Laminate
A multilayer laminate with ethylene-vinyl alcohol copolymer and ethylene-acid copolymer ionomer layers, bonded to a polyethylene film, addresses recyclability issues of existing laminates by maintaining performance and enabling faster packaging speeds.
Patent Information
- Application Number
- BR112022024835
- Authority / Receiving Office
- BR · BR
- Patent Type
- Patents
- Current Assignee / Owner
- Publication Date
- 2026-11-17
AI Technical Summary
Existing laminates incorporating polypropylene, polyamide, and poly(ethylene terephthalate) are difficult to recycle due to incompatible materials, limiting their recyclability and sustainability.
A laminate comprising a multilayer film with a barrier layer of ethylene-vinyl alcohol copolymer, a sealing layer of ethylene-acid copolymer ionomer or polyethylene elastomer with a peak melt temperature of 100 °C or less, and a bonding layer, bonded to a polyethylene film with a density of 0.900 to 0.970 g/cm³, allowing for compatibility in polyethylene recycling streams.
The laminate maintains or enhances properties like barrier sealing performance, oxygen transmission rate, water vapor transmission rate, heat seal initiation temperature, heat seal strength, and heat adhesion strength, while enabling faster packaging speeds and improved recyclability.
Smart Images

Figure 00000033_0000 
Figure 00000034_0000
Abstract
Description
"LAMINATE" TECHNICAL FIELD
[001] The embodiments of the present disclosure generally relate to laminates and, more particularly, to laminates including polyethylene. INTRODUCTION
[002] Laminates incorporating polypropylene, polyamide, and poly(ethylene terephthalate) contain multiple layers and are widely used in flexible packaging for consumer products. For example, a typical flexible packaging laminate might include an outer printing substrate of biaxially oriented polypropylene (BOPP), a barrier layer of metallized films, an adhesive layer of solvent-based adhesive, and a sealing layer of polyethylene. The combination of layers and materials can provide heat resistance for a wide sealing window, good printability, high barrier performance, and shrink-free sealing. However, such laminates can be difficult, if not impossible, to recycle together due to the different types of materials that are not compatible for recycling with each other.As the demand for sustainable and recyclable materials continues to increase, there remains a strong need for laminates that can be recycled more easily and that exhibit comparable or improved performance properties compared to existing structures. SUMMARY
[003] The embodiments of the present disclosure meet the aforementioned needs by providing laminates that can be fully compatible for recycling in polyethylene recycling streams. The performance of the laminates of the invention may be better than, or at least comparable to, other laminates, such as laminates comprising BOPP, and may allow for the use of faster packaging speeds during manufacturing. For example, in certain aspects, the laminates may exhibit enhanced or maintained properties such as barrier sealing performance, oxygen transmission rate (OTR), water vapor transmission rate (WVTR), heat seal initiation temperatures (HSIT), heat seal strength, heat adhesion strength, Petition 870250007322, dated 01 / 29 / 2025, page 12 / 77 2 / 30th of the hot bonding initiation temperature, and / or shrinkage, when compared to existing laminates.
[004] A laminate is disclosed herein. In embodiments, the laminate comprises: (a) a multilayer film comprising: (1) a barrier layer comprising an ethylene-vinyl alcohol copolymer; (2) a sealing layer, wherein the sealing layer comprises at least 70% by weight of an ethylene-acid copolymer ionomer or a polyethylene elastomer / plastomer having a higher peak melt temperature (Tm) of 100 °C or less; and (3) a bonding layer between the barrier layer and the sealing layer; (b) a polyethylene film comprising an ethylene-based polymer having a density of 0.900 to 0.970 g / cm3; and (c) an adhesive that bonds the multilayer film to the polyethylene film.
[005] These and other modalities are described in detail in the Detailed Description. BRIEF DESCRIPTION OF THE DRAWINGS
[006] Figure 1 is a hot seal strength graph of the Comparative and Inventive Examples discussed below.
[007] Figure 2 is a hot adhesion strength graph of the Comparative and Inventive Examples discussed below. DETAILED DESCRIPTION
[008] Aspects of the disclosed laminates are described in more detail below. The laminates of the present disclosure may have a wide variety of applications, including, for example, bags, bags with support base, cushioned bags, bulk bags, pre-produced packaging, sachets, or the like. This disclosure, however, should not be interpreted as limiting the embodiments presented below.
[009] As used herein, the term polymer means a polymeric compound prepared by the polymerization of monomers, whether of the same type or of a different type. The generic term polymer thus encompasses the term homopolymer (used to refer to polymers prepared from only one type of monomer), and the term copolymer or interpolymer. Trace amounts of impurities (e.g., catalyst residues) may be incorporated into and / or within the polymer. A polymer may be a single polymer, a blend of polymers, or a Petition 870250007322, dated 01 / 29 / 2025, page 13 / 77 3 / 30 polymer blends, including blends of polymers that are formed in situ during polymerization.
[0010] As used herein, the terms polyethylene or ethylene-based polymer shall mean polymers comprising a predominant amount (>50 mol %) of units that are derived from ethylene monomer. This includes polyethylene homopolymers or copolymers (meaning units derived from two or more comonomers).Common forms of polyethylene known in the art include low-density polyethylene (LDPE); linear low-density polyethylene (LLDPE); ultra-low-density polyethylene (ULDPE); very low-density polyethylene (VLDPE); single-site catalyst-produced linear low-density polyethylene, including both linear and substantially linear low-density resins (m-LLDPE); ethylene-based plastomers (POP) and ethylene-based elastomers (POE); medium-density polyethylene (MDPE); and high-density polyethylene (HDPE).These polyethylene materials are generally known in the art; however, the following descriptions may be helpful in understanding the differences between some of these different polyethylene resins.
[0011] The term LDPE may also be referred to as high-pressure ethylene polymer or highly branched polyethylene and should mean that the polymer is partially or fully homopolymerized or copolymerized in autoclaves or tubular reactors at pressures above 14,500 psi (100 MPa) using free radical initiators such as peroxides (see, for example, US patent 4,599,392, which is incorporated herein by reference). LDPE resins typically have a density in the range of 0.916 to 0.935 g / cm3.
[0012] The term LLDPE includes resin produced using traditional Ziegler-Natta catalyst systems and chromium-based catalyst systems, as well as single-site catalysts, including but not limited to substituted mono- or bis-cyclopentadienyl catalysts (typically called metallocene), restricted geometry catalysts, phosphinimine catalysts, and aryloxyether catalysts. Petition 870250007322, dated 01 / 29 / 2025, page 14 / 77 4 / 30 polyvalent (typically called bisphenylphenoxy), and includes linear, substantially linear, or heterogeneous copolymers or homopolymers of polyethylene. LLDPEs contain fewer long-chain branches than LDPEs and include the substantially linear ethylene polymers that are further defined in U.S. Patent No. 5,272,236, U.S. Patent No. 5,278,272, U.S. Patent No. 5,582,923, and U.S. Patent No. 5,733,155; the homogeneously branched linear ethylene polymer compositions, such as those in U.S. Patent No. 3,645,992; the heterogeneously branched ethylene polymers, such as those prepared according to the process disclosed in U.S. Patent No. 4,076,698; and / or blends thereof (such as those disclosed in U.S. Document 3,914,342 or U.S. Document 5,854,045).LLDPEs can be produced via gas-phase, solution-phase, or slurry polymerization, or any combination thereof, using any type of reactor or reactor configuration known in the art.
[0013] The term MDPE refers to polyethylenes that have densities of 0.926 to 0.935 g / cm3. MDPE is typically produced using chromium or Ziegler-Natta catalysts or using single-site catalysts including, but not limited to, substituted mono- or bis-cyclopentadienyl catalysts (typically called metallocene), restricted geometry catalysts, phosphinimine catalysts and polyvalent aryloxyether catalysts (typically called bisphenylphenoxy) and typically have a molecular weight distribution (MWD) greater than 2.5.
[0014] The term HDPE refers to polyethylenes with densities greater than about 0.935 g / cm3 and up to about 0.980 g / cm3, which are generally prepared with Ziegler-Natta catalysts, chromium catalysts or single-site catalysts including, but not limited to, substituted mono- or bis-cyclopentadienyl catalysts (typically called metallocene), restricted geometry catalysts, phosphinimine catalysts and polyvalent aryloxyether catalysts (typically called bisphenylphenoxy).
