Ethylene polymers, manufacturing art, products molded by sopro and olefin polymerization process

A double metallocene catalyst system addresses the trade-off in ethylene polymer properties by concentrating long-chain branches in lower molecular weight fractions, enhancing extrusion processability and meltability while maintaining hardness for blow molding applications.

BR112022025254B1Active Publication Date: 2026-11-17CHEVRON PHILLIPS CHEMICAL COMPANY LP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
BR112022025254
Authority / Receiving Office
BR · BR
Patent Type
Patents
Current Assignee / Owner
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing ethylene polymers produced with metallocene catalysts have excellent impact and toughness properties but poor extrusion processability and meltability, while Ziegler-Natta and chromium-based catalysts offer good extrusion processability and meltability but lack hardness properties, making it difficult to achieve both in blow molding applications.

Method used

A double metallocene catalyst system is used to produce ethylene polymers with long-chain branches concentrated in lower molecular weight fractions, maintaining meltability and parison stability while improving extrusion processability, characterized by a unique molecular weight distribution and branching profile.

Benefits of technology

The ethylene polymers exhibit improved extrusion processability and meltability with maintained hardness properties, suitable for producing blow-molded products like bottles and containers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000073_0000
    Figure 00000073_0000
  • Figure 00000074_0000
    Figure 00000074_0000
  • Figure 00000075_0000
    Figure 00000075_0000
Patent Text Reader

Abstract

Dual catalyst system for producing long-chain branched polyethylene for blow molding applications. These are ethylene-based polymers characterized by a melting index of less than 1 g / 10 min, a density of 0.94 to 0.965 g / cm3, a Mw of 100,000 to 250,000 g / mol, a relaxation time of 0.5 to 3, an average number of long-chain branches (LCBs) per 1,000,000 total carbon atoms in a molecular weight range of 300,000 to 900,000 g / mol that is greater than that in a molecular weight range of 1,000,000 to 2,000,000 g / mol, or an average number of LCBs per 1,000,000 total carbon atoms in a molecular weight range of 1,000,000 to 2,000,000 g / mol less than or equal to about 5, and a maximum ratio of ΔE / 3Δ at an extension rate of 0.1 s-1 from 1.2 to 10.These polymers do not have substantially long-chain branching in the high molecular weight fraction of the polymer; instead, they have significant long-chain branching in a lower molecular weight fraction, so that the meltability and parison stability of the polymer are maintained during the manufacture of blow-molded products and other fabricated articles. These ethylene polymers can be produced using a dual catalyst system containing a single-atom bridged metallocene compound or a two-atom bridged metallocene compound with two indenyl groups, and a single-atom bridged metallocene compound with a fluorenyl group and a cyclopentadienyl group.
Need to check novelty before this filing date? Find Prior Art

Description

"ETHYLENE POLYMERS, MANUFACTURING ARTICLES, BLOW-MOLDED PRODUCTS AND OLEFIN POLYMERIZATION PROCESS" FUNDAMENTALS OF THE INVENTION

[001] Polyolefins, such as homopolymer and copolymer of high-density polyethylene (HDPE) and linear low-density polyethylene (LLDPE), can be produced using various combinations of catalyst systems and polymerization processes. Ziegler-Natta and chromium-based catalyst systems can, for example, produce ethylene polymers that have good extrusion processability, polymer meltability in blow molding and pipe applications, and bubble stability in blown film applications, typically due to their wide molecular weight distribution (MWD). Metallocene-based catalyst systems can, for example, produce ethylene polymers that have excellent impact and toughness properties, but often at the cost of poor extrusion processability, meltability, and bubble stability.

[002] In some end uses, such as blow molding, it may be beneficial to have the hardness properties of a metallocene-catalyzed copolymer, but with improved processability, stress hardening and meltability. Consequently, it is to these purposes that the present invention generally relates. SUMMARY OF THE INVENTION

[003] This summary is provided to present a selection of concepts that are better described below in the detailed description. This summary is not intended to identify necessary or essential features of the claimed subject matter. Nor is it intended to be used to limit the scope of the claimed subject matter.

[004] The present invention relates generally to ethylene polymers (for example, ethylene / α-olefin copolymers) characterized by a melting index less than or equal to about 1 g / 10 min, a density in a range of about 0.94 to about 0.965 g / cm3, a Mw in a range of about 100000 to about 250000 g / mol and a relaxation time of about 0.5 to about 3 seconds. Petition 870240096702, dated 12 / 11 / 2024, p. 12 / 192 2 / 68

[005] These ethylene polymers can be further characterized by an average number of long-chain branches (LCBs) per 1,000,000 total carbon atoms of the polymer in a molecular weight range of 300,000 to 900,000 g / mol that is greater (by at least 50%, at least 100%, or at least 200%) than that in a molecular weight range of 1,000,000 to 2,000,000 g / mol. Beneficially, most LCBs are present in lower molecular weight portions of the ethylene polymer and not in the very high molecular weight fraction (often referred to as the high molecular weight tail of the molecular weight distribution).Alternatively, these ethylene polymers can be further characterized by an average number of LCBs per 1,000,000 total carbon atoms of the polymer in a molecular weight range of 1,000,000 to 2,000,000 g / mol less than or equal to about 5 (effectively, from little to no long-chain branching at the high molecular weight end), and a maximum nE / 3n ratio at an extension rate of 0.1 s⁻¹ in a range of about 1.2 to about 10 (the ratio of extension viscosity to 3 times the shear viscosity; for Newtonian fluids, the ratio is 1 and stress hardening results in ratios greater than 1).

[006] Unexpectedly, there is substantially no long-chain branching in the high molecular weight fraction of these polymers that could adversely impact the properties of blow-molded products. However, beneficially, there is a significant amount of long-chain branching in lower molecular weight fractions of the polymer, so that the meltability and parison stability of the polymer are maintained, as well as the extrusion processability. The ethylene polymers disclosed herein can be used to produce various manufactured articles, such as blow-molded bottles and containers.

[007] Another aspect of this invention relates to a double catalyst system, and in this aspect, the double catalyst system may comprise catalyst component I comprising a metallocene compound bridged to a single atom or bridged to two atoms with two indenyl groups, catalyst component II comprising a metallocene compound bridged to a single atom with a fluorenyl group and a cyclopentadienyl group, and Petition 870240096702, dated 12 / 11 / 2024, p. 13 / 192 3 / 68 with an alkenyl substituent on the single-atom bridge and / or on the cyclopentadienyl group, an activator and, optionally, a cocatalyst.

[008] In yet another aspect, an olefin polymerization process is provided, and in this aspect, the process may comprise placing any catalyst composition disclosed herein in contact with an olefin monomer and an optional olefin comonomer in a polymerization reactor system under polymerization conditions to produce an olefin polymer. For example, the olefin monomer may be ethylene and the olefin comonomer may be 1-butene, 1-hexene, 1-octene or a mixture thereof.

[009] Both the aforementioned summary and the following detailed description provide examples and are explanatory only. Consequently, the preceding summary and the detailed description below should not be considered restrictive. Furthermore, features or variations may be provided beyond those set forth herein. For example, certain aspects and modalities may be directed to various combinations and subcombinations of features described in the detailed description. BRIEF DESCRIPTION OF THE FIGURES

[010] Figure 1 presents a plot of the molecular weight distributions of the polymers from Examples 1-2 and Comparative Example 3.

[011] Figure 2 presents a plot of the short-chain branching distributions across the molecular weight distributions of the polymers from Examples 1-2.

[012] Figure 3 presents a plot of the long-chain branching distribution across the molecular weight distribution of the polymer from Example 1.

[013] Figure 4 presents a plot of the long-chain branching distribution across the molecular weight distribution of the polymer from Example 2.

[014] Figure 5 shows a plot of the radius of gyration in relation to molecular weight for a linear standard and the polymers of Examples 1-2.

[015] Figure 6 shows a plot of extension viscosity (extension viscosity as a relation to time) for the polymer of Example 1.

[016] Figure 7 shows a plot of extension viscosity (extension viscosity as a relation to time) for the polymer of Example 2. Petition 870240096702, dated 12 / 11 / 2024, page 14 / 192 4 / 68

[017] Figure 8 presents a plot of extension viscosity (extension viscosity as a relation to time) for the polymer of Comparative Example 4.

[018] Figure 9 presents a plot of the maximum ηΞ / 3η ratio at extension rates in the range of 0.03 to 10 s-1 for the polymers of Examples 1-2.

[019] Figure 10 presents a dynamic rheology plot comparing the viscosities of the polymers in Examples 1-2 to those of the polymer in Comparative Example 3. DEFINITIONS

[020] To define more clearly the terms used in this document, the following definitions are provided. Unless otherwise indicated, the following definitions apply to this disclosure. If a term is used in the disclosure but is not specifically defined in this document, the definition from the IUPAC Compendium of Chemical Terminology, 2nd Edition (1997), may be applied, provided that such definition does not conflict with any other disclosure or definition applied in this document, or render indefinitely void or void any claim for that definition to apply. To the extent that any definition or usage provided by any document incorporated by means of this document conflicts with the definition or usage of controls provided in this document.

[021] In this document, material features are described in such a way that, within particular aspects, a combination of different features can be anticipated. For any and all aspects and / or features disclosed in this document, all combinations that do not adversely affect the designs, compositions, processes and / or methods described in this document are contemplated with or without explicit description of the particular combination. Additionally, unless explicitly stated otherwise, any aspect and / or feature disclosed in this document may be combined to describe inventive features consistent with the present disclosure.

[022] Although compositions and methods are described in this document in terms of “comprising” various components or steps, compositions and methods may also “consist essentially of” or Petition 870240096702, dated 12 / 11 / 2024, p. 15 / 192 5 / 68 “consist of” the various components or steps, unless stated otherwise. For example, a catalyst composition consistent with aspects of the present invention may comprise; alternatively, it may consist essentially of; or alternatively, it may consist of; catalyst component I, catalyst component II, an activator and a cocatalyst.

