Polyethylene homopolymer compositions with balanced properties, films prepared from these compositions and the process to prepare these compositions

A dual-reactor polymerization process using a single-site catalyst produces a polyethylene blend with tailored molecular weights and low long-chain branching, addressing the poor barrier properties of conventional polyethylene homopolymers and achieving films with enhanced optical and barrier performance.

BR112022021674B1Active Publication Date: 2026-11-17NOVA CHEM (INT) SA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
BR112022021674
Authority / Receiving Office
BR · BR
Patent Type
Patents
Current Assignee / Owner
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing polyethylene homopolymers, particularly those produced with peroxide initiators in high-pressure polymerization, exhibit poor barrier properties despite having desirable optical properties, and linear ethylene homopolymers lack sufficient density and stiffness.

Method used

A polyethylene composition comprising two ethylene homopolymer blend components, each with specific molecular weight ratios and distributions, is prepared using a single-site catalyst in a dual-reactor polymerization process to achieve a balanced density, molecular weight distribution, and low long-chain branching, enhancing both optical and barrier properties.

Benefits of technology

The resulting films exhibit a good balance of optical properties, such as high gloss and low turbidity, along with improved barrier properties, specifically low water vapor transmission rates, while maintaining desirable mechanical properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Polyethylene homopolymer compositions with balanced properties. A polyethylene homopolymer composition with a weight-average molecular weight Mw of 75,000 to 95,000; a Mz of 200,000 to 325,000; a molecular weight distribution Mw / Mn of 6 to 12 and a melting index, I2 of 1.5 to 2.8 grams per 10 minutes can be used to prepare films with a good balance of optical properties and resistance to moisture transmission.
Need to check novelty before this filing date? Find Prior Art

Description

“Polyethylene homopolymer compositions with balanced properties, films prepared from said compositions and process for preparing said compositions” TECHNICAL FIELD

[001] A polyethylene homopolymer composition can be used to prepare films with a good balance of optical and barrier properties. PREVIOUS TECHNIQUE

[002] Polyethylene homopolymer that is prepared with a peroxide initiator in a high-pressure polymerization process is a widely available commercial item that is commonly referred to as high-pressure / low-density polyethylene (or HPLD). Such HPLD typically contains a significant amount of long-chain branching (or “LCB”). The presence of LCB reduces the density of the polyethylene homopolymer. In addition, the presence of LCB modifies the melt rheology of polyethylene in a way that is desirable for many manufacturing processes – especially blown film production. Films made from HPLD typically exhibit very good optical properties (high gloss and low turbidity), but poor “barrier” properties (i.e., these films are comparatively permeable to moisture).It is also generally accepted that the presence of LCB can reduce some physical properties of polyethylene compared to a linear polyethylene homopolymer with the same melt index.

[003] The production of linear ethylene homopolymers by homopolymerization of ethylene with a coordination catalyst (such as a Ziegler Natta or Z / N catalyst) is also known. The resulting ethylene homopolymers are essentially LCB-free when prepared with a Z / N catalyst. These linear ethylene homopolymers have sharp melting points, which Petition 870240100453, dated 11 / 26 / 2024, page 10 / 67 2 / 25 makes them suitable for some injection molding applications. Furthermore, plastic film prepared from linear ethylene homopolymer has high resistance to moisture transmission (or, alternatively, a low water vapor transmission rate or low “WVTR”). SUMMARY OF THE INVENTION

[004] In one embodiment, a polyethylene composition is provided that includes at least two ethylene homopolymer blend components, wherein the composition has: (i) a density of 0.96 to 0.97 g / cm3; (ii) a Mw of 75,000 to 90,000; (iii) a Mn of 7,000 to 12,000; (iv) a Mz of 200,000 to 325,000; (v) a molecular weight distribution, Mw / Mn, of 6 to 12; (vi) a melting index, I2, as determined by ASTM D1238 at 190°C, using a charge of 2.16 kilograms, from 1.5 to 2.8 grams for 10 minutes; and further characterized by (vii) 25 to 55% by weight of the composition having a molecular weight less than or equal to 20,000; wherein the composition includes a first mixing component containing 45 to 60% by weight of the composition and a second mixing component containing 55 to 40% by weight of the composition, where the first mixing component has: A1) an Mw / Mn ratio of 1.8 to 2.5; and A2) a melting index, I2, as determined by ASTM D1238 at 190°C, using a charge of 2.16 kilograms, from 3,000 to 25,000 grams for 10 minutes; and, wherein the second component of the mixture has: B1) an Mw / Mn ratio of 1.8 to 2.5; and B2) a melting index, I2, as determined by ASTM D1238 at 190°C, Petition 870240100453, dated 11 / 26 / 2024, page 11 / 67 3 / 25 using a load of 2.16 kilograms, from 0.05 to 0.5 grams for 10 minutes.

[005] In one embodiment, a polyethylene composition is provided that includes at least two ethylene homopolymer blend components, wherein the composition has: (i) a density of 0.96 to 0.97 g / cm3; (ii) a Mw of 75,000 to 90,000; (iii) a Mn of 7,000 to 12,000; (iv) a Mz of 200,000 to 325,000; (v) a molecular weight distribution, Mw / Mn, of 6 to 12; (vi) a melting index, I2, as determined by ASTM D1238 at 190°C, using a charge of 2.16 kilograms, from 1.5 to 2.8 grams for 10 minutes; and further characterized by; (vii) 25 to 55% by weight of the composition has a molecular weight less than or equal to 20,000, wherein the composition includes a first mixing component containing 45 to 60% by weight of the composition and a second mixing component containing 55 to 40% by weight of the composition, wherein the first mixing component has: A1) an Mw / Mn ratio of 1.8 to 2.5; and A2) a melting index, I2, as determined by ASTM D1238 at 190°C, using a charge of 2.16 kilograms, from 3,000 to 8,500 grams for 10 minutes; and wherein the second component of the mixture has: B1) an Mw / Mn ratio of 1.8 to 2.5; and B2) a melting index, I2, as determined by ASTM D1238 at 190°C, using a charge of 2.16 kilograms, from 0.05 to 0.5 grams for 10 minutes.