[0015] The term ULDPE refers to polyethylenes that have densities of 0.855 to 0.912 g / cm3, which are generally prepared with Ziegler-Natta catalysts, catalysts of Petition 870250007322, dated 01 / 29 / 2025, p. 15 / 77 5 / 30 chromium or single-site catalysts including, but not limited to, substituted mono- or bis-cyclopentadienyl catalysts (typically called metallocene), restricted geometry catalysts, phosphinimine catalysts, and polyvalent aryloxyether catalysts (typically called bisphenylphenoxy). ULDPEs include, but are not limited to, polyethylene plastomers (ethylene-based) and polyethylene elastomers (ethylene-based).
[0016] As used in this document, the term polyethylene elastomer / plastomer shall mean substantially linear, or linear, ethylene / α-olefin copolymers containing a homogeneous distribution of short-chain branching comprising ethylene-derived units and units derived from at least one C3-C10 α-olefin comonomer, or at least one C4-C8 α-olefin comonomer, or at least one C6-C8 α-olefin comonomer. Polyethylene elastomers / plastomers have a density of 0.865 g / cm3, or 0.870 g / cm3, or 0.880 g / cm3, or 0.890 g / cm3 to 0.900 g / cm3, or 0.902 g / cm3, or 0.904 g / cm3, or 0.909 g / cm3, or 0.910 g / cm3. Non-limiting examples of polyethylene elastomers / plastomers include AFFINITY™ plastomers and elastomers (available from The Dow Chemical Company), EXACT™ plastomers (available from ExxonMobil Chemical), Tafmer (available from Mitsui), Nexlene™ (available from SK Chemicals Co.) and Lucene (available from LG Chem Ltd.).
[0017] The terms comprising, including, having and their derivatives are not intended to exclude the presence of any additional component, step or procedure, whether or not specifically disclosed. In order to avoid any doubt, all compositions claimed through the use of the term comprising may include any additional additive, adjuvant or compound, whether polymeric or otherwise, unless otherwise indicated. Conversely, the term consisting essentially excludes from the scope of any subsequent recitation any other component, step or procedure, except those that are not essential for operability. The term consisting excludes any component, step or procedure not specifically outlined or listed. Multilayer laminate film
[0018] The laminate disclosed here comprises a multi-layered film. The film Petition 870250007322, dated 01 / 29 / 2025, p. 16 / 77 6 / 30 of multiple layers according to the embodiments disclosed herein includes a barrier layer, a sealing layer, and a fixing layer, wherein the fixing layer is positioned between the barrier layer and the sealing layer. For example, the multilayer film according to the embodiments disclosed herein may have an A / B / C structure, wherein A is the barrier layer, B is the fixing layer, and C is the sealing layer. In other embodiments, the multilayer film additionally comprises an outer layer and a second fixing layer, wherein the second fixing layer is positioned between the outer layer and the barrier layer. For example, the multilayer film according to the embodiments disclosed herein may have an A / B / C / D / E structure, wherein A is the outer layer, B is the second fixing layer, C is the barrier layer, D is the fixing layer, and E is the sealing layer.In such configurations, the second fixing layer, B, may have the same or a different composition as the fixing layer, D. Multilayer film barrier layer
[0019] The multilayer film of the laminate comprises a barrier layer.
[0020] In embodiments, the barrier layer of the multilayer film may be positioned adjacent to or in close proximity to a fixation layer described below and may be the outermost layer of the multilayer film. In other embodiments, an outer layer, as described below, is part of the multilayer film and is the outermost layer of the multilayer film, and a second fixation layer, also described below, is positioned between the outer layer and the barrier layer. The barrier layer according to the embodiments disclosed herein comprises an ethylene-vinyl alcohol copolymer (EVOH).
[0021] In embodiments, the barrier layer EVOH has an ethylene content of 20 to 50 mol%. All subranges and individual values of an ethylene content of 20 to 50 mol% are disclosed and included herein. For example, in embodiments, the barrier layer EVOH has an ethylene content of 20 to 50 mol%, or 22 to 45 mol%, or 25 to 40 mol%. One skilled in the art will recognize that the ethylene content of the EVOH can contribute to lower or higher OTR of the laminate disclosed herein (i.e., in general, the lower the ethylene content, the lower the achievable OTR value). One skilled in the art will also recognize that Petition 870250007322, dated 01 / 29 / 2025, p. 17 / 77 7 / 30 A barrier layer comprising an EVOH with a lower ethylene content may be suitable for flexible bottle and tube applications, and a barrier layer comprising an EVOH with a higher ethylene content may allow for easier processing, long-term performance stability, and packaging types that require flexibility (resistance to bending cracks), such as thermoformability.
[0022] Commercially available examples of EVOH that can be used in the barrier layer include those commercially available from Kuraray Co., Ltd. (Tokyo, Japan) under the name EVAL™, including, for example, EVAL™ H171B (ethylene content of 38 mol%) and EVAL™ F171B (ethylene content of 32 mol%).
[0023] Various thicknesses are considered for the multilayer film. In embodiments, the barrier layer is 5 to 25% of the total thickness of the multilayer film. Multi-layer film sealing layer
[0024] The multi-layered laminate film comprises a sealing layer.
[0025] The sealing layer of the multilayer film comprises at least 70% by weight of a (meth)acrylic acid copolymer ionomer (referred to herein as an ethylene-acid copolymer ionomer) or a polyethylene elastomer / plastomer, based on the total weight of the sealing layer. All individual values and subranges of at least 70% by weight are disclosed and included herein. For example, in the embodiments, the sealing layer may comprise at least 70% by weight, at least 80% by weight, at least 90% by weight, at least 95% by weight, at least 99% by weight, at least 99.5% by weight, or from 70% by weight to 100% by weight, 75% by weight to 99% by weight, 80% by weight to 95% by weight, or 90% to 95% by weight of an ethylene-acid copolymer ionomer or a polyethylene elastomer / plastomer, based on the total weight of the sealing layer.
[0026] The sealing layer of the multilayer film comprises at least 70% by weight of an ethylene-acid copolymer or a polyethylene elastomer / plastomer having a higher peak melting temperature (Tm) of 100 °C or less. All individual values and subranges of 100 °C or less are disclosed and included herein. For example, in embodiments, the ionomer of Petition 870250007322, dated 01 / 29 / 2025, page 18 / 77 The 8 / 30 ethylene-acid copolymer or the polyethylene elastomer / plastomer of the sealing layer has a higher peak melt temperature (Tm) of 100 °C or less, 98 °C or less, 96 °C or less, 94 °C or less, or 92 °C or less, or in the range of 70 °C to 100 °C, 70 °C to 95 °C, 75 °C to 100 °C, or 75 °C to 95 °C, where the higher peak melt temperature (Tm) can be measured according to the DSC test method described below.
[0027] In embodiments, the sealing layer comprises at least 70% by weight of a polyethylene elastomer / plastomer that has a higher peak melting temperature (Tm) of 100 °C or less. In such embodiments, the polyethylene elastomer / plastomer of the sealing layer may have a density in the range of 0.865 to 0.910 g / cm3. All individual values and subranges of a density of 0.865 to 0.910 g / cm3 are disclosed and included in this document; for example, the polyethylene elastomer / plastomer may have a density in the range of 0.865 to 0.910 g / cm3, 0.865 to 0.900 g / cm3, 0.865 to 0.890 g / cm3, 0.865 to 0.880 g / cm3, 0.865 to 0.870 g / cm3, 0.870 a0.910 g / cm3, 0.870 to 0.900 g / cm3, 0.870 to 0.890 g / cm3, 0.870 to 0.880 g / cm3, 0.880 to 0.910 g / cm3, 0.880 to 0.900 g / cm3, 0.880 to 0.890 g / cm3, 0.890 to 0.910 g / cm3, 0.890 to 0.900 g / cm3, or 0.900 to 0.910 g / cm3.
[0028] In embodiments where the sealing layer comprises a polyethylene elastomer / plastomer, the polyethylene elastomer / plastomer may have a melt index (I2) in the range of 0.50 to 20 g / 10 minutes (g / 10 min). All individual values and subranges of a melt index (I2) of 0.50 to 20 g / 10 min are disclosed and included herein; for example, the polyethylene elastomer / plastomer may have a melt index (I2) from a lower limit of 0.50, 1.0, 2.0, 5.0, 10.0, 15 or 18 g / 10 min to an upper limit of 1.0, 2.0, 5.0, 10.0, 15, 18, 19 or 20 g / 10 min.
