Lapis Sunlight T20-04 WNT are stirred with a dissolving disc. Application is done with a SATA minijet spray gun onto sandblasted steel plates (wet film thickness of 80 to 100 µm), curing occurs for 30 minutes at 200°C. This gives a bright, homogeneous, well-adherent golden-green layer.

[00156] After the complete test set (autoclave, SST, CC / TT) was performed, it can be observed that this example meets the requirements as can be derived from table 2. Also for this example, the fatigue test (figure 2a) and the tests in environments with the presence of H2S (table 3 and table 4) were successfully performed. Example 7: Composition for corrosive gaseous media G 053

[00157] 9.60 g of bisphenol A type epichlorohydrin epoxy resin (Cytec Beckopox EP307) are dissolved in 19.50 g of methoxypropyl acetate (CAS 108-65-6). For this, 4.50 g of Petition 870260066502, dated 06 / 07 / 2026, page 51 / 234 39 / 49 solution of Cytec Phenodur PR722 / 53BG / B phenolic resin, 0.06 g of Fluorolink D10H, 3.60 g of BYK Cerafak 100 (CFK) and 1.80 g of cyanoguanidine (CAS 461-58-5). The mixture is milled in a ball mill (VMA Getzmann Dispermat CA with APS grinding system, 1.2 to 1.4 mm zirconium oxide balls). The balls are then removed and the yield is determined. At a 75% yield, 2.67 g (= 3.56 g * 75%) of Merck Colorstream Lapis Sunlight T20-04 WNT is stirred with a dissolving disc. The application is made with a SATA minijet spray gun on sandblasted steel sheets (wet film thickness of 80 to 100 µm), curing takes 30 minutes at 200°C.

[00158] This gives a bright, homogeneous, well-adherent golden-green layer.

[00159] After the complete test set (autoclave, SST, CC / TT) has been performed, it can be observed that this example meets the requirements as can be derived from table 2. Example 8: Composition for corrosive gaseous media G 039

[00160] 13.60 g of bisphenol A type epichlorohydrin epoxy resin (Cytec Beckopox EP307) are dissolved in 13.60 g of methoxypropyl acetate (CAS 108-65-6). To this end, 6.40 g of Cytec Phenodur PR722 / 53BG / B phenolic resin solution, 0.09 g of Fluorolink D10H and 5.13 g of BYK Cerafak 100 (CFK) are added. The mixture is stirred with a dissolving disc (VMA Getzmann Dispermat CA). 5.55 g of Merck Colorstream Lapis Sunlight T20-04 WNT is stirred with a dissolving disc. The application is done with a SATA minijet spray gun on sandblasted steel sheets (wet film thickness of 80 to 100 µm), curing takes 30 minutes at 200°C. This gives a bright, homogeneous, well-adherent green-gold layer.

[00161] After the complete test set (autoclave, SST, CC / TT) has been performed, it can be observed that this example meets the requirements as can be derived from table 2. Petition 870260066502, dated 06 / 07 / 2026, page 52 / 234 40 / 49 Example 9: Composition for corrosive gaseous media G 037

[00162] 13.60 g of bisphenol A type epichlorohydrin epoxy resin (Cytec Beckopox EP307) are dissolved in 13.60 g of methoxypropyl acetate (CAS 108-65-6). To this end, 4.50 g of Cytec Phenodur PR722 / 53BG / B phenolic resin solution, 0.09 g of Fluorolink D10H and 9.38 g of BYK Ceratix 8461 (CTX) are added. The mixture is stirred with a dissolving disc (VMA Getzmann Dispermat CA). 6.62 g of Merck Colorstream Lapis Sunlight T20-04 WNT is stirred with a dissolving disc. The application is done with a SATA minijet spray gun on sandblasted steel sheets (wet film thickness of 80 to 100 µm), curing takes 30 minutes at 200°C.

[00163] This gives a bright, even, well-adherent golden-green layer.

