Water saturated carbon molecular peneira membrane, membrana preparation process, gas separation process and mpmc uses

A water-saturated carbon molecular sieve membrane, with tailored pore sizes and pretreated with water vapor, addresses the challenges of selectivity and efficiency in gas separation and solvent dehydration, enhancing permeation and selectivity in membrane reactors.

BR112022010864B1Active Publication Date: 2026-11-17FUNDACION TECNALIA RESEARCH & INNOVATION +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
BR112022010864
Authority / Receiving Office
BR · BR
Patent Type
Patents
Current Assignee / Owner
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing gas separation processes using carbon molecular sieve membranes face challenges in achieving high selectivity and efficiency, particularly in separating hydrogen from methane and solvent dehydration, with a need for improved processes that enhance purity and efficiency in membrane reactors and solvent dehydration.

Method used

The use of a water-saturated carbon molecular sieve membrane, prepared by pretreating the membrane with water vapor to fill its pores, enhances selectivity and permeation of adsorbable gases while reducing the permeation of non-adsorbable gases, achieved by specific pore size distribution and defect-free structure.

Benefits of technology

The water-saturated membrane significantly increases selectivity and permeation efficiency, overcoming external mass transfer limitations and achieving linear hydrogen flow rate dependence on partial pressure, thereby improving gas separation and solvent dehydration processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000063_0000
    Figure 00000063_0000
  • Figure 00000063_0001
    Figure 00000063_0001
  • Figure 00000064_0000
    Figure 00000064_0000
Patent Text Reader

Abstract

CARBON MOLECULAR SIEVE MEMBRANE AND ITS USE IN SEPARATION PROCESSES. This paper presents a water-saturated carbon molecular sieve membrane obtained by: a) providing a hydrophilic carbon molecular sieve membrane (CMSM) comprising pores with a pore size of 0.25 nm to 0.55 nm for molecular sieving, and with a pore size greater than 0.55 nm up to 0.90 nm for adsorption diffusion, and an insignificant number of pores larger than 0.90 nm, such that a graph of N2 permeance versus permeation pressure at room temperature and at a pressure of 1 to 4 bar has a zero or negative slope; and b) wetting the membrane until a water-saturated carbon molecular sieve membrane is obtained. A process for separating a gas from a gas mixture with such a water-saturated membrane is also provided, and its use for solvent dehydration and as a membrane reactor.
Need to check novelty before this filing date? Find Prior Art

Description

1 / 56 “Water-Saturated Carbon Molecular Sieve Membrane, Membrane Preparation Process, Gas Separation Process and Uses of MMS”

[001] This patent application claims the benefit of European Patent Application 19383095.7 filed on December 11, 2019. TECHNICAL FIELD

[002] The present invention relates to the field of gas separation processes. More specifically, it relates to a particular carbon-based molecular sieve membrane pre-treated with water vapor, as well as its use in gas separation processes, solvent dehydration and as membrane reactors. FUNDAMENTALS OF THE INVENTION

[003] Compared to other techniques, membrane separation processes have relatively low energy requirements and low maintenance costs. Two parameters characterize the separation performance of membranes: permeation and selectivity.

[004] Carbon molecular sieve membranes (CMSMs) have been considered the latest generation of membrane technology because they possess a unique microporous structure. The main advantage of carbon molecular sieve membranes is that their pore size distribution (PSD) can be tailored to suit a desired separation. The distribution consists of 0.5-2 nm pores (known as micropores or galleries). Petition 870260086072, dated 08 / 24 / 2026, page 14 / 148 2 / 56 connected by smaller pores, smaller than 0.7 nm in size (known as ultramicropores). Large micropores offer larger permeation and sorption sites for strongly adsorbable molecules, while simultaneously decreasing the passage of less adsorbent molecules (adsorption diffusion mechanism); ultramicropores are responsible for separation by molecular sieving mechanism, which will permeate only molecules smaller than the pore size. The combination of these two transport mechanisms offers the high permeability and selectivity characteristics of these materials.

[005] MA Llosa et al. (Alumina-carbon composite molecular sieve membranes prepared from novolac resin and boehmite. Part I: Studies, characterization and gas permeation studies, in Int. J. Hydrogen Energy, 2015, Vol. 40, pages 5653-5663) first reported the preparation of supported and defect-free 3 μm thick carbon-alumina composite molecular sieve membranes (MPMC-Al) using novolac and boehmite phenolic resins as precursors in alumina tubes (200 nm pore size) in a soak-dry-carburization cycle. The pore size, pore size distribution, and pore hydrophilicity were adjusted by altering the carbonization temperature of the membrane (MA Llosa et al. Composite-alumina-carbon molecular sieve membranes prepared from novolac resin and boehmite. Part II: Effect of the carbonization temperature on the gas permeation properties, in Int. J.(Hydrogen Energy, 2015, Volume 40, pages 3485-3496). In this way, they reported the influence. Petition 870260086072, dated 08 / 24 / 2026, page 15 / 148 3 / 56 of the carbonization temperature affects the pore size distribution and permeation properties of these carbon-alumina composite molecular sieve membranes (MCMP-Al) carbonized at temperatures from 450 °C to 1000 °C. The selectivity and permeation properties of the membrane can also be controlled by altering the amount of water adsorbed in the pores, through adjustment of the permeation temperature.

[006] Separating hydrogen present at low concentrations in a mixture with methane is of great interest for the anticipated hydrogen economy. Hydrogen can be stored and distributed using existing natural gas networks. For safety reasons, the hydrogen content in distribution gas mixtures must be low (approximately 10%). Therefore, the hydrogen must be separated at the end-user site.

[007] On the other hand, researchers are continuously working on developing better processes, catalysts, and adsorbents to increase the efficiency of petrochemical and fuel production, which are highly dependent on separation processes and their improvement. A good alternative to solve this problem is to develop membrane reactors. A membrane reactor (MR) is a device that simultaneously performs a reaction (steam reforming, dry reforming, autothermal reforming, methanol synthesis, etc.) and membrane-based separation in the same physical device. Continuous extraction of one of the products can alter the equilibrium, increasing the Petition 870260086072, dated 08 / 24 / 2026, page 16 / 148 4 / 56 efficiency and selectivity, compared to a traditional system.

[008] Furthermore, highly concentrated and anhydrous solvents are of great importance in the chemical industry, so efficient dehydration processes are being developed. In this context, hydrophilic carbon molecular sieve membranes are excellent candidates.

[009] Therefore, there is still a need for improved processes, through the use of carbon molecular sieve membranes (CMSMs), which allow for higher purities in gas separation processes and better efficiencies in membrane reactors and solvent dehydration. SUMMARY OF THE INVENTION

[010] The inventors discovered that pretreating a certain carbon molecular sieve membrane (CMSM) with water vapor, to obtain a water-saturated membrane before carrying out a gas separation process, significantly increases the membrane's selectivity, and this is done in a reproducible manner. Particularly, in the water-saturated membrane, filling the pores with water helps to increase the permeation of adsorpable gases (adsorption-diffusion mechanism) and, at the same time, increases selectivity by decreasing the permeation of non-adsorbable gases.

[011] Therefore, one aspect of the present invention relates to the water-saturated carbon molecular sieve membrane obtained by the following steps: Petition 870260086072, dated 08 / 24 / 2026, page 17 / 148 5 / 56 i) providing a hydrophilic carbon molecular sieve membrane (CMSM) comprising pores with a pore size of 0.25 nm to 0.55 nm for molecular sieving, and with a pore size greater than 0.55 nm up to 0.90 nm for adsorption diffusion, and an insignificant number of pores larger than 0.90 nm, such that the CMSM has an insignificant number of pores larger than 0.90 nm, such that a graph of N2 permeance versus permeation pressure at room temperature and at a pressure of 1 to 4 bar has a zero or negative slope; and ii) humidifying the MPMC prepared in step i) to obtain a water-saturated MPMC, through the following steps: treatment of MPMC with water vapor at a temperature of 5 °C to 180 °C and at atmospheric pressure and a relative humidity greater than 95%, such as 99%, for a period of time, such that, after further treatment with water vapor, the permeation flux of a non-adsorbable gas, such as N2 or He, at 4 bar at the temperature at which the MPMC was treated with water vapor, is constant for a given period, such as 3 hours; or alternatively, by exposing the MPMC to a stream of water-saturated N2 or He gas by bubbling the gas at a temperature of 5 °C to 180 °C in a tank filled with water, such that after further exposure to the water-saturated N2 or He gas stream, the permeation flux of a non-adsorbable gas, such as N2 or He, at Petition 870260086072, dated 08 / 24 / 2026, page 18 / 148 6 / 56 bars and at the mentioned temperature, be constant for a given period, such as, for example, a period of 3 hours.

[012] The MPMC membranes used in step i) comprise pores of specific pore sizes, as defined in this document, and a “defect-free structure,” i.e., a structure that does not exhibit defects that could affect the gas separation properties of the membrane (i.e., its permeability and selectivity). An MPMC comprising pores whose pore size is considered “defect-free” is when the number of pores larger than 0.90 nm is negligible, i.e., when a graph of N2 permeance versus permeation pressure at room temperature and at a pressure of 1 to 4 bar has a zero or negative slope. The combination of these characteristics, i.e., having pores with the mentioned pore size and the absence of defects in the porous structure, allows obtaining the intended effect when wetting the MPMC, as defined in step ii).