[006] In one embodiment, the Mz of the polyethylene composition is less than or equal to 300,000.

[007] In one embodiment, the Mn of the polyethylene composition is less than or Petition 870240100453, dated 11 / 26 / 2024, page 12 / 67 4 / 25 equals 10,000.

[008] In one embodiment, the polyethylene composition comprises a nucleating agent.

[009] In one embodiment, the polyethylene composition comprises a nucleating agent comprising a calcium salt of hexahydrophthalic acid.

[010] In one embodiment, a film prepared from the polyethylene composition provides a good balance of optical properties (good gloss and low turbidity) and barrier properties (low water vapor transmission rate, WVTR).

[011] One embodiment is a film made of polyethylene composition with a turbidity of less than 30%.

[012] In one embodiment, a process is provided for preparing a polyethylene composition that includes at least two ethylene homopolymer mixture components, said process comprising contacting at least one single-site polymerization catalyst system with ethylene under polymerization conditions for said ethylene in at least two polymerization reactors, including a first polymerization reactor and a second polymerization reactor, and mixing together the polyethylene produced in each polymerization reactor, wherein hydrogen is added to said first polymerization reactor so as to provide a concentration of 0.5 to 2 ppm in said first polymerization reactor, and wherein hydrogen is added to the second polymerization reactor so as to provide a hydrogen concentration of 35 to 55 ppm in said second polymerization reactor. DESCRIPTION OF THE MODALITIES

[013] The polyethylene homopolymer compositions of this invention are made of at least two ethylene homopolymer blend components. As used herein, the term homopolymer is intended to convey a meaning Petition 870240100453, dated 11 / 26 / 2024, page 13 / 67 5 / 25 conventional - that is, the polymer is prepared substantially only with ethylene monomer (although it is recognized by those skilled in the art that much smaller quantities - less than 1% - of higher alpha olefins may be present in a conventional homopolymer as a result of contamination of the ethylene stream and / or the polymerization medium).

[014] In one embodiment, the present compositions contain at least one homopolymer blend component that has a very high melt index (also referred to as I2) of 3,000 to 25,000 grams per 10 minutes.

[015] In one embodiment, the present compositions contain at least one homopolymer blend component that has a very high melting index (also referred to as I2) of 3,000 to 8,500 grams per 10 minutes.

[016] In one embodiment, the overall polyethylene composition will have: (i) a density of 0.96 to 0.97 g / cm3; (ii) a Mw of 75,000 to 95,000; (iii) a Mn less than or equal to 12,000 (or in another form, less than or equal to 10,000); (iv) a Mz of 200,000 to 325,000 (or in another form, less than or equal to 300,000); (v) an Mw / Mn of 6 to 12; (vi) an I2, as determined by ASTM D1238 at 190°C, using a 2.16 kilogram load, from 1.5 to 2.8 grams for 10 minutes; and (vii) a molecular weight distribution such that 25 to 55% by weight (or in other embodiments greater than 30% by weight) of the composition has a molecular weight less than 20,000 (i.e., when the molecular weight distribution of the homopolymer composition is plotted as a conventional molecular weight versus mass fraction graph, the cumulative % by weight of the composition of this invention is such that at least 25% by weight and up to 55% by weight has a molecular weight less than 20,000). Petition 870240100453, dated 11 / 26 / 2024, p. 14 / 67 6 / 25 20,000).

[017] In one embodiment, the overall polyethylene composition will have: (i) a density of 0.96 to 0.97 g / cm3; (ii) a Mw of 75,000 to 95,000; (iii) a Mn less than or equal to 12,000 (or in another form, less than or equal to 10,000); (iv) a Mz of 200,000 to 325,000 (in another modality, less than or equal to 300,000); (v) an Mw / Mn of 6 to 12; (vi) an I2, as determined by ASTM D1238 at 190°C, using a charge of 2.16 kilograms, from 1.5 to 2.8 grams for 10 minutes; and (vii) a molecular weight distribution such that 25 to 45% by weight (or in other embodiments greater than 30% by weight) of the composition has a molecular weight less than 20,000 (i.e., when the molecular weight distribution of the homopolymer composition is plotted as a conventional molecular weight versus mass fraction graph, the cumulative % by weight of the composition of this invention is such that at least 25% by weight and up to 45% by weight has a molecular weight less than 20,000).

[018] In one embodiment, the composition is essentially free of any polyethylene with a molecular weight greater than 900,000 (for greater certainty, less than 1% by weight has a molecular weight greater than 900,000).

[019] In one embodiment, the polyethylene composition has a number average molecular weight, Mn, of 7,000 to 10,000.

[020] In one embodiment, the polyethylene composition has an average molecular weight Z, Mw of 200,000 to 300,000.

[021] In one form, at least 25% by weight, or at least 30% by weight, or at least 35% by weight, or at least 40% by weight of the composition Petition 870240100453, dated 11 / 26 / 2024, page 15 / 67 7 / 25 of polyethylene has a molecular weight of less than 20,000.

[022] In one embodiment, at least 99% by weight of the polyethylene composition has a molecular weight of less than 900,000.

[023] Both components of the homopolymer blend will often also have a narrow molecular weight distribution (Mw / Mn of 2.5 or less).

[024] In one embodiment of the invention, the polyethylene composition comprises at least two ethylene homopolymer blend components: a first blend component containing 45 to 60% by weight of the polyethylene composition and a second blend component containing 55 to 40% by weight of the polyethylene composition.

[025] In one embodiment, the first mixture component has a lower weight-average molecular weight, Mw, than the second mixture component.

[026] In one embodiment, the first mixing component has a higher melting index, I2 (as determined by ASTM D1238 at 190°C, using a charge of 2.16 kilograms) than the second mixing component.

[027] In one embodiment of the invention, the first mixing component has an Mw / Mn of 1.8 to 2.5.

[028] In one embodiment of the invention, the first mixing component has a melting index, I2, as determined by ASTM D1238 at 190°C, using a charge of 2.16 kilograms, from 3,000 to 25,000 grams for 10 minutes, or from 3,000 to 20,000 grams for 10 minutes, or from 3,000 to 15,000 grams for 10 minutes, or from 3,000 to 10,000 grams for 10 minutes, or from 3,000 to 8,500 grams for 10 minutes.