[023] The terms “a”, “an”, “the”, “the”, etc., are intended to include plural alternatives, for example, at least one, unless otherwise specified. For example, the disclosure of an activator-support or a metallocene compound is intended to cover one, or mixtures or combinations of more than one, activator-support or metallocene compound, respectively, unless otherwise specified.

[024] Groups of elements in the table are indicated using the numbering scheme indicated in the version of the periodic table of elements published in Chemical and Engineering News, 63(5), 27, 1985. In some cases a group of elements may be indicated using a common name assigned to the group; for example, alkaline earth metals (or alkali metals) for elements of Group 1, alkaline earth metals (or alkali metals) for elements of Group 2, transition metals for elements of Groups 3-12 and halogens for elements of Group 17.

[025] For any particular compound disclosed in this document, the general structure or name presented is also intended to encompass all structural isomers, conformational isomers, and stereoisomers that may arise from a given set of substituents, unless otherwise indicated. Thus, a general reference to a compound includes all structural isomers unless explicitly indicated otherwise; for example, a general reference to pentane includes n-pentane, 2-methylbutane, and 2,2-dimethylpropane, while a general reference to a butyl group includes an n-butyl group, a sec-butyl group, an isobutyl group, and a tert-butyl group. Furthermore, a reference to a general structure or name encompasses all enantiomers, diastereomers, and other optical isomers, whether in enantiomeric or racemic forms, as well as mixtures of stereoisomers, as the context permits or requires.For any particular formula or name that is displayed, any general formula or name. Petition 870240096702, dated 12 / 11 / 2024, p. 16 / 192 Figure 6 / 68 also covers all conformational isomers, regioisomers, and stereoisomers that can arise from a given set of substituents.

[026] The term substituted, when used to describe a group, for example, when referring to a substituted analogue of a particular group, is intended to describe any non-hydrogen chemical moiety that formally replaces a hydrogen in that group and is intended to be non-limiting. A group or groups may also be referred to in this document as substituted or by equivalent terms such as non-substituted, which refer to the original group in which a non-hydrogen radical does not replace a hydrogen within that group. Unless otherwise specified, substituted is intended to be non-limiting and includes inorganic substituents or organic substituents, as understood by one skilled in the art.

[027] The term hydrocarbon, whenever used in this specification and claims, refers to a compound containing only carbon and hydrogen. Other identifiers may be used to indicate the presence of specific groups in the hydrocarbon (for example, halogenated hydrocarbon indicates the presence of one or more halogen atoms replacing an equivalent number of hydrogen atoms in the hydrocarbon). The term hydrocarbyl group is used in this document in accordance with the definition specified by IUPAC: a univalent group formed by the removal of a hydrogen atom from a hydrocarbon (i.e., a group containing only carbon and hydrogen). Examples without limitation of hydrocarbyl groups include alkyl, alkenyl, aryl, and aralkyl groups, among others.

[028] The term polymer as used in this document includes, but is not limited to, homopolymers, copolymers, terpolymers, etc., and alloys and mixtures thereof. The term polymer as used in this document also includes impact, block, graft, random, and alternating copolymers. A copolymer is derived from an olefin monomer and an olefin comonomer, while a terpolymer is derived from an olefin monomer and two olefin comonomers. Therefore, polymer encompasses copolymers and terpolymers derived from any olefin monomer and comonomer(s) disclosed in this document. Similarly, the scope of the term polymerization includes homopolymerization, Petition 870240096702, dated 12 / 11 / 2024, page 17 / 192 7 / 68 Copolymerization and terpolymerization. Therefore, an ethylene polymer includes ethylene homopolymers, ethylene copolymers (e.g., ethylene / α-olefin copolymers), ethylene terpolymers and the like, as well as mixtures or blends thereof. Thus, an ethylene polymer encompasses polymers frequently referred to in the art as LLDPE (linear low-density polyethylene) and HDPE (high-density polyethylene). As an example, an olefin copolymer, such as an ethylene copolymer, may be derived from ethylene and a comonomer, such as 1-butene, 1-hexene, or 1-octene. If the monomer and comonomer were ethylene and 1-hexene, respectively, the resulting polymer may be categorized as an ethylene / 1-hexene copolymer. The term "polymer" also includes all possible geometric configurations, unless otherwise stated, and such configurations may include isotactic, syndiotactic, and random symmetries.Furthermore, unless stated otherwise, the term "polymer" is also intended to include all polymers of molecular weight and is inclusive of polymers of lower molecular weight.

[029] The term “cocatalyst” is used generally in this document to refer to compounds such as aluminoxane compounds, organoboron or organoborate compounds, ionizing ionic compounds, organoaluminum compounds, organozinc compounds, organomagnesium compounds, organolithium compounds and the like, which may constitute a component of a catalyst composition when used, for example, in addition to an activating support. The term cocatalyst is used independently of the actual function of the compound or of any chemical mechanism by which the compound may operate.

[030] The terms chemically treated solid oxide, treated solid oxide compound, and the like, are used in this document to indicate a solid inorganic oxide of relatively high porosity, which may exhibit Lewis acid or Bronsted acid behavior, and which has been treated with an electron-withdrawing component, typically an anion, and which is calcined. The electron-withdrawing component is typically a source compound of electron-withdrawing anions. The chemically treated solid oxide may comprise the contact product of one or more solid oxides with one or more electron-withdrawing anion sources. Petition 870240096702, dated 12 / 11 / 2024, page 18 / 192 8 / 68 of electrons. Typically, the chemically treated solid oxide comprises at least one acidic solid oxide compound. The activator support of the present invention may be a chemically treated solid oxide. The terms support and activator-support are not used to imply that these components are inert, and such components should not be interpreted as an inert component of the catalyst composition. The term activator, as used herein, generally refers to a substance that is capable of converting a metallocene component into a catalyst that can polymerize olefins or converting a contact product of a metallocene component and a component that provides an activatable ligand (e.g., an alkyl, a hydride) to the metallocene, when the metallocene compound does not yet comprise such a ligand, into a catalyst that can polymerize olefins. This term is used independently of the actual activation mechanism.Illustrative activators include activator holders, aluminoxanes, organoboron or organoborate compounds, ionizing ionic compounds, and the like. Aluminoxanes, organoboron or organoborate compounds, and ionizing ionic compounds are generally referred to as activators if used in a catalyst composition in which an activator holder is not present. If the catalyst composition contains an activator holder, then the aluminoxane, organoboron or organoborate, and ionizing ionic materials are typically termed cocatalysts.

[031] The term “metallocene,” as used herein, describes compounds comprising at least one chemical moiety of the type η3a η5-cycloalkadienyl, wherein the η3a η5-cycloalkadienyl moieties include cyclopentadienyl ligands, indenyl ligands, fluorenyl ligands, and the like, including partially saturated or substituted derivatives or analogues of any of these. Possible substituents on these ligands may include H, therefore, this invention comprises ligands such as tetrahydroindenyl, tetrahydrofluorenyl, octahydrofluorenyl, partially saturated indenyl, partially saturated fluorenyl, partially saturated substituted indenyl, partially saturated substituted fluorenyl, and the like. In some contexts, the metallocene is referred to simply as the “catalyst,” similarly, the term “cocatalyst” is used herein to refer to, by Petition 870240096702, dated 12 / 11 / 2024, p. 19 / 192 9 / 68 example, to an organoaluminum compound.

[032] The terms “catalyst composition”, “catalyst mixture”, “catalyst system” and the like, are independent of the actual product or composition resulting from the contact or reaction of the initial components of the disclosed or claimed catalyst composition / mixture / system, the nature of the active catalytic site, or the fate of the cocatalyst, catalyst component I, catalyst component II or activator (e.g., activator carrier), after combination of these components. Therefore, the terms “catalyst composition”, “catalyst mixture”, “catalyst system” and the like encompass the initial starting components of the composition, as well as any product (or products) that may result from the contact of these initial starting components, and this is inclusive of both heterogeneous and homogeneous catalyst systems or compositions.The terms catalyst composition, catalyst mixture, catalyst system, and similar terms may be used interchangeably throughout this disclosure.

[033] The term contact product is used in this document to describe compositions in which the components are brought into contact in any order, in any manner, and for any period of time, unless otherwise specified. For example, the components may be contacted by mixing or blending. Furthermore, the contact of any component may occur in the presence or absence of any other component of the compositions described herein. The combination of additional materials or components may be made by any suitable method. In addition, the term contact product includes mixtures, combinations, solutions, pastes, reaction products and the like, or combinations thereof. Although the contact product may include reaction products, it is not necessary that the respective components react with each other.Similarly, the term contact is used in this document to refer to materials that can be mixed, blended, pasted, dissolved, reacted, treated, or otherwise combined in some other way.

[034] Although methods and materials similar or equivalent to those described in this document may be used in practice or in testing the Petition 870240096702, dated 12 / 11 / 2024, page 20 / 192 10 / 68 of the present invention, the preferred methods, devices and materials are described below.

[035] All publications and patents mentioned in this document are incorporated herein by reference in their entirety for the purpose of describing and disclosing, for example, the constructs and methodologies described in the publications, which may be used in connection with the methods, compositions and compounds described in this document.

[036] Various types of ranges are disclosed in the present invention. When a range of any type is disclosed or claimed, the intention is to disclose or claim individually every possible number that such a range could reasonably encompass, including endpoints of the range, as well as any subranges and combinations of subranges covered therein. For example, when a chemical fraction with a certain number of carbon atoms is disclosed or claimed, the intention is to disclose or claim individually every possible number that such a range could encompass, in accordance with the disclosure in this document.For example, the disclosure that a chemical moiety is a C1 to C18 hydrocarbyl group, or in alternative language, a hydrocarbyl group having from 1 to 18 carbon atoms, as used in this document, refers to a chemical moiety that may have 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17 or 18 carbon atoms, as well as any range between these two numbers (e.g., a C1 to C8 hydrocarbyl group), and also including any combination of ranges between these two numbers (e.g., a C2 to C4 and C12 to C16 hydrocarbyl group).