[013] Another aspect of the present invention relates to a process for preparing a water-saturated carbon-alumina molecular sieve membrane (water-saturated Al-MCM) comprising: i) Preparation of a hydrophilic MPMC-Al using the following steps: - provide a porous support ο-Α^Οι; - Prepare a solution containing 5% to 20% by weight of phenol-formaldehyde resin, 0.5% to 5% by weight of formaldehyde, 0.1% to 2% by weight of ethylenediamine, 0.1% Petition 870260086072, dated 08 / 24 / 2026, p. 19 / 148 7 / 56 at 5% by weight of boehmite in N-methyl-2-pyrrolidone, and heat the solution (e.g., from 80 °C to 110 °C, for 30 minutes to 3 hours) to perform a pre-polymerization process to obtain a coating solution; - to coat the porous substrate «-Al2Oa» in the coating solution by immersion, in order to obtain a coated substrate; - Dry the coated substrate at a temperature of 70 °C to 120 °C to complete the polymerization process; - Carbonize the dry coated support at a carbonization temperature of 450 °C to 750 °C, to obtain an MPMC-Al; ii) humidify the MPMC-Al prepared in step i) to obtain a water-saturated MPMC-Al by following these steps: - Treat the MPMC-Al with steam at a temperature of 5 °C to 180 °C, at atmospheric pressure and a relative humidity greater than 95%, such as 99%, for a period of time, in such a way that, after the additional steam treatment, the permeation flux of a non-adsorbable gas, such as N2 or He, at 4 bar and at the temperature at which the MPMC was treated with steam, is constant for a given period, such as 3 hours; or Alternatively, by exposing the MPMC to a stream of water-saturated N2 or He gas, by bubbling the gas at a temperature of 5 °C to 180 °C in a tank filled with water, such that, after further exposure to the water-saturated N2 or He gas stream, the permeation flow of a non-adsorbable gas, such as N2 or He, at 4 Petition 870260086072, dated 08 / 24 / 2026, page 20 / 148 8 / 56 bars and at the mentioned temperature, be constant for a given period, such as, for example, a period of 3 hours.

[014] Another aspect of the present invention relates to a water-saturated MPMC-Al, which can be obtained by the process defined above.

[015] Another aspect of the present invention relates to the process for separating a gas from a mixture of gases, wherein said process comprises: a) supply of a water-saturated membrane as defined above and below; b) supply of a gas mixture comprising at least two gases; c) Feeding the water-saturated MPMC with the gas mixture at a temperature of 5 °C to 300 °C to obtain a retentate and a permeate, wherein the feed is carried out at a pressure such that the partial pressure of the gas in the retentate is greater than the partial pressure of the gas in the permeate and such that the membrane is still a water-saturated membrane, i.e., a difference in permeation is observed compared to the same MPMC without having been subjected to a humidification step, to obtain a water-saturated membrane under the feed temperature and pressure.

[016] Surprisingly, as shown in the examples, the water-saturated MPMC is not affected by external mass transfer limitations (concentration polarization) when working with gas mixtures. Thus, Petition 870260086072, dated 08 / 24 / 2026, page 21 / 148 9 / 56 For example, in the separation of hydrogen present in a gas mixture, the dependence of the difference in the partial pressure of hydrogen and the hydrogen flow rate is almost linear, regardless of the H2 concentration in the mixture.

[017] Another aspect of the present invention relates to the use of a water-saturated MPMC, as defined above and below, for the separation of a gas from a mixture of gases.

[018] The inventors also realized that the water-saturated MPMC, as defined above and below, is also useful for the dehydration of organic solvents and as membrane reactors. Thus, these uses are also part of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[019] Figure 1 shows the micropore size distribution of carbonized carbon membranes at: a) 450 °C and 650 °C; b) 550 °C and 750 °C. PM: Molecular sieving region. DA: Adsorption diffusion region.

[020] Figure 2 shows the changes undergone in MPMC: i) during carbonization, functional groups are removed, leaving active carbon groups, which can react with active molecules; then, ii) water can be chemisorbed (i.e., active atoms react with water), producing oxygen-containing functional groups, making the pores hydrophilic; then, iii) the hydrophilic groups can absorb water, physically filling the pores, reducing the pore size. Petition 870260086072, dated 08 / 24 / 2026, page 22 / 148 10 / 56

[021] Figure 3 shows (a, b) the permeation of N2 at a pressure difference of 400 kPa, heating time 0.7 °C min-1.

[022] Figures 4a and 4b show the derivative of the polynomial fit of the flow from Figures 3a and 3b, respectively.

[023] Figure 5 shows the N2 and H2 permeability of an Al-MCP-MPC carbonized at 600 °C, before and after wetting (outside the reactor).

[024] Figure 6 shows the H2 and CH4 permeation results of dry MPMC-550 and MPMC-600 membranes obtained as in Example 3 at 20 °C, with the respective Robeson upper limit plot.

[025] Figure 7 shows a comparison of the hydrogen flow rate permeation of a mixture consisting of 50% H2 - 50% CH4, using a dry MPMC-550 (after water desorption at 150 °C) or a humidified (wet) MPMC-550. Permeation temperature: 20 °C.

[026] Figure 8 shows a comparison of the hydrogen purity of the permeate obtained by permeation of a mixture consisting of 50% H2 - 50% CH4, using a dry MPMC-550 (after desorption at 150 °C) and a humidified (wet) MPMC-550. Permeation temperature: 20 °C.

[027] Figure 9 shows the comparison between the hydrogen flow rates of two mixtures consisting of H2CH4 containing 10% and 50% hydrogen, respectively, at 20 °C, 35 °C, 50 °C and 70 °C, in a humidified MPMC-550. Petition 870260086072, dated 08 / 24 / 2026, page 23 / 148 11 / 56

[028] Figure 10 shows the comparison between the purity of hydrogen in the permeate obtained by permeating two H2-CH4 mixtures containing 10% and 50% hydrogen, respectively, at 20 °C, 35 °C, 50 °C and 70 °C, using a humidified MPMC-550.

[029] Figure 11 shows the comparison between the hydrogen permeation flow rate of two H2CO2 mixtures containing 10% and 50% hydrogen, respectively, at 20 °C, 35 °C, 50 °C, in a humidified MPMC-550.

[030] Figure 12 shows the comparison between the purity of hydrogen in the permeate obtained by permeating two H2-CO2 mixtures containing 10% and 50% hydrogen, respectively, at 20 °C, 35 °C, 50 °C and 70 °C, using an MPMC-550 humidification device.

[031] Figure 13 shows the comparison between the hydrogen flow rate of two H2-N2 mixtures containing 10% and 50% hydrogen, respectively, at 20 °C, 35 °C, 50 °C and 70 °C, in a humidification MPMC-550.

[032] Figure 14 shows the comparison between the purity of hydrogen in the permeate obtained by permeating two H2-N2 mixtures containing 10% and 50% hydrogen, respectively, at 20 °C, 35 °C, 50 °C and 70 °C, using an MPMC-550 humidification device.

[033] Figure 15 shows the comparison between the hydrogen flow rate in an H2-CH4 mixture containing 10% hydrogen at 20 °C, 50 °C, 70 °C and 100 °C in a dry MPMC-600 and in a humidified MPMC-600. Petition 870260086072, dated 08 / 24 / 2026, page 24 / 148 12 / 56

[034] Figure 16 shows the comparison between the purity of hydrogen in the permeate obtained by permeating an H2-CH4 mixture containing 10% hydrogen at 20 °C, 50 °C, °C and 100 °C, using a dry MPMC-600 and a humidified MPMC-600.

[035] Figure 17 shows the relative increase in purity obtained under the wetted membrane condition.

[036] Figure 18 shows an example of the effect of flux against the partial pressure difference for a Pd-based membrane (flux ~ AP0.5) and for an Al-MCP (flux is proportional to AP), considering that they have the same permeance (mol-m-2s-1-Pa-1) at 1 bar pressure.

[037] Figure 19 shows the hydrogen permeate flux for a binary mixture of H2 / CH4 at 400 °C with 100-50% H2 purity by volume, as a function of the difference between the square root of the partial pressure of H2 in the retentate (on average) and the permeate side for a supported Pd-Ag membrane.

[038] Figure 20 shows the hydrogen flux rate at different hydrogen concentrations in the H2-CH4 inlet mixture tested at 400 °C for a supported Pd-Ag membrane,

[039] Figure 21 shows the hydrogen purity at different hydrogen concentrations in the H2-CH4 input mixture tested at 400 °C for a supported Pd-Ag membrane.

[040] Figure 22 shows the hydrogen flux as a function of the percentage of hydrogen in the mixture for Petition 870260086072, dated 08 / 24 / 2026, page 25 / 148 13 / 56 H2 / N2, H2 / CO2 and H2 / CH4 at 400 °C, 3 bar total pressure and vacuum on the permeate side, for a supported Pd-Ag membrane.

[041] Figure 23 shows the hydrogen flow rate as a function of the hydrogen partial pressure difference for various H2 / CH4 mixtures, at a working temperature of 20 °C, when testing an MPMC-550, after exposure to ambient humidity.

[042] Figure 24 shows: a) a sketch of a hydrophilic pore filled with water; b) water permeability at various temperatures and pressures of the carbonized MPMC-Al of Example 2.2 at 550 °C.

[043] Figure 25 shows the water permeation at various temperatures and 3 bar pressure differences for the MPMC-Al membranes of Example 2.2 carbonized at different temperatures,

[044] Figure 26 shows the gas / water selectivity against various gases as a function of the permeation temperature of the MPMC-Al membranes of Example 2.2 carbonized at different temperatures. DETAILED DESCRIPTION OF THE INVENTION

[045] All terms and expressions used herein in this patent application, unless otherwise indicated, shall be understood in their common meaning as known in the art. Other terms of more specific definitions, as used in this patent application, are those set forth below and shall be applied uniformly throughout the descriptive report and Petition 870260086072, dated 08 / 24 / 2026, page 26 / 148 14 / 56 claims, unless an expressly established definition provides a broader definition.

[046] The expression “permeation flux” is defined as the volume of gas that passes through the membrane per unit of time. This value is determined experimentally with a soap flow meter.

[047] The expression “permeation flux” is defined as the volume that flows through the membrane per unit area per unit time. This value is calculated from the “permeation flux” divided by the membrane area.

[048] The term “permeability” is defined as the volume of feed gas that passes through a unit area of ​​the membrane in a unit time and under a unit pressure gradient. The common unit used in MPMC is mol-m2s-1-Pa-1. This value is calculated from the “permeation flux” divided by the pressure difference between the retentate and the permeate.

[049] The term “permeability” is defined as the flow of material transport through the membrane per unit of motive force per unit of membrane thickness.

[050] The expression “permeability selectivity” or ideal selectivity related to a gas refers to the ratio of the permeability of two gases at the same temperature.