[0029] Commercially available examples of polyethylene elastomers / plastomers that can be used in the sealing layer include those commercially available from The Dow Chemical Company (Midland, MI, USA) under the name AFFINITY™, including, for example, AFFINITY™ VP 8770G1, AFFINITY™ PF7266, AFFINITY™ PL 1881G and AFFINITY™ PF1140G.
[0030] In embodiments, the sealing layer comprises an ethylene-acid copolymer ionomer having a higher peak melting temperature (Tm) of 100 °C or Petition 870250007322, dated 01 / 29 / 2025, p. 19 / 77 9 / 30 less. The cation source of the ethylene-acid copolymer ionomer can be a source of monovalent or divalent cations, including formates, acetates, hydroxides, nitrates, carbonates, and bicarbonates. In various embodiments, the ethylene-acid copolymer can be treated with one or more cations or cation sources that may comprise magnesium, sodium, zinc, or combinations thereof.
[0031] In the embodiments, the ethylene content of the ethylene-acid copolymer ionomer is greater than 50% by weight or greater than 60% by weight, based on the total weight of the ethylene-acid copolymer ionomer. For example, the ethylene content of the ethylene-acid copolymer ionomer may be from 50% by weight to 95% by weight, from 50% by weight to 90% by weight, from 50% by weight to 85% by weight, or from 60% by weight to 80% by weight, based on the total weight of the ethylene-acid copolymer ionomer.
[0032] In embodiments, the ethylene-acid copolymer ionomer has a melting index (I2) of 0.1 g / 10 min to 16 g / 10 min, 3 g / 10 min to 13 g / 10 min, 3.5 g / 10 min to 10 g / 10 min, or 5 g / 10 min to 8 g / 10 min. Commercially available ethylene-acid copolymer ionomers include those available under the name SURLYN™ from The Dow Chemical Company (Midland, MI, USA).
[0033] In addition to an ethylene-acid copolymer ionomer or a polyethylene elastomer / plastomer, the sealing layer, in the embodiments, may further comprise at least one additional polymer and / or at least one additive. For example, the at least one additional polymer may be selected from the group of polyethylene, ethylene-vinyl acetate, ethylene-acrylic acid, or combinations thereof in an amount of less than 30% by weight of the sealing layer. And, for example, the at least one additive may be selected from the group of antioxidants, UV stabilizers, thermal stabilizers, slip agents, anti-adherent agents, antistatic agents, pigments or colorants, processing aids, crosslinking catalysts, flame retardants, fillers, foaming agents, or combinations thereof in an amount of less than 30% by weight of the sealing layer.
[0034] In embodiments, the sealing layer further comprises a polyethylene having a higher peak melt temperature (Tm) of 108 °C or less. For example, in embodiments, the sealing layer further comprises a Petition 870250007322, dated 01 / 29 / 2025, p. 20 / 77 10 / 30 Linear low-density polyethylene (LLDPE). Linear low-density polyethylene has a density less than or equal to 0.930 g / cm3. All individual values and subranges less than or equal to 0.930 g / cm3 are included and disclosed in this document; for example, the density of linear low-density polyethylene may have a lower limit of 0.870 g / cm3 and an upper limit of 0.928, 0.925, 0.920, or 0.915 g / cm3. All individual values and subranges between 0.870 and 0.930 cm3 are included and disclosed in this document.
[0035] Commercially available examples of polyethylenes that have a higher peak melt temperature (Tm) of 108 °C or less that can be used in the sealing layer include those commercially available from The Dow Chemical Company under the name ELITE™ AT, including, for example, ELITE™ AT 6202 and ELITE™ AT 6410.
[0036] In embodiments, the sealing layer is at least 10 microns thick, or alternatively at least 15 microns thick, or alternatively at least 20 microns thick. In other embodiments, the sealing layer is 25 to 60% of the total thickness of the multilayer film. Multilayer film fixation layer
[0037] The multi-layered laminate film comprises an attachment layer between the barrier layer and the sealing layer. The attachment layer may adhere the barrier layer to the sealing layer.
[0038] In embodiments, the fixing layer comprises an adhesive resin selected from the group consisting of an ethylene-based polymer grafted with anhydride, ethylene acid copolymer and ethylene-vinyl acetate. Examples of anhydride graft moieties may include, but are not limited to, maleic anhydride, citraconic anhydride, 2-methylmaleic anhydride, 2-chloromaleic anhydride, 2,3-dimethylmaleic anhydride, bicyclo[2,2,1]-5-heptene-2,3-dicarboxylic anhydride and 4-methyl-4-cyclohexene-1,2-dicarboxylic anhydride, bicyclo(2.2.2)oct-5-ene-2,3-dicarboxylic anhydride, 10-octahydronaphthalene-2,3-dicarboxylic acid anhydride, 2-oxa-1,3-diketospiro(4.4)non-7-ene, bicyclo(2.2.1)hept-5-ene-2,3-dicarboxylic acid anhydride, tetrahydrophthalic anhydride, anhydride of norborn-5-ene-2,3-dicarboxylic acid, nadic anhydride, methylnadic anhydride, hymic anhydride, methyl anhydride Petition 870250007322, dated 01 / 29 / 2025, p. 21 / 77 11 / 30 hymic and x-methyl-bi-cyclo(2.2.1)hept-5-ene-2,3-dicarboxylic acid anhydride. In one embodiment, the anhydride-grafted chemical portion comprises maleic anhydride.
[0039] In embodiments, the fixation layer comprises an anhydride-modified linear low-density polyethylene. In embodiments, the anhydride-modified linear low-density polyethylene has a density in the range of 0.860 g / cm3 to 0.935 g / cm3. All individual values and subranges from 0.860 g / cm3 to 0.935 g / cm3 are disclosed and included in this document; For example, anhydride-modified linear low-density polyethylene may have a density in the range of 0.875 g / cm3 to 0.935 g / cm3, 0.900 g / cm3 to 0.925 g / cm3, 0.910 g / cm3 to 0.935 g / cm3, 0.910 g / cm3 to 0.925 g / cm3, 0.915 g / cm3 to 0.935 g / cm3 or 0.920 g / cm3 to 0.930 g / cm3. In embodiments, anhydride-modified linear low-density polyethylene has a melt index (I2) of 0.1 g / 10 min to 50 g / 10 min, or 0.5 g / 10 min to 20 g / 10 min, or 1.0 g / 10 min to 10 g / 10 min.
[0040] In embodiments, the fixation layer comprises from 0 to 100% by weight of anhydride-modified linear low-density polyethylene, based on the total weight of the fixation layer. All individual values and subranges from 0 to 100% by weight are disclosed and included herein. For example, in embodiments, the fixation layer may comprise from 10 to 90% by weight, 20 to 80% by weight, 30 to 70% by weight, or 40 to 60% by weight of anhydride-modified linear low-density polyethylene, based on the total weight of the fixation layer.
[0041] Examples of commercially available anhydride-modified linear low-density polyethylenes that can be used in embodiments include BYNEL™ Series 4100 resins, such as BYNEL™ 41E710 and BYNEL™ 41E687, available from The Dow Chemical Company (Midland, MI, USA).
[0042] In embodiments, the anchoring layer further comprises at least one of linear low-density polyethylene, low-density polyethylene, medium-density polyethylene, or high-density polyethylene. For example, in embodiments, the anchoring layer further comprises high-density polyethylene having a density in the range of 0.945 g / cm3 to 0.970 g / cm3. All individual values and subranges from 0.945 g / cm3 to 0.970 g / cm3 are disclosed and included herein; for example, high-density polyethylene may have a Petition 870250007322, dated 01 / 29 / 2025, page 22 / 77 12 / 30 density in the range of 0.945 g / cm3a 0.965 g / cm3, 0.950 g / cm3a 0.970 g / cm3, 0.950 g / cm3a 0.965 g / cm3, 0.955 g / cm3a 0.970 g / cm3, 0.955 g / cm3a 0.965 g / cm3, or 0.955 g / cm3 to 0.965 g / cm3.
[0043] In embodiments where high-density polyethylene is present, the high-density polyethylene of the fixation layer may be a copolymer of ethylene and C3-C12 comonomer. In embodiments, the fixation layer additionally comprises 0 to 90% by weight of high-density polyethylene, based on the total weight of the fixation layer. All individual values and subranges from 0 to 90% by weight are disclosed and included herein. For example, in embodiments, the fixation layer may comprise 10 to 90% by weight, 20 to 80% by weight, 30 to 70% by weight, or 40 to 60% by weight of high-density polyethylene, based on the total weight of the fixation layer. In the various forms, the melt index (I2) of high-density polyethylene can be 0.3 to 10.0 g / 10 min, 0.3 to 7.0 g / 10 min, 0.3 to 5.0 g / 10 min, 0.3 to 4.0 g / 10 min, 0.3 to 3.0 g / 10 min, 0.3 to 2.0 g / 10 min, 0.3 to 1.5 g / 10 min, or 0.5 to 1.0 g / 10 min.