[029] In one embodiment of the invention, the second mixing component has an Mw / Mn of 1.8 to 2.5.

[030] In one embodiment of the invention, the second mixing component has a melting index, I2, as determined by ASTM D1238 at 190°C, using Petition 870240100453, dated 11 / 26 / 2024, p. 16 / 67 8 / 25 a load of 2.16 kilograms, from 0.05 to 0.5 grams for 10 minutes.

[031] The present compositions can be used to prepare films with a good balance of optical and barrier properties, as will be illustrated in the Examples.

[032] While not wishing to be limited by theory, it is believed that: 1) The good optical properties of films made from these compositions are a result of Mz being controlled to a value less than or equal to 325,000 (especially less than or equal to 300,000); 2) The excellent barrier properties (low WVTR) of the films are a result of a combination of: (i) the low molecular weight of the first component of the mixture (i.e., at least 25% by weight of the mixture has an absolute molecular weight of less than 20,000); the Mn of the composition is low (less than or equal to 12,000, especially less than or equal to 10,000); (ii) both components of the mixture having a molecular weight distribution (Mw / Mn) less than or equal to 2.5; and (iii) the large difference in the molecular weight of the components of the mixture - with the result that the molecular weight distribution of the composition is 6 to 12.

[033] The homopolymer compositions of this invention can generally be used to prepare a wide variety of molded or extruded products. However, they will frequently be used in films, especially blown films. Certain plastic films produced with the present compositions have a desirable balance of optical properties and barrier properties (or, alternatively, low WVTR state). Such films can be single-layer or multi-layer. In multi-layer films, the compositions can be suitably employed in at least one skin layer or, alternatively, in a core layer of a 3, 5 or 7-layer film. In one embodiment, the compositions are used in the core layer of a multi-layer film with conventional HDPE resins (such as those prepared with Petition 870240100453, dated 11 / 26 / 2024, page 17 / 67 9 / 25 a Zeigler Natta or chromium catalyst) being used in the skin layers. In one embodiment, a multilayer film may also contain a core layer made of ethylene-vinyl alcohol copolymer (EVOH) to further enhance barrier properties.

[034] The present compositions can be prepared by any conventional mixing technique or alternatively, by homopolymerization of ethylene in a multireactor polymerization system. If the compositions are produced by a polymerization method, then a catalyst capable of producing polyethylene with a molecular weight distribution, Mw / Mn, less than or equal to 2.5 is used in all polymerization reactors. The use of a double reactor solution polymerization process using a single-site catalyst is suitable and is illustrated in the Examples.

[035] Multireactor polymerization systems are well known to those skilled in the art. A description of the dual reactor solution polymerization system that can be used in this invention is given in U.S. Patent No. 6,372,864 (Brown).

[036] The term single-site catalyst is also well known to those skilled in the art and is used here to convey its conventional meaning. In general, a single-site catalyst will produce ethylene homopolymers with a narrow molecular weight distribution (i.e., Mw / Mn less than or equal to 2.5) in a well-mixed polymerization reactor and will copolymerize ethylene with a higher alpha olefin (such as butene, hexene, or octene) in a manner that produces a regular distribution of the comonomer within the copolymers.

[037] Examples of single-site catalyst systems include the following catalysts: metallocenes, restricted geometry catalysts, or phosphinimine catalysts when used in combination with a methylaluminoxane (MAO) cocatalyst or a boron activator (such as a trityl or aniline salt of Petition 870240100453, dated 11 / 26 / 2024, p. 18 / 67 10 / 25 tetraquis (pentafluorophenyl) boron).

[038] Other descriptions of single-site catalysts are provided in U.S. Patent No. 6,689,847 (including the references therein).

[039] Additional examples of linear ethylene homopolymers that have been produced with single-site catalysts (such as metallocene catalysts or constrained geometry catalysts) are suggested in U.S. Patent No. 6,419,966 (Davis). Similarly, a review of linear ethylene homopolymers prepared with “constrained geometry” catalysts is suggested in 2003 / 0088021 A1 (Van Dun '03). Furthermore, Van Dun's invention provides a review of resin blends containing an ethylene homopolymer blend component with a molecular weight distribution greater than 2.5 (i.e., a blend component that is not prepared with a single-site catalyst).Van Dun specifically teaches that homopolymers derived from typical single-site catalysts have the dual disadvantage of (a) being unable to achieve as high a density for a given molecular weight as comparable Ziegler products; and (b) exhibiting a narrow Mw / Mn ratio across the entire molecular weight range.

[040] It should be noted that catalysts that do not readily produce long-chain branching (LCB) are generally used in this invention. This is because the presence of LCB can reduce the density and / or stiffness (as evidenced by the lower modulus) of films made from the polyethylene homopolymer compositions of this invention.

[041] LCB is determined using 13C nuclear magnetic resonance (NMR) and is quantified using the method defined by Randall (Rev. Macromol. Chem. Phys. C29 (2 and 3) p. 285-297). In one embodiment, the compositions of this invention contain less than 0.3 long-chain branches per 100 carbon atoms, especially less than 0.1 long-chain branches per 1,000 carbon atoms. Petition 870240100453, dated 11 / 26 / 2024, p. 19 / 67 11 / 25

[042] The use of a single-site phosphinimine catalyst system in a double-reactor polymerization process to prepare compositions according to this invention is described in the following non-limiting Examples. Additives

[043] HDPE is often sold with an additive package containing a primary antioxidant (part 1, below) and a secondary antioxidant (part 3, below). The primary antioxidant can be used in an amount of 200 to 2,000 ppm. Similarly, the secondary antioxidant can also be used in an amount of 200 to 2,000 ppm. Other (optional) additives are also described below. 1. Primary Antioxidants 1.1 Alkylated Monophenols

[044] For example, 2,6-di-tert-butyl-4-methylphenol; 2-tert-butyl-4,6-dimethylphenol; 2,6-di-tert-butyl-4-ethylphenol; 2,6-di-tert-butyl-4-n-butylphenol; 2,6-di-tert-butyl-4isobutylphenol; 2,6-dicyclopentyl-4-methylphenol; 2-(alpha-methylcyclohexyl)-4,6 dimethylphenol; 2,6di-octadecyl-4-methylphenol; 2,4,6,-tricyclohexyphenol; and 2,6-di-tert-butyl-4-methoxymethylphenol. 1.2 Alkylated Hydroquinones