[051] The expression “carbon-alumina composite molecular sieve membrane” or “MPMC-Al” refers to a carbon membrane with alumina nanoparticles dispersed in the carbon matrix. Petition 870260086072, dated 08 / 24 / 2026, p. 27 / 148 15 / 56

[052] The expression “water-saturated MPMC” or “hydrated MPMC” refers to an MPMC (including an Al-supported MPMC) containing an amount of water corresponding to that which would be contained in an MPMC that has been treated at a temperature of 5 °C to 180 °C, such as ambient temperature, and at atmospheric pressure and relative humidity greater than 95%, such as 99%, with water vapor, for a period, in such a way that, after further treatment with water vapor, the permeation flux of a non-adsorbable gas, such as N2 or He at 4 bar at the temperature at which the MPMC was treated with water vapor, is constant for a given period, such as a period of 3 hours.Alternatively, a “water-saturated MPMC” can be obtained by exposing the MPMC to a stream of water-saturated N2 or He gas by bubbling the gas at a temperature of 5 °C to 180 °C, such as room temperature, in a tank filled with water, in such a way that, after further exposure to the water-saturated N2 or He gas stream, the permeation flux of a non-adsorbable gas, such as N2 or He, at 4 bar and the aforementioned temperature, is constant for a given period, such as a period of 3 hours.

[053] In general, and particularly at temperatures above 180 °C, a water-saturated MPMC must contain at least an amount of water equivalent to that which would be contained in an MPMC that has undergone a humidification treatment carried out at the temperature and pressure at which permeation will be carried out in order to fill the Petition 870260086072, dated 08 / 24 / 2026, page 28 / 148 16 / 56 pores filled with water until there is no more water retention, such that, due to the presence of water in the pores, a difference in permeation is observed compared to the same MPMC without having been subjected to such a humidification process.

[054] The expression “hydrophilic MPMC” refers to an MPMC that, before being humidified to obtain a water-saturated MPMC, has a N2 permeability at 300 °C and a pressure difference of 4 bar greater than 7 x 10-9 mol m2s-1Pa-1 and, after being humidified to obtain a water-saturated MPMC, has a N2 permeability at room temperature and a pressure difference of 1 bar less than 1 x 10-9 mol m2s-1Pa-1.

[055] Membrane processes are characterized by the fact that a feed stream, which is a mixture of gases, is divided into two streams: the retentate and the permeate. The retentate is the part of the feed that does not pass through the membrane, while the permeate is the part of the feed that passes through the membrane, i.e., the separated gas. To separate a gas from a mixture of gases, the partial pressure of the gas in the retentate must be greater than the pressure of the permeate.

[056] Thus, the permeation of a desired gas will depend on the difference in the partial pressure of that gas in the retentate and in the permeate. For example, for a feed that is a mixture consisting of 10% H2 and 90% CH4, if the pressure in the permeate is atmospheric pressure (1 bar), the pressure in Petition 870260086072, dated 08 / 24 / 2026, p. 29 / 148 17 / 56 The feed pressure must be greater than 10 bar, meaning the partial pressure of H2 in the feed must be greater than 1 bar.

[057] The expression “pressure difference” refers to the difference in gas pressure in the retentate and gas pressure in the permeate.

[058] The expression “partial pressure difference” for a given gas refers to the difference in the partial pressure of the gas in the retentate and the partial pressure of the gas in the permeate.

[059] The term “negligible” refers to a value that coincides with zero in the context of measurement precision or that is less than a defined limit value, which, for example, takes into account a deviation from zero, which is hardly avoidable for structural reasons or which has no significant effect on performance, in terms of permeability and selectivity of the MPMC. To verify whether the MPMC has a “negligible” amount of pores larger than 0.90 nm, i.e., whether it has a defect-free structure, the MPMC must be able to present a graph of N2 permeance versus permeation pressure at room temperature and at a pressure of 1 to 4 bar with zero or negative slope.

[060] The expression “room temperature” refers to a temperature of approximately 20 °C to approximately 25 °C.

[061] The expression “atmospheric pressure”, as used in this document, is intended to refer to a Petition 870260086072, dated 08 / 24 / 2026, page 30 / 148 18 / 56 atmospheric pressure substantially at 101,325 kPa (i.e., 760 mm Hg) ± 15 kPa.

[062] As used in this document, the term percentage or concentration of a gaseous component in a gas mixture refers to the amount by volume of the single gaseous component relative to the total volume of the gas mixture or, if specifically mentioned, of another gaseous component or components of the gas mixture.

[063] Note that, as used in this descriptive report and in the attached claims, the singular forms a, an, the and include plural referents, unless the context clearly indicates otherwise.

[064] As mentioned above, the present invention relates to a water-saturated carbon molecular membrane, as described above.

[065] These carbon membranes have a porous structure whose permeation mechanism is the result of molecular sieving (pore range of 0.25-0.55 nm) and / or surface diffusion (0.5-0.90 nm). MPMC membranes, such as MPMC-Al membranes, are produced by carbonization of a polymeric precursor under an inert atmosphere or vacuum, for example, at a temperature of 250 °C to 2500 °C, or 450 °C to 1500 °C, particularly 500 °C to 800 °C (cf. Llosa MA et al. (Part I) 2015; Campo MC et al. 2010). Examples of polymeric precursors include, but are not limited to, polyimides, polyfurfuryl alcohol, phenolic resins, cellulose, cellulosic derivatives, and poly(vinylidene chloride). Phenolic resins, such as, for example Petition 870260086072, dated 08 / 24 / 2026, p. 31 / 148 19 / 56 For example, resol and novolac resins are desirable precursors for preparing MPMC membranes, as they have the advantage of being inexpensive and having a high carbon yield, withstanding high temperatures without losing their shape.

[066] Phenolic resins are a product of the polycondensation reaction of phenol with formaldehyde; their structure and properties depend on the formaldehyde / phenol ratio (F / F), catalyst, pH, and temperature. There are two forms of phenolic resins: resol and novolac. Resol resins are a product of basic catalysis in excess formaldehyde (F / F>1). Novolac resins are obtained in an acidic medium and the amount of formaldehyde is lower, generally with a formaldehyde / phenol ratio (F / F) of approximately 0.75-0.85.

[067] In one embodiment of the process for preparing water-saturated MPMC-Al of the present invention and water-saturated MPMCAl obtained by this process, the phenol formaldehyde resin is a novolac resin.

[068] In another embodiment of the process for preparing the water-saturated MPMC-Al of the present invention and the water-saturated MPMC-Al obtained by this process, optionally, in combination with one or more features of the particular embodiments defined above, the carbonization temperature is from 450 °C to 700 °C, particularly from 500 °C to 650 °C, such as, for example, 550 °C or 600 °C.

[069] Before carbonization, for self-supporting membranes, the polymeric precursor is molded (e.g., films, hollow fiber); for the supported membrane, Petition 870260086072, dated 08 / 24 / 2026, page 32 / 148 20 / 56 They are generally produced by immersing (coating) a porous support in a solution containing the polymeric precursor.

[070] As mentioned above, membrane humidification is performed to obtain a MPMC containing at least an amount of water corresponding to that which an MPMC would contain that was: - treated with water vapor at a temperature of 5 °C to 180 °C (for example, at 20 °C, 25 °C, 40 °C, 70 °C, 100 °C or 120 °C), atmospheric pressure and relative humidity greater than 95% (particularly 99%) for a period, such that, after further treatment with water vapor, the membrane gas permeation flux at the temperature at which the MPMC was treated with water vapor and at 4 bar for a non-adsorbable gas, such as N2 or He, is constant for a given period, such as for 3 hours; or - exposed to a flow of water-saturated N2 or He gas by bubbling the gas at a temperature of 5 °C to 180 °C (for example, at 20 °C, 25 °C, 40 °C, 70 °C, 100 °C or 120 °C), in a tank filled with water, in such a way that, after further exposure to the water-saturated N2 or He gas flow, the permeation flux of a non-adsorbable gas, such as N2 or He, at 4 bar and the aforementioned temperature, is constant for a given period, such as a period of 3 hours. Petition 870260086072, dated 08 / 24 / 2026, page 33 / 148 21 / 56

[071] The permeation flux was determined with a soap flow meter under the temperatures and pressure mentioned.

[072] In another embodiment of the water-saturated carbon molecular sieve membrane of the present invention, optionally, in combination with one or more features of the particular embodiments defined above, under temperatures above 180 °C (such as, for example, 200 °C, 250 °C or 300 °C), the membrane is humidified to obtain a CMM containing at least an amount of water corresponding to that which would be contained in a CMM that has been subjected to a humidification treatment carried out under temperature and pressure under which permeation will be carried out, in order to fill the pores with water until there is no more water, in such a way that, due to the presence of water in the pores, a difference in permeation is observed, compared with the same CMM without having been subjected to such a humidification process.

[073] In one embodiment of the present invention, the humidification of the membrane is carried out under ambient temperature, atmospheric pressure and relative humidity greater than 95%, such as 99%, for a period, in such a way that, after further treatment with water vapor, the permeation flux of the membrane gas at the temperature at which the MPMC was treated with water vapor and at 4 bar for a non-adsorbable gas such as N2 or He, is constant for a given period such as 3 hours. Petition 870260086072, dated 08 / 24 / 2026, page 34 / 148 22 / 56

[074] In one embodiment of the water-saturated carbon molecular sieve membrane of the present invention, optionally, in combination with one or more features of the particular embodiments defined above, the MPMC is an alumina-carbon composite molecular sieve membrane (MPMC-Al). In particular, MPMC-Al has a nitrogen content of 0.1% by weight to 4.0% by weight, an alumina content of 2.5% to 50%, and a carbon content of 50% by weight to 95% by weight relative to the total weight of the membrane.

[075] MPMC-Al membranes can be prepared using the materials and immersion-drying-carbonization method on porous alumina supports described in Llosa MA et al. (Part I) 2015 (see Experimental section on page 5655), but the carbonization temperature is selectable at will. Other examples of MPMC-Al are reported, for example, by Teixeira et al., 2011, Teixeira et al., 2012, Rodrigues et al., 2014. CHARACTERIZATION OF PORE SIZE

[076] The pore size and pore size distribution of carbon molecular sieve membranes were calculated using data obtained from CO2 adsorption equilibrium at 0 °C. The CO2 adsorption equilibrium isotherm was acquired by the gravimetric method on a Rubotherm magnetic suspension balance with a precision of 10-5 mg. Details on how to determine the pore size distribution of MPMC membranes can be found in Nguyen C. and Do. DD, 1999, and Nguyen C., et al., 2003. Petition 870260086072, dated 08 / 24 / 2026, page 35 / 148 23 / 56

[077] Pre-treatment of the membrane with water vapor to obtain a water-saturated MPMC can be carried out inside or outside the permeator. Pre-treatment with steam outside the permeator.

