Lí mineral manufacturing process
A recycled raw material-based process for mineral wool manufacturing addresses the issues of explosive fracturing and high CO2 emissions, ensuring high melt quality and environmental sustainability with improved high-temperature resistance and biosolubility.
Patent Information
- Application Number
- BR112022010502
- Authority / Receiving Office
- BR · BR
- Patent Type
- Patents
- Current Assignee / Owner
- Publication Date
- 2026-11-17
AI Technical Summary
The use of dolomite and magnesia as magnesium carriers in mineral wool manufacturing leads to explosive fracturing, poor melt quality, and high CO2 emissions, posing operational and environmental challenges.
A process using a recycled raw material comprising at least 8.5% magnesium oxide, free of dolomite and magnesia, with a specific chemical composition, ensuring high liquidus temperature and glass transition temperature, and employing electric or fuel-fired furnaces with electrodes for melting, followed by internal centrifugation for fiber formation.
The process enhances melt quality, reduces the risk of explosive fracturing, and significantly decreases CO2 emissions while producing mineral wool with improved high-temperature resistance and biosolubility.
Abstract
Description
"Mineral Wool Manufacturing Process"
[0001] The present invention relates to the field of artificial mineral fibers. It aims more specifically at a process for manufacturing mineral wool, intended notably for manufacturing thermal and / or acoustic insulation products.
[0002] Mineral wools are traditionally obtained by melting a mixture of raw materials in a melting furnace, the resulting molten material then being poured into a fiber-forming device whereby the mineral wool is formed. The raw materials, generally natural, are selected, and their proportions adapted, according to the desired target chemical composition of the mineral wool. Magnesium oxide may be included in the composition of mineral wools to impart certain properties or to improve their processability. Dolomite and magnesia are the main magnesium carriers used in the manufacture of mineral wools. These raw materials, however, have certain disadvantages. They can, in fact, cause explosive fracturing or "decrepitation" phenomena during the melting of the raw material mixture.This leads to the formation of a layer composed of fragments and decay dust on the furnace dome, which can be detrimental to both the furnace's operation and the quality of the molten material bath. On the other hand, due to their chemical compositions, these raw materials contribute significantly to CO2 emissions during the melting of the raw material mixture.
[0003] The objective of the present invention is to overcome the aforementioned drawbacks by proposing an economical process for manufacturing mineral wool that includes magnesium oxide while ensuring good processability, maintaining, and even improving, the quality of the molten bath and the properties of the mineral wool, particularly from the point of view of resistance to high temperatures, and thus reducing the environmental impact.
[0004] Thus, a first aspect of the present invention relates to a process for manufacturing mineral wool that has a chemical composition, expressed as a weight percentage of oxides, comprising: Petition 870260094621, dated 09 / 15 / 2026, page 11 / 36 2 / 11 SiO2 30-50 % Al2O3 15-35 % CaO 5-25 % MgO 1-25 % Fe2O3 2-15 % Na2O + K2O > 10 % the said process comprising: - the supply of a mixture of raw materials; - the fusion of said mixture of raw materials to obtain a molten material; - the formation of fibers from the molten material; characterized in that the raw material mixture comprises at least 8.5% by weight of a recycled raw material comprising at least 3.5% magnesium, expressed as oxides by weight, said recycled raw material being essentially free of carbonates, and in that the raw material mixture is free of dolomite and magnesia.
[0005] The process according to the invention relates to the manufacture of mineral wool whose chemical composition causes a high liquidus temperature and a high fluidity at the fiber formation temperature, associated with a high glass transition temperature.
[0006] The silica (SiO2) content is comprised within a range of 30 to 50%, preferably 35 to 48%, and even 37 to 45%.
[0007] The alumina content (AUOa) is comprised within a range of 15 to 35%, preferably 18 to 30%, and even 20% to 28%.
[0008] The alumina content (AUOa) is comprised within a range of 15 to 35%, preferably 18 to 30%, and even 20% to 28%.