[00164] After the complete test set (autoclave, SST, CC / TT) has been performed, it can be observed that this example meets the requirements as can be derived from table 2. Example 10: Composition for corrosive gaseous media G 035

[00165] 13.60 g of bisphenol A type epichlorohydrin epoxy resin (Cytec Beckopox EP307) are dissolved in 27.20 g of methoxypropyl acetate (CAS 108-65-6). To this, 6.40 g of Cytec Phenodur PR722 / 53BG / B phenolic resin solution, 0.09 g of Fluorolink D10H and 4.27 g of Merck Colorstream Lapis Sunlight T20-04 WNT are added. The mixture is mixed with a dissolving disc (VMA Getzmann Dispermat CA). Application is done with a SATA minijet gun on sandblasted steel plates (wet film thickness of 80 to 100 µm), curing occurs for 30 minutes at 200°C. This gives a bright, homogeneous, well-adherent golden-green layer. A cross-sectional view from scanning electron microscopy is shown in Figure 3a.

[00166] After the complete test set (autoclave, SST, CC / TT) is Petition 870260066502, dated 06 / 07 / 2026, page 53 / 234 41 / 49 completed, it can be observed that this example meets the requirements as can be derived from table 2. Example 11: Composition for corrosive gaseous media G 049

[00167] 9.70 g of bisphenol A type epichlorohydrin epoxy resin (Cytec Beckopox EP307 is dissolved in 19.40 g of methoxypropyl acetate (CAS 108-65-6). To this, 4.50 g of Cytec Phenodur PR722 / 53BG / B phenolic resin solution, 0.06 g of Fluorolink D10H, 6.60 g of Byk Ceratix 8461, and 3.09 g of Merck Colorstream Lapis Sunlight T20-04 WNT are added. The mixture is mixed with a dissolving disc (VMA Getzmann Dispermat CA). Application is done with a SATA minijet gun on sandblasted steel plates (wet film thickness of 80 to 100 µm), curing occurs for 30 minutes at 200°C. This gives a bright, homogeneous, well-adherent golden-green layer. A cross-sectional view from scanning electron microscopy is shown in Figure 3b.

[00168] After the complete test set (autoclave, SST, CC / TT) has been performed, it can be observed that this example meets the requirements as can be derived from table 2. Example 12: Composition for corrosive gaseous media G 048

[00169] 9.70 g of bisphenol A type epichlorohydrin epoxy resin (Cytec Beckopox EP307) are dissolved in 19.40 g of methoxypropyl acetate (CAS 108-65-6). To this end, 4.50 g of Cytec Phenodur PR722 / 53BG / B phenolic resin solution, 0.06 g of Fluorolink D10H, 3.60 g of Byk Cerafak 100, and 3.11 g of Merck are added. Colorstream Lapis Sunlight T20-04 WNT. The mixture is mixed with a dissolving disc (VMA Getzmann Dispermat CA). Application is done with a SATA minijet spray gun on sandblasted steel plates (wet film thickness of 80 to 100 µm), curing occurs for 30 minutes at 200°C. This gives a bright, homogeneous, well-adherent golden-green layer. A cross-sectional view from the Petition 870260066502, dated 06 / 07 / 2026, page 54 / 234 42 / 49 scanning electron microscopy is shown in figure 3c.

[00170] After the complete test set (autoclave, SST, CC / TT) has been performed, it can be observed that this example meets the requirements as can be derived from table 2. Comparative example 2 (without flakes and without comonomer 1): for corrosive gaseous media G 046

[00171] 12.20 g of bisphenol A type epichlorohydrin epoxy resin (Cytec Beckopox EP307) are dissolved in 24.40 g of methoxypropyl acetate (CAS 108-65-6). To this, 5.70 g of Cytec Phenodur PR722 / 53BG / B phenolic resin solution and 0.08 g of Fluorolink D10H are added. The mixture is mixed with a dissolving disc (VMA Getzmann Dispermat CA). Application is done with a SATA minijet gun on sandblasted steel plates (wet film thickness of 80 to 100 µm), curing occurs for 30 minutes at 200°C. This gives a transparent, glossy, homogeneous, well-adherent yellow-brown layer.