[037] Similarly, another representative example follows for the Mw / Mn ratio of an ethylene polymer consistent with aspects of this invention. By a disclosure that the Mw / Mn ratio may be in a range of about 5 to about 15, the intention is to state that the Mw / Mn ratio may be any ratio in the range and, for example, may be equal to about 5, about 6, about 7, about 8, about 9, about 10, about 11, about 12, about 13, about 14 or about 15. Additionally, the Mw / Mn ratio may be within any range from about 5 to about 15 (for example, from about 6 to about 10) and this also includes any combination of ranges between about 5 and about 15 (for example, from about 6 to about 10). Petition 870240096702, dated 12 / 11 / 2024, p. 21 / 192 11 / 68 For example, the Mw / Mn ratio may be in a range of about 6 to about 9 or about 11 to about 14). Moreover, in all cases, when “about” a particular value is revealed, then that value itself is revealed. Thus, the revelation that the Mw / Mn ratio may be from about 5 to about 15 also reveals an Mw / Mn ratio of 5 to 15 (for example, from 6 to 10), and this also includes any combination of ranges between 5 and 15 (for example, the Mw / Mn ratio may be in a range of 6 to 9 or from 11 to 14). Similarly, all other ranges revealed in this document should be interpreted in a manner similar to these examples.

[038] The term about means that quantities, sizes, formulations, parameters, and other quantities and characteristics are not and need not be exact, but may be approximate and / or greater or less, as desired, reflecting tolerances, conversion factors, rounding, measurement errors and the like, and other factors known to those skilled in the art. In general, a quantity, size, formulation, parameter, or other quantity or characteristic is about or approximate, whether or not expressly stated as such. The term about also encompasses values ​​that differ due to different equilibrium conditions for a composition resulting from a particular initial mixture. Whether or not modified by the term about, the claims include equivalents to the quantities. The term about may mean within 10% of the reported numerical value, preferably within 5% of the reported numerical value. DETAILED DESCRIPTION OF THE INVENTION

[039] The present invention relates generally to metallocene-based double ethylene polymers that have similar processability to chromium-based polymers, but with improved ESCR and hardness properties. Articles produced from these ethylene-based polymers may include blow-molded products, such as blow-molded bottles.

[040] In general, metallocene-derived ethylene-based polymers with long-chain branches have these long-chain branches concentrated in the high molecular weight fraction of the polymer. Advantageously, the ethylene polymers disclosed in this document do not have Petition 870240096702, dated 12 / 11 / 2024, page 22 / 192 12 / 68 substantially no long-chain branching in the high molecular weight fraction of the polymer; instead, significant amounts of long-chain branching are present in lower molecular weight fractions of the polymer.

[041] These ethylene polymers can be produced, for example, with a double metallocene catalyst system in a single reactor. It has been found that the use of a first metallocene catalyst that preferentially produces lower molecular weight polyethylene with a relatively high LCB content in combination with a second metallocene catalyst that preferentially produces essentially linear polyethylene of higher molecular weight can result in the unique combination of polymer properties described in this document. ETHYLENE POLYMERS

[042] Generally, the polymers disclosed here are ethylene-based polymers or ethylene polymers, encompassing ethylene homopolymers as well as copolymers, terpolymers, etc., of ethylene and at least one olefin comonomer. Comonomers that can be copolymerized with ethylene can often have from 3 to 20 carbon atoms in their molecular chain. For example, typical comonomers may include, but are not limited to, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene and the like, or combinations thereof.In one aspect, the olefin comonomer may comprise a C3C18 olefin; alternatively, the olefin comonomer may comprise a C3C10 olefin; alternatively, the olefin comonomer may comprise a C4C10 olefin; alternatively, the olefin comonomer may comprise a C3C10 α-olefin; alternatively, the olefin comonomer may comprise a C4-C10 α-olefin; alternatively, the olefin comonomer may comprise 1-butene, 1-hexene, 1-octene, or any combination thereof; or alternatively, the comonomer may comprise 1-hexene. Typically, the amount of comonomer, based on the total weight of monomer (ethylene) and comonomer, can range from about 0.01 to about 20 by weight %, from about 0.1 to about 10 by weight %, from about 0.5 to about 15 by weight %, from about 0.5 to about 8 by weight %, or from about 1 to about 15 by weight %. Petition 870240096702, dated 12 / 11 / 2024, page 23 / 192 13 / 68

[043] In one aspect, the ethylene polymer of this invention may comprise an ethylene / α-olefin copolymer, while in another aspect, the ethylene polymer may comprise an ethylene homopolymer, and in yet another aspect, the ethylene polymer of this invention may comprise an ethylene / α-olefin copolymer and an ethylene homopolymer. For example, the ethylene polymer may comprise an ethylene / 1-butene copolymer, an ethylene / 1-hexene copolymer, an ethylene / 1-octene copolymer, an ethylene homopolymer, or any combination thereof; alternatively, an ethylene / 1-butene copolymer, an ethylene / 1-hexene copolymer, an ethylene / 1-octene copolymer, or any combination thereof; or alternatively, an ethylene / 1-hexene copolymer.

[044] An illustrative and non-limiting example of an ethylene polymer (for example, comprising an ethylene copolymer) of the present invention may have a melting index less than or equal to about 1 g / 10 min, a density in a range of about 0.94 to about 0.965 g / cm3, a Mw in a range of about 100000 to about 250000 g / mol, a relaxation time of about 0.5 to about 3 if an average number of long-chain branches (LCBs) per 1000000 total carbon atoms of the polymer in a molecular weight range of 300000 to 900000 g / mol that is greater (for example, at least 50% greater, or at least 75% greater, or at least 100% greater, or at least 150% greater, or at least 200% greater) that is, in a molecular weight range of 1,000,000 to 2,000,000 g / mol.Another illustrative and non-limiting example of an ethylene polymer (for example, comprising an ethylene copolymer) of the present invention may have a melting index less than or equal to about 1 g / 10 min, a density in a range of about 0.94 to about 0.965 g / cm3, a Mw in a range of about 100000 to about 250000 g / mol, a relaxation time of about 0.5 to about 3 s, an average number of long-chain branches (LCBs) per 1,000,000 total carbon atoms of the polymer in a molecular weight range of 1,000,000 to 2,000,000 g / mol less than or equal to about 5, and a maximum nE / 3n ratio at an extension rate of 0.1 s-1 in a range of about 1.2 to about 10. These ethylene polymers may also have any one of the polymer properties listed below and, in any combination, unless. Petition 870240096702, dated 12 / 11 / 2024, p. 24 / 192 14 / 68 may be indicated otherwise.

[045] The densities of ethylene-based polymers disclosed in this document are frequently greater than or equal to about 0.94 g / cm3 and less than or equal to about 0.965 g / cm3. Furthermore, in particular aspects, the density may be in a range of about 0.942 to about 0.965 g / cm3, about 0.94 to about 0.96 g / cm3, about 0.95 to about 0.965 g / cm3, about 0.955 to about 0.962 g / cm3 or about 0.955 to about 0.96 g / cm3.

[046] Ethylene polymers described in this document may often have a melting index (MI) less than or equal to about 1 g / 10 min, less than or equal to about 0.7 g / 10 min, or less than or equal to about 0.5 g / 10 min. In further aspects, ethylene polymers described in this document may have a melting index (MI) in a range of about 0.1 to about 0.7 g / 10 min, about 0.1 to about 0.5 g / 10 min, about 0.2 to about 0.7 g / 10 min, or about 0.2 to about 0.4 g / 10 min.

[047] Although not limited to this, the ethylene polymer may also have a high charge melt index (HLMI) in a range of about 10 to about 65 g / 10 min; alternatively, from about 35 to about 55 g / 10 min; alternatively, from about 20 to about 60 g / 10 min; or alternatively, from about 40 to about 55 g / 10 min.

[048] The ratio of high load melt index (HLMI) to melt index (MI), termed the HLMI / MI ratio, is not particularly limited, however, it is typically in the range of about 80 to about 220, about 100 to about 200, about 120 to about 170 or about 130 to about 160. At this HLMI / MI ratio, the melt index is not equal to zero.

[049] In one aspect, ethylene polymers described in this document may have an Mw / Mn ratio, or polydispersity index, in a range of about 5 to about 15, about 6 to about 12, about 6 to about 10, about 7 to about 13 or about 7 to about 10. Additionally or alternatively, the ethylene polymer may have an Mz / Mw ratio in a range of about 3.5 to about 10, about 4 to about 8, about 4 to about 6 or about 4.5 to about 5.5.

[050] In one aspect, ethylene polymers described in the present Petition 870240096702, dated 12 / 11 / 2024, p. 25 / 192 15 / 68 document may have a weight-average molecular weight (Mw) in a range of about 125000 to about 250000 g / mol, about 100000 to about 200000 g / mol, about 110000 to about 190000 g / mol or about 125000 to about 175000 g / mol. Additionally or alternatively, the ethylene polymer may have a number-average molecular weight (Mn) in a range of about 10000 to about 30000 g / mol, about 10000 to about 25000 g / mol, about 15000 to about 25000 g / mol or about 15000 to about 20000 g / mol. Alternatively, the ethylene polymer may have an average molecular weight z (Mz) in a range of about 500,000 to about 2,000,000 g / mol, about 600,000 to about 1,200,000 g / mol, about 650,000 to about 1,000,000 g / mol, or about 700,000 to about 900,000 g / mol.

[051] Polyethylene polymers consistent with certain aspects of the invention may frequently have a bimodal molecular weight distribution (as determined using gel permeation chromatography (GPC) or other related analytical technique). Frequently, in a bimodal molecular weight distribution, there is a valley between the peaks, and the peaks may be separated or deconvoluted. Typically, a bimodal molecular weight distribution can be characterized by having an identifiable high molecular weight component (or distribution) and an identifiable low molecular weight component (or distribution). Illustrative unimodal MWD curves and bimodal MWD curves are shown in U.S. Patent No. 8,383,754, which is incorporated herein by reference in its entirety.