[045] For example, 2,6-di-tert-butyl-4-methoxyphenol; 2,5-di-tertbutylhydroquinone; 2,5-di-tert-amylhydroquinone; and 2,6-diphenyl-4-octadecyloxyphenol. 1.3 Hydroxylated Thiodiphenyl Ethers

[046] For example, 2,2'-thio-bis-(6-tert-butyl-4-methylphenol); 2,2'-thio-bis-(4octylphenol); 4,4'-thio-bis-(6-tertbutyl-3-methylphenol); and 4,4'-thio-bis-(6-tert-butyl-2-methylphenol). 1.4 Alkylidene-Bisphenols

[047] For example, 2,2'-methylene-bis-(6-tert-butyl-4-methylphenol); 2,2'-methylene-bis-(6-tert-butyl-4-ethylphenol); 2,2'-methylene-bis-(4-methyl-6-(alpha-methylcyclohexyl)phenol); 2,2'-methylene-bis-(4-methyl-6-cyclohexyphenol); 2,2'-methylene-bis-(6-nonyl-4-methylphenol); 2,2'-methylene-bis-(6-nonyl-4-methylphenol); 2,2'-methylene-bis-(6-(alpha-methylbenzyl)-4-Petition 870240100453, dated 11 / 26 / 2024, page 20 / 67 12 / 25 nonylphenol); 2,2'-methylene-bis-(6-(alpha, alpha-dimethylbenzyl)-4-nonyl-phenol); 2,2'-methylenebis-(4,6-di-tert-butylphenol); 2,2'-ethylidene-bis-(6-tert-butyl-4-isobutylphenol); 4,4'-methylenebis-(2,6-di-tert-butylphenol); 4,4'-methylene-bis-(6-tert-butyl-2-methylphenol); 1,1-bis-(5-tert-butyl-4-hydroxy-2-methylphenol)butane 2,6-di-(3-tert-butyl-5-methyl-2-hydroxybenzyl)-4methylphenol; 1,1,3-tris-(5-tert-butyl-4-hydroxy-2-methylphenyl)butane; 1,1-bis-(5-tert-butyl-4-hydroxy-2-methylphenyl)-3-dodecyl-mercaptobutane; ethylene glycol-bis-(3,3-bis-(3'-tert-butyl4'-hydroxyphenyl)-butyrate)-di-(3-tert-butyl-4-hydroxy-5-methylphenyl)-dicyclopentadiene; di-(2(3'-tert-butyl-2'-hydroxy-5'-methylbenzyl)-6-tert-butyl-4-methylphenyl)terephthalate; and other phenolics such as bisphenol monoacrylate esters such as ethylidiene bis-2,4-di-t-butylphenol monoacrylate ester. 2. UV Absorbers and Light Stabilizers 2.1 2-(2'-hydroxyphenyl)-benzotriazoles

[048] For example, the derivatives of 5'-methyl-,3'5'-di-tert-butyl-, 5'-tert-butyl,5'(1,1,3,3-tetramethylbutyl)-, 5-chloro-3',5'-di-tert-butyl-, 5-chloro-3'-tert-butyl-5'-methyl-3'sec-butyl-5'-tert-butyl-, 4'-octoxy, 3',5'-diterc-amyl-3',5'-bis-(alpha,alpha-dimethylbenzyl). 2,2-Hydroxy-Benzophenones

[049] For example, the derivative of 4-hydroxy-4-methoxy-, 4-octoxy, 4-decyloxy-, 4-dodecyloxy-, 4-benzyloxy, 4,2',4'-trihydroxy- and 2'-hydroxy-4,4'-dimethoxy. 2.3 Sterically Inhibited Amines

[050] For example, bis(2,2,6,6-tetramethylpiperidyl)-sebacate; bis-5 (1,2,2,6,6-pentamethylpiperidyl)-sebacate; bis(1,2,2,6,6-pentamethylpiperidyl)ester of n-butyl-3,5-di-tert-butyl-4-hydroxybenzyl malonic acid; condensation product of 1-hydroxyethyl-2,2,6,6-tetramethyl-4-hydroxy-piperidine and succinic acid; condensation product of N,N'-(2,2,6,6-tetramethylpiperidyl)-hexamethylenediamine and 4-tert-octylamino-2,6-dichloro-1,3,5-s-triazine; tris-(2,2,6,6-tetramethylpiperidyl)-nitrilotriacetate, tetrakis(2,2,6,6-tetramethyl-4-piperidyl)-1,2,3,4-butanetetracarbonic acid; and 1,1'(1,2-ethanediyl)-bis(3,3,5,5-tetramethylpiperazinone). These amines are commonly called HALS. Petition 870240100453, dated 11 / 26 / 2024, page 21 / 67 13 / 25 (Hindered Amines Light Stabilizing) and include 2,2,6,6-tetramethylpiperidinol esters of butane tetracarboxylic acid. Such amines include hydroxylamines derived from hindered amines, such as di(1-hydroxy-2,2,6,6-tetramethylpiperidin-4-yl)sebacate; 1-hydroxy-2,2,6,6-tetramethyl-4-benzoxypiperidine; 1-hydroxy-2,2,6,6-tetramethyl-4-(3,5-di-tert-butyl-4-hydroxyhydrocinnamoyloxy)-piperdine; and N-(1-hydroxy-2,2,6,6-tetramethylpiperidin-4-yl)-epsiloncaprolactam. 3. Secondary Antioxidants 3.1 Phosphites and Phosphonites

[051] For example, triphenyl phosphite; diphenylalkyl phosphates; phenyldialkyl phosphates; tris(nonyl-phenyl) phosphite; trilauryl phosphite; trioctadecyl phosphite; distearyl pentaerythritol diphosphite; tris(2,4-di-tert-butylphenyl) phosphite; diisodecyl pentaerythritol diphosphite; 2,4,6-tri-tert-butylphenyl-2-butyl-2-ethyl-1,3-propanediol phosphite; bis(2,4-ditert-butylphenyl) pentaerythritol diphosphite Trisaryl sorbitol triphosphite; and tetrakis(2,4-di-tertbutylphenyl)4,4'-biphenylene diphosphonite. 3.2 Hydroxylamines and Amine Oxides