[0044] Commercially available examples of high-density polyethylene that can be used in the bonding layer include those commercially available from The Dow Chemical Company (Midland, MI, USA) under the names ELITE™ 5960 G1 and DOWLEX™ 2006G. Outer layer and second layer of multilayer film fixation.
[0045] In embodiments, the multilayer film may comprise an outer layer and a second fixation layer, wherein the second fixation layer is positioned between the outer layer and the barrier layer.
[0046] According to embodiments disclosed herein, the outer layer of the multilayer film comprises polyethylene. In the embodiments, the polyethylene of the outer layer has a density of 0.900 to 0.970 g / cm3. All individual values and subranges of a density of 0.900 to 0.970 g / cm3 are disclosed and included in this document; for example, the polyethylene may have a density in the range of 0.900 to 0.970 g / cm3, 0.910 to 0.957 g / cm3, 0.920 to 0.947 g / cm3, 0.920 to 0.937 g / cm3, 0.920 to 0.930 g / cm3 or 0.920 to 0.927 g / cm3.
[0047] In the embodiments, the polyethylene of the outer layer has a melt index of 0.1 Petition 870250007322, dated 01 / 29 / 2025, p. 23 / 77 13 / 30 g / 10 min to 10 g / 10 min, or from 0.5 g / 10 min to 8 g / 10 min, or from 0.5 g / 10 min to 5 g / 10 min.
[0048] In embodiments, the polyethylene of the outer layer comprises at least 50% by weight of the outer layer, based on the total weight of the outer layer. All individual values and subranges of at least 50% by weight are disclosed and included herein. For example, the polyethylene may comprise at least 50% by weight, at least 75% by weight, at least 90% by weight, at least 99% by weight or at least 99.9% by weight of the outer layer, based on the total weight of the outer layer.
[0049] In addition to polyethylene, the outer layer, in the embodiments, may further comprise at least one additional polymer, and the at least one additional polymer may be selected from the group of ultra-low density polyethylene, low density polyethylene, polyethylene elastomer / plastomer, ethylene-vinyl acetate, ethylene-acrylic acid, or combinations thereof in an amount of less than 50% by weight of the outer layer.
[0050] In embodiments, the multilayer film additionally comprises a second bonding layer between the outer layer and the barrier layer. The second bonding layer may adhere the outer layer to the barrier layer.
[0051] In embodiments, the second bonding layer includes an adhesive resin selected from the group consisting of an ethylene-based polymer grafted with anhydride, ethylene acid copolymer and ethylene-vinyl acetate. Examples of anhydride graft moieties may include, but are not limited to, maleic anhydride, citraconic anhydride, 2-methylmaleic anhydride, 2-chloromaleic anhydride, 2,3-dimethylmaleic anhydride, bicyclo[2,2,1]-5-heptene-2,3-dicarboxylic anhydride and 4-methyl-4-cyclohexene-1,2-dicarboxylic anhydride, bicyclo(2.2.2)oct-5-ene-2,3-dicarboxylic anhydride, 10-octahydronaphthalene-2,3-dicarboxylic acid anhydride, 2-oxa-1,3-diketospiro(4.4)non-7-ene, bicyclo(2.2.1)hept-5-ene-2,3-dicarboxylic acid anhydride, tetrahydrophthalic anhydride, anhydride of norborn-5-ene-2,3-dicarboxylic acid, nadic anhydride, methylnadic anhydride, himic anhydride, methylhimic anhydride and x-methyl-bi-cyclo(2.2.1)hept-5-ene-2,3-dicarboxylic acid anhydride.In one embodiment, the anhydride-grafted chemical moiety comprises maleic anhydride.
[0052] In some forms, the second fixing layer comprises a polyethylene Petition 870250007322, dated 01 / 29 / 2025, page 24 / 77 14 / 30 linear low-density polyethylene, anhydride-modified. In embodiments, linear low-density polyethylene, anhydride-modified, has a density in the range of 0.860 g / cm3 to 0.935 g / cm3. All individual values and subranges from 0.860 g / cm3 to 0.935 g / cm3 are disclosed and included in this document; For example, anhydride-modified linear low-density polyethylene may have a density in the range of 0.875 g / cm3 to 0.935 g / cm3, 0.900 g / cm3 to 0.925 g / cm3, 0.910 g / cm3 to 0.935 g / cm3, 0.910 g / cm3 to 0.925 g / cm3, 0.915 g / cm3 to 0.935 g / cm3 or 0.920 g / cm3 to 0.930 g / cm3. In embodiments, anhydride-modified linear low-density polyethylene has a melt index (I2) of 0.1 g / 10 min to 50 g / 10 min, or 0.5 g / 10 min to 20 g / 10 min, or 1.0 g / 10 min to 10 g / 10 min.
[0053] In embodiments, the second fixing layer comprises from 0 to 100% by weight of anhydride-modified linear low-density polyethylene, based on the total weight of the second fixing layer. All individual values and subranges from 0 to 100% by weight are disclosed and included herein. For example, in embodiments, the second fixing layer may comprise from 10 to 90% by weight, 20 to 80% by weight, 30 to 70% by weight, or 40 to 60% by weight of anhydride-modified linear low-density polyethylene, based on the total weight of the second fixing layer.
[0054] Examples of commercially available anhydride-modified linear low-density polyethylenes that can be used in embodiments include BYNEL™ Series 4100 resins, such as BYNEL™ 41E710 and BYNEL™ 41E687, available from The Dow Chemical Company (Midland, MI, USA).
[0055] In embodiments, the second fixing layer further comprises at least one of linear low-density polyethylene, low-density polyethylene, medium-density polyethylene, or high-density polyethylene. For example, in embodiments, the second fixing layer further comprises high-density polyethylene having a density in the range of 0.945 g / cm3 to 0.970 g / cm3. All individual values and subranges of 0.945 g / cm3 to 0.970 g / cm3 are disclosed and included herein; for example, the high-density polyethylene of the second fixing layer may have a density in the range of 0.945 g / cm3 to 0.965 g / cm3, 0.950 g / cm3 to 0.970 g / cm3, 0.950 g / cm3 to 0.965 g / cm3, 0.955 Petition 870250007322, dated 01 / 29 / 2025, page 25 / 77 15 / 30 g / cm3a 0.970 g / cm3, 0.955 g / cm3a 0.965 g / cm3or 0.955 g / cm3a 0.965 g / cm3.
[0056] In embodiments where a high-density polyethylene is present, the high-density polyethylene of the second fixing layer may be a copolymer of ethylene and C3-C12 comonomer. In embodiments, the second fixing layer comprises from 0 to 90% by weight of a high-density polyethylene, based on the total weight of the second fixing layer. All individual values and subranges from 0 to 90% by weight are disclosed and included herein. For example, in embodiments, the second fixing layer may comprise from 10 to 90% by weight, 20 to 80% by weight, 30 to 70% by weight, or 40 to 60% by weight of a high-density polyethylene, based on the total weight of the second fixing layer.In embodiments, the high-density polyethylene of the second bonding layer may have a melt index (I2) of 0.3 to 10.0 g / 10 min, 0.3 to 7.0 g / 10 min, 0.3 to 5.0 g / 10 min, 0.3 to 4.0 g / 10 min, 0.3 to 3.0 g / 10 min, 0.3 to 2.0 g / 10 min, or 0.3 to 1.5 g / 10 min, or 0.5 to 1.0 g / 10 min.
[0057] Commercially available examples of high-density polyethylene that can be used in the second bonding layer include those commercially available from The Dow Chemical Company (Midland, MI, USA) under the names ELITE™ 5960G1 and DOWLEX™ 2006G. Sticker
[0058] The laminate comprises an adhesive that bonds the multilayer film described above to the polyethylene film described below. The adhesive may be applied to the outermost layer of the multilayer film (e.g., to the barrier layer in embodiments or to the outer layer in other embodiments) to act as an adhesive layer and bond the multilayer film to the polyethylene film described below.