[078] For a water-saturated Al MPMC, a hydrophilic MPMC, as defined above, is introduced at a temperature of 5 °C to 180 °C, such as, for example, 5 °C to 120 °C, particularly at room temperature and relative humidity above 95%, such as 99%, in a closed container containing water, until there is no more water to fill the pores.

[079] To determine when the membrane is saturated with water, the membrane gas permeation flux at the mentioned temperature, such as room temperature, and at 4 bar, is monitored until it is constant over a given period, such as a period of 3 hours. The gas used is a non-adsorbable gas at the permeation temperature (e.g., room temperature), such as N2 or He. Pre-treatment with steam inside the permeator.

[080] As an alternative method for a water-saturated Al MPMC, the MPMC is introduced into a permeator and the permeator is fed, preferably at ambient temperature, with: (i) a water-saturated gas stream obtained, for example, by bubbling the gas stream into a tank filled with water before feeding it into the permeator; or (ii) water vapor or a mixture of gases. Petition 870260086072, dated 08 / 24 / 2026, page 36 / 148 24 / 56 containing water. Treatment time can range from 1 minute to several hours.

[081] After treatment, the gas flow of the non-adsorbable gas (i.e., N2 or He) at 4 bar is measured. The gas treatment and permeation cycles are repeated until the gas permeation is constant over a period of 3 hours. USES OF THE WATER-SATURATED MPMC OF THE INVENTION

[082] As mentioned above, the present invention also relates to a process for separating a gas in a gas mixture, by means of the use of a water-saturated MPMC, as defined above, having some specific characteristics.

[083] Therefore, a MPMC with some specific characteristics of pore size, pore size distribution and hydrophilicity is subjected to a pre-treatment of humidification until it is saturated with water (under the permeation pressure and temperature conditions). The gas mixture comprises at least two gases and is fed to the water-saturated MPMC at a pressure such that the partial pressure of the gas in the retentate is greater than the partial pressure of the gas in the permeate and such that the membrane is still a water-saturated membrane, i.e., a difference in permeation is observed compared to the same MPMC without having been subjected to a humidification step, to obtain a water-saturated membrane under the feed pressure and temperature. The process can be carried out at a temperature of 5 °C to 300 °C. Petition 870260086072, dated 08 / 24 / 2026, page 37 / 148 25 / 56

[084] In one embodiment of the present invention, optionally, in combination with one or more features of the particular embodiments defined above, step (c) is carried out at a temperature of 5 °C to 250 °C, 5 °C to 120 °C, 15 °C to 120 °C, 15 °C to 100 °C, 15 °C to 70 °C, or 20 °C to 50 °C, such as, for example, 40 °C. In a particular embodiment of the present invention, step (c) is carried out at room temperature.

[085] The gas, pure or in the form of a mixture, can be fed into the permeator via digital mass flow controllers, while the pressure can be controlled with a digital backpressure regulator. The maximum retentate pressure can be, for example, 40 bar, while the permeate can be operated at different pressures down to vacuum (by means of the use of a vacuum pump). Several thermocouples can be used to record temperature profiles along the permeator.

[086] The separation of gases in the hydrophilic membranes of the present invention is based on molecular sieving (MS; gases smaller than the pores will permeate) and adsorption diffusion (AD; difference in affinity of gases with the water present in the pores). The pores of the MPMC of the present invention are divided into two groups (Figure 1a): a) pores from 0.25 nm to 0.55 nm, in which separation is done by molecular sieving; and b) pores with a pore size greater than 0.55 nm up to 0.90 nm, in which water is adsorbed. In the adsorption diffusion (AD) region, the water adsorbed in the pores reduces the pore size; the amount of water adsorbed will depend on the temperature and, consequently, Petition 870260086072, dated 08 / 24 / 2026, page 38 / 148 26 / 56 also depends on the size of the pores. Gases will pass through according to their size (smaller ones will pass through more quickly), and gases with greater interaction (adsorption) with water in the pores (gases with more adsorption) will permeate preferentially. The interaction with water will depend on the polarity of the gases; gaseous gases with a dipole moment (i.e., water) will have more permeation. When the gases are non-polar, gases with greater polarizability will permeate more quickly (example: CO2 and H2 over He). Polarizability [m3] Kinetic diameter [nm] He 2 0.26 H 8.2 0.29 Co2 26.3 0.33 Ar 16.6 0.364 N2 17.7 0.365 Ch4 26 0.38

[087] The polarizability of an atom or molecule is a measure of the ease with which electrons and nuclei can be displaced from their average positions, forming an instantaneous dipole. The kinetic diameter expresses the probability of a molecule in a gas colliding with another molecule. This is an indication of the size of the molecule as a target. The polarizability and kinetic diameter of gases can be found in chemical and physical data textbooks.

[088] In another embodiment of the present invention, optionally, in combination with one or more features of the particular embodiments defined above, the at least two gases have a polarizability of 2 to 27, or of 2 to Petition 870260086072, dated 08 / 24 / 2026, p. 39 / 148 27 / 56 26.3 and at least one of the at least two gases has a kinetic diameter less than 0.55 nm. If more than two gases have a kinetic diameter less than 0.55 nm, separation will occur when: the difference in kinetic diameter between the at least two gases is equal to or greater than 0.01 nm; the difference in polarizability between the at least two gases is equal to or greater than 1 m3; or both.

[089] In particular, at least two gases are selected from the group consisting of He, H2O, Ne, H2, NO, Ar, NH3, N2, O2, CO2, CO, CH4, C2H4, C2H6, propene, C3H8 (propane), H2S, methanol, ethanol, propanol, dioxane, dimethylformamide, dimethyl sulfoxide, acetone, and N-methyl-2-pyrrolidone. Examples of gases with a kinetic diameter greater than 0.55 nm are n-butane or isobutane. Examples of solvents with a kinetic diameter greater than 0.55 nm are CHCl3, CHCl2, methanol, ethanol, dimethyl ether, dimethyl carbonate, acetone, acetonitrile, dioxane. In particular, at least two gases are a mixture selected from the group consisting of H2 / CH4; H2 / N2; H2 / CO2; CO2 / CH4; CO2 / N2; O2 / N2; and biogas.

[090] In a particular embodiment of the present invention, optionally, in combination with one or more features of the particular embodiments defined above, the gas mixture comprises 5% to 20% H2 and 95% to 80% CH4, particularly approximately 10% H2 and approximately 90% CH4, wherein step c) is carried out at a hydrogen partial pressure difference equal to or greater than 3 bar, such as, for example, 3 bar. Petition 870260086072, dated 08 / 24 / 2026, p. 40 / 148 28 / 56 at 8 bars, and at a temperature of 40 °C or lower, such as 20 °C or room temperature.

[091] Advantageously, unlike other known processes, the water-saturated MPMC of the present invention allows H2 to be separated from a mixture with CH4 at low temperature and, consequently, the purity of the permeate is increased.

[092] In a particular embodiment of the present invention, optionally, in combination with one or more features of the particular embodiments defined above, the at least two gases are CO2 and N2. In particular, the gas mixture comprises 10% to 20% CO2 and 65% to 75% N2, particularly approximately 15% CO2 and approximately 70% N2.

[093] In a particular embodiment of the present invention, optionally, in combination with one or more features of the particular embodiments defined above, the at least two gases are H2 and CO2. In particular, the gas mixture comprises 55% to 65% H2 and 30% to 40% CO2, more specifically, approximately 60% H2 and approximately 35% CO2.

[094] In another embodiment of the present invention, optionally, in combination with one or more features of the particular embodiments defined above, the gas mixture is anhydrous.

[095] In another embodiment of the present invention, optionally, in combination with one or more features of the particular embodiments defined above, the mixture of Petition 870260086072, dated 08 / 24 / 2026, page 41 / 148 29 / 56 gases comprising at least two gases is biogas, and CO2 is removed from the biogas).

[096] As mentioned above, another aspect of the present invention relates to the use of a water-saturated MPMC, as defined above, for the separation of a gas from a gas mixture.

[097] Biogas is a mixture of gases produced by the decomposition of organic matter in the absence of oxygen (anaerobically), comprising methane and carbon dioxide. Specifically, biogas is a mixture of gases containing mainly methane and carbon dioxide and small amounts of other gases, such as H2, H2S, N2 and water vapor. The use of biomethane is preferable to biogas because it increases the energy density of the fuel source and can be used directly in all existing and installed plants and can also be sent to the natural gas network.

[098] In another embodiment of the present invention, the use of water-saturated MPMC is intended for biogas enhancement, i.e., to remove CO2 from biogas.

[099] In another embodiment of the present invention, the use of water-saturated MPMC is intended for the removal of CO2 from a gas mixture comprising at least 50% nitrogen. In particular, the gas mixture comprises 5% to 10% CO2 and 65% to 75% N2, more specifically, approximately 5% CO2 and approximately 70% N2. Petition 870260086072, dated 08 / 24 / 2026, page 42 / 148 30 / 56

[0100] In another embodiment of the present invention, the use of the water-saturated MPMC is intended for the separation of H2 from a gas mixture also comprising CO2, particularly from the product of pre-combustion, after the water-gas displacement reaction, wherein the gas mixture comprises 50% to 70% H2 and 50% to 30% CO2; or it is intended for the separation of alkanes from alkenes, such as, for example, C2H4 from C2H6, for example, in a gas mixture comprising 30-70% C2H4 and 70-30% C2H6; or propane from propene, for example, in a gas mixture comprising 30-70% propene and 70-30% propane; or propane, propene or a mixture of these with butane, for example, in a gas mixture comprising 70-30% propane, propene or a mixture thereof and 30-70% butane.

[0101] As mentioned above, another aspect of the present invention relates to the use of a water-saturated MPMC, as defined above, for solvent dehydration, i.e., for the removal of water from an organic solvent, to obtain an organic solvent containing 0.1% to 1% water. Examples of organic solvents include methanol, ethanol, propanol, n-butanol, isobutanol, tert-butanol, acetone, dimethyl ether, dimethyl carbonate, tetrahydrofuran, acetonitrile, dioxane, acetic acid, and ethyl acetate.