[052] Although not limited to this, ethylene polymers described in this document may have a zero shear viscosity at 190 °C in a range of about 1 x 103 to about 1 x 108 Pa-s, about 1 x 104 to about 1 x 107 Pa-s or about 1 x 104 to about 1 x 106 Pa-s. In addition, these ethylene polymers may have a CY-a parameter of about 0.15 to about 0.45, about 0.2 to about 0.4, about 0.22 to about 0.35 or about 0.22 to about 0.32. Additionally or alternatively, these ethylene polymers may have a relatively short relaxation time given their relatively high molecular weight, with the relaxation time typically in the range of about 0.5 to about 3 s, such as from about 0.75 to about 2.5 s. Petition 870240096702, dated 12 / 11 / 2024, p. 26 / 192 16 / 68 about 1 to about 2 s or about 1 to about 1.5 s. Additionally or alternatively, these ethylene polymers can be characterized by a viscosity in HLMI (eta in HLMI or η in HLMI) at 190 °C in a range of about 250 to about 800 Pa-s and more frequently, in a range of about 300 to about 750, about 300 to about 500, about 300 to about 450 or about 350 to about 450 Pa-s. Alternatively, these ethylene polymers may have a viscosity at 100 s-1 (eta at 100 or η at 100) at 190 °C in a range of about 750 to about 1750, about 850 to about 1300, about 1000 to about 1500, or about 1000 to about 1300 Pa-s.Alternatively, these ethylene polymers may have a η ratio of 0.1 / η in 100 (viscosity at 0.1 s⁻¹ divided by viscosity at 100 s⁻¹) in a range of about 20 to about 45, about 20 to about 35, about 22 to about 32, or about 25 to about 30. These rheological parameters are determined from viscosity data measured at 190 °C and using the Carreau-Yasuda (CY) empirical model, as described in this document.

[053] The average number of long-chain branches (LCBs) per 1,000,000 total carbon atoms of ethylene polymer in a molecular weight range of 1,000,000 to 2,000,000 g / mol may be less than or equal to about 5 (there are effectively no LCBs in the high molecular weight fraction of the polymer). All average LCB numbers disclosed herein are numerical averages. In some respects, the average number of LCBs per 1,000,000 total carbon atoms of polymer in the molecular weight range of 1,000,000 to 2,000,000 g / mol may be less than or equal to about 4, less than or equal to about 3.5, less than or equal to about 3, or less than or equal to about 1. In further respects, the average number of LCBs in this molecular weight range may be below the detection limit.

[054] The average number of LCBs per 1,000,000 total carbon atoms of ethylene polymer in a molecular weight range of 300,000 to 900,000 g / mol may be greater (by any amount disclosed herein, for example, at least 50%, at least 75%, at least 100%, at least 150% or at least 200%, and often up to 400-800%, or more) than the number Petition 870240096702, dated 12 / 11 / 2024, p. 27 / 192 17 / 68 average of LCBs per 1,000,000 total carbon atoms in a molecular weight range of 1,000,000 to 2,000,000 g / mol. In some respects, the average number of LCBs per 1,000,000 total carbon atoms of ethylene polymer in a molecular weight range of 300,000 to 900,000 g / mol may be at least 50% higher (or at least 75% higher, or at least 100% higher, or at least 150% higher, or at least 200% higher and often up to 400-800% higher) than that in a molecular weight range of 1,000,000 to 2,000,000 g / mol. As disclosed in this document, all average LCB numbers are numerical averages.

[055] The average number of LCBs per 1,000,000 total carbon atoms of ethylene polymer in the molecular weight range of 300,000 to 900,000 g / mol is not particularly limited, however, it is frequently within a range of about 3 to about 15; alternatively, about 4 to about 13; alternatively, about 4 to about 10; alternatively, about 5 to about 9; or alternatively, about 6 to about 8.

[056] Similarly, the average number of LCBs per 1000000 total carbon atoms of ethylene polymer in the molecular weight range of 400000 to 600000 g / mol is not particularly limited, however, it is frequently within a range of about 4 to about 15; alternatively, about 5 to about 14; alternatively, about 5 to about 12; alternatively, about 7 to about 10; or alternatively, about 8 to about 9.

[057] In general polymer (using the Janzen-Colby model), ethylene polymers typically have long chain branching (LCB) levels in a range of about 4 to about 20 LCBs, about 5 to about 15 LCBs, about 6 to about 14 LCBs, or about 8 to about 12 LCBs per 1,000,000 total carbon atoms.

[058] Unexpectedly, the ethylene polymers described in this document may have a maximum ηΞ / 3η ratio at an extension rate of 0.1 s⁻¹ in a range of about 1.2 to about 10. For Newtonian fluids, the extension viscosity ratio for 3 times the shear viscosity is equal to 1, while stress hardening due to long-chain branching may result in ratios greater than 1. In one respect, the maximum ratio of Petition 870240096702, dated 12 / 11 / 2024, p. 28 / 192 The 18 / 68 ηE / 3η ratio at an extension rate of 0.1 s⁻¹ may be in the range of about 1.2 to about 10 or about 1.5 to about 8, while in another aspect the maximum ratio may be in the range of about 1.5 to about 5 or about 1.2 to about 4, and in yet another aspect the maximum ratio may be in the range of about 1.2 to about 3 or about 1.4 to about 3.5, and in yet another aspect the maximum ratio may be in the range of about 1.4 to about 3 or about 1.5 to about 2.5. These extension viscosity ratios for three times the shear viscosity are determined using a Sentmanat Extension Rheometer (SER) at 150 °C.

[059] Additionally, although not limited to this, the ethylene polymer can be further characterized by a maximum nE / 3n ratio at an extension rate of 0.03 s-1 in a range of about 1.2 to about 10; alternatively, from about 1.5 to about 8; alternatively, from about 2 to about 7; alternatively, from about 2 to about 5; alternatively, from about 2.5 to about 4.5; or alternatively, from about 3 to about 4.

[060] In addition, ethylene polymers (e.g., ethylene copolymers) can typically have a planar short-chain branching distribution (planar SCBD; uniform comonomer distribution).A flat SCBD can be characterized by a slope of a plot of the number of short-chain branches (SCBs) per 1000 total carbon atoms relative to the logarithm of the molecular weight of the ethylene polymer (determined by linear regression over the range D15 to D85) that is in a range of about -0.6 to about 0.6 and / or a percentage of data points that deviate from the average short-chain branching content by more than 0.5 SCBs per 1000 total carbon atoms (determined over the range D15 to D85) that is less than or equal to about 20% and / or a percentage of data points that deviate from the average short-chain branching content by more than 1 SCB per 1000 total carbon atoms (determined over the range D15 to D85) that is less than or equal to about 10%. Polymers that have a flat or uniform SCBD are disclosed, for example, in US Patent documents No. 9,217,049 and 9,574.031, which are incorporated into this document by reference in their entirety.

[061] Aspects of this invention also relate to the performance of Petition 870240096702, dated 12 / 11 / 2024, p. 29 / 192 19 / 68 Ethylene polymer (e.g., an ethylene / 1-hexene copolymer) in representative blow molding equipment, as described below in this document. The ethylene polymers may have a cycle time of about 13 to about 20, about 14 to about 19, about 15 to about 18, or about 16 to about 17 seconds; unexpectedly, these polymers may have cycle times that are substantially equal to those of comparable chromium-based resins. Additionally or alternatively, ethylene polymers described in this document may have a partial weight in a range of about 95 to about 115, about 100 to about 115, about 95 to about 110, or about 100 to about 110 grams.Additionally or alternatively, ethylene polymers described herein may have a layflat (top) in a range of about 13.2 to about 15.2, about 12.7 to about 14.4, about 13.2 to about 14.4 centimeters (about 5.2 to about 6, about 5 to about 5.7, about 5.2 to about 5.7 inches).

[062] Consistent with aspects of this disclosure, ethylene polymers may have an environmental stress cracking resistance (ESCR) of at least 200 hours. In addition, in some aspects, ethylene polymers may have an ESCR of at least 250 hours, at least 300 hours, at least 400 hours, or at least 500 hours, and may frequently be in the range as high as 600 to 1000 hours. The ESCR test is typically stopped after a certain number of hours is reached, and given the long duration of the test, the upper limit of ESCR (in hours) is generally not determined. The "bottle" ESCR test is conducted in 10% Igepal at 60 °C (140 °F) (ASTM D2561), which is a much more stringent test than the ESCR test conducted using a 100% Igepal solution.Alternatively, ethylene polymers may have a “folded strip” (ESCR) of at least 50 hours, such as at least 60 hours, at least 75 hours, at least 85 hours, or at least 100 hours, and may frequently be in the range as high as 150 to 300 hours. As mentioned above, the “folded strip” ESCR test is typically stopped after a certain number of hours is reached, and given the long duration of the test, the upper limit of ESCR (in hours) is generally not determined. The “folded strip” ESCR test is conducted in 10% Igepal at 50°C for a... Petition 870240096702, dated 12 / 11 / 2024, p. 30 / 192 20 / 68 thickness of 1.9 mm (75 mils) (ASTM D1693).

[063] In one respect, the ethylene polymer may be a reactor product (e.g., a single reactor product), for example, not a post-reactor blend of two polymers, for example, having different molecular weight characteristics. As a person skilled in the art would readily recognize, physical blends of two different polymer resins may be produced, however, this necessitates additional processing and complexity not required for a reactor product. Additionally, the ethylene polymer may further contain any suitable additive, examples without limitation thereof include an antioxidant, an acid scavenger, an antiblocking additive, a slip additive, a colorant, a filler, a polymer processing aid, a UV additive and the like, as well as any combination thereof.