[052] For example, N,N-dibenzylhydroxylamine; N,N-diethylhydroxylamine; N,N-dioctylhydroxylamine; N,N-dilaurylhydroxylamine; N,N-ditetradecylhydroxylamine; N,N-dihexadecylhydroxylamine; N,N-dioctadecylhydroxylamine; N-hexadecyl-N-octadecylhydroxylamine; N-heptadecyl-N-octadecylhydroxylamine; and N,N-dialkylhydroxylamine derived from hydrogenated tallow amines. Analogous amine oxides are also suitable. 4. Slip Agents

[053] For example, oleamide; erucamide; stearamide; behenamide. 5. Fillers, Antiblocking Agents and Reinforcing Agents

[054] For example, calcium carbonate; diatomaceous earth; natural and synthetic silica; silicates; glass fibers; asbestos; talc; kaolin; mica; barium sulfate; metallic oxides and hydroxides; carbon black; and graphite. Petition 870240100453, dated 11 / 26 / 2024, page 22 / 67 14 / 25 6. Various Additives

[055] For example, plasticizers; epoxidized vegetable oils, such as epoxidized soybean oils; lubricants; emulsifiers; pigments; optical brighteners; fireproofing agents; antistatic agents; antifogging agents; blowing agents; and thiosynergis, such as dilaurylthiodipropionate or distearylthiodipropionate. 7. Nucleating Agents

[056] In one embodiment, the compositions of this invention are used to prepare films containing a nucleating agent. Examples of suitable nucleating agents include the cyclic organic structures described in U.S. Patent No. 5,981,636 (and salts thereof, such as disodium bicyclo[2.2.1]heptene dicarboxylate); saturated versions of the structures described in U.S. Patent No. 5,981,636 (as described in U.S. Patent No. 6,465,551; Zhao et al., for Milliken); salts of certain cyclic dicarboxylic acids with a hexahydrophthalic acid structure (or “HHPA” structure) as described in U.S. Patent No. 6,599,971 (Dotson et al., for Milliken); zinc glycerol; and phosphate esters, such as those described in U.S. Patent No. 5,342,868 and sold under the trade names NA-11 and NA-21 by Asahi Denka Kogyo.In one embodiment, the nucleating agent is a cyclic dicarboxylate or a salt thereof, especially divalent metal or metalloid salts (particularly calcium salts) of the HHPA structures described in U.S. Patent 6,599,971. For clarity, the HHPA structure generally comprises a ring structure with six carbon atoms in the ring and two carboxylic acid groups that are substituents on adjacent atoms of the ring structure. The other four carbon atoms in the ring may be substituted as described in U.S. Patent No. 6,599,971. In one embodiment, the nucleating agent is 1,2-cyclohexanedicarboxylic acid, calcium salt (CAS Registry Number 491589-22-1) – and – in another embodiment, this nucleating agent is added in an amount of 200 to 2,000 ppm (especially 500 to 1,500). Petition 870240100453, dated 11 / 26 / 2024, page 23 / 67 15 / 25 ppm), based on HDPE weight.

[057] In the Examples, the physical properties of the polymers were measured using the methods described below:

[058] Melting index, I2, measurements were made in accordance with ASTM D1238 (I2 using a load of 2.16 kg at 190°C and I21 using a load of 21 kg at 190°C).

[059] Density (g / cm3) was measured according to ASTM D792. Film density was measured according to ASTM D1505.

[060] The turbidity of the films was measured in accordance with ASTM D1003.

[061] The film brightness was measured in accordance with ASTM D2457.

[062] Mn, Mw and Mz (g / mol) were determined by Gel Permeation Chromatography and measured according to ASTM D6474-99.

[063] If the mixture components are made as separate polymers, then the methods described above can be used to directly measure the properties (such as melt index, density, Mn, Mw, and Mw / Mn) of the mixture components and the overall composition. However, if the composition is made in a multireactor process that produces an in situ mixture, then curve fitting techniques can be used to deconvolve / estimate properties and quantities of the mixture components in the overall composition. In general, this type of deconvolution is performed starting with the GPC chromatogram / curve for the overall resin and then using various Flory distributions to arrive at a “best fit” for the chromatogram / curve. This deconvolution technique is well known to those skilled in the art.

[064] A technique for estimating the melt index of the low molecular weight blend component is described below. It will be recognized by those skilled in the art that the melt index (I2) is inversely proportional to the molecular weight for polyethylene resins. This has been confirmed for HDPE resins of Petition 870240100453, dated 11 / 26 / 2024, page 24 / 67 16 / 25 homopolymer with a narrow molecular weight distribution (less than 3) preparing a graph of log(I2) versus log (weight-average molecular weight, Mw). In order to prepare this graph, the melt index (I2) and weight-average molecular weight (Mw) of more than 15 different homopolymer HDPE resins were measured. These homopolymer HDPE resins had a narrow molecular weight distribution (less than 3), but had different Mw values ​​- ranging from about 30,000 to 150,000. (As will be appreciated by those skilled in the art, it is difficult to obtain reproducible I2 values ​​for polyethylene resins with a molecular weight that is outside this range).

[065] A log / log plot of these I2 and Mw values ​​was used to calculate the following relationship between I2 and Mw for such homopolymer HDPE resins: I2 = (1.774 x 1019) x (Mw-3.86).

[066] Extrapolation (based on the relationship above) was used to estimate the I2 values ​​of the low molecular weight fractions of the compositions of the invention shown in the examples. That is, Mw values ​​were used to estimate the I2 values.

[067] Water Vapor Transmission Rate (WVT, expressed in grams of water vapor transmitted per 100 square inches of film per day at a specified film thickness (mils), or g / 100 in² / day) was measured in accordance with ASTM F1249-90 with a MOCON permatron developed by Modern Controls Inc. under conditions of 100°F (37.8°C) and 100% relative humidity. Oxygen Transmission Rate (OTR, expressed in cubic centimeters of oxygen per 100 square inches of film per day at a specified film thickness (mils), or cc / 100 in² / day) was measured using an instrument sold under the MOCON OXTRA System brand, model 2 / 21T.