[0102] In the solvent dehydration process, water gas is passed through the pores by applying a vacuum from the permeate side of the membrane. Because solvent molecules are larger than or equal to the largest pore for molecular sieving (>0.55 nm) and water is very small, only water will pass through. Furthermore, Petition 870260086072, dated 08 / 24 / 2026, page 43 / 148 31 / 56 Water is preferentially adsorbed in the hydrophilic pores of the adsorption diffusion (DA) region of the pores, blocking the passage of other less hydrophilic molecules. Dipolar aprotic solvents are used in organic synthesis and in the dissolution of polymers, where very small amounts or traces of water can be harmful.

[0103] As mentioned above, another aspect of the present invention relates to the use of a water-saturated MPMC, as defined above, as a membrane reactor. The water-saturated MPMC of the present invention can be used in process intensification for the in situ removal of water during catalytic reactions in the chemical, petrochemical, food and cosmetic sectors. Particularly in processes for the production of methane, methanol, dimethyl ether, dimethyl carbonate (DMC), or other organic solvents, in which water is produced in the reactions.Examples of processes in which the water-saturated MPMC of the present invention can be used as a membrane reactor are the reaction of CO2 and H2 to produce CH4; the synthesis of esters by reacting alcohols with carboxylic acids; biodiesel and biolubricants; methanol produced from CO2 and H2; dimethyl ether obtained by dehydration of methanol or by direct synthesis from CO2 and H2; and the synthesis of dimethyl carbonate from CO2 and methanol. By using the water-saturated MPMC of the present invention, water is removed from the reaction product and the production of the compound of interest, such as esters and oxygenated solvents, is achieved. Petition 870260086072, dated 08 / 24 / 2026, p. 44 / 148 32 / 56

[0104] The water-saturated MPMCs of the present invention have great potential because they are easier to prepare, are cheaper, and have better permeation properties than zeolite membranes that are currently being studied in the field of membrane reactors, especially with regard to the reaction of CO2 and H2.

[0105] As mentioned above, one aspect of the present invention relates to a process for preparing water-saturated MPMC-Al, as defined above. A water-saturated MPMC-Al obtained by the process mentioned above is also part of the present invention.

[0106] Similarly, the process for separating a gas from a mixture of gases of the present invention can also be defined as comprising the following steps: a) provide a water-saturated MPMC-Al, as defined above. (b) to provide a gas mixture comprising at least two gases, as defined above; c) Feeding the water-saturated MPMC-Al with the gas mixture at a temperature of 5 °C to 300 °C, particularly 5 °C to 250 °C, in order to obtain a retentate and a permeate, with the feed being carried out at a pressure such that the partial pressure of the gas in the retentate is greater than the partial pressure of the gas in the permeate.

[0107] Throughout the descriptive report and claims, the word "understand" and its variations are not intended to exclude other technical features, additives, components, or steps. Furthermore, the word Petition 870260086072, dated 08 / 24 / 2026, p. 45 / 148 33 / 56 includes the case of "consisting of." Additional objects, advantages, and features of the present invention will become apparent to individuals skilled in the art after examining the descriptive report or may be learned through practice of the invention. The examples below and the drawings are provided by way of illustration and are not intended to be limiting of the present invention. Furthermore, the present invention encompasses all possible combinations of particular and preferred embodiments described herein. EXAMPLES Example 1. Membrane preparation

[0108] Several MPMC-Al membranes were prepared using the materials and immersion-drying-carbonization method on porous alumina supports described by Llosa MA et al. (Part I), (see Experimental section on page 5655), but for the carbonization temperature. In particular, this document discloses the preparation of an MPMC-Al membrane by carbonizing the membrane at 500 °C. Similarly, MPMC-Al membranes were prepared by carbonization at 500 °C, 550 °C, 600 °C, 650 °C, 750 °C, 850 °C and 1000 °C.

[0109] Since permeation depends on humidity and storage time (variation in the amount of water in the pores), the effectiveness of vapor pretreatment of an AlMP was demonstrated by comparison with the performance of dry membranes, obtained by removing most of the water present in the pores through heat treatment. A Petition 870260086072, dated 08 / 24 / 2026, page 46 / 148 34 / 56 Water-saturated MPMC-Al membrane after pretreatment with steam will be called a "wetted membrane". Distribution of micropore size:

[0110] The micropore size distribution of carbonized membranes under various temperatures is shown in Figure 1. The membranes show the presence of ultramicropores (ranging from 0.25-0.55 nm, molecular sieving region - PM) and larger micropores (0.55 nm - 0.90 nm, adsorption diffusion region - DA). The membrane carbonized at 450 °C has a small pore volume, with pores ranging from 0.4 nm to 0.90 nm; the membrane carbonized at 550 °C has a similar pore size distribution pattern, but with a significantly larger pore volume. When carbonized at 650 °C, a bidisperse pore size distribution with a significantly larger volume in the molecular sieving range - MSR (from 0.25 to 0.55 nm; in the adsorption diffusion (AD) region, most pores are in the range of more than 0.55 to 0.65 nm), which could provide a good compromise between selectivity and permeation.Finally, compared to 650 °C, the 750 °C sample shows a smaller volume of small micropores in the molecular sieving (MS) region and a larger volume in the adsorption diffusion (AD) region with a very well-defined pore size distribution, which could contribute to greater permeation. These results show that as the carbonization temperature increases, the volume and number of smaller micropores increase up to 650 °C, and larger pores are formed under higher carbonization temperatures. Petition 870260086072, dated 08 / 24 / 2026, page 47 / 148 35 / 56 Permeation test

[0111] A shell-and-tube type apparatus equipped with a backpressure regulator (lower limit <20 kilopascal) and a soap flow meter (detection limit <0.2 ml / minute) was used to measure gas permeation through the supported MPMC. The selected gas was introduced into the membrane tube from the outer shell and the gas permeated through the membrane was carried to a soap flow meter to determine the flow rate. Gas permeation for N2 was determined at ambient temperature (unless otherwise specified) and at different pressures, while the permeate side was at atmospheric pressure. Hydrophilicity and water adsorption in pores

[0112] Immediately after carbonization and avoiding contact with air, the N2 permeability of the membranes was measured.

[0113] As shown in Figure 2, during carbonization, functional groups are removed, leaving active carbon groups, which can react with active molecules; thus, water can be chemisorbed, producing oxygen-containing functional groups, making the pores hydrophilic. Then, the hydrophilic groups can absorb water, physically filling the pores, reducing the pore size.

[0114] The desorption of water from carbonized membranes at various temperatures was studied by measuring N2 permeation at a pressure difference of 400 kPa, as a function of permeation temperature (Figure 3a and Petition 870260086072, dated 08 / 24 / 2026, pp. 48 / 148 36 / 56 Figure 3b). In Figure 3a, it can be observed that as the carbonization temperature of the membranes increases from 450 °C to 600 °C, the N2 flux increases. At 450 °C, the flux of N2 is low and there is no maximum, which indicates that the carbonization temperature is low and few pores have formed. The flux derivative and permeation temperature curves of Figures 3a and 3b are shown in Figures 4a and 4b, respectively. The intensity of the derivative and the permeation temperature corresponding to the maximum increases with the carbonization temperature; the maximum changes with the carbonization temperature; for carbonization temperatures of 500 °C, 550 °C, and 600 °C, the maximum temperatures are 150 °C, 175 °C, and 280 °C, respectively. This behavior is related to the strength of the interaction of water with the pores. At 750 °C and 850 °C, N2 permeation is low and no maxima are observed; at these temperatures, the pores become less hydrophilic. It can be deduced that among the carbonization temperatures tested, around 600-650 °C, the membrane has the highest hydrophilicity, retaining more water in the pores.

[0115] For the membrane carbonized at 500 °C, the system was cooled to room temperature and, without removing the membrane from the permeation reactor, a boat containing water was introduced and the permeability of N2 at 400 kPa was recorded as a function of time. At the beginning of the experiment, a sharp decrease in permeation is observed; water is being adsorbed in the most accessible locations of the membrane. Adsorption is rapid in the first 20 minutes, after which a small gradual decrease in permeation is observed; the Petition 870260086072, dated 08 / 24 / 2026, page 49 / 148 37 / 56 Water is being adsorbed in the internal pores of the membrane. Therefore, the increase in nitrogen permeation with temperature in Figure 3 is a consequence of the gradual removal of water from the pores. The same membrane was again treated at 300 °C under nitrogen to remove the physisorbed water from the pores, and the N2 permeability over time was measured as explained above, but this time a boat containing hexane was introduced into the reactor. The N2 permeability remains constant; this is a clear indication that the membrane pores are hydrophilic (i.e., hexane is hydrophobic and is not adsorbed by the pores). Example 2. Steam pretreatment of an Al MPMC outside the permeator. 2.1 Dry membrane

[0116] A carbonized MPMC-Al at 500 °C was heated to 200 °C under N2, to remove the adsorbed water from the pores. 2.2 Wetted membrane

[0117] A dry MPMC-Al prepared as described above was removed from the permeator and subjected to hydration (pre-treatment with water vapor outside the permeator), placing the membrane in a box containing water at ambient temperature, atmospheric pressure and relative humidity greater than 95%, such as 99%, until it reached water saturation (wetted membrane). 2.3 Permeation test for N2 and H2

[0118] N2 and H2 permeation was performed before and after wetting an Al-MCP prepared as Petition 870260086072, dated 08 / 24 / 2026, p. 50 / 148 38 / 56 disclosed in Example 2, but to be carbonized at 600 °C. The effect of hydration was evident: the permeability of both N2 and H2 decreases significantly (see Figure 5). However, the reduction in N2 permeability is greater than that of H2, which is reflected in the selectivity to H2; thus, the ideal H2 / N2 permeability selectivity at 1 bar for the humidified membrane is 70 times greater than without humidification. Example 3. Steam pretreatment of an Al MPMC inside the permeator.

[0119] Two carbon molecular sieve membranes were prepared as disclosed in Example 2, but to be carbonized at 550 °C and 600 °C. They were referred to as MPMC-550 and MPMC-600 membranes, respectively. 3.1 Dry membrane

[0120] MPMC-550 and MPMC-600 membranes were placed inside a permeator. Nitrogen was then introduced into the permeator and the temperature was increased to 150 °C at a heating rate of 2 °C / minute. The aforementioned temperature was maintained for 6 hours to obtain the corresponding dehydrated membranes.