[064] In addition, ethylene polymers can be produced with a metallocene catalyst system containing zirconium and hafnium, discussed further below. Metallocene-based ZieglerNatta, chromium, and titanium catalyst systems are not required. Therefore, the ethylene polymer may not contain any measurable amount of chromium or titanium (catalyst residue), i.e., less than 0.1 ppm by weight. In some respects, the ethylene polymer may independently contain less than 0.08 ppm, less than 0.05 ppm, or less than 0.03 ppm of chromium and titanium. ARTICLES AND PRODUCTS

[065] Articles of manufacture may be formed from and / or may comprise the olefin polymers (e.g., ethylene polymers) of this invention and, consequently, are encompassed in this document. For example, articles that may comprise the polymers of this invention may include, but are not limited to, an agricultural film, an automotive part, a bottle, a container for chemicals, a drum, a fiber or cloth, a food packaging film or container, a food service article, a fuel tank, a geomembrane, a household container, a lining, a molded product, a medical device or material, an outdoor storage product (e.g., wall panels of a Petition 870240096702, dated 12 / 11 / 2024, page 31 / 192 21 / 68 outdoor shed), outdoor recreational equipment (e.g., kayaks, basketball hoop bases), a pipe, sheet or tape, a toy or traffic barrier, and the like. Various processes may be employed to form these articles. Examples, without limitation, of such processes include injection molding, blow molding, spin molding, film extrusion, sheet extrusion, profile extrusion, thermoforming, and the like. Additionally, additives and modifiers are frequently added to these polymers in order to provide beneficial polymer processing or end-use product attributes. Such processes and materials are described in Modern Plastics Encyclopedia, mid-November 1995 issue, volume 72, no. 12; and Film Extrusion Manual Process, Materials, Properties, TAPPI Press, 1992; disclosures thereof are incorporated herein by reference in their entirety.In some aspects of this invention, a manufactured article may comprise any of the olefin polymers (or ethylene polymers) described herein, and the manufactured article may be or may comprise a blow-molded product.

[066] Also contemplated in this document is a method for forming or preparing a manufactured article comprising any polymer disclosed in this document. For example, a method may comprise (i) bringing a catalyst composition into contact with an olefin monomer (e.g., ethylene) and an optional olefin comonomer under polymerization conditions in a polymerization reactor system to produce an olefin polymer (e.g., an ethylene polymer), wherein the catalyst composition may comprise catalyst component I, catalyst component II, an activator (e.g., an activator support comprising a solid oxide treated with an electron-withdrawing anion) and an optional cocatalyst (e.g., an organoaluminum compound); and (ii) forming a manufactured article comprising the olefin polymer (or ethylene polymer).The forming stage may include mixing, melt processing, extrusion, molding (e.g., blow molding) or thermoforming, and the like, including combinations thereof. Any suitable additive may be combined with the polymer in the melt processing stage (stage of). Petition 870240096702, dated 12 / 11 / 2024, page 32 / 192 22 / 68 extrusion), such as antioxidants, acid scavengers, antiblocking agents, slip additives, colorants, fillers, processing aids, UV inhibitors and the like, as well as combinations thereof. Catalyst systems and polymerization processes

[067] According to aspects of the present invention, the olefin polymer (e.g., the ethylene polymer) can be produced using a double catalyst system. In these aspects, the catalyst component I can comprise any suitable single-atom bridge-linked or two-atom bridge-linked metallocene compound with two indenyl groups, or any single-atom bridge-linked or two-atom bridge-linked metallocene compound disclosed herein with two indenyl groups.Catalyst component II may comprise any suitable single-atom bridged metallocene compound with a fluorenyl group and a cyclopentadienyl group, and with an alkenyl substituent on the single-atom bridge and / or on the cyclopentadienyl group, or any single-atom bridged metallocene compound disclosed herein with a fluorenyl group and a cyclopentadienyl group, and with an alkenyl substituent on the single-atom bridge and / or on the cyclopentadienyl group. The catalyst system may also comprise any suitable activator or any activator disclosed herein and, optionally, any suitable cocatalyst or any cocatalyst disclosed herein.

[068] With reference, first, to catalyst component II, which may comprise a metallocene compound bridged to a single atom with a fluorenyl group and a cyclopentadienyl group; an alkenyl substituent may be present on the single atom bridge, or on the cyclopentadienyl group, or on both. In one aspect, the fluorenyl group may be substituted, while in another aspect, the fluorenyl group may be unsubstituted. Additionally, the bridged metallocene compound of catalyst component II may contain zirconium, hafnium, or titanium, or alternatively, zirconium or hafnium. Furthermore, the single atom bridge may be a single carbon atom or a single silicon atom, although it is not limited to them. In some aspects, this bridging atom may have two substituents independently selected from H or any Ci group. Petition 870240096702, dated 12 / 11 / 2024, p. 33 / 192 23 / 68 a C18 hydrocarbyl disclosed in this document (for example, one or both substituents may be a phenyl group). The alkenyl substituent on the cyclopentadienyl group (or on the bridging atom) may be any suitable alkenyl group, such as a C3 to C18 alkenyl group or a terminal C3 to C8 alkenyl group.

[069] Catalyst component II may comprise, in particular aspects of this invention, a bridged metallocene compound having formula (II): CP (II).

[070] Within formula (II), M, Cp, RX, RY, E and each X are independent elements of the bridged metallocene compound. Consequently, the bridged metallocene compound having formula (II) can be described using any combination of M, Cp, RX, RY, E and X disclosed herein.

[071] According to aspects of this invention, the metal in formula (II), M, can be Ti, Zr or Hf. In one aspect, for example, M can be Zr or Hf, while in another aspect, M can be Ti; alternatively, M can be Zr; or alternatively, M can be Hf.

[072] Each X in formula (II) may independently be a monoanionic ligand. In some respects, suitable monoanionic ligands may include, but are not limited to, H (hydride), BH4, a halide, a C1 to C36 hydrocarbyl group, a C1 to C36 hydrocarboxy group, a C1 to C36 hydrocarbylaminyl group, a C1 to C36 hydrocarbylsilyl group, a C1 to C36 hydrocarbylaminylsilyl group, —OBR12 or —OSO2R1, wherein R1 is a C1 to C36 hydrocarbyl group. It is contemplated that each X may be the same or different monoanionic ligand. In addition to the representative sections for each X that are disclosed herein, additional suitable hydrocarbyl groups, hydrocarboxy groups, hydrocarbylaminyl groups, hydrocarbylsilyl groups and hydrocarbylaminylsilyl groups are disclosed, for example, Petition 870240096702, dated 12 / 11 / 2024, p. 34 / 192 24 / 68 in Patent document US 9,758,600, incorporated herein by reference in its entirety.

[073] In one aspect, each X can independently be H, BH4, a halide (e.g., F, Cl, Br, etc.), a C18 to C18 hydrocarbyl group, a C18 to C18 hydrocarboxy group, a C18 to C18 hydrocarbylaminyl group, a C18 to C18 hydrocarbysilyl group, or a C18 to C18 hydrocarbylaminylsilyl group. Alternatively, each X can independently be H, BH4, a halide, OBR12, or OSO2R1, where R1 is a C18 to C18 hydrocarbyl group. In another aspect, each X can independently be H, BH4, a halide, a C1 to C12 hydrocarbyl group, a C1 to C12 hydrocarboxy group, a C1 to C12 hydrocarbylaminyl group, a C1 to C12 hydrocarbysilyl group, a C1 to C12 hydrocarbylaminylsilyl group, OBR12 or OSO2R1, where R1 is a C1 to C12 hydrocarbyl group.In another aspect, each X can independently be H, BH4, a halide, a C1 to C10 hydrocarbyl group, a C1 to C10 hydrocarboxy group, a C1 to C10 hydrocarbylaminyl group, a C1 to C10 hydrocarbysilyl group, a C1 to C10 hydrocarbylaminylsilyl group, OBR12, or OSO2R1, where R1 is a C1 to C10 hydrocarbyl group. In yet another aspect, each X can independently be H, BH4, a halide, a C1 to C8 hydrocarbyl group, a C1 to C8 hydrocarboxy group, a C1 to C8 hydrocarbylaminyl group, a C1 to C8 hydrocarbysilyl group, a C1 to C8 hydrocarbylaminylsilyl group, OBR12, or OSO2R1, where R1 is a C1 to C8 hydrocarbyl group. In yet another aspect, each X can independently be a halide or a C18 hydrocarbyl group. For example, each X can be Cl.

[074] In one aspect, each X can independently be H, BH4, a halide, or a C1 to C36 hydrocarbyl group, hydrocarboxylic group, hydrocarbylamynyl group, hydrocarbylsilyl group, or hydrocarbylamynylsilyl group, while in another aspect, each X can independently be H, BH4, or a C1 to C18 hydrocarboxylic group, hydrocarbylamynyl group, hydrocarbylsilyl group, or hydrocarbylamynylsilyl group. In yet another aspect, each X can independently be a halide; alternatively, a C1 to C18 hydrocarbyl group; alternatively, a C1 to C18 hydrocarboxylic group; alternatively, a C1 to C18 hydrocarbylamynyl group; alternatively, a C1 to C18 hydrocarbylsilyl group; or alternatively, a C1 to C18 hydrocarbylamynylsilyl group. In yet another aspect, Petition 870240096702, dated 12 / 11 / 2024, p. 35 / 192 25 / 68 each X can be H; alternatively, F; alternatively, Cl; alternatively, Br; alternatively, I; alternatively, BH4; alternatively, a C18 hydrocarbyl group; alternatively, a C18 hydrocarboxy group; alternatively, a C18 hydrocarbylaminyl group; alternatively, a C18 hydrocarbysilyl group; or alternatively, a C18 hydrocarbylaminylsilyl group.

[075] Each X may independently be, in some respects, H, a halide, methyl, phenyl, benzyl, an alkoxy, an aryloxy, acetylacetonate, formate, acetate, stearate, oleate, benzoate, an alkylaminyl, a dialkylaminyl, a trihydrocarbylsilyl or a hydrocarbylaminylsilyl; alternatively, H, a halide, methyl, phenyl or benzyl; alternatively, an alkoxy, an aryloxy or acetylacetonate; alternatively, an alkylaminyl or a dialkylaminyl; alternatively, a trihydrocarbylsilyl or hydrocarbylaminylsilyl; alternatively, H or a halide; alternatively, methyl, phenyl, benzyl, an alkoxy, an aryloxy, acetylacetonate, an alkylaminyl or a dialkylaminyl; alternatively, H; Alternatively, a halide; alternatively, methyl; alternatively, phenyl; alternatively, benzyl; alternatively, an alkoxy; alternatively, an aryloxy; alternatively, acetylacetonate; alternatively, an alkylamynyl; alternatively, a dialkylamynyl;Alternatively, a trihydrocarbylsilyl; or alternatively, a hydrocarbylaminylsilyl. In these and other respects, alkoxy, aryloxy, alkylaminyl, dialkylaminyl, trihydrocarbylsilyl and hydrocarbylaminylsilyl may be a C1 to C36, a C1 to C18, a C1 to C12 or a C1 to C8 alkoxy, aryloxy, alkylaminyl, dialkylaminyl, trihydrocarbylsilyl and hydrocarbylaminylsilyl.