[068] The polymerization conditions and polymer properties are shown in Table 1. Petition 870240100453, dated 11 / 26 / 2024, page 25 / 67 17 / 25 EXAMPLES Polymerizations

[069] These examples used a dual reactor solution polymerization process in which the contents of the first reactor flow into the second reactor. The use of the two reactors provides “in situ” polymer mixtures. Both reactors were sufficiently stirred to provide well-mixed conditions. The volume of the first reactor was 12 liters and the volume of the second reactor was 24 liters. The first reactor was operated at a reactor pressure of approximately 13,000 kPa (approximately 2.0 x 10³ psi). The second reactor was at a sufficiently lower pressure to facilitate continuous flow from the first reactor to the second. The solvent used was methyl pentane. The process is continuous in all feed streams.

[070] The catalyst used in all experiments was a titanium (IV) complex with a cyclopentadienyl ligand (“Cp”), two chloride ligands and a tri(butyl tertiary) phosphinimine ligand, namely: CpTi(NP(tBu)3)Cl2. The concentration of catalyst that was added to each reactor is shown in Table 1, expressed in parts per million (ppm) of Ti (based on the total weight of the reactor contents).

[071] A boron cocatalyst (namely triphenyl carbene or tetrakis pentafluorophenyl boron trityl salt) was used in an approximately stoichiometric amount (based on the titanium content in the catalyst). A commercially available methylaluminoxane (“MMAO7”, from Akzo Nobel) was also included at an Al / Ti ratio of about 40 / 1. 2,6-di-tertiary butylhydroxy 4-ethylbenzene was added to the MAO to eliminate free trimethylaluminum (TMA) in the MAO (at an Al / OH ratio of about 0.5 to 1, based on the Al content in the TMA).

[072] Hydrogen is added to the reactor as a chain transfer agent. In one embodiment, 0.5 to 2 parts per million by weight (ppm) of hydrogen are added to the first reactor and 35 to 55 ppm to the second reactor (based on the total weight of the reactor contents). Petition 870240100453, dated 11 / 26 / 2024, page 26 / 67 18 / 25

[073] The term “ethylene separation” refers to the fraction of total ethylene that is directed to this reactor.

[074] Other polymerization conditions and some properties of the resulting high-density polyethylene (HDPE) compositions are shown in Table 1. TABLE 1 Pilot Plant Process Conditions and Resin Parameters for a HDPE (targeting a fusion index, I2 = approximately 2) Pilot Plant 2 MIHDPE From Invention 1 From Invention 2 From Invention 3 From Invention 4 From Invention 5 Comparative 1 Comparative 2 Reactor 1 Ethylene separation (%) 50 45 45 50 50 35 50 Hydrogen for reactor (ppm) 1.1 0.91 1.1 1.78 1.68 0.85 1.97 Solvent (kg / h) 374 347 347 381 383 270 381 Reactor inlet temperature (°C) 35 35 35 30 35 30 30 Reactor temperature (°C) 163 163 163 163 163 163 163 Catalyst for reactor (ppm) 0.15 0.15 0.11 0.11 0.09 0.11 0.1 Percentage of ethylene converted 93 93.5 93.5 93.5 93.5 93.5 93.5 Reactor 2 Ethylene separation (%) 50 55 55 50 50 65 50 Hydrogen for reactor (ppm) 40 45 40 40 45 12 15 Solvent (kg / h) 226 253 253 219 217 330 219 Reactor inlet temperature (°C) 40 35 35 42 45 40 41 Reactor temperature (°C) 193 193 193 193 193 193 193 Catalyst 0.5 0.55 0.24 0.24 0.29 0.12 0.15 Petition 870240100453, dated 11 / 26 / 2024, page 27 / 67 19 / 25 For reactor (ppm) Percentage of ethylene converted 85.2 84.0 84.0 81.9 81.7 82.1 82.0 Whole polymer Density (g / cm3) - Total 0.965 0.966 0.965 0.967 0.967 0.963 0.963 Melting index (g / 10 min) - Total 1.9 2.1 2.0 2.0 2.2 1.9 2.0 Melt flow index ratio - Total 44 59 56 45 38 47 37 Mn - Total 8887 8044 9792 7437 10521 23536 21630 Mw - Total 86068 80396 84166 86432 91284 97512 88991 Mz - Total 261506 253136 274454 322204 248611 301957 225814 Mw / Mn - Total 9.7 10.0 8.6 11.6 8.7 4.14 4.11 % by weight @ MW < 20000 Total 47 53 49 49 45 24 28 Reactor 1 % by weight of reactor polymer 1 48 43 43 47 51 36 47 Melting index (g / 10 min) 0.13 0.10 0.09 0.12 0.13 0.05 0.15 Mw 167000 176000 181000 173000 167000 211000 159000 Reactor 2 % by weight of polymer reactor 2 52 57 57 53 49 64 53 Melting index (g / 10 min) 8250 8250 3000 12500 4750 60 150 Mw 9450 9450 12200 8480 11100 34000 27000 Part C.1: Blown Film

[075] The HDPE compositions shown in Table 1 were used to prepare films on a blown film line manufactured by Gloucester Engineering Corporation of Gloucester, MA. The compositions contained 500 parts per million by weight (ppm) of a primary antioxidant (a hindered phenol, sold under the trademark IRGANOX® 1076), 500 ppm of a secondary antioxidant (a phosphite, Petition 870240100453, dated 11 / 26 / 2024, page 28 / 67 20 / 25 sold under the trademark IRGAFHOS® 168) and a nucleating agent. The nucleating agent was purchased from Milliken (and is reported to be a combination of a) the calcium salt of HHPA and; b) zinc stearate, in a weight ratio of 2 / 1) and was added in an amount of 1200 ppm. The blown film line was equipped with a single-screw extruder with a 2.5-inch (6.35 cm) diameter screw, a 24:1 length / diameter screw ratio, and an annular die with a diameter of 4 inches (10.16 cm). The die clearance was set at 35 mils. A conventional temperature profile for HDPE extrusion was used. A double air ring was used for film cooling. The film thickness was 1.5 mils and a burst ratio (BUR) of 2:1 was used to prepare the films.