[0121] After desorption of water from the pores, the membrane was cooled to the permeation temperature (i.e., from 20 °C to 100 °C) and then permeation studies of the dry membrane were carried out. 3.2 Wetted membrane Petition 870260086072, dated 08 / 24 / 2026, p. 51 / 148 39 / 56

[0122] The dry membranes obtained above were exposed to a stream of water-saturated N2 gas by bubbling the gas at room temperature through a tank filled with water, before feeding the permeator. To ensure consistent humidification, the membranes were saturated with water from the humidified stream every night for 12 hours before conducting the experiments. A pure nitrogen permeation test was performed to confirm that nitrogen permeation at 4 bar pressure was constant. Example 4. Permeation studies of dry and moistened membranes.

[0123] Permeation of pure hydrogen and a mixture of gases containing hydrogen was performed, and the permeation and purity values ​​of hydrogen were measured under various pressures and temperatures. Vacuum was used on the permeate side.

[0124] With regard to the wet membrane, the first interesting result is the excellent selectivity and permeability, compared to the Robeson upper limit, as illustrated in Figure 6. This limit provides a reference against which new membrane materials can be compared.

[0125] The differences in flow rate and hydrogen purity in a carbonized MPMC-Al at 550 °C (MPMC-550) before (dry) and after treatment with water vapor (humidified) of a gas mixture containing 50% hydrogen and 50% methane at 20 °C and various differences in partial pressure of hydrogen are illustrated in Figures 7 Petition 870260086072, dated 08 / 24 / 2026, page 52 / 148 40 / 56 and 8, respectively. Without intending to limit ourselves to theory, it is believed that water treatment causes the pore walls to become moistened with water and, as a consequence, the pore size is reduced (pore filling). The results show that, although the hydrogen flow is decreased (Figure 7), the purity of the hydrogen is considerably increased (Figure 8). Example 5. Permeation of gas mixtures using a humidified MPMC-Al-550.

[0126] An MPMC-550 was pretreated with a stream of N2 gas saturated with water vapor, using the procedure described in Example 3, section 3.2, and was used to measure the permeation and purity of hydrogen in the permeate of binary mixtures of hydrogen with CH4, CO2 or N2 with 10% or 50% hydrogen under various temperatures (from 20 °C to 70 °C) and various partial pressure differences, applying vacuum on the permeate side.

[0127] The separation of hydrogen present in mixtures with methane containing 10% and 50% hydrogen was studied using the MPMC-550. The hydrogen flux rate in the permeate obtained from a mixture of H2 and CH4 (10% and 50% H2) under various temperatures and differences in the partial pressure of H2 is shown in Figure 9, and the corresponding H2 purity is shown in Figure 10. It can be observed that by increasing the permeation temperature, the permeability of hydrogen increases at the expense of hydrogen purity. It is important to note that for the carbon membrane saturated with water vapor, the hydrogen purity obtained is Petition 870260086072, dated 08 / 24 / 2026, page 53 / 148 41 / 56 remarkably high, especially when considering a 10% H2 content in the mixture. Similarly, particularly at 20 °C, with a partial pressure of hydrogen of 0.55 bar, a purity of 97.5% is obtained.

[0128] Similar tests were carried out with binary mixtures of hydrogen with N2 or with CO2. The results are shown in Figures 11 and 12 for CO2 and in Figures 13 and 14 for N2.

[0129] For the separation of H2 from a mixture with CO2, the purity of the permeate is lower than with CH4, probably because CO2 is smaller and more absorbable than CH4 (Figure 12).

[0130] In Figures 13 and 14, the H2-N2 results in terms of flow rate and hydrogen purity are represented under different hydrogen partial pressure differences. When the membrane was saturated with water, high hydrogen purity was achieved with all the different mixtures considered. Under higher temperatures, such as 100 °C, a real improvement in performance is expected when the membrane is wetted.

[0131] Similar results (to those obtained with H2 / N2, H2 / CH4 and H2 / CO2) are expected for gases with a notable difference in molecular size or an extremely distinct adsorption capacity, such as, for example, CO2 / CH4 or CO2 / N2. Thanks to their high water adsorption capacity, carbonized membranes from 500 °C to 750 °C, mainly from 500 °C to 700 °C, will perform similarly when tested under humidified conditions with dry gases. High selectivity and purity are expected to be achieved up to a Petition 870260086072, dated 08 / 24 / 2026, page 54 / 148 42 / 56 working temperature of 100 °C, when working with the corresponding moistened membranes.

[0132] Similarly, a carbonized humidified MPMCAl at 500 °C was used to purify hydrogen from a mixture containing 10% H2 and 90% N2. This separation is important because the existing natural gas infrastructure can be used to store and distribute hydrogen. For safety reasons, a low concentration of H2 (i.e., 10%) can be mixed in. It was observed that the purity strongly depended on the permeation temperature. In particular, at 30 °C, the purity of the hydrogen obtained was 99.4%. Example 6. Differences in hydrogen permeation properties of a dry MPMC-600 and a moistened MPMC-600.

[0133] A dry MPMC-600 was obtained by heating the membrane to 150 °C under a nitrogen environment, inside the permeator (most of the water was removed from the pores). Then, the permeator temperature was cooled to 100 °C and hydrogen permeation of a mixture of 10% H2 and 90% CH4 was carried out at various partial pressures of hydrogen (membrane dried at 100 °C).

[0134] Next, the same gas mixture was saturated with water by bubbling it through water for 15 hours before entering the permeator, which was at 100 °C. In this way, water was selectively adsorbed onto the hydrophilic membrane (wetted) at 100 °C, and hydrogen permeation was carried out (membrane wetted at 100 °C) under Petition 870260086072, dated 08 / 24 / 2026, page 55 / 148 43 / 56 various partial pressures of hydrogen. The same procedure was performed at different temperatures: 70 °C, 50 °C and 20 °C.

[0135] By wetting the membrane, the hydrogen flow rate was reduced (Figure 15), resulting in a notable increase in purity (Figure 16). This was more pronounced at higher temperatures. The average increase in purity that occurs after wetting the membrane (wet versus dry) was 18% at 100 °C, 14% at 70 °C, 10% at 50 °C, and only 4% at 20 °C (Figure 17). This indicates that pretreatment by conditioning the carbon membrane with a steam stream will be more important at temperatures above 100 °C.

[0136] Therefore, according to the results above, membrane humidification confers an excellent advantage to purification, especially under higher temperatures. Comparative Example 1. Palladium-based membranes versus MPMC-Al membranes

[0137] Palladium-based membranes are used for hydrogen separation due to their high hydrogen permeation and unique selectivity. Permeation is preferably carried out at 400 °C, as they can be damaged at temperatures below 300 °C and above 500 °C. In palladium-based membranes, the hydrogen flux is a function of the square root difference of the partial pressure difference on both sides of the membrane (Sievert's law). In MPMC-Al, the flux is proportional to the partial pressure difference. Petition 870260086072, dated 08 / 24 / 2026, page 56 / 148 44 / 56

[0138] Figure 18 shows an example of the pressure dependence versus hydrogen flux for a palladium-based membrane and for a wetted MPMC-Al membrane inside the reactor to water saturation, considering that both have the same permeance at a pressure difference of 1 bar. It can be observed that at low pressures, the flux for both cases is similar. However, as the pressure increases, the gain in permeation is much greater for MPMC-Al membranes than for palladium-based membranes. Under low pressures, the H2 permeation for MPMC-Al membranes is approximately 10 times lower than for a palladium-based membrane of the same thickness.Selectivity is also lower for MPMC-Al membranes (in practical terms, 20 to 40 times lower than for palladium-based membranes); however, permeation of MPMC-Al can be achieved at low temperatures (i.e., room temperature), while palladium membranes can be permeated at high temperatures (generally 400 °C). Comparative Example 2. Effect of hydrogen concentration in a mixture with other gases on hydrogen permeation.

[0139] Figure 19 shows the hydrogen permeation flux for pure hydrogen and various binary H2 / CH4 mixtures (from 100% to 50% hydrogen) at 400 °C in a supported Pd-Ag membrane 1.2 μm thick, as a function of the square root difference in the partial pressure of hydrogen (cf. Melendez, J. et al., in “Preparation and characterization of ceramic supported ultra-thin (~1 pm) Pd-Ag membranes”, J. Memb. Sci. 528 Petition 870260086072, dated 08 / 24 / 2026, page 57 / 148 45 / 56 (2017), pages 12-23). ​​Pure hydrogen follows Sieverts' law (linear dependence of H2 flux on the square root of the pressure difference), but as the hydrogen concentration in the binary mixture decreases, the fluxes are not linear, showing a downward convexity towards the pressure axis. Since the dilution effect is already included when using partial pressure, and given that CH4 can be considered inert, the limitation of mass transfer from the bulk to the membrane surface (concentration polarization) is the most likely explanation for this phenomenon; this becomes more important in the case of highly selective, high-flux membranes. Similar behavior was observed in supported Pd 0.8 and Ag 0.2 membranes, 2.5 μm thick.

[0140] The results of the flow rate (Figure 20) and hydrogen purity (Figure 21) are shown for different H2-CH4 mixtures from a hydrogen concentration of 10% to 70%. A supported 20 cm Pd-Ag ceramic membrane was used for the aforementioned tests. The trend was also compared with pure gas tests. The retentate pressure was changed from 8 to 40 bar, while the permeate pressure was maintained at 0.15 bar with a vacuum pump. Hydrogen permeance decreased significantly due to concentration polarization, especially when working with low hydrogen content. Purity was also notably lower compared to that obtained with pure H2. Probably, the reason was the higher concentration of contaminants near the Petition 870260086072, dated 08 / 24 / 2026, page 58 / 148 46 / 56 membrane surface area, due to high hydrogen permeation.