[076] Furthermore, each X may independently be, in certain respects, a halide or a C1 to C18 hydrocarbyl group; alternatively, a halide or a C1 to C8 hydrocarbyl group; alternatively, F, Cl, Br, I, methyl, benzyl or phenyl; alternatively, Cl, methyl, benzyl or phenyl; alternatively, a C1 to C18 alkoxy, aryloxy, alkylamynyl, dialkylamynyl, trihydrocarbylsilyl or hydrocarbylaminylsilyl group; alternatively, a C1 to C8 alkoxy, aryloxy, alkylamynyl, dialkylamynyl, trihydrocarbylsilyl or hydrocarbylaminylsilyl group; or alternatively, methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, ethenyl, propenyl, butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, phenyl, tolyl, benzyl, naphthyl, trimethylsilyl, triisopropylsilyl, triphenylsilyl or Petition 870240096702, dated 12 / 11 / 2024, p. 36 / 192 26 / 68 allyl dimethylsilyl.

[077] In formula (II), Cp can be a cyclopentadienyl group, optionally with an alkenyl substituent. In some respects, Cp may contain no additional substituents other than the alkenyl substituent. In other respects, Cp may be additionally substituted by one substituent, two substituents, and so forth. If present, each substituent on Cp may independently be H, a halide, a C1 to C36 hydrocarbyl group, a C1 to C36 halogenated hydrocarbyl group, a C1 to C36 hydrocarboxy group, or a C1 to C36 hydrocarbylsilyl group. Importantly, each substituent on Cp may be the same substituent group or a different one. Furthermore, each substituent may be in any position in the cyclopentadienyl ring structure that conforms to the rules of chemical valence.In general, any substituent on Cp can independently be H or any halide, C1 to C36 hydrocarbyl group, C1 to C36 halogenated hydrocarbyl group, C1 to C36 hydrocarboxylic group, or C1 to C36 hydrocarbylsilyl group described herein. In addition to representative substituents disclosed herein, suitable additional hydrocarbyl groups, halogenated hydrocarbyl groups, hydrocarboxylic groups, and hydrocarbylsilyl groups are disclosed, for example, in U.S. Patent No. 9,758,600, which is incorporated herein by reference in its entirety.

[078] In one aspect, for example, each substituent at Cp can independently be a C12 to C12 hydrocarbyl group or a C12 to C12 hydrocarbylsilyl group. In another aspect, each substituent at Cp can independently be a C8 to C8 alkyl group or a C3 to C8 alkenyl group. In yet another aspect, each substituent in Cp can independently be H, Cl, CF3, a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an ethenyl group, a propenyl group, a butenyl group, a pentenyl group, a hexenyl group, a heptenyl group, an octenyl group, a nonenyl group, a decenyl group, a phenyl group, a tolyl group, a benzyl group, a naphthyl group, a trimethylsilyl group, a tri-isopropylsilyl group, a triphenylsilyl group, or an allyldimethylsilyl group. Petition 870240096702, dated 12 / 11 / 2024, p. 37 / 192 27 / 68

[079] Similarly, RXe RY in formula (II) can independently be H or any halide, C1 to C36 hydrocarbyl group, C1 to C36 halogenated hydrocarbyl group, C1 to C36 hydrocarboxy group or C1 to C36 hydrocarbylsilyl group disclosed herein. In one aspect, for example, RXe RY can independently be H or a C1 to C12 hydrocarbyl group. In another aspect, RXe RY can independently be a C1 to C10 hydrocarbyl group or, alternatively, a C1 to C6 alkyl group.In yet another aspect, RX and RY can independently be H, Cl, CF3, a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an ethenyl group, a propenyl group, a butenyl group, a pentenyl group, a hexenyl group, a heptenyl group, an octenyl group, a nonenyl group, a decenyl group, a phenyl group, a tolyl group, a benzyl group, a naphthyl group, a trimethylsilyl group, a tri-isopropylsilyl group, a triphenylsilyl group or an allyldimethylsilyl group, and the like.In yet another aspect, RX and RY can independently be a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an ethenyl group, a propenyl group, a butenyl group, a pentenyl group, a hexenyl group, a heptenyl group, an octenyl group, a nonenyl group, a decenyl group, a phenyl group, a tolyl group, or a benzyl group.

[080] The bridging group E in formula (II) may be a bridging group having the formula >EARARB, where EA may be C, Si or Ge, and RA and RB may independently be H or a C1 to C18 hydrocarbyl group. In some aspects of this invention, RA and RB may independently be a C1 to C12 hydrocarbyl group; alternatively, RA and RB may independently be a C1 to C8 hydrocarbyl group; alternatively, RA and RB may independently be a phenyl group, a C1 to C8 alkyl group or a C3 to C8 alkenyl group; Alternatively, RA and RB can independently be a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an ethenyl group, a propenyl group, a butenyl group, a pentenyl group, a Petition 870240096702, dated 12 / 11 / 2024, p. 38 / 192 28 / 68 a hexenyl group, a heptenyl group, an octenyl group, a nonenyl group, a decenyl group, a phenyl group, a cyclohexylphenyl group, a naphthyl group, a tolyl group, or a benzyl group; or alternatively, RA and RB may independently be a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a propenyl group, a butenyl group, a pentenyl group, a hexenyl group, a phenyl group, or a benzyl group. In these and other respects, RA and RB may be the same or different.

[081] Illustrative and non-limiting examples of bridged metallocene compounds having formula (II) and / or suitable for use as catalyst component II may include the following compounds (Me = methyl, Ph = phenyl; t-Bu = tert-butyl): and similar items, as well as combinations thereof.

[082] Catalyst component II is not limited to bridged metallocene compounds as described above. Other suitable bridged metallocene compounds are disclosed in US Patent Documents Nos. 7,026,494, 7,041,617, 7,226,886, 7,312,283, 7,517,939 and 7,619,047, which are incorporated into this document in their entirety by reference. Petition 870240096702, dated 12 / 11 / 2024, p. 39 / 192 29 / 68

[083] With reference now to catalyst component I, which may comprise, in particular aspects of this invention, a metallocene compound bridged to a single atom or bridged to two atoms (two-atom chain) with two indenyl groups. In some aspects, the metallocene compound contains two unsubstituted indenyl groups. The bridge may be a single carbon atom; alternatively, a single silicon atom; alternatively, a two-carbon atom bridge; or alternatively, a two-silicon atom bridge.Independently, any bridging atom (or atoms) may have two substituents independently selected from H or a C18 to C18 hydrocarbyl group, or from H or a C18 to C8 hydrocarbyl group; alternatively, two substituents independently selected from H or a C16 to C6 alkyl group; or alternatively, two substituents independently selected from a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an ethenyl group, a propenyl group, a butenyl group, a pentenyl group, a hexenyl group, a heptenyl group, an octenyl group, a nonenyl group, a decenyl group, a phenyl group, a cyclohexylphenyl group, a naphthyl group, a tolyl group, or a benzyl group. The two substituents may be the same or different.

[084] If the metallocene compound is a two-carbon-atom-bridged metallocene compound, the bridging group may have the formula —CRCRD—CRERF—, wherein RC, RD, RE, and RF may independently be H or any C1 to C18 hydrocarbyl group disclosed herein (and similarly for a two-silicon-atom bridge). For example, RC, RD, RE, and RF may independently be H or a C1 to C6 alkyl group, or alternatively, H or a methyl group.

[085] In other respects, at least one indenyl group is substituted (thus, one or both indenyl groups may be substituted). As stated above, the bridge may be a single carbon atom, a single silicon atom, a bridge of two carbon atoms, or a bridge of two silicon atoms, and additionally, each bridging atom (or atoms) may have two substituents independently selected from H or a C1 to C18 group. Petition 870240096702, dated 12 / 11 / 2024, page 40 / 192 30 / 68 hydrocarbyl (e.g., a C1 to C2 alkyl group). Any substituent on any indenyl group may also be independently selected from H or a C1 to Cw hydrocarbyl group (e.g., a C1 to C2 alkyl group). Although not limited to this, catalyst component I typically contains zirconium.

[086] Illustrative and non-limiting examples of metallocene compounds suitable for use as catalyst component I may include the following compounds: and similar, as well as a combination thereof.

[087] Catalyst component I is not limited to bridged metallocene compounds as described above. Other suitable metallocene compounds are disclosed in U.S. Patent Nos. 8,288,487 and 8,426,538, which are incorporated herein by reference in their entirety.

[088] According to one aspect of this invention, the weight ratio of catalyst component I to catalyst component II in the catalyst composition may be in a range of about 25:1 to about 1:25, about 10:1 to about 1:10, about 8:1 to about 1:8, about 5:1 to about 1:5, about 3:1 to about 1:3; about 2:1 to about 1:2, about 1.5:1 to about 1:1.5, about 1.25:1 to about 1:1.25 or about 1.1:1 to about 1:1.1. In another aspect, catalyst component II is the smaller component of the catalyst composition, and in such aspects, the weight ratio of catalyst component I to catalyst component II in the catalyst composition may be in a range of about 1:1 to about 10:1, about 1.2:1 to about 5:1, about 1.5:1 to about 4:1, or about 1.5:1 to about 2.5:1.

[089] Additionally, the dual catalyst system contains an activator. Petition 870240096702, dated 12 / 11 / 2024, page 41 / 192 31 / 68 For example, the catalyst system may contain an activating support, an aluminoxane compound, an organoboron or organoborate compound, an ionizing ionic compound, and the like, or any combination thereof. The catalyst system may contain one or more activators.