[076] The properties of the films are shown in the attached Tables. TABLE 2 Barrier Data HDPE Resins WVTR** (g / 100 in² / day) OTR** (cc / 100 in² / day) HDPE- 1 MI (Comparative) 0.0775 33 From invention 1 0.061 25 From invention 2 0.06 23 From invention 3 0.0454 25 From invention 4 0.0711 28 From invention 5 0.0637 28 Comparative 1 0.0903 38 Comparative 2 0.0867 37

[077] The WVTR values ​​shown in Table 2 are as measured for films that are 1.5 mil thick (i.e., they have not been normalized to a value that would be expected for a 1 mil thick film). HDPE-1 MI is comparative - the melting index of this HDPE is 1.2 grams per 10 minutes, which is very low for the compositions of this invention. HDPE-1 MI is a commercial product that has achieved commercial success for the preparation of barrier films that are used for packaging dry foods. TABLE 3 Petition 870240100453, dated 11 / 26 / 2024, page 29 / 67 21 / 25 Optical Data HDPE Resins Turbidity** (%) Gloss @ 45o** (%) HDPE- 1 MI (Comparative) 32 28 Of the invention 1 22 41 Of the invention 2 24 38 Of the invention 3 27 30 Of the invention 4 28 29 Of the invention 5 34 24 Comparative 1 28 25 Comparative 2 26 30 **Turbidity and brightness data for 1.5 mil blown films. Discussion of Optical Properties.**

[078] Again, the values ​​are reported as measured for the 1.5 mil thick films (i.e., not normalized) and HDPE-1 is comparator and made with a commercially available HDPE with a melt index of 1.2 grams per 10 minutes, which is very low for the compositions of this invention. The films of invention 1-5 were shown to exhibit better barrier properties than the film made with HDPE-1 (in Table 2). The data in Table 3 showed that the films of invention 1-4 also exhibit better optical properties than the comparator film made of HDPE-1. The films of invention 1-4 also exhibit better optical properties than the two comparator films shown at the bottom of Table 3, which is interesting because comparators 1-2 were also made with HDPE resins with a melt index of about 2 (as is required for the compositions of this invention). The films of invention 1-3 have especially good optical properties.All compositions of invention 1-3 have an Mn of less than 10,000; an Mz of less than 300,000 and an Mw of less than 90,000. Preparation of Multilayer Films

[079] Multilayer films with three layers (structure A / B / C) were prepared in this example. The skin layers (A and C) were 25% by weight (each) of the total structure and were made with conventional HDPE (prepared with a Petition 870240100453, dated 11 / 26 / 2024, page 30 / 67 22 / 25 Zeigler Natta catalyst in a conventional solution polymerization reactor, with a melting index, I2, of about 1 gram / 10 minutes and a density of about 0.95 g / cm3). The core layer (50% by weight of the total structure) was made with the composition of invention 1 or 2 from example 1. The barrier properties of the films are shown in Table 4. TABLE 4 Multilayer Films HDPE core layer 3-layer film structure Normalized WVTR (g.mil / 100 in2 / day) Normalized OTR (cc.mil / 100 in2 / day) HDPE-1 (Comparative) 0.1669 72.9 From invention 1 0.1294 57.1 From invention 2 0.1545 62.1 TABLE 5 Secant Modulus MD at 1% of Deformation Data. HDPE Resins Drying Modulus (MPa) HDPE-1 (Comparative) 819 From invention 1 933 From invention 2 976 From invention 3 915 From invention 4 1212 From invention 5 832 Comparative 1 1045 Comparative 2 1076 Module Discussion

[080] It is desirable that HDPE films have relatively high stiffness (as evidenced by having relatively high modulus values). The compositions of this invention have a higher melt index than the melt index of HDPE1 and a higher melt index normally causes a lower stiffness / modulus. However, the data in Table 5 show that the compositions of this invention can also be used to prepare films that have desirable stiffness / modulus. The secant modulus was measured generally in accordance with ASTM D882.

[081] Non-limiting embodiments of the present invention include the following: Petition 870240100453, dated 11 / 26 / 2024, page 31 / 67 23 / 25

[082] Modality A. A polyethylene composition comprising at least two ethylene homopolymer mixture components, wherein said composition has: (i) a density of 0.96 to 0.97 g / cm3; (ii) a Mw of 75,000 to 95,000; (iii) a Mn of 7,000 to 12,000; (iv) a Mz of 200,000 to 325,000; (v) a molecular weight distribution, Mw / Mn, of 6 to 12; (vii) a melting index, I2, as determined by ASTM D1238 at 190°C, using a charge of 2.16 kilograms, from 1.5 to 2.8 grams for 10 minutes; and further characterized by; (viii) 25 to 55% by weight of said composition has a molecular weight less than or equal to 20,000; wherein the said composition comprises a first mixing component containing 45 to 60% by weight of said composition and a second mixing component containing 55 to 40% by weight of said composition, wherein said first mixing component has: A1) an Mw / Mn ratio of 1.8 to 2.5; and A2) a melting index, I2, as determined by ASTM D1238 at 190°C, using a charge of 2.16 kilograms, from 3,000 to 25,000 grams for 10 minutes; and wherein said second mixing component has: B1) an Mw / Mn ratio of 1.8 to 2.5; and B2) Melting index, I2, as determined by ASTM D1238 at 190°C, using a charge of 2.16 kilograms, from 0.05 to 0.5 grams for 10 minutes.

[083] Modality B. The polyethylene composition of Modality A, where the aforementioned Mn is from 7,000 to 10,000.

[084] Modality C. The polyethylene composition of Modality A or B, in Petition 870240100453, dated 11 / 26 / 2024, p. 32 / 67 24 / 25 that the aforementioned Mz is between 200,000 and 300,000.

[085] Modality D. The polyethylene composition of Modality A, B or C, wherein said first mixing component has a melt index, I2, as determined by ASTM D1238 at 190°C, using a charge of 2.16 kilograms, from 3,000 to 8,500 grams for 10 minutes.