[0009] The lime (CaO) content is comprised within a range of 5 to 25%, preferably 7 to 20%, and even 8% to 18%.
[0010] The magnesium (MgO) content is comprised within a range of 1 to 25%, preferably 1 to 15%, and even 1% to 10%. Petition 870260094621, dated 09 / 15 / 2026, page 12 / 36 3 / 11
[0011] Mineral wool generally does not comprise other alkaline earth oxides besides CaO and MgO. It may, however, contain small amounts of BaS or SrO, at levels that can reach up to 2%, and even 1%, 0.20%, or even 0.1%, these oxides being present as impurities in certain raw materials.
[0012] The total content of alkaline oxides (R2O), notably soda ash (Na2O) and potash (K2O), is greater than 10%, preferably from 10.2 to 20%, and even from 10.5 to 15%. The Na2O content is typically comprised within a range of 4 to 20%, preferably from 5 to 15%, and even from 6% to 13%. The K2O content is typically of a maximum of 20%, preferably from 1 to 15%, and even from 2 to 10%. The mineral wool preferably does not comprise any other alkaline oxide than Na2 and K2O. It may, however, contain small amounts of Li2O, sometimes present as impurities in certain raw materials, at levels that can reach up to 0.5%, and even 0.2%, or even 0.1%.
[0013] The iron oxide content (total iron expressed as F2O3) is comprised within a range of 2 to 15%, preferably 2 to 12%, and even 2.5 to 10%.
[0014] The sum of the contents of SiO2, Al2O3, CaO, MgO, R2O and Fe2O3 preferably represents at least 95%, notably at least 97%, and even at least 98% by weight of the mineral wool composition.
[0015] The chemical composition of mineral wool may also contain P2O5, notably at levels that can reach up to 3%, and even up to 1.2%. However, it is preferably free of P2O5.
[0016] The composition of mineral wool may also include other elements, notably present as unavoidable impurities. It may include titanium oxide (TiO2) and zirconium oxide (ZrO2) at levels within a range of up to 3%, notably from 0.1 to 2.0%, and even 1.0%.
[0017] The chemical composition of mineral wool typically comprises less than 0.1% by weight of halogen, notably fluorine.
[0018] It is evident that the different preferred ranges described above can be freely combined with each other, the different combinations not being able to Petition 870260094621, dated 09 / 15 / 2026, page 13 / 36 4 / 11 all of them to be numbered for the sake of brevity.
[0019] Due to its composition, mineral wool can offer the advantage of being both biosoluble, meaning it can dissolve rapidly in a physiological environment, thus preventing any potential pathogenic risk linked to the eventual accumulation of finer fibers in the body through inhalation, and exhibiting good resistance at very high temperatures. The fire resistance of a building element corresponds to the duration during which the element retains its load-bearing function, ensures flame tightness, and maintains its role as thermal insulation. The standard fire test generally consists of a temperature rise according to ISO 834, based on the temperature curve of a cellulosic fire.
[0020] Conventionally, the mineral wool composition as described above is obtained by preparing and melting a mixture of raw materials. The process according to the invention comprises a step of supplying a mixture of raw materials comprising at least 8.5% by weight of a recycled raw material comprising at least 3.5%, preferably at least 4%, and even at least 5% of magnesium, expressed as oxide weight. The use of such a raw material allows for the release of dolomite and magnesia and allows for better melt quality. The other raw materials can be chosen from those conventionally used in the manufacture of mineral wools such as limestone, phonolite, nepheline syenite, feldspar, basalt, sodium carbonate, iron oxides.Their respective proportions in the raw material mixture are determined by the professional based on their chemical compositions and the target chemical composition of mineral wool to be obtained. In particular, the raw material mixture preferably comprises at least 1%, more preferably at least 2%, and even at least 3%, by weight of bauxite as an alumina carrier.