[090] The activator may comprise a supporting activator, an aluminoxane compound, an organoboron or organoborate compound, an ionizing ionic compound, and the like, or combinations thereof. Examples of such activators are disclosed, for example, in U.S. Patents Nos. 3,242,099, 4,794,096, 4,808,561, 5,576,259, 5,807,938, 5,919,983 and 8,114,946, the disclosures of which are incorporated herein by reference in their entirety. In another aspect, the catalyst system may comprise an aluminoxane compound. In yet another aspect, the catalyst system may comprise an organoboron or organoborate compound. In yet another aspect, the catalyst system may comprise an ionizing ionic compound.

[091] In other respects, the catalyst system may comprise an activator support, for example, an activator support comprising a solid oxide treated with an electron-withdrawing anion. Examples of such materials disclosed, for example, in U.S. Patent Nos. 7,294,599, 7,601,665, 7,884,163, 8,309,485, 8,623,973 and 9,023,959, which are incorporated herein by reference in their entirety.For example, the activating support may comprise fluorinated alumina, chlorinated alumina, brominated alumina, sulfated alumina, fluorinated silica and alumina, chlorinated silica and alumina, brominated silica and alumina, sulfated silica and alumina, fluorinated silica and zirconia, chlorinated silica and zirconia, brominated silica and zirconia, sulfated silica and zirconia, fluorinated silica and titania, alumina coated with fluorinated and chlorinated silica, alumina coated with fluorinated silica, alumina coated with sulfated silica or alumina coated with phosphated silica, and the like, as well as any combination thereof. In some respects, the activating support may comprise a fluorinated solid oxide and / or a sulfated solid oxide.

[092] Various processes can be used to form activator supports useful in the present invention. Methods for bringing the solid oxide into contact with the electron-withdrawing component, suitable electron-withdrawing components Petition 870240096702, dated 12 / 11 / 2024, p. 42 / 192 32 / 68 and quantities of addition, impregnation with metals or metal ions (for example, zinc, nickel, vanadium, titanium, silver, copper, gallium, tin, tungsten, molybdenum, zirconium and the like, or combinations thereof), and various calcination procedures and conditions are disclosed, for example, in US Patent documents Nos. 6,107,230, 6,165,929, 6,294,494, 6,300,271, 6,316,553, 6,355,594, 6,376,415, 6,388,017, 6,391,816, 6,395,666, 6,524,987, 6,548,441, 6,548,442 6,576,583, 6,613,712, 6,632,894, 6,667,274, 6,750,302, 7,294,599, 7,601,665 7,884,163 and 8,309,485, which are incorporated into this document by reference in their entirety. Other suitable processes and procedures for preparing activating supports (e.g., fluorinated solid oxides, sulfated solid oxides, etc.) are well known to those skilled in the art.

[093] The present invention may employ catalyst compositions containing catalyst component I, catalyst component II, an activator (one or more of one) and, optionally, a cocatalyst. When present, the cocatalyst may include, but without limitation, metal alkyl or organometal cocatalysts, wherein the metal includes boron, aluminum, zinc and the like. Optionally, the catalyst systems provided in this document may comprise a cocatalyst or a combination of cocatalysts. For example, alkylboron, alkylaluminum and alkylzinc compounds may be used as cocatalysts in such catalyst systems. Representative boron compounds may include, but without limitation, tri-n-butylborane, tripropylborane, triethylborane and the like, and this includes combinations of two or more of these materials.Organoaluminum compounds comprise trimethylaluminum, triethylaluminum, tri-n-propylaluminum, tri-n-butylaluminum, triisobutylaluminum, tri-n-hexylaluminum hydride, tri-n-octylaluminum, diisobutylaluminum, diethylaluminum ethoxide, diethylaluminum chloride, and the like or combinations thereof. Exemplary zinc compounds (e.g., organozinc compounds) that may be used as cocatalysts may include, but are not limited to, dimethylzinc, diethylzinc, dipropylzinc, dibutylzinc, dinepentylzinc, di(trimethylsilyl)zinc, di(triethylsilyl)zinc, di(triisopropylsilyl)zinc, di(triphenylsilyl)zinc, di(allyldimethylsilyl)zinc, di(trimethylsilylmethyl)zinc and the like, or combinations thereof. Consequently, in one aspect of this invention, a. Petition 870240096702, dated 12 / 11 / 2024, page 43 / 192 33 / 68 double catalyst composition may comprise catalyst component I, catalyst component II, an activating support and an organoaluminum compound (and / or an organozinc compound).

[094] In another aspect of the present invention, a catalyst composition is provided comprising catalyst component I, catalyst component II, an activating support and an organoaluminum compound, wherein this catalyst composition is substantially free of aluminoxane, organoboron or organoborate compounds, ionizing ionic compounds and / or other similar materials; alternatively, substantially free of aluminoxanes; alternatively, substantially free of organoboron or organoborate compounds; or alternatively, substantially free of ionizing ionic compounds. In these aspects, the catalyst composition has catalyst activity, discussed herein, in the absence of these additional materials.For example, a catalyst composition of the present invention may consist essentially of catalyst component I, catalyst component II, an activating support, and an organoaluminum compound, wherein no other material is present in the catalyst composition that would increase / decrease the activity of the catalyst composition by more than about 10% of the catalyst activity of the catalyst composition in the absence of said materials.

[095] Catalyst compositions of the present invention generally have a catalyst activity greater than about 250 grams of ethylene polymer (homopolymer and / or copolymer, as the context requires) per gram of activator support per hour (abbreviated as g / g / h). In another aspect, the catalyst activity may be greater than about 350, greater than about 450, or greater than about 550 g / g / h. Still in another aspect, the catalyst activity may be greater than about 700 g / g / h, greater than about 1000 g / g / h, or greater than about 2000 g / g / h, and frequently as high as 3500-6000 g / g / h. Illustrative and non-limiting ranges for catalyst activity include from about 500 to about 5000, from about 750 to about 4000, or from about 1000 to about 3500 g / g / h, and the like. These activities are measured under paste polymerization conditions with a tri-isobutylaluminum cocatalyst, using Petition 870240096702, dated 12 / 11 / 2024, p. 44 / 192 34 / 68 isobutane as diluent, at a polymerization temperature of about 95 °C and a reactor pressure of about 4 MPa (590 psig). In addition, in some aspects, the activator support may comprise sulfated alumina, fluorinated silica alumina, or fluorinated silica-coated alumina, although it is not limited to these.

[096] This invention further encompasses methods for producing such catalyst compositions, such as, for example, contacting the respective catalyst components in any order or sequence. In one aspect, for example, the catalyst composition can be produced by a process comprising contacting, in any order, catalyst component I, catalyst component II and the activator, while in another aspect, the catalyst composition can be produced by a process comprising contacting, in any order, catalyst component I, catalyst component II, the activator and the cocatalyst.

[097] Olefin polymers (e.g., ethylene polymers) can be produced from the disclosed catalyst systems using any suitable olefin polymerization process using various types of polymerization reactors, polymerization reactor systems, and polymerization reaction conditions. One such olefin polymerization process for polymerizing olefins in the presence of a catalyst composition of the present invention may comprise contacting the catalyst composition with an olefin monomer and, optionally, an olefin comonomer (one or more) in a polymerization reactor system under polymerization conditions to produce an olefin polymer, wherein the catalyst composition may comprise, as disclosed herein, catalyst component I, catalyst component II, an activator, and an optional cocatalyst.This invention also encompasses any olefin polymers (e.g., ethylene polymers) produced through any of the polymerization processes disclosed herein.

[098] As used in this document, “polymerization reactor” includes any polymerization reactor capable of polymerizing olefin monomers and comonomers (one or more comonomers) to produce homopolymers. Petition 870240096702, dated 12 / 11 / 2024, page 45 / 192 35 / 68 copolymers, terpolymers and the like. The various types of reactors include those that may be referred to as a batch reactor, fluidized paste reactor, gas phase reactor, solution reactor, high pressure reactor, tubular reactor, autoclave reactor, and the like, or combinations thereof. The polymerization conditions for the various types of reactors are well known to those skilled in the art. Gas phase reactors may comprise fluidized bed reactors or horizontal stepped reactors. Fluidized paste reactors comprise vertical and / or horizontal circuits. High pressure reactors comprise autoclave and / or tubular reactors. Reactor types may include batch or continuous processes. Continuous processes could use intermittent or continuous product discharge. Processes may also include partial or complete direct recycling of unreacted monomer, unreacted comonomer, and / or diluent.

[099] A polymerization reactor system may comprise a single reactor or multiple reactors (2 reactors, more than 2 reactors, etc.) of the same or different types. For example, the polymerization reactor system may comprise a slurry reactor, a gas-phase reactor, a solution reactor, or a combination of two or more of these reactors. Polymer production in multiple reactors may include several stages in at least two separate polymerization reactors interconnected by a transfer device that makes it possible to transfer the resulting polymers from the first polymerization reactor to the second reactor. The desired polymerization conditions in one of the reactors may be different from the operating conditions of other reactors. Alternatively, polymerization in multiple reactors may include the manual transfer of the polymer from one reactor to subsequent continuous polymerization reactors.Multiple reactor systems may include any combination including, but not limited to, multiple cycle reactors, multiple gas phase reactors, a combination of gas phase and cycle reactors, multiple high-pressure reactors, or a combination of high-pressure reactors with gas phase and / or cycle reactors. Multiple reactors may be operated in series, in parallel, or in both. Consequently, the present invention encompasses polymerization reactor systems comprising a single reactor, which... Petition 870240096702, dated 12 / 11 / 2024, page 46 / 192 36 / 68 comprise two reactors and comprise more than two reactors. The polymerization reactor system may comprise a fluid paste reactor, a gas phase reactor, a solution reactor, in certain aspects of this invention, as well as combinations of multiple reactors thereof.