[0059] In the embodiments, the adhesive is a solvent-based adhesive, a solvent-free adhesive, or a water-based adhesive. Examples of commercially available adhesives that can be used in the embodiments include those available from The Dow Chemical Company (Midland, MI, USA) under the names ADCOTE™, MOR-FREE™, and ROBOND™. Polyethylene film laminate Petition 870250007322, dated 01 / 29 / 2025, page 26 / 77 16 / 30
[0060] The laminate disclosed herein comprises a polyethylene film. The polyethylene film according to the embodiments disclosed herein adheres to the barrier layer or the outer layer of the multilayer film via the adhesive described above. The polyethylene film comprises an ethylene-based polymer having a density of 0.900 to 0.970 g / cm3.
[0061] In embodiments, the ethylene-based polymer of the polyethylene film has a density of 0.900 to 0.970 g / cm3. All individual values and subranges of a density of 0.900 to 0.970 g / cm3 are disclosed and included in this document. For example, the ethylene-based polymer may have a density in the range of 0.900 to 0.970 g / cm3, 0.910 to 0.957 g / cm3, 0.920 to 0.947 g / cm3, 0.920 to 0.937 g / cm3, 0.920 to 0.930 g / cm3 or 0.920 to 0.927 g / cm3.
[0062] In embodiments, the ethylene-based polymer has a melting index (I2) of 0.1 g / 10 min to 10 g / 10 min, or 0.5 g / 10 min to 8 g / 10 min, or 0.5 g / 10 min to 5 g / 10 min.
[0063] In the embodiments, the ethylene-based polymer comprises at least 50% by weight of the polyethylene film, based on the total weight of the polyethylene film. All individual values and subranges of at least 50% by weight are disclosed and included herein. For example, the ethylene-based polymer may comprise at least 50% by weight, at least 75% by weight, at least 90% by weight, at least 99% by weight, or at least 99.9% by weight of the polyethylene film, based on the total weight of the polyethylene film.
[0064] In addition to the ethylene-based polymer, the polyethylene film, in the embodiments, may further comprise at least one additional polymer, and the at least one additional polymer may be selected from the group of a second ethylene-based polymer, polyethylene elastomer / plastomer, ethylene-vinyl acetate, ethylene-acrylic acid, or combinations thereof. For example, the polyethylene film may further comprise at least 20% by weight of a second ethylene-based polymer having a density of 0.958 g / cm3 or greater.
[0065] Polyethylene film can be a multilayer film or a single-layer film. In some embodiments, the film is a single-layer film. In other embodiments, the polyethylene film comprises at least two layers. The Petition 870250007322, dated 01 / 29 / 2025, page 27 / 77 17 / 30 embodiments of the polyethylene film may include, for example, a fixing layer, sealing layers or barrier layers. In the embodiments, the polyethylene film additionally comprises a barrier layer comprising an ethylene-vinyl alcohol copolymer (EOVH).
[0066] In embodiments, the polyethylene film is an oriented film. In embodiments, the polyethylene film is a machine-direction oriented film. In such embodiments, the polyethylene film may be a machine-direction oriented (MDO) polyethylene film. In other embodiments, the polyethylene films are biaxially oriented. In such embodiments, the polyethylene film may be a biaxially oriented polyethylene film (BOPE). In embodiments where the polyethylene film is a BOPE, the BOPE may be biaxially oriented using a sequential biaxial orientation process in a drawing oven, and may be referred to as oven-drawing biaxially oriented polyethylene (TF-BOPE). Such techniques are generically known to those skilled in the art.In other embodiments, the polyethylene film can be biaxially oriented using other techniques known to those skilled in the art based on the teachings of this document, such as a double bubble orientation process. Generally, with a sequential biaxial orientation process in a stretching oven, the stretching oven is incorporated as part of a multi-layer co-extrusion line. After extrusion from a flat die, the film is cooled on a cooling cylinder and immersed in a water bath filled with water at room temperature. The cast film is then passed through a series of cylinders with different rotational speeds to achieve stretching in the machine direction. There are several pairs of cylinders in the stretching segment of the DM of the manufacturing line, and all are oil-heated.The paired cylinders function sequentially as preheating cylinders, stretching cylinders, and cylinders for relaxing and annealing. The temperature of each pair of cylinders is controlled separately. After stretching in the machine direction, the film sheet is passed inside a hot air stretching oven with heating zones to perform stretching in the transverse direction. The first several zones are for preheating, followed by... Petition 870250007322, dated 01 / 29 / 2025, p. 28 / 77 18 / 30 by zones for stretching and then the last zones for annealing.
[0067] In the embodiments, the polyethylene film has a transverse directional stretch ratio greater than its machine-direction stretch ratio, and the polyethylene film has a ratio between the percentage elongation at break in the machine direction and the percentage elongation at break in the transverse direction of at least 2 to 1. In the embodiments, the polyethylene film may exhibit a percentage elongation at break in the machine direction that is at least 2 times greater than the percentage elongation at break in the transverse direction, when measured in accordance with ASTM D882, or alternatively, at least 5 times greater, or alternatively, at least 8 times greater, or alternatively, at least 10 times greater.
[0068] In the embodiments, the polyethylene film can be oriented in the machine direction at a stretch ratio of 2:1 to 6:1, or alternatively, at a stretch ratio of 3:1 to 5:1. The polyethylene film, in the embodiments, can be oriented in the transverse direction at a stretch ratio of 2:1 to 9:1, or alternatively, at a stretch ratio of 3:1 to 8:1. In the embodiments, the polyethylene film is oriented in the machine direction at a stretch ratio of 2:1 to 6:1 and in the transverse direction at a stretch ratio of 2:1 to 9:1.
[0069] In the embodiments, depending for example on the end-use application, the polyethylene film may be corona treated or printed using techniques known to those skilled in the art before or after being adhered to the multilayer film.
[0070] The multilayer film and polyethylene film disclosed herein may have a variety of thicknesses depending, for example, on the number of layers. For example, in the embodiments, the multilayer film or polyethylene film may have a thickness of 10 to 200 microns, or alternatively, 15 to 100 microns. Additives
[0071] It should be understood that any of the preceding layers of the multilayer film or polyethylene film may additionally comprise one or more additives as known to those skilled in the art, such as, for example, antioxidants, UV stabilizers, thermal stabilizers, slip agents, antiblocking agents, antistatic agents, pigments or colorants, processing aids, crosslinking catalysts, flame retardants, fillers. Petition 870250007322, dated 01 / 29 / 2025, page 29 / 77 19 / 30 and foaming agents. For example, in embodiments, the sealing layer of the multilayer film comprises at least one of a slip agent or anti-adherent agent. The Laminate
[0072] As noted above, the polyethylene film is adhered to the outermost layer (e.g., the barrier layer in embodiments or the outer layer in other embodiments) of the multilayer film, and the combination of the multilayer film and the polyethylene film provides the laminate.
[0073] The laminate of the present invention may have several desirable properties. For example, the laminate of the present invention may have one or more of the following properties: an OTR of at least 6.75 cm3 / day / m2; a WVTR of less than 4.50 g / day / m2; a hot seal initiation temperature at 5N of less than 97 °C; a seal strength at 120 °C of at least 10.0 N / 25 mm; a hot adhesion initiation at 1N of less than 83 °C; a hot adhesion strength at 110 °C of at least 0.30 N; and zero percent (0%) shrinkage over a temperature range of 70 °C to 110 °C.
[0074] In the models, the laminate has a sealing window of at least 40 °C.