[0021] The recycled raw material may be a by-product from the treatment of aluminum slag (also called salt slag, black dross, white dross or salt cake) that comes from the manufacture and / or recycling of aluminum metal. In aluminum manufacture, the first transformation slags that form in. Petition 870260094621, dated 09 / 15 / 2026, page 14 / 36 5 / 11 The surface of the vats contains a high percentage of metallic aluminum. These slags are therefore generally treated, for example in rotary kilns, to recover the aluminum they contain. In particular, in certain technologies, treatment salts may be added during this second transformation. The second-transformation slags, which contain small proportions of metallic aluminum, can in turn be treated to extract the residual metallic aluminum and recycle the treatment salts. Certain by-products of this treatment, consisting mainly of oxide mixtures and essentially devoid of metallic residue, can be used as recycling raw material in the process according to the invention. These by-products can in turn be subjected to certain treatments (granulation, drying, calcination, etc.) before their use in the process according to the invention.In addition to reducing the amount of wastewater and other volatile elements such as halogens and ammonia, calcination, for example in a rotary kiln, improves particle size distribution. However, the potential for recycling raw materials is not limited to these examples.
[0022] Recycling raw material typically has a chemical composition, expressed in oxide weights, comprising: Al2O3 50 to 80%, preferably 60 to 75%, SiO2 2 to 25%, preferably 5 to 50%, MgO 3 to 20%, preferably 5 to 15%, Fe2O3 0.5 to 10%, preferably 1 to 8%,
[0023] It typically comprises less than 0.9%, preferably less than 0.6%, by weight of halogen, notably fluorine and chlorine. The presence of halogens necessitates costly fume treatment facilities. In a particular embodiment, the recycled raw material is notably fluorine-free, meaning that it comprises less than 0.1% by weight of fluorine.
[0024] The recycled raw material preferably has a composition such that the Al2O3 / MgO mass ratio is greater than 8. Such a ratio is particularly advantageous for obtaining the mineral oil according to the invention without the need for addition. Petition 870260094621, dated 09 / 15 / 2026, page 15 / 36 6 / 11 of dolomite.
[0025] The recycled raw material is preferably free of metallic particles, particularly metallic aluminum. Small amounts of metallic aluminum (typically up to 2%, preferably up to 1%, more preferably up to 0.5% by weight) may, however, be present, especially when the recycled raw material is a byproduct of aluminum slag processing. Similarly, small amounts of aluminum nitride (typically up to 3%, preferably up to 2%, more preferably up to 1% by weight) may also be present, especially when the recycled raw material is a byproduct of aluminum slag processing.
[0026] From a mineralogical point of view, the recycled raw material is essentially free of carbonates, meaning that it comprises at most 5%, preferably at most 2%, more preferably at most 1%, and even at most 0.5% by weight of carbonates. It preferably comprises at least 20%, and even at least 30%, and generally up to 80%, and even up to 60%, by weight of amorphous phase. Large proportions of amorphous phase favor melting. It may comprise at least 10%, and even at least 20%, and generally up to 50%, by weight of spinel-type crystalline phase comprising magnesium (Mg1xMxAl2-yM'yO4, M and M' being transition metals).
[0027] The raw material mixture is typically in powder form. In particular, the raw material mixture preferably does not comprise briquettes.
[0028] The melting step can be carried out in different known ways, notably by melting inside a fuel-fired furnace or by electric melting. It is not generally carried out inside a cupola-type furnace. The mineral fiber compositions targeted by the present invention are poorly compatible with this melting method, notably due to the relatively high alkali content. The mixtures of materials necessary to achieve these compositions tend to rapidly change from a solid state to a low-viscosity liquid that can coat the coke particles and impede combustion. Cupola furnaces also favor the evaporation of alkalis, generating not only losses of Petition 870260094621, dated 09 / 15 / 2026, page 16 / 36 7 / 11 matter, but also environmental or safety problems due to the high reactivity of the latter with other scattering substances such as sulfur.
[0029] The fuel-fired furnace comprises at least one burner, either overhead (the flames are arranged above the molten material bath and heated by radiation) or immersed (the flames are heated directly within the molten material bath). The burner or burners may be fed with various fuels such as natural gas or fuel oil.