[00172] After the complete test set (autoclave, SST, CC / TT) was performed, it can be observed that this example did not meet the requirements as can be derived from table 2 in CC / TT. Comparative example 3 (with glass flakes having NO metal oxide on the surface): for corrosive gaseous media G 014

[00173] 13.60 g of bisphenol A type epichlorohydrin epoxy resin (Cytec Beckopox EP307) are dissolved in 27.20 g of methoxypropyl acetate (CAS 108-65-6). To this, 6.40 g of Cytec Phenodur PR722 / 53BG / B phenolic resin solution, 0.09 g of Fluorolink D10H and 1.90 g of Microglas RCF 015 (Muhlmeier) are added. The mixture is mixed with a dissolving disc (VMA Getzmann Dispermat CA). Application is done with a SATA minijet gun on sandblasted steel sheets (wet film thickness of 80 to 100 µm), curing occurs for 30 minutes at 200°C. This gives a yellow-brown layer. Petition 870260066502, dated 06 / 07 / 2026, page 55 / 234 43 / 49 transparent, shiny, homogeneous, well-adhering.

[00174] After the complete test set (autoclave, SST, CC / TT) was performed, it can be observed that this example did not meet the requirements, as can be derived from table 2 in CC / TT.

[00175] While the present inventions have been described and illustrated along with various specific embodiments, those skilled in the art will appreciate that variations and modifications can be made without departing from the principles of the inventions as illustrated herein, as described and claimed. The present inventions can be incorporated in other specific forms without departing from their spirit or essential characteristics. The embodiments described are considered in all respects to be illustrative and not restrictive. The scope of the inventions is therefore indicated by the appended claims, rather than by the description above. All changes that come within the meaning and range of equivalence of the claims shall be embraced within their scope. List of tables and figures

[00176] Table 1: The table shows different results for different coating compositions with the following abbreviations: CS = Crystal Silver Flakes (Merck); LS = Lapis Sunlight Flakes (Merck); CTX = Ceratix 8461 (Byk); CF = Cerafak 100 (Byk); PS = P 104 S (Byk); FL = Fluorolink D10H (Solvay). Samples labeled with H are compositions specifically for liquid environments.

[00177] Table 2: The table shows different results for different coating compositions with the following abbreviations: CS = Crystal Silver Flakes (Merck); LS = Lapis Sunlight Flakes (Merck); CTX = Ceratix 8461 (Byk); CF = Cerafak 100 (Byk); PS = P 104 S (Byk); FL = Fluorolink D10H (Solvay). Samples labeled with G are preferred for gaseous environments.

[00178] Table 3: Results of the NACE Method A tests. Petition 870260066502, dated 06 / 07 / 2026, p. 56 / 234 44 / 49 Coated samples passed the test, uncoated samples failed < 200 h (*TS: tensile strength).

[00179] Table 4: Results of cyclic slow deformation rate tests. All samples coated with G055 show crack propagation less than 0.1 mm, while uncoated samples show crack propagation less than 0.2 mm and also failures during testing (*TS: tensile strength).

[00180] Figure 1: The figure shows the classification for the Cross-Cut Tape Test (CC / TT) according to DIN ISO 2409

[00181] Figure 2A: The figure shows the Fatigue test results for sample G055.

[00182] Figure 2B: The figure shows the Fatigue test results for the different sample G089.

[00183] Figure 3: SEM images of a cross-section of different samples. From top: a) G035 20% by weight Lapis Sunlight; b) G049 20% by weight Lapis Sunlight + 2.0% Ceratix 8461; c) GO 48 20% by weight Lapis Sunlight + 2.3% Cerafak 100.