[0075] In embodiments, the laminate of the present invention comprises at least 90% by weight of polyethylene, or at least 95% by weight of polyethylene, or at least 99% by weight of polyethylene, or at least 99.5% by weight of polyethylene, or at least 99.9% by weight of polyethylene, based on the total weight of the laminate. Articles
[0076] The embodiments of the present invention also provide articles formed from the laminate described herein. Examples of such articles may include packaging, flexible packaging, and bags. In the embodiments, the packaging of the present invention may comprise a liquid, a powder, a food product, or other items. The articles and packaging of the present invention may be formed from the laminate disclosed herein using techniques known to those skilled in the art, taking into account the teachings of this document. Testing methods Density Petition 870250007322, dated 01 / 29 / 2025, page 30 / 77 20 / 30
[0077] Density is measured according to ASTM D792 and expressed in grams / cm3 (g / cm3). Melting index (K)
[0078] The melting index (I2) is measured according to ASTM D-1238 at 190 °C at 2.16 kg. Values are reported in g / 10 min, which corresponds to grams eluted during 10 minutes. Oxygen Transmission Rate (OTR)
[0079] Oxygen transmission rate (OTR) is measured according to ASTM D3985. Samples are tested at 23 °C, 0% RH (relative humidity), sample size of 50 cm2. Values are reported in cm3 / day / m2. Water Vapor Transmission Rate (WVTR)
[0080] Water Vapor Transmission Rate (WVTR) is measured according to ASTM F1249. Samples are tested at 37.8 °C, 100% RH and a sample size of 50 cm2. Values are reported in g / day / m2. Hot adhesion initiation and hot adhesion resistance
[0081] A hot adhesion test is performed using a J&B 4000 hot adhesion tester at a sealing width of 25 mm, a dwell time of 0.5 s, a sealing pressure of 0.275 N / mm2 (40 psi), and a hot adhesion pull speed of 200 mm / s. The hot adhesion initiation is reported as the minimum temperature in degrees Celsius to achieve a strength of 1 newton. The hot adhesion strength is measured in units of newtons per 25 mm (N / 25 mm). Hot seal initiation temperature and sealing resistance
[0082] To determine the hot seal initiation temperature (HSIT) and seal strength, samples are sealed using a J&B Hot Tack 4000 Tester. The sample width is 25 mm, the dwell time is 0.5 seconds, and the seal pressure is 0.275 N / mm². The hot-sealed samples are conditioned for 24 hours and then measured using a Zwick tensile testing machine equipped with a 200 N load cell and a tensile speed of 500 mm / min. The HSIT is reported as a minimum temperature in degrees Celsius to achieve a force of 5 newtons. Seal strength values are reported in N / 25 mm. Petition 870250007322, dated 01 / 29 / 2025, page 31 / 77 21 / 30 Shrinkage
[0083] Shrinkage (%) is obtained by measuring the length and width of the sealing area in both MD and DT directions after hot-sealing the films together and by calculating the percentage change compared to the width of the sealing bar, which can be between 1 mm and 15 mm. Standard hot-sealing machines, including the PULSA impulse sealing device or the J&B Hot Tack tester, can be used, provided the machines have an accurate and adjustable temperature controller. Sealing conditions include grip pressure (40 to 80 psi or 0.275 to 0.552 N / mm2), dwell time (0.1 to 1.5 seconds) and sealing temperature window (60 to 150oC) and depend on the packaging speed, with typical conditions for high-speed packaging machines being a grip pressure of 40 psi (0.275 N / mm2) and a dwell time of 0.5 seconds. Highest Peak Melting Temperature (Tm)
[0084] Differential scanning calorimetry (DSC) is used to measure the melting and crystallization behavior of a polymer over a wide temperature range. For example, the TA Instruments Q1000 DSC, equipped with a refrigerated cooling system (RCS) and an autosampler, is used to perform this analysis. The instrument is first calibrated using the calibration assistant computer program. A baseline is obtained by heating a cell from -80 °C to 280 °C without any sample in an aluminum crucible for DSC. Sapphire standards are then used, as instructed by the calibration assistant. Next, 1 to 2 milligrams (mg) of a new indium sample are analyzed by heating the standard sample to 180 °C, cooling it to 120 °C at a cooling rate of 10 °C / minute, and then by isothermal maintenance of the standard sample at 120 °C for 1 minute.The standard sample is then heated from 120 °C to 180 °C at a heating rate of 10 °C / minute. It is then determined that the standard indium sample has a heat of fusion (Hf) = 28.71 ± 0.50 joules per gram (J / g) and an onset of fusion = 156.6 °C ± 0.5 °C. The test samples are then analyzed using a DSC instrument.
[0085] During the test, a nitrogen purge gas flow of 50 mL / min is used. Petition 870250007322, dated 01 / 29 / 2025, page 32 / 77 22 / 30 Each sample is pressed as a molten mass into a thin film at approximately 175 °C; the molten sample is then air-cooled to room temperature (approximately 25 °C). The film sample is formed by pressing a 0.1 to 0.2 gram sample at 175 °C at 1500 psi for 30 seconds to form a film 0.1 to 0.2 mils thick. A 3 to 10 mg specimen, 6 mm in diameter, is extracted from the cooled polymer, weighed, placed in a lightweight aluminum crucible (approximately 50 mg), and sealed by crimping. Analysis is then performed to determine its thermal properties.
[0086] The thermal behavior of the sample is determined by varying the sample temperature up and down in order to create a heat flow versus temperature profile. First, the sample is rapidly heated to 180 °C and held isothermally for five minutes, in order to remove its thermal history. Then, the sample is cooled to -40 °C at a cooling rate of 10 °C / minute and held isothermally at -40 °C for five minutes. The sample is then heated to 150 °C (this is the second heating ramp) at a heating rate of 10 °C / minute. The cooling and second heating curves are recorded. The cooling curve is analyzed by fitting the baseline endpoints from the beginning of crystallization to -20 °C. The heating curve is analyzed by fitting the baseline endpoints from -20 °C to the end of melting.The determined values are the highest peak melting temperature (Tm), peak crystallization temperature (Tc), initial crystallization temperature (Tc initial), heat of fusion (Hf) (in joules per gram), and the % crystallinity calculated for polyethylene samples using: % Crystallinity for PE = ((Hf) / (292 J / g)) x 100 and the % crystallinity calculated for polypropylene samples using: % Crystallinity for PP = ((Hf) / 165 J / g)) x 100. The heat of fusion (Hf) and the highest peak melting temperature are reported from the second heating curve. The highest peak crystallization temperature and the initial crystallization temperature are determined from the cooling curve. Examples
[0087] The following examples illustrate features of the present disclosure, but are not intended to limit the scope of the disclosure. Petition 870250007322, dated 01 / 29 / 2025, page 33 / 77 23 / 30 Polymers / Film used
[0088] The following materials were used in the example slides discussed below.
[0089] ELITE™ 5960G, an improved polyethylene resin that has a density of 0.962 g / cm3 and a melt index (I2) of 0.85 g / 10 min and is commercially available from The Dow Chemical Company (Midland, MI, USA).
[0090] ELITE™ 5960G1, an improved polyethylene resin that has a density of 0.962 g / cm3 and a melt index (I2) of 0.85 g / 10 min and is commercially available from The Dow Chemical Company (Midland, MI, USA).
[0091] ELITE™ 5940ST, an improved polyethylene resin that has a density of 0.941 g / cm3 and a melt index (I2) of 0.8 g / 10 min and is commercially available from The Dow Chemical Company (Midland, MI, USA).
[0092] ELITE™ 5400G, an improved polyethylene resin that has a density of 0.916 g / cm3 and a melt index (I2) of 1.0 g / 10 min and is commercially available from The Dow Chemical Company (Midland, MI, USA).
[0093] ELITE™ 5400GS, an improved polyethylene resin that has a density of 0.916 g / cm3 and a melt index (I2) of 1.0 g / 10 min and is commercially available from The Dow Chemical Company (Midland, MI, USA).
[0094] DOW™ LDPE 450E, a low-density polyethylene resin that has a density of 0.923 g / cm3 and a melt index (I2) of 2.0 g / 10 min, and is commercially available from The Dow Chemical Company (Midland, MI).
[0095] BYNEL™ 41E710, an anhydride-modified linear low-density polyethylene resin having a density of 0.922 g / cm3 and a melt index (I2) of 2.7 g / 10 min, and commercially available from The Dow Chemical Company (Midland, MI).
[0096] EVAL™ H171B, an ethylene-vinyl alcohol copolymer with an ethylene content of 38 mol% having a density of 1.17 g / cm3 and a melting index (I2) of 1.7 g / 10 min, and commercially available from Kuraray Co., Ltd. (Tokyo, Japan).
[0097] SURLYN™ 1707, an ethylene-acid copolymer ionomer neutralized with a sodium cation source, which has a higher peak melting temperature (Tm) of 92 °C, a density of 0.95 g / cm3 and a melting index (I2) of 0.9 g / 10 min, and Petition 870250007322, dated 01 / 29 / 2025, page 34 / 77 24 / 30 commercially available from The Dow Chemical Company (Midland, MI, USA).
[0098] AFFINITY™ PF 7266, a polyethylene elastomer / plastomer that has a higher peak melt temperature (Tm) of 76 °C, a density of 0.885 g / cm3 and a melt index (I2) of 2.5 g / 10 min, and commercially available from The Dow Chemical Company (Midland, MI, USA).