[0030] By “electric melting” it is understood that the vitrifiable mixture is melted by the Joule effect, by means of electrodes immersed in the molten bath, excluding any use of other heating means, such as flames. The vitrifiable mixture is normally distributed homogeneously over the surface of the molten bath with the aid of a mechanical device, and thus constitutes a thermal screen that limits the temperature above the molten bath, so that the presence of a superstructure is not always necessary. The electrodes may be suspended so as to be immersed in the molten bath from above, installed on the hearth, or even installed on the side walls of the tank. The first two options are generally preferred for large tanks in order to distribute the heating of the molten bath as best as possible.The electrodes are preferably made of molybdenum, and even occasionally of tin oxide. The passage of the molybdenum electrode through the hearth is preferably done by means of an electrode holder made of water-cooled steel.
[0031] The melting stage can also perform both fuel-fired and electric melting simultaneously, for example by employing a fuel-fired furnace also equipped with electrodes on the side walls that serve to accelerate the melting of the vitrifiable mixture.
[0032] Conventionally, the type of mineral wool targeted by the process according to the invention is transformed into fiber by so-called “external” centrifugal processes, for example, of the type that uses a cascade of centrifugal wheels fed with molten material by a distribution device. Petition 870260094621, dated 09 / 15 / 2026, page 17 / 36 8 / 11 static, as notably described in patents EP 0465310 or EP 0439385. The mineral wool composition described above, however, also allows for fiber formation by so-called "internal" centrifugation, meaning that it uses centrifuges that rotate at high speed and are perforated with holes, significantly reducing the amount of unprocessed fiber. This process is notably described in patents EP 0189354 or EP 0519797. The fiber formation step is thus preferably carried out by internal centrifugation.
[0033] The present invention also relates to the use of a recycled raw material, or a mixture of raw materials comprising at least 8.5% of the latter, for the manufacture of mineral wool having a chemical composition, expressed as a weight percentage of oxides, comprising: SiO2 30-50 % Al2O3 15-35 % CaO 5-25 % MgO 1-25 % Fe2O3 2-15 % Na2O + K2O > 10 % characterized by the fact that the recycled raw material comprises at least 3.5% magnesium, expressed as oxides by weight, and is essentially free of carbonates. The raw material mixture is, on the other hand, preferably free of dolomite and magnesia. The use of the recycled raw material as described above, and more generally of a raw material mixture comprising the latter, allows for a significant reduction in carbon dioxide emissions resulting from the melting of the raw materials.
[0034] The present invention also relates to a mineral wool obtainable by the process described above. Such mineral wool comprises at least 8.5% by weight of a recycled feedstock comprising at least 3% magnesium, expressed as a weight of oxides, said recycled feedstock being essentially free of carbonates, and has a chemical composition, expressed as a weight percentage of oxides, comprising: Petition 870260094621, dated 09 / 15 / 2026, page 18 / 36 9 / 11 SiO2 30-50 % Al2O3 15-35 % CaO 5-25 % MgO 1-25 % Fe2O3 2-15 % Na2O + K2O > 10 %
[0035] The invention also relates to a thermal insulation product comprising mineral wool as described above. Such a product is notably presented in the form of rolls or panels. It can be used, for example, in construction, industry or means of transport, particularly rail or maritime. It is especially suited to applications in which it may be subjected to high temperatures, either continuously (insulation of domestic or industrial ovens or furnaces, fluid transport conduits) or accidentally, in a fire protection role (fire doors, insulation of ships, tunnels or offshore platforms...).
[0036] More generally, the product according to the invention can be used to thermally insulate any type of building, whether commercial or residential (collective or individual). For example, it can be used in exterior insulation systems, for insulating houses with a timber frame, in sandwich panels, in ventilation ducts, etc.
[0037] The characteristics described above in relation to the process according to the invention, particularly with regard to the mineral wool composition, the mixture of raw materials and the recycled raw material, also apply to the other aspects of the invention (uses of the recycled raw material or the mixture of raw materials comprising the latter, the mineral wool or the insulation product) even though these latter are not repeated for the sake of brevity.