[00184] Figure 4: Sample for cyclic slow deformation rate tests with artificial transverse groove. Petition 870260066502, dated 06 / 07 / 2026, page 57 / 234 45 / 49 Table 1 Sample Flake 1 Sunglight Pencil % by weight Flake 2 Crystal Silver % by weight Boron carbonate HD 20 % by weight Rheology Additive % by weight Thickness [pm] Thickness [pm] CC / TT liquid CC / TT gaseous SST [h] Taber Δm [mg] 72% PR by weight weight Comon number 2 FL % by weight H193 - - - - 30.40 720h 2 / 3 5 / 5 6.8 79.60 19.90 0.50 H139 - - 25% HD20 - 7.00 720h 0 / 0 0 / 0 - 5.00 720.393 H226 5% LS - 15% HD20 - 7.81 720h 0 / 0 0 / 0.5 408 2.0 63.68 15.92 0.40 H144 10% LS - - - 15.46 720h 0 / 1 0 / 2 67 2.71 71.96 0.45 H228 10% LS - 10% HD20 - 7.88 720h 0 / 0 0 / 0 408 1.5 63.68 15.92 0.40 H229 10% LS - 15% HD20 - 8.37 720h / 000 7.859 14.93 0.38 H246 10% LS - 15% HD20 1% CTX 11.08 720h 0 / 0 0 / 0 1008 3.2 58.90 14.73 0.38 H247 10% LS - 15% HD20 260 720h CTX 0 / 0 0 / 0 1008 3.1 58.10 14.53 0.38 H248 10% LS - 15% HD20 3% CTX 14.85 720h 0 / 0 0 / 0 HD20 - 9.96 720h 0 / 0 0 / 0 576 2.5 51.74 12.94 0.33 H232 20% LS - 15% HD20 - 11.68 720h 0 / 0 0 / 0 1080 4,3 51,74 12,94 0,33 H235 - 5% CS 15% HD20 - 16,90 720h 0 / 0,5 1 / 3,5 408 2,8 63,68 15,92 0,40 H237 - 10% CS 10% HD20 - 21,91 720h 0 / 1,5 0 / 2,5 408 3,3 63,68 15,92 0,40 H238 - 10% CS 15% HD20 - 17,35 720h 0 / 0 0 / 1,5 1080 2,8 59,70 14,93 0,38 H252 - 10% CS 15% HD20 1% CTX 22,91 720h 0 / 0 0 / 0 504 3,2 58,90 14,73 0,38 H253 - 10% CS 15% HD20 2% CTX 26,21 720h 0 / 0 0 / 1 1008 3,6 58,10 14,53 0,38 H254 - 10% CS 15% HD20 3% CTX 28,30 720h 0 / 0 0 / 1 840 3,4 57,30 14,33 0,38 H239 - 10% CS 25% HD20 - 58,36 720h 0 / 1 0 / 1,5 1080 3,4 51,74 12,94 0,33 H240 - 20% CS 10% HD20 - 16,09 720h 0 / 0 0 / 0 1080 4,0 55,72 13,93 0,35 H241 - 20% CS 15% HD20 - 19,12 720h 0 / 1,5 0 / 0,5 1080 3,9 51,74 12,94 0,33 H242 - 20% CS 25% HD20 - 23,39 720h 0 / 2,5 0 / 1,5 1080 5,4 43,78 10,95 0,28 H168 5% LS - 10% HD15 2% CF 25,8 720h 0 / 1 0 / 1 480 4,2 66,06 16,52 0,43 H169 5% LS - 10% HD15 0,25% PS 19,5 720h 1 / 2 0 / 0 984 3,4 67,46 16,87 0,43 H170 5% LS - 10% HD15 0,5% PS 17,7 720h 0 / 0 0 / 1 1032 3,7 67,26 16,81 0,43, Petition 870260066502, dated 06 / 07 / 2026, p. 58 / 234 46 / 49 Sample Flake 1 Lapis Sunglight % by weight Flake 2 Crystal Silver % by weight Flake 3 Glass Flakes % by weight Comonomer 1 cyanoguanidine % by weight Rheology additive 1 CTX % by weight Rheology additive 2 CFK % by weight Thickener [□m] Autoclave test with H2S CC / TT gas. Fatigue test EP307 % by weight PR722 % by weight Comonomer 2 FL % by weight G046 - - - - - - 11.96 720 h 2 / 4 79.60 19.90 0.50 G014 - - 10.00 - - - 23.82 720 h 5 / 5 71.64 19.90 0.45 G099 - - - 10.54 2.24 - 19 720 h 1 / 2 69.43 17.63 0.43 G095 5.00 - - 2.93 2.31 - 29 720 h 0 / 0 71.45 17.86 0.45 G096 5.00 - - 5.29 2.25 - 28 720 h 0 / 0 69.62 17.41 0.44 G094 5.00 - - 10.01 2.13 - 23 720 h 0 / 0 65.96 16.49 0.41 G097 5.00 - - 14.73 2.01 - 24 720 h 0 / 0 62.29 15.57 0.39 G098 5.00 - - 19.45 1.89 - 20 720 h 0 / 1 58.63 14.66 0.37 G090 10.00 - - 2.77 2.19 - 27 720 h 0 / 0 67.69 16.92 0.42 G091 10.00 - - 5.01 2.13 - 22 720 h 0 / 0 65.96 16.49 0.41 G089 10.00 - - 9.48 2.02 - 27 720 h 0 / 0 