[0141] In Figure 22, the hydrogen permeation of binary mixtures of H2 / N2, H2 / CO2 and H2 / CH4 as a function of the H2 content in the mixture at 400 °C and 3 bar total pressure (vacuum on the permeate side) for a supported Pd-Ag membrane (cf. Melendez J. et al., 2017). It is clearly observed that when the percentage of hydrogen in the feed decreases, the hydrogen permeation rate also drops. Furthermore, the permeate hydrogen flux decreases quite linearly from 100% to 0% H2 and is quite similar for the different H2 mixtures. Example 7. Dependence of partial pressure difference and hydrogen flux in water-saturated MPMC-Al membranes

[0142] The hydrogen flux rate as a function of the hydrogen partial pressure difference was tested at 20 °C for various H2 / CH4 and H2 / N2 mixtures and a carbonized MPMC-Al at 550 °C (MPMC-550) after exposure to ambient humidity. It was found that the dependence of the hydrogen partial pressure difference on the hydrogen flux was almost linear, regardless of the H2 concentration in the mixture and the gases tested (Figure 23), which proves that concentration polarization does not affect the membrane H2 flux. Results and advantages of the water-saturated MPMC-Al membranes of the present invention. Petition 870260086072, dated 08 / 24 / 2026, page 59 / 148 47 / 56

[0143] The effect of water adsorbed on a membrane was also tested on a carbonized MPMC-Al at 600 °C. First, the water was removed by heating at 150 °C under N2, and a permeation test was performed with dry gas and humidified gas to study the effect of water vapor treatment on the purity of the gaseous permeate. Tests were carried out under various partial pressures of H2, for H2 / CH4 mixtures containing 10% H2 at various temperatures (20 °C, 50 °C, 70 °C, and 100 °C), and the relative increase in purity obtained under humidified conditions was evaluated. A clear improvement in performance was shown after humidification of the membranes, especially at high temperatures.

[0144] Similar effects are expected with gaseous mixtures consisting of H2 / CH4, H2 / N2, H2 / CO2, CO2 / CH4 and CO2 / N2, thanks to the adsorption of water on the pore walls, which facilitates the permeation of the smaller and more absorbable molecule.

[0145] Therefore, water-saturated MPMC-Al membranes exhibit competitive and promising performance compared to commercial membranes for gas separation in mixtures, especially under high pressure, due to the absence of mass transfer limitations. Furthermore, when operating under humidified conditions, improved gas purity is achieved thanks to water adsorption, particularly at high temperatures.

[0146] As seen in Comparative Examples 1 and 2 and in the Examples above, the water-saturated MPMC-Al of the present invention is advantageous for the following reasons: Petition 870260086072, dated 08 / 24 / 2026, page 60 / 148 48 / 56 Water-saturated MPMC-Al membranes offer significantly higher purities compared to dry MPMC-Al membranes, especially at higher temperatures. - H2 permeation in palladium membranes is carried out between 300 °C and 500 °C, while in MPMC-Al it can be carried out at room temperature; therefore, the operational cost is lower for MPMC-Al, considering similar permeation. Palladium-based membranes are very expensive, while MPMC-Al membranes are produced from very inexpensive phenolic resins. - The flux in palladium membranes depends on ΔP°, while the flux in MPMC-Al membranes depends on ΔP. Therefore, the H2 flux under high pressures and low temperatures is greater for MPMC-Al membranes. - In the permeation of the gas mixture, for palladium membranes, the hydrogen flux decreases as the H2 concentration decreases; for MPMC-Al, the flux is almost constant (without concentration polarization). Example 8 Carbon membranes for water vapor permeation

[0147] In water permeation, depending on the water pressure and temperature, condensation can occur, leading to the presence of both adsorbed monolayer and free water (gas) - (Figure 24). The water in the pores will increase with increasing pressure and decreasing temperature. Petition 870260086072, dated 08 / 24 / 2026, page 61 / 148 49 / 56 Effect of carbonization temperature on water permeation

[0148] As discussed above, the hydrophilicity of the carbon membrane can be modified by altering the carbonization temperature. Water permeability under different temperatures and a pressure difference of 3 bar was measured for the MPMC-Al membranes of Example 2.2 and is shown in Figure 25. Regardless of the carbonization temperature, the lowest permeances were obtained when the experiments were performed at 150 °C; as explained previously, this is due to water condensation in the pores. For membranes carbonized at 500 °C and 550 °C, the highest permeances were obtained at a permeation temperature of 200 °C; for membranes carbonized at 600 °C and 650 °C, the maximum shifted to 250 °C (Figure 25). When the carbonization temperature of the membranes was increased to 750 °C and 850 °C, the permeance peak shifted again to 200 °C.

[0149] Permeation peaks have been related to pore hydrophilicity. Without intending to limit oneself to theory, it is believed that as the carbonization temperature increases from 550 °C to 600 °C, the number and size of pores increase, exposing more hydrophilic groups; the number of activated carbons, which will react with water, also increases, forming new hydrophilic groups. Increasing the temperature from 650 °C, the hydrophilic groups are removed, and condensation reactions between the activated carbons occur, reducing the porosity of the membrane and, consequently, the permeation of water. This is more Petition 870260086072, dated 08 / 24 / 2026, page 62 / 148 50 / 56 pronounced for the carbonized membrane at 850 °C; therefore, the water permeance at this temperature is lower than at 750 °C. The presence of more hydrophilic groups in the pores allows water to be more strongly bound to the pores, which requires more energy (higher temperature) to be removed. Ideal water / gas permeability selectivity

[0150] The permeance of various gases (N2, H2, CH4, CO, CO2) under different temperatures was measured for the MPMC-Al membranes of Example 2.2, and their ideal water / gas selectivity (i.e., water permeability selectivity) was calculated. The results are illustrated in Figure 26. For the gases tested, all membranes showed selectivity towards water, due to having the smallest kinetic diameter (0.26 nm, transport by molecular sieving) and greater affinity to the pores (transport by adsorption diffusion).

[0151] The selectivity of water permeability depends on the carbonization temperature and the permeation temperature.

[0152] Regardless of the carbonization temperature, the highest selectivities were obtained when permeations were performed at approximately 200 °C, with the exception of the H2O / N2 mixture, where the maximum was obtained at approximately 250 °C for the membrane carbonized at 750 °C. Probably, around this carbonization temperature, the number and size of pores are optimal for water permeation; below this temperature, the pores are smaller, and above it, water begins to condense in the pores. Petition 870260086072, dated 08 / 24 / 2026, page 63 / 148 51 / 56 reducing porosity, hydrophilicity and pore size. In fact, the lowest selectivities are obtained with the membrane carbonized at 1000 °C.

[0153] In general, for the gases tested, the highest selectivities are obtained with the membrane carbonized at 750 °C.

[0154] The ideal water / gas selectivities as a function of kinetic diameter and permeation temperature of the MPMC-Al membranes of Example 2.2 carbonized under different temperatures are shown in Figure 26. For all carbonization temperatures, the highest selectivities are obtained for water / N2. The selectivity of water against CO2 and H2 is lower than N2, probably due to the larger kinetic diameter of the latter. CO, being larger than N2, has lower selectivity. CO is a polar compound that can be adsorbed in the hydrophilic pores of the carbon membrane, which increases the adsorption diffusion mechanism of permeation. Comparing CO with CH4, CH4 is larger than CO, therefore its permeation is lower. In relation to N2 and CH4, CH is a symmetrical molecule that cannot be easily polarized; on the other hand, N2 is less symmetrical and can be more easily polarized, increasing the dipole-induced dipolar interaction with the polar pores.

[0155] The lowest selectivity is observed with H2, as the molecule size is slightly larger than water; in addition, water can form hydrogen bonds with the pores, increasing permeation by adsorption diffusion. LIST OF QUOTES Petition 870260086072, dated 08 / 24 / 2026, page 64 / 148 52 / 56 1. MA Llosa et al. Composite-alumina-carbon molecular sieve membranes prepared from novolac resin and boehmite. Part I: Preparation, characterization and gas permeation studies”, Int. J. Hydrogen Energy. 2015, vol. 40, pp. 5653-5663. 2. MA Llosa et al. Composite-alumina-carbon molecular sieve membranes prepared from novolac resin and boehmite. Part II: Effect of the carbonization temperature on the gas permeation properties”, Int. J. Hydrogen Energy. 2015, Vol. 40, pp. 3485-3496 3. Campo, MC et al. Molecular carbon sieves membranes from cellophane paper”Journal of Membrane Science, 2010, vol. 350, pp. 180-188; 4. Teixeira M et al. Composite phenolic resin-based carbon molecular sieve membranes for gas separation”, Carbon 2011, vol. 49, pp. 4348-4358; 5. Teixeira M et al. Carbon-Al2O3-Ag composite molecular sieve membranes for gas separation” Chem. Eng. Res Des. 2012, vol. 90, pp. 2338-2345; 6. Rodrigues SC, et al. Preparation and characterization of carbon molecular sieve membranes based on resorcinoleformaldehyde resin” J. Memb. Sci. 2014, vol. 459, pp. 207-216; 7. Nguyen C., Do, D.D. Adsorption of supercritical gases in porous media: determination of micropore size distribution”. J. Phys. Chem. B. 1999, 103 (33), 6900-8, and [sic]; Petição 870260086072, de 24 / 08 / 2026, pág. 65 / 148 53 / 56 8. Nguyen C et al. “The structural characterization of carbon molecular sieve membrane (CMSM) via gas adsorption” J. Memb. Sci., 2003, 220 (1-2) 177-82; 9. Melendez J et al., “Preparation and characterization of ultrathin (~1 pm) ceramic-supported PdAg membranes”, J. Memb. Sci. 2017, vol. 528, pp.12-23;