[086] Modality E. The polyethylene composition of Modality A, B, C or D, in which at least 40% by weight of said composition has a molecular weight of less than 20,000.

[087] Modality F. The polyethylene composition of Modality A, B, C, D or E, in which at least 99% by weight of said composition has a molecular weight less than or equal to 900,000.

[088] Modality G. The polyethylene composition of Modality A, B, C, D, E or F comprising a nucleating agent.

[089] Embodiment H. The polyethylene composition of Embodiment G, in which the nucleating agent comprises a salt of a dicarboxylic acid.

[090] Modality I. The polyethylene composition of Modality G, wherein the nucleating agent comprises a calcium salt of hexahydrophthalic acid.

[091] Modality J. A film made from the polyethylene composition of Modality A, B, C, D, E, F, G, H or I.

[092] Modality K. A film made from the polyethylene composition of Modality A, B, C, D, E, F, G, H or I with a turbidity value of less than 30%.

[093] Embodiment L. A process for preparing the polyethylene composition of Embodiment A, said process comprising contacting at least one single-site polymerization catalyst system with ethylene under polymerization conditions for said ethylene in at least two polymerization reactors, including a first polymerization reactor and a second polymerization reactor, and mixing the polyethylene produced in each polymerization reactor, Petition 870240100453, dated 11 / 26 / 2024, page 33 / 67 25 / 25 wherein hydrogen is added to said first polymerization reactor so as to provide a concentration of 0.5 to 2 ppm in said first polymerization reactor, and wherein hydrogen is added to the second polymerization reactor so as to provide a hydrogen concentration of 35 to 55 ppm in said second polymerization reactor.

[094] Mode M. The process according to Mode L, in which the aforementioned polymerization conditions are solution polymerization conditions.

[095] Modality N. The process according to Modality M, wherein said at least two polymerization reactors are operated in such a way that there is a temperature difference of at least 30°C between said at least two polymerization reactors. INDUSTRIAL APPLICABILITY

[096] A polyethylene homopolymer composition is provided that can be used to prepare polymer films with a good balance of optical properties and resistance to moisture transmission.

Claims

1. Polyethylene composition CHARACTERIZED in that it comprises at least two ethylene homopolymer blend components, wherein said composition has: (i) a density of 0.96 to 0.97 g / cm3; (ii) a Mw of 75,000 to 95,000; (iii) a Mn of 7,000 to 12,000; (iv) a Mz of 200,000 to 325,000; (v) a molecular weight distribution, Mw / Mn, of 6 to 12; (vii) a melt index, I2, as determined by ASTM D1238 at 190 °C, using a charge of 2.16 kilograms, of 1.5 to 2.8 grams for 10 minutes; and further (viii) 25 to 55% by weight of said composition has an absolute molecular weight less than or equal to 20.000, as determined by Gel Permeation Chromatography and measured in accordance with ASTM D6474-99; wherein said composition comprises a first mixing component containing 45 to 60% by weight of said composition and a second mixing component containing 55 to 40% by weight of said composition, wherein said first mixing component has: A1) an Mw / Mn of 1.8 to 2.5; and A2) a melting index, I2, as determined by ASTM D1238 at 190 °C, using a charge of 2.16 kilograms, from 3,000 to 25,000 grams for 10 minutes; and wherein said second mixing component has: B1) an Mw / Mn of 1.8 to 2.5; and B2) a melting index, I2, as determined by ASTM D1238 at 190 °C, using a charge of 2.16 kilograms, from 0.05 to 0.5 grams for 10 minutes.

2. Polyethylene composition, according to claim 1, CHARACTERIZED in that said Mn is from 7,000 to 10,000. Petition 870260097533, dated 09 / 22 / 2026, page 8 / 13 2 / 3 3. Polyethylene composition, according to claim 2, CHARACTERIZED in that said Mz is from 200,000 to 300,000.

4. Polyethylene composition, according to claim 1, CHARACTERIZED in that said first component of the mixture has a melt index, I2, as determined by ASTM D1238 at 190 °C, using a charge of 2.16 kilograms, from 3,000 to 8,500 grams for 10 minutes.

5. Polyethylene composition, according to claim 1, CHARACTERIZED in that at least 40% by weight of said composition has an absolute molecular weight of less than 20,000.

6. Polyethylene composition, according to claim 1, CHARACTERIZED in that at least 99% by weight of said composition has an absolute molecular weight of less than or equal to 900,000.

7. Polyethylene composition, according to any one of claims 1 to 6, CHARACTERIZED in that it comprises a nucleating agent.

8. Polyethylene composition according to claim 7, CHARACTERIZED in that the nucleating agent comprises a salt of a dicarboxylic acid.

9. Polyethylene composition according to claim 7, CHARACTERIZED in that the nucleating agent comprises a calcium salt of hexahydrophthalic acid.

10. Film CHARACTERIZED by the fact that it is made from a polyethylene composition as defined in any one of claims 1 to 9.

11. Film CHARACTERIZED by the fact that it is made from a polyethylene composition, as defined in any of claims 1 to 9, with a turbidity of less than 30%. Petition 870260097533, dated 09 / 22 / 2026, page 9 / 13 3 / 3 12. Film CHARACTERIZED by the fact that it is made from a polyethylene composition, as defined in claim 3, with a turbidity of less than 30%.

13. Process for preparing the polyethylene composition, as defined in claim 1, CHARACTERIZED in that said process comprises contacting at least one single-site polymerization catalyst system with ethylene under polymerization conditions for said ethylene in at least two polymerization reactors, including a first polymerization reactor and a second polymerization reactor, and mixing together the polyethylene produced in each polymerization reactor, wherein hydrogen is added to said first polymerization reactor so as to provide a concentration of 0.5 to 2 ppm in said first polymerization reactor, and wherein hydrogen is added to the second polymerization reactor so as to provide a hydrogen concentration of 35 to 55 ppm in said second polymerization reactor.

14. Process according to claim 13, CHARACTERIZED in that said polymerization conditions are solution polymerization conditions.

15. Process according to claim 14, CHARACTERIZED in that said at least two polymerization reactors are operated such that there is a temperature difference of at least 30 °C between said at least two polymerization reactors.