ok 62.49 15.62 0.39 D092 10.00 - - 13.95 1,91 - 26 720 h 0 / 0 59.02 14.75 0.37 G093 10.00 - - 18.43 1.79 - 28 720 h 0 / 1 55.54 13.89 0.35 G035 20.00 - - - - - 15.67 720 h 0 / 1 63.68 15.92 0.45 G049 20.00 - - - 2.00 - 24.25 720 h 1 / 1 62.09 15.52 0.39 G048 20.00 - - - - 2.30 26.58 720 h 1 / 1 61.85 15.46 0.39 G085 20.00 - - 2.46 1.96 - 33 720 h 0 / 0 60.17 15.04 0.38 G086 20.00 - - 4.45 1.89 - 34 720 h 0 / 0 58.63 14.66 0.37 G051 20.00 - - 10.40 - - 23.19 720 h 0 / 0 55.40 13.85 0.35, Petition 870260066502, dated 06 / 07 / 2026, page 59 / 234 47 / 49 Table 2 Sample Flake 1 Lapis Sunglight % by weight Flake 2 Crystal Silver % by weight Flake 3 Glass Flakes % by weight Comonomer 1 cyanoguanidine % by weight Rheology additive 1 CTX % by weight Rheology additive 2 CFK % by weight Thickener [□m] Autoclave test with H2S CC / TT gas. Fatigue test EP307 % by weight PR722 % by weight Comonomer 2 FL % by weight G055 20.00 - - 10.16 1.75 - 29.72 720 h 0 / 0 ok 54.21 13.55 0.34 G053 20.00 - - 10.12 - 2.02 35.40 720 h 0 / 0 53.97 13.49 0.34 G039 27.40 - - - 1.83 - 25.66 720 h 0 / 0 56.33 14.08 0.35 G037 23.99 - - - - 2.22 29.69 720 h 0 / 0 58.74 14.69 0.37 G060 20.00 10.40 24.42 720 h 0 / 0 55.40 13.85 0.35 G064 20.00 10.16 1.75 34.49 720 h 0 / 0 54.21 13.55 0.34 G062 20.00 10.12 2.02 30.73 720 h 0 / 0 53.97 13.49 0.34 Petition 870260066502, dated 06 / 07 / 2026, page 60 / 234 48 / 49 Table 2 (continued) Sample No. TS* [MPa] Applied Stress [MPa] Result Classification 1 1170 744 Passed [1500h] Coated with G055 2 1170 744 Passed [1500h] Coated with G055 3 1170 744 Failed Not coated 4 1170 744 Failed Not coated 5 1170 744 Failed Not coated 6 980 730 Failed Not coated 7 980 730 Failed Not coated 8 980 730 Failed Not coated 9 860 744 Failed Not coated 10 860 744 Failed Not coated 11 860 744 Failed Not coated Table 3: Results of the NACE Method A tests. Coated samples passed the test, uncoated samples failed < 200 h (*TS: tensile strength) Sample No. TS Steel* [MPa] Applied delta stress [MPa] Number of cycles Crack length [pm] Classification 5 1050 418 2000 4800 (sample failure) Uncoated 6 1050 418 500 4800 (sample failure) Uncoated 7 1050 239 4000 1050 Uncoated 8 1050 239 2000 220 Uncoated 9 1050 318 950 5000 (sample failure) Uncoated 10 1050 318 980 5000 (sample failure) Uncoated 11 1170 418 2000 80 Coated with G055 13 1170 418 440 Failed during testing Uncoated Table 4: Results of the cyclic slow deformation rate tests. Petition 870260066502, dated 06 / 07 / 2026, p. 61 / 234 49 / 49 All samples coated with G055 show crack propagation of less than 0.1 mm, while uncoated samples show crack propagation greater than 0.2 mm and also failures during testing (*TS: tensile strength). References Cited WO 2004 / 022806 A1 JP S54-011938 A WO 2006 / 079643 A1 US 2009 / 0277625 A1 JP S62-050368 A DE 10 2006 062 500 A1 WO 2005 / 044551 A1 DE 10 2009 037 323 A1 DE 102 009 031 266 A1 DE 603 ​​19 674 T2 WO 2006 / 007385 A1 EP 1 718 690 A1 EP 0 387 692 A2 DE 42 12 633 A1 WO 93 / 21127 A1 WO 96 / 31572 A1 US 3,705,109 EN 2083621 G. Buxbaum and G. Pfaff Industrial inorganic pigments, 3aed. Wiley-VCH Pages 243–248 FJ Maile et al. Progress in Organic Coating 2005, 54, 150-163