[0038] The following examples illustrate the invention in a non-limiting manner. Examples
[0039] Mineral wool products that have a target chemical composition such as Petition 870260094621, dated 09 / 15 / 2026, p. 19 / 36 The 10 / 11 examples presented in Table 1 were made from different mixtures of materials. The raw material mixture in comparative example C1 is a classic mixture comprising dolomite as a magnesium carrier. In example I1 according to the invention, the dolomite has been completely replaced by a recycled material according to the invention. The compositions of the raw material mixtures are detailed in Table 2. Table 3 presents the chemical composition of the recycled material. [Table 1] SiO2 Al2O3 CaO MgO Fe2O3 Na2O K2O TiO2 Other % by weight 42.7 22.9 14.4 1.7 5.6 6.7 4.0 1.0 1.0 [Table 2] Composition of the raw material mixture (kg) C1 I1 Dolomite 63 - Recycled raw material - 100 Bauxite 135.4 45 Limestone 209 238.4 Phonolite 606 606 Nepheline Syenite 65 65 Iron oxide 37.5 34.7 Sodium carbonate 36 33 [Table 3] SiO2 Al2O3 CaO MgO Fe2O3 Na2O Cl F Other % by weight 11.3 68.8 3.2 7.5 4 1.7 0.05 0 3.4 Petition 870260094621, dated 09 / 15 / 2026, page 20 / 36 11 / 11
[0040] During the different production campaigns, no decay was observed during the melting of raw material mixtures of example I1. This has the effect of significantly reducing the amount of spillage and the risk of clogging of the regenerators compared to the use of a raw material mixture of example C1. The reliability of the molten bath composition is also improved compared to example C1. Finally, a 2 to 5% decrease in CO2 emissions was also observed during the melting of raw material mixtures of example I1 compared to that of example C1.
Claims
CLAIMS 1. A process for manufacturing mineral wool having a chemical composition, expressed as a weight percentage of oxides, comprising: SiO2 30-50% Al2O3 15-35% CaO 5-25% MgO Fe2O3 1-25% 2-15% Na2O + K2O > 10% said process comprising: - the supply of a mixture of raw materials; - the melting of said mixture of raw materials to obtain a molten material; - the formation of fibers from the molten material; characterized in that the raw material mixture is in powder form and comprises at least 8.5% by weight of a recycled raw material comprising at least 3% magnesium, expressed as oxides by weight, said recycled raw material being essentially free of carbonates, and in that the raw material mixture is free of dolomite and magnesia, in that the raw material mixture is free of briquettes, and in that the raw material mixture is melted in a fuel-fired furnace and / or by electric melting.
2. Process according to claim 1, characterized in that the chemical composition of the mineral wool comprises less than 0.1% by weight of halogen.
3. Process according to claim 1, characterized in that the recycled feedstock comprises less than 0.9% by weight of halogen.
4. Process in accordance with any of claims 1 to 3, Petition 870260094621, dated 09 / 15 / 2026, page 22 / 36 2 / 2 characterized by the fact that the recycled raw material is fluorine-free.
5. Process according to any one of claims 1 to 4, characterized in that the recycled feedstock comprises up to 2% by weight of metallic aluminum.
6. Process according to any one of claims 1 to 5, characterized in that the recycled raw material has a chemical composition, expressed as a weight of oxides, comprising: Al2O3 50 to 80%, SiO2 2 to 25%, MgO 3 to 20%, Fe2O3 0.5 to 10%.
7. Process according to any one of claims 1 to 6, characterized in that the recycled raw material has a chemical composition, expressed as a weight of oxides, in which the Al2O3 / MgO mass ratio is greater than 8.
8. Process according to any one of claims 1 to 7, characterized in that the raw material mixture comprises at least 1% by weight of bauxite.
9. Process according to any one of claims 1 to 8, characterized in that the fuel-fired furnace is a submerged combustion furnace.
10. Process according to any one of claims 1 to 9, characterized in that fiber formation is carried out by internal centrifugation.