[0156] For completeness, several aspects of the present invention are set forth in the following listed clauses: 1. Water-saturated carbon molecular sieve membrane obtained by: a) providing a hydrophilic carbon molecular sieve membrane (CMSM) comprising pores with a pore size of 0.25 nm to 0.55 nm for molecular sieving, and with a pore size greater than 0.55 nm up to 0.90 nm for adsorption diffusion, and a negligible number of pores larger than 0.90 nm, such that a graph of N2 permeance versus permeation pressure at room temperature and at a pressure of 1 to 4 bar has a zero or negative slope; and b) wetting the membrane until a water-saturated carbon molecular sieve membrane is obtained. 2. Water-saturated carbon molecular sieve membrane of clause 1, wherein the MPMC is an alumina-carbon composite molecular sieve membrane (MPMC-Al). 3. Water-saturated carbon molecular sieve membrane from clause 2, wherein the MPMC-Al has a content of Petition 870260086072, dated 08 / 24 / 2026, page 66 / 148 54 / 56 nitrogen from 0.1% by weight to 4.0% by weight, an alumina content from 2.5% to 50% and a carbon content from 50% by weight to 95% by weight, relative to the total weight of the membrane. 4. A process for separating a gas from a mixture of gases, characterized by comprising the following steps: a) provide a water-saturated membrane as defined in any of clauses 1 to 3; b) to provide a gas mixture comprising at least two gases; c) Feeding the water-saturated MPMC with a gas mixture at a temperature of 5 °C to 300 °C, to obtain a retentate and a permeate, with the feed being carried out at a pressure such that the partial pressure of the gas in the retentate is greater than the partial pressure of the gas in the permeate, and such that the membrane is a water-saturated membrane. 5. Process, in accordance with clause 4, wherein the temperature of step (c) is 5 °C to 250 °C, 5 °C to 120 °C, 15 °C to 120 °C, 15 °C to 100 °C, 15 °C to 70 °C or 20 °C to 50 °C. 6. Process, according to clause 4 or 5, wherein at least two gases have a polarizability of 2 to 27 and at least one of the at least two gases has a kinetic diameter less than 0.55 nm, and wherein if the at least two gases have a kinetic diameter less than 0.55 nm, the difference in kinetic diameter between the at least two gases is equal to or greater than 0.01 nm and / or the difference in Petition 870260086072, dated 08 / 24 / 2026, page 67 / 148 55 / 56 polarizability between at least two gases is equal to or greater than 1 m3. 7. Process, in accordance with clause 6, wherein at least two gases are selected from He, H2O, Ne, H2, NO, Ar, NH3, N2, O2, CO, CO2, CH4, C2H4, C2H6, propene, propane, H2S, methanol and ethanol. 8. Process, in accordance with any one of clauses 4 to 7, wherein the gas mixture comprises at least two gases selected from the group consisting of H2 / CH4; H2 / N2; H2 / CO2; CO2 / CH4; CO2 / N2; O2 / N2; and biogas. 9. Process, according to clause 8, wherein the gas mixture comprises 5% to 20% H2 and 95% to 80% CH4 and wherein step c) is carried out at a partial pressure difference of hydrogen equal to or greater than 3 bar and at a temperature equal to or less than 40 °C. 10. Process, in accordance with clause 8, wherein at least two gases are CO2 and N2 and the gas mixture comprises 10% to 20% CO2 and 65% to 75% N2, in particular, approximately 15% CO2 and approximately 70% N2. 11. Process, in accordance with clause 8, wherein at least two gases are CO2 and N2 and the gas mixture comprises 55% to 65% H2 and 30% to 40% CO2, in particular, approximately 60% H2 and approximately 35% CO2. 12. Process, in accordance with clause 8, wherein the gas mixture comprising at least two gases is biogas and CO2 is removed from the biogas. Petition 870260086072, dated 08 / 24 / 2026, page 68 / 148 56 / 56 13. Use of a water-saturated MPMC, as defined in clauses 1 to 3, for the separation of a gas from a gas mixture. 14. Use of a water-saturated MPMC, as defined in clauses 1 to 3, for solvent dehydration. 15. Use of a water-saturated MPMC, as defined in clauses 1 to 3, as a membrane reactor. Petition 870260086072, dated 08 / 24 / 2026, page 69 / 148

Claims

1 / 6 CLAIMS 1. Water-saturated carbon molecular sieve membrane characterized in that it is obtained by: i) providing a hydrophilic carbon molecular sieve membrane (CMSM) comprising pores with a pore size of 0.25 nm to 0.55 nm, for molecular sieving, and with a pore size greater than 0.55 nm up to 0.90 nm, for adsorption diffusion, and a negligible amount of pores larger than 0.90 nm, wherein a negligible amount of pores larger than 0.90 nm in the CMSM means that, when the N2 permeance of the CMSM is measured as a function of permeation pressure, at room temperature and at a pressure of 1 to 4 bar, the resulting graph has a zero or negative slope;and ii) humidify the MPMC obtained in step i) to obtain a water-saturated MPMC, by means of the following steps: - treat the MPMC obtained in step i) with water vapor at a temperature of 5 °C to 180 °C and at atmospheric pressure and a relative humidity greater than 95%, such as 99%, for a period, in such a way that, after the additional treatment with water vapor, the permeation flux of a non-adsorbable gas selected from N2 and He, at 4 bar at the temperature at which the MPMC was treated with water vapor, is constant for a period of 3 hours;or - alternatively, by exposing the MPMC obtained in step i) to a flow of N2 or He gas saturated with water by bubbling the gas at a temperature of 5 °C to 180 °C in a tank filled with water, in such a way that, after further exposure to the flow of N2 or He gas saturated with water, the permeation flux of a non-adsorbable gas selected from N2 and He, at 4 bar and at the aforementioned temperature, is constant for a period of 3 hours; wherein a hydrophilic MPMC is an MPMC that, before being humidified to obtain a water-saturated MPMC, exhibits a N2 permeance at 300 °C and a pressure difference of 4 bar greater than 7x10-9 mol m-2 s-1 Pa-1 and, after being humidified to obtain a water-saturated MPMC, exhibits a N2 permeance at room temperature and a pressure difference of 1 bar less than 1x10-9 mol m-2 s-1 Pa-1.

2. Water-saturated carbon molecular sieve membrane, according to claim 1, characterized in that the MPMC is a molecular sieve membrane composed of alumina-carbon (MPMC-Al).

3. Water-saturated carbon molecular sieve membrane, according to claim 2, characterized in that the MPMC-Al has a nitrogen content of 0.1% by weight to 4.0% by weight, an alumina content of 2.5% to 50%, and a carbon content of 50% by weight to 95% by weight, relative to the total weight of the membrane.

4. Process for the preparation of a water-saturated alumina-carbon composite molecular sieve membrane (water-saturated MPMC-AL), characterized in that it comprises: i) preparing a hydrophilic MPMC-Al by the following steps: - providing a porous support to A^Os; - preparing a solution containing 5% to 20% by weight of phenol-formaldehyde resin, 0.5% to 5% by weight of formaldehyde, 0.1% to 2% by weight of ethylenediamine, 0.1% to 5% by weight of boehmite in N-methyl-2-pyrrolidone and heating the solution (e.g., from 80 °C to 110 °C, for 30 minutes to 3 hours), to perform a pre-polymerization process, to obtain a coating solution; - Immerse the porous α-Al2Os substrate in the coating solution to obtain a coated substrate; - Dry the coated substrate at a temperature of 70 °C to 120 °C to complete the polymerization process;- carbonize the dry coated support at a carbonization temperature of 450 °C to 750 °C to obtain an Al-MPMC; ii) humidify the Al-MPMC prepared in step i) to obtain a water-saturated Al-MPMC by the following steps: - treat the Al-MPMC prepared in step i) with water vapor at a temperature of 5 °C to 180 °C, at atmospheric pressure and a relative humidity greater than 95%, such as 99%, for a period of time, such that, after the additional treatment with water vapor, the permeation flux of a non-adsorbable gas selected from N2 and He, at 4 bar and at the temperature at which the MPMC was treated with water vapor, is constant for a period of 3 hours;or - alternatively, by exposing the MPMCAl prepared in step i) to a stream of water-saturated N2 or He gas, by bubbling the gas at a temperature of 5 °C to 180 °C in a tank filled with water, such that, after further exposure to the water-saturated N2 or He gas stream, the permeation flux of a non-adsorbable gas selected from N2 and He, at 4 bar and at the aforementioned temperature, is constant for a period of 3 hours.

5. Process according to claim 4, characterized in that the phenol-formaldehyde resin is a novolac resin.

6. Process, according to any one of claims 4 or 5, characterized in that the carbonization temperature is from 450 °C to 700 °C.

7. Water-saturated MPMC-AL characterized in that it is obtained by the process defined in any one of claims 4 to 6.

8. Process for separating a gas from a gas mixture, characterized in that the process comprises: a) providing a water-saturated membrane as defined in any one of claims 1 to 3 or 7; b) providing a gas mixture comprising at least two gases; and c) feeding the water-saturated MPMC with a gas mixture at a temperature of 5 °C to 300 °C in order to obtain a retentate and a permeate, wherein the feed is carried out at a pressure such that the partial pressure of the gas in the retentate is greater than the partial pressure of the gas in the permeate and in such a way that a permeation difference is observed in comparison with the same MPMC without having been subjected to a humidification step, in order to obtain a water-saturated membrane under feed pressure and temperature.

9. Process, according to claim 8, characterized in that at least two gases have a polarizability of 2 to 27 and at least one of the at least two gases has a kinetic diameter less than 0.55 nm, wherein, if the at least two gases have a kinetic diameter less than 0.55 nm, the difference in kinetic diameter between the at least two gases is equal to or greater than 0.01 nm and / or the difference in polarizability between the at least two gases is equal to or greater than 1 m3.

10. Process according to claim 9, characterized in that at least two gases are selected from He, H2O, Ne, H2, NO, Ar, NH3, N2, O2, CO, CO2, CH4, C2H4, C2H6, propene, propane, H2S, methanol and ethanol.

11. A process according to any one of claims 8 to 10, characterized in that the gas mixture comprising at least two gases is selected from the group consisting of H2 / CH4; H2 / N2; H2 / CO2; CO2 / CH4; CO2 / N2; O2 / N2; and biogas, which is a gas mixture containing mainly methane and carbon dioxide and smaller amounts of other gases, such as H2, H2S, N2 and water vapor.

12. Process according to claim 11, characterized in that the gas mixture comprises 5% to 20% H2 and 95% to 80% CH4 and in which step c) is carried out at a partial pressure difference of hydrogen equal to or greater than 3 bar and at a temperature equal to or less than 40 °C.

13. Process, according to claim 11, characterized in that at least two gases are CO2 and N2 and the gas mixture comprises 10% to 20% CO2 and 65% to 75% N2; or Petition 870260086072, dated 08 / 24 / 2026, page 74 / 148 6 / 6 at least two gases are H2 and CO2 and the gas mixture comprises 55% to 65% H2 and 30% to 40% CO2.

14. Process according to claim 11, characterized in that the gas mixture comprising at least two gases is biogas and CO2 is removed from the biogas, wherein the biogas is a gas mixture comprising methane and carbon dioxide.

15. Use of a water-saturated MPMC, as defined in any one of claims 1 to 3, or of a water-saturated MPMC-AL, according to claim 7, characterized in that said membrane is used for solvent dehydration or as a membrane reactor. Petition 870260086072, dated 08 / 24 / 2026, p. 75 / 148