Claims

1. Equipment comprising oil and / or gas drilling, finishing, storage and transport equipment coated with a coating as a barrier against corrosive gaseous or liquid environments, characterized in that the coating comprises a) 40 to 98% of a cured binder comprising at least one cured crosslinkable resin selected from polyepoxides, phenolic resin, and phenoxy resin, aminoplast resin, polyisocyanate-derived polyurethane resin and acrylic resin, wherein the resin comprises at least one polar group comprising a heteroatom selected from the group including nitrogen, oxygen, sulfur and phosphorus; b) 2 to 60% of at least one type of hydrophilic flakes with at least one type of hydrophilic flakes having an aspect ratio of more than 10, wherein the surface of the flakes, at least partially, comprises a metal oxide, wherein the coating further comprises a fluorine-containing polymer or oligomer;and wherein the oil and / or gas equipment is selected from the group consisting of pipe, casing pipe, tubing, pipeline, coiled pipe, artificial lifting parts, tools and high-pressure gas cylinders.

2. Equipment according to claim 1, characterized in that the metal oxide is a transition metal oxide.

3. Equipment according to claim 2, characterized in that the transition metal oxide is selected from TiO2, Fe2O3, ZrO2 or mixtures thereof.

4. Equipment, according to any of the claims 1 to 3, characterized by the fact that the hydrophilic flakes are obtained through a warp coating process and then precipitation coated.

5. Equipment according to any one of claims 1 to 4, characterized in that the cured crosslinkable resin is an acrylic resin.

6. Equipment according to any one of claims 1 to 5, characterized in that the polar group is selected from the group including hydroxyl, alkoxysilyl, epoxy, carboxyl, ester, carbonyl, oxycarbonyl, sulfide, disulfide, sulfonyl, sulfinyl, thiol, thiocarbonyl, imino, amino, nitrile, ammonium, imide, amide, hydrazo, azo, diazo, cyanide, guanidine, oxygen-containing heterocyclic groups, nitrogen-containing heterocyclic groups, sulfur-containing heterocyclic groups.

7. Equipment according to any one of claims 1 to 6, characterized in that the crosslinkable resin is of the class of epoxy resins, phenol resins, phenoxy resins or mixtures thereof.

8. Equipment according to any one of claims 1 to 7, characterized in that the composition further comprises inorganic particles.

9. Equipment according to claim 8, characterized in that the inorganic particles are hard particles.

10. Equipment according to claim 9, characterized in that the hard particles are selected from particles consisting of at least one of the oxides, nitrides, carbides, carbonitrides, silicides and borides.

11. Equipment according to claim 10, characterized in that the hard particles are selected from particles consisting of at least one of boron carbide, Petition 870260066502, dated 06 / 07 / 2026, pp. 226 / 234 3 / 3 silicon carbide and / or silicon nitride.

12. Equipment according to any one of claims 1 to 11, characterized in that the cured binder is further crosslinked by a comonomer, oligomer or crosslinking polymer.

13. Equipment according to claim 12, characterized in that the crosslinking comonomer is selected from the group comprising a comonomer comprising at least one cyano group, a functionalized perfluoropolyether and / or mixtures thereof.

14. Equipment according to claim 12, characterized in that the comonomer comprising at least one cyano group is a cyanoguanidine-derived compound.

15. Equipment according to any one of claims 1 to 14, characterized in that the coating further comprises at least one rheological additive.

16. Equipment according to any one of claims 1 to 15, characterized in that the coating comprises 40 to 95% by weight of the binder.

17. Equipment according to claim 16, characterized in that the binder consists of a mixture of epoxy resins, and phenoxy resins are used in a ratio of 10:1 to 1:1 by weight.