[0099] ADCOTE™ 545S / Coreagent F, a commercially available solvent-based, 2-component polyurethane adhesive from The Dow Chemical Company (Midland, MI, USA).
[00100] INNATE™ ST70, a precision packaging resin that has a density of 0.926 g / cm3 and a melting index (I2) of 0.85 g / 10 min, and is commercially available from The Dow Chemical Company (Midland, MI, USA).
[00101] POLYBATCH® CE505, a standard slip mixture, commercially available near Lyondell Basell (Houston, TX, USA).
[00102] POLYBATCH® AB5, a standard nonstick mixture commercially available from Lyondell Basell (Houston, TX, USA).
[00103] CONPOL™ 13B, a commercially available nonstick standard mixture from The Dow Chemical Company (Midland, MI, USA).
[00104] CONPOL™ 20S1, a commercially available standard slip mixture from The Dow Chemical Company (Midland, MI, USA).
[00105] TF-BOPE 20 substrate, a biaxially oriented linear low-density polyethylene film, furnace-stretched in the machine direction at a stretch ratio of 3-5X and in the transverse direction at a stretch ratio of 79X to a thickness of 20 microns. The linear low-density polyethylene has a density of 0.926 g / cm3 and a melt index (I2) of 1.7 g / 10 min, and is commercially available from The Dow Chemical Company, Midland, MI, USA, under the name INNATE™ XUS 59910.08.
[00106] TF-BOPE 40 substrate, a biaxially oriented linear low-density polyethylene film, furnace-stretched in the machine direction at a stretch ratio of 3-5X and in the transverse direction at a stretch ratio of 79X to a thickness of 40 microns. The linear low-density polyethylene has a density of 0.926 g / cm3 and a melt index (I)2) of 1.7 g / 10 min, and is available Petition 870250007322, dated 01 / 29 / 2025, page 35 / 77 25 / 30 commercially available from The Dow Chemical Company, Midland, MI, USA, under the name INNATE™ XUS 59910.08.
[00107] MDO Substrate, a machine-oriented, multilayer film of five-layer polyethylene, which has a thickness of 25 microns. The MDO Substrate comprises ELITE™ 5960G, ELITE™ 5940ST, INNATE™ ST70 and ELITE™ 5400GS.
[00108] HDPE substrate, a multi-layer film, five layers that is 25 microns thick and has a layer structure of (1) 100% ELITE™ 5960G1; (2) 100% ELITE™ 5960G1; (3) 100% ELITE™ 5960G1; (4) 100% ELITE™ 5960G1; (5) 100% DOW™ LDPE 450E. The film is created on a Collin 5-layer co-extrusion casting line with 4 extruders, Configuration: A / B / C / B / D; Layer Ratio: 1 / 1 / 1 / 1 / 1; melt temperature of each extruder from 250 to 260oC; Slit die with coat hanger geometry; total production capacity of 8 kg / h; line speed of 21.5 m / min.
[00109] BOPP substrate, a printed biaxially oriented propylene film treated to 36 dynes and having a thickness of 18 microns.
[00110] Laminates, designated as Examples of the Invention 1 to 8 and Comparative Examples 1 and 2, are formed in a PRINT-ABCBD construction, where PRINT corresponds to TF-BOPE 20 Substrate, TF-BOPE 40 Substrate, MDO Substrate or HDPE Substrate for the Examples of the Invention or BOPP Substrate for the Comparative Examples and ABCBD corresponds to a five-layer multilayer film. For each of the Comparative Examples, the PRINT substrate is laminated to layer A of the multilayer film using ADCOTE™ 545S / Co-agent F applied at a coating weight of 3 to 3.5 g / m2. The samples are cured at room temperature (25 °C) for two days and a hot cylinder rolling process is carried out on ChemInstruments #007416 at a temperature of 75 °C, a pressure of 60 psi and a speed of 1.66 m / min.
[00111] The five-layer multilayer films for each of the Examples of the Invention and Comparative Examples are formed on a 5-layer Collin blow molding co-extrusion line with the following parameters - target film thickness: 55 µm; extruders: 4 extruders; layer configurations: A / B / C / B / D; layer ratio: Petition 870250007322, dated 01 / 29 / 2025, page 36 / 77 26 / 30 2 / 1.5 / 2 / 1.5 / 4; layer thickness (pm): 10 / 7.5 / 10 / 7.5 / 20; die diameter (mm): 50; blow ratio (BUR): 3.0; flat width (mm): 235; total production capacity of 8 kg / h; line speed of 5.4 m / min; melting temperature (oC) of extruders A, B, C and D of 174 °C, 191 °C, 197 °C and 177 °C, respectively.
[00112] Table 1 below provides the structure and composition of the laminate examples, Examples of the Invention 1 to 8 and Comparative Examples 1 and 2. Table 1 - Structure and composition of the laminate Example Print Layer A Layer B Layer C Layer B Layer D Comp. 1 Substrate BOPP DOW™ LDPE 450E 50% BYNEL™ 41E710 + 50% ELITE™ 5960G1 EVAL™ H171B 50% BYNEL™ 41E710 + 50% ELITE™ 5960G1 80% AFFINITY™ pf 7266* Comp. 2 Substrate BOPP DOW™ LDPE 450E 50% BYNEL™ 41E710 + 50% ELITE™ 5960G1 EVAL™ H171B 50% BYNEL™ 41E710 + 50% ELITE™ 5960G1 93.5% SURLYN™ 1707** Inv. 1 Substrate TF-BOPE 40 DOW™ LDPE 450E 50% BYNEL™ 41E710 + 50% ELITE™ 5960G1 EVAL™ H171B 50% BYNEL™ 41E710 + 50% ELITE™ 5960G1 80 % of AFFINITY™ pf 7266* Inv. 2 Substrate TF-BOPE 40 DOW™ LDPE 450E 50% of BYNEL™ 41E710 + 50% of ELITE™ 5960G1 EVAL™ H171B 50% of BYNEL™ 41E710 + 50% of ELITE™ 5960G1 93.5% of SURLYN™ 1707** Inv. 3 Substrate TF-BOPE 20 DOW™ LDPE 450E 50% of BYNEL™ 41E710 + 50% of ELITE™ 5960G1 EVAL™ H171B 50% of BYNEL™ 41E710 + 50% ELITE™ 5960G1 80% AFFINITY™ pf 7266* Petition 870250007322, dated 01 / 29 / 2025, page 37 / 77 27 / 30 Example Print Layer A Layer B Layer C Layer B Layer D Inv. 4 Substrate TF-BOPE 20 DOW™ LDPE 450E 50% BYNEL™ 41E710 + 50% ELITE™ 5960G1 EVAL™ H171B 50% BYNEL™ 41E710 + 50% ELITE™ 5960G1 93.5% SURLYN™ 1707** Inv. 5 Substrate HDPE DOW™ LDPE 450E 50% BYNEL™ 41E710 + 50% ELITE™ 5960G1 EVAL™ H171B 50% BYNEL™ 41E710 + 50% ELITE™ 5960G1 80% AFFINITY™ pf 7266* Inv. 6 HDPE Substrate DOW™ LDPE 450E 50% BYNEL™ 41E710 + 50% ELITE™ 5960G1 EVAL™ H171B 50% BYNEL™ 41E710 + 50% ELITE™ 5960G1 93.5% SURLYN ™ 1707** Inv. 7 MDO Substrate DOW™ LDPE 450E 50% BYNEL™ 41E710 + 50% ELITE™ 5960G1 EVAL™ H171B 50 % of BYNEL™ 41E710 + 50% of ELITE™ 5960G1 80% of AFFINITY™ pf 7266* Inv. 8 Substrate MDO DOW™ LDPE 450E 50% of BYNEL™ 41E710 + 50% of ELITE™ 5960G1 EVAL™ H171B 50% of BYNEL™ 41E710 + 50% of ELITE™ 5960G1 93.5% of SURLYN™ 1707** * In addition to 80% AFFINITY™ PF 7266, Layer D includes 10% POLYBATCH® CE505 and 10% POLYBATCH® AB5. ** In addition to 93.5% SURLYN™ 1707, Layer D includes 4% CONPOL™ 13B and 2.5% CONPOL™ 20S1.
[00113] The thickness, oxygen transmission rate (OTR), and water vapor transmission rate (WVTR) of the examples are measured. Table 2 provides the results. Laminates with a BOPP substrate are known to exhibit slightly better WVTR properties than comparable polyethylene laminates. Comparative Examples 1 and 2, which contain a BOPP printing substrate, are not compatible with polyethylene recycling streams, although they have Petition 870250007322, dated 01 / 29 / 2025, p. 38 / 77 28 / 30 performance comparable to or better than OTR and WVTR than Examples of the Invention 1 to 8. Also, one skilled in the art will recognize that the OTR of the laminate can be adjusted depending on the thickness and ethylene content of the barrier layer EVOH (i.e., in general, the thicker the barrier layer or the lower the ethylene content, the lower the achievable OTR value). As noted above, the Inventive Examples are non-limiting examples, not intended to limit the scope of disclosure, and a multilayer film according to embodiments of the present invention may include a barrier layer comprising an EVOH having an ethylene content of 20 to 50 mol%. Table 2 - Thickness, OTR and WVTR Exemplo Espessura (pm) OTR (cm3 / dia / m2) WVTR (g / dia / m2) Comp. 1 73 2,68 2,85 Comp. 2 73 1,82 2,49 Inv. 1 95 0,42 3,19 Inv. 2 95 1,56 3,27 Inv. 3 75 2,37 4,06 Inv. 4 75 2,15 4,01 Inv. 5 80 2,05 3,15 Inv. 6 80 2,00 2,83 Inv. 7 80 2,00 4,42 Inv. 8 80 6,51 2,69
[00114] The hot seal initiation temperature (HSIT), seal strength, hot adhesion initiation temperature at 1 Newton, and hot adhesion strength at 110 °C are measured. Figure 1 shows the hot seal strength curves of Comparative Example 1 and Invention Examples 1, 3, 5, and 7. Figure 2 shows the hot adhesion strength curves of Comparative Example 2 and Invention Examples 2, 4, 6, and 8. Tables 3 and 4 provide the results. The shrinkage (%) at 70 °C, 80 °C, 90 °C, 100 °C, 110 °C, 120 °C, and 130 °C of the examples is measured. None of the examples show shrinkage at 70 °C, 80 °C, 90 °C, 100 °C, or 110 °C in the machine direction (MD) or cross or transverse direction (DT). The shrinkage results (%) between 70 °C and 130 °C for the examples are reported in Table 5.
[00115] Examples of the Invention 1, 3, 5 and 7 have comparable or, in aspects, comparable HSIT, seal strength, hot adhesion initiation and hot adhesion strength. Petition 870250007322, dated 01 / 29 / 2025, page 39 / 77 29 / 30 improved compared to Comparative Example 1. Similarly, Examples of the Invention 2, 4, 6, and 8 have comparable or, in some respects, improved HSIT, seal strength, hot adhesion initiation, and hot adhesion resistance compared to Comparative Example 2. The Examples of the Invention exhibit a desirable or maintained low hot adhesion initiation temperature and low HSIT, and achieve, in some respects, maintained or improved seal strength performance. The Examples of the Invention have heat resistance performance and seal performance comparable to the Comparative Examples in the temperature range of 70 °C to at least 120 °C, and thus have a seal window of at least 40 °C or about 50 °C.
[00116] Table 3 - HSIT, sealing strength, hot adhesion initiation and hot adhesion strength for Comparative Example 1 and Examples of the Invention 1, 3, 5 and 7. Example HSIT at 5N (°C) Sealing strength at 120°C (N / 25 mm) Hot adhesion initiation at 1N (°C) Hot adhesion strength at 110°C (N / 25 mm) Comp. 1 74 47.9 78 1.51 Inv. 1 74 50.8 82 1.23 Inv. 3 81 52.8 79 1.31 Inv. 5 76 38.4 78 0.35 Inv. 7 74 59.3 75 2.13
[00117] Table 4 - HSIT, sealing strength, hot adhesion initiation and hot adhesion strength for Comparative Example 2 and Examples of the Invention 2, 4, 6 and 8. Example HSIT at 5N (°C) Sealing strength at 120°C (N / 25 mm) Hot adhesion initiation at 1N (°C) Hot adhesion strength at 110°C (N / 25 mm) Comp. 2 97 12.2 75 6.43 Inv. 2 95 13.2 75 4.84 Inv. 4 96 11.0 75 4.33 Inv. 6 95 12.2 74 5.27 Inv. 8 96 10.6 73 6.23 Petition 870250007322, dated 01 / 29 / 2025, p. 40 / 77 30 / 30
[00118] Table 5 - Shrinkage (%) between 70 and 130 °C inside the heat-seal window Example Shrinkage (%) in DM at 70 to 110 °C* Shrinkage (%) in DT at 70 to 110 °C* Shrinkage (%) in DM at 120 °C* Shrinkage (%) in DT at 120 °C* Shrinkage (%) in DM at 130 °C* Shrinkage (%) in DT at 130 °C* Comp. 1 0 0 0 0 0 0 Comp. 2 0 0 0 0 0 0 Inv 1 0 0 >8 4 >12 12 Inv 2 0 0 >8 4 >12 12 Inv 3 0 0 >8 8 >12 4 Inv 4 0 0 >8 4 >12 8 Inv 5 0 0 0 0 0 0 Inv 6 0 0 0 0 0 0 Inv. 7 0 0 0 0 0 0 Inv. 8 0 0 0 0 0 0 *Dimensions of the sealing bar: 0.5 cm (DM direction) x 2.5 cm (DT direction).
[00119] Each document cited in the present invention, if any, including any patent or patent application by reference or related reference, and any patent application or patent to which the present application claims priority or benefit, is hereby incorporated by reference in its entirety, except where expressly excluded or otherwise limited. Reference to any document is not an admission that it is prior art in relation to any invention disclosed or claimed herein or that it alone, or in any combination with any other reference or references, teaches, suggests or reveals any such invention. Furthermore, to the extent that any meaning or definition of a term in this document conflicts with any meaning or definition of the same term in a document incorporated by reference, the meaning or definition ascribed to that term in this document shall prevail.
[00120] Although specific embodiments of the present invention have been illustrated and described, it will be evident to those skilled in the art that various other alterations and modifications can be made without departing from the spirit and scope of the invention. Therefore, it is intended to cover, in the appended claims, all such alterations and modifications that are within the scope of this invention.
Claims
1. Laminate, characterized in that it comprises: (a) a multilayer film comprising: (1) a barrier layer comprising an ethylene-vinyl alcohol copolymer; (2) a sealing layer, wherein the sealing layer comprises at least 70% by weight of an ethylene-acid copolymer ionomer or a polyethylene elastomer / plastomer having a higher peak melting temperature (Tm) of 100 °C or less; and (3) a bonding layer between the barrier layer and the sealing layer; (b) a polyethylene film comprising an ethylene-based polymer having a density of 0.900 to 0.970 g / cm3; and (c) an adhesive that bonds the multilayer film to the polyethylene film; wherein the polyethylene film is an oriented film.
2. Laminate according to claim 1, characterized in that the multilayer film further comprises an outer layer comprising a polyethylene having a density of 0.900 to 0.970 g / cm3 and a second bonding layer between the outer layer and the barrier layer. 3.Laminate, according to any one of claims 1 or 2, characterized in that the polyethylene film is a biaxially oriented film.
4. Laminate, according to any one of claims 1 to 2, characterized in that the polyethylene film is a machine-oriented film.
5. Laminate, according to any one of claims 1 to 4, characterized in that the polyethylene film additionally comprises at least 20% by weight of a second ethylene-based polymer having a density of 0.958 g / cm3 or greater.
6. Laminate, according to any one of claims 1 to 5, characterized in that the polyethylene film additionally comprises a barrier layer comprising an ethylene-vinyl alcohol copolymer.
7. Laminate, according to any one of claims 1 to 6, characterized in that the barrier layer of the multilayer film is 5 to 25% of the total thickness of the multilayer film. 8.Laminate, according to any one of claims 1 to 7, characterized by the fact that the sealing layer is at least 10 microns thick.
9. Laminate, according to any one of claims 1 to 8, characterized by the fact that the sealing layer is 25 to 60% of the total thickness of the multilayer film.
10. Laminate, according to any one of claims 1 to 9, characterized by the fact that the fixing layer comprises an anhydride-modified linear low-density polyethylene and at least one of linear low-density polyethylene, low-density polyethylene, medium-density polyethylene, or high-density polyethylene.
11. Laminate, according to any one of claims 1 to 10, characterized in that the adhesive comprises a solvent-based adhesive, a solvent-free adhesive, or a water-based adhesive.