[100] According to one aspect, the polymerization reactor system may comprise at least one cycle fluid paste reactor comprising vertical or horizontal cycles. The monomer, diluent, catalyst, and comonomer may be continuously fed into a cycle reactor where polymerization occurs. Generally, continuous processes may comprise the continuous introduction of the monomer / comonomer, a catalyst, and a diluent into a polymerization reactor and the continuous removal from this reactor of a suspension comprising polymer and diluent particles. The reactor effluent may be instantaneously evaporated to remove the continuous polymer from the liquids comprising the diluent, monomer, and / or comonomer.Several technologies can be used for this separation step, including, but not limited to, flash evaporation, which may include any combination of heat addition and pressure reduction; cyclonic separation in a cyclone or hydrocyclone; or centrifugal separation.

[101] Typical flow paste polymerization processes (also known as particle-form processes) are disclosed in U.S. Patents Nos. 3,248,179, 4,501,885, 5,565,175, 5,575,979, 6,239,235, 6,262,191, 6,833,415 and 8,822,608, for example; each of which is incorporated herein by reference in its entirety.

[102] Suitable diluents used in fluidized polymerization include, but are not limited to, the monomer being polymerized and hydrocarbons that are liquid under reaction conditions. Examples of suitable diluents include, but are not limited to, hydrocarbons such as propane, cyclohexane, isobutane, n-butane, n-pentane, isopentane, neopentane, and n-hexane. Some circuit polymerization reactions can occur under bulk conditions where no diluent is used.

[103] According to yet another embodiment, the polymerization reactor may comprise at least one gas-phase reactor. Such systems may Petition 870240096702, dated 12 / 11 / 2024, page 47 / 192 37 / 68 employ a continuous recycling stream containing one or more monomers continuously cycled through a fluidized bed in the presence of catalyst under polymerization conditions. A recycling stream can be withdrawn from the fluidized bed and recycled back to the reactor. Simultaneously, the polymer product can be withdrawn from the reactor and new or fresh monomer can be added to replace the polymerized monomer. Such gas-phase reactors may comprise a process for a multi-stage gas-phase polymerization of olefins, in which olefins are polymerized in the gas phase in at least two independent gas-phase polymerization zones while feeding a catalyst-containing polymer formed in a first polymerization zone to a second polymerization zone. One type of gas-phase reactor is disclosed in US Patents Nos. 5,352,749, 4,588,790, 5,436,304, 7,531,606 and 7,598.327, each of which is incorporated herein by reference in its entirety.

[104] According to another aspect of the invention, a high-pressure polymerization reactor may comprise a tubular reactor or an autoclave reactor. Tubular reactors may have several zones where fresh monomer, initiators or catalysts are added. The monomer may be entrained in an inert gas stream and introduced into one zone of the reactor. The initiators, catalysts and / or catalyst components may be entrained in a gas stream and introduced into another zone of the reactor. The gas streams may be intermixed for polymerization. Heat and pressure may be appropriately employed to obtain ideal polymerization reaction conditions.

[105] According to another aspect of the invention, the polymerization reactor may comprise a solution polymerization reactor in which the monomer / comonomer is contacted with the catalyst composition by means of agitation or other suitable means. A carrier comprising an inert organic diluent or excess monomer may be employed. If desired, the monomer / comonomer may be placed in the vapor phase in contact with the product of the catalytic reaction, in the presence or absence of liquid material. The polymerization zone may be maintained at temperatures and pressures that will result in the formation of a polymer solution in a reaction medium. Agitation may be Petition 870240096702, dated 12 / 11 / 2024, page 48 / 192 38 / 68 is employed to obtain better temperature control and to maintain uniform polymerization mixtures throughout the polymerization zone. Appropriate means are used to dissipate the exothermic heat of polymerization.

[106] Polymerization reactors suitable for the present invention may further comprise any combination of at least one raw material feeding system, at least one feeding system for the catalyst or catalyst components, and / or at least one polymer recovery system. Reactor systems suitable for the present invention may further comprise systems for raw material purification, catalyst storage and preparation, extrusion, reactor cooling, polymer recovery, fractionation, recycling, storage, discharge, laboratory analysis, and process control. Depending on the desired properties of the olefin polymer, hydrogen may be added to the polymerization reactor as required (e.g., continuously, pulsed, etc.).

[107] The polymerization conditions that are controlled for efficiency and to provide the desired polymer properties may include temperature, pressure, and the concentrations of various reagents. The polymerization temperature can affect catalyst productivity, polymer molecular weight, and molecular weight distribution. Several polymerization conditions can be kept substantially constant, for example, for the production of a particular grade of olefin polymer (or ethylene polymer). A suitable polymerization temperature can be any temperature below the depolymerization temperature, according to the Gibbs free energy equation. Typically, this includes from about 60 °C to about 280 °C, for example, or from about 60 °C to about 120 °C, depending on the type of polymerization reactor (or reactors).In some reactor systems, the polymerization temperature can generally be within a range of about 70 °C to about 100 °C, or about 75 °C to about 95 °C.

[108] Suitable pressures will also vary depending on the type of reactor and polymerization. The pressure for liquid-phase polymerization in a cycle reactor is typically less than 1000 psig (6.9 MPa). The pressure for polymerization of Petition 870240096702, dated 12 / 11 / 2024, page 49 / 192 39 / 68 gas phase is generally approximately 1.4 to 3.4 MPa (200 to 500 psig). High-pressure polymerization in tubular or autoclave reactors is generally performed at about 138 to 517 MPa (20,000 to 75,000 psig). Polymerization reactors can also be operated in a supercritical region, generally occurring at higher temperatures and pressures. Operation above the critical point of a pressure / temperature diagram (supercritical phase) can offer advantages.

[109] Olefin monomers that can be employed with catalyst compositions and polymerization processes of this invention may include olefin compounds having from 2 to 30 carbon atoms per molecule and having at least one olefinic double bond, such as ethylene or propylene. In one aspect, the olefin monomer may comprise a C2-C20 olefin; alternatively, a C2-C20 alpha-olefin; alternatively, a C2-C10 olefin; alternatively, a C2C10 alpha-olefin; alternatively, the olefin monomer may comprise ethylene; or alternatively, the olefin monomer may comprise propylene (for example, to produce a polypropylene homopolymer or a propylene-based copolymer).

[110] When a copolymer (or, alternatively, a terpolymer) is desired, the olefin monomer and the olefin comonomer may independently comprise, for example, a C2-C20 alpha-olefin. In some aspects, the olefin monomer may comprise ethylene or propylene, which is copolymerized with at least one comonomer (for example, a C2-C20 alpha-olefin, a C3-C20 alpha-olefin group, etc.). According to one aspect of this invention, the hydrogen-to-olefin monomer ratio in the polymerization process is controlled.In this respect, the comonomer may comprise a C3-C10 alpha-olefin group; alternatively, the comonomer may comprise 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, styrene, or any combination thereof; alternatively, the comonomer may comprise 1-butene, 1-hexene, 1-octene, or any combination thereof; alternatively, the comonomer may comprise 1-butene; alternatively, the comonomer may comprise 1-hexene; or alternatively, the comonomer may comprise 1-octene. Petition 870240096702, dated 12 / 11 / 2024, page 50 / 192 40 / 68 EXAMPLES

[111] This invention is further illustrated by the following examples, which should not be interpreted in such a way as to impose limitations on the scope of the invention in any way. Various other aspects, embodiments, modifications, and equivalents thereof, which, after reading the description in this document, may be suggested by themselves to a person skilled in the art without departing from the principles of the present invention or the scope of the appended claims.

[112] Melting index (MI, g / 10 min) was determined according to ASTM D1238 at 190 °C with a weight of 2160 grams and the high load melting index (HLMI, g / 10 min) was determined according to ASTM D1238 at 190 °C with a weight of 21600 grams. Density was determined in grams per cubic centimeter (g / cm3) in a compression-molded sample, cooled at 15 °C per hour and conditioned for 40 hours at room temperature according to ASTM D1505 and ASTM D4703.

[113] Molecular weights and molecular weight distributions were obtained using a PL-GPC 220 system (Polymer Labs, an Agilent company) equipped with an IR4 detector (Polymer Char, Spain) and three Styragel HMW-6E GPC columns (Waters, MA) run at 145 °C. The flow rate of the 1,2,4-trichlorobenzene (TCB) mobile phase containing 0.5 g / l of 2,6-di-t-butyl-4-methylphenol (BHT) was set at 1 ml / min, and the polymer solution concentrations were in the range of 1.0–1.5 mg / ml, depending on the molecular weight. Sample preparation was conducted at 150 °C for approximately 4 h with occasional gentle stirring before the solutions were transferred to sample vials for injection. An injection volume of approximately 400 μL was used. The integral calibration method was used to deduce molecular weights and molecular weight distributions using a Chevron Phillips Chemical Company HDPE polyethylene resin, MARLEX®BHB5003, as the standard.The complete standard table was predetermined in a separate experiment with SEC-MALS. Mn is the number-average molecular weight, Mw is the weight-average molecular weight, Mz is the z-average molecular weight, and Mp is the peak molecular weight (location, in molecular weight, of the highest point on the molecular weight distribution curve).

[114] Rheological characterizations of castings were carried out as the Petition 870240096702, dated 12 / 11 / 2024, page 51 / 192 41 / 68 follow. Oscillatory shear measurements (10%) of small stress were performed on an Anton Paar MCR rheometer using parallel plate geometry. All rheological tests were performed at 190 °C. The complex viscosity data | η*\ versus frequency (0) were then fitted to the curve using the three modified parameters, the Carreau-Yasuda (CY) empirical model to obtain the zero shear viscosity - ηο, the characteristic viscous relaxation time - τη and the amplitude parameter - a (CY-a parameter). The simplified Carreau-Yasuda (CY) empirical model is as follows. I η*(0)|ηο [1 + (τηω)a](1-n>'aem where: \ η*(0) \ = magnitude of complex shear viscosity; ηο = zero shear viscosity; τη = viscous relaxation time (Tau(n)); a = “amplitude” parameter (CY-a parameter); n = corrects the final slope of the power law, corrected by 2 / 11; e = angular frequency of oscillating shear strain.

[115] Details of the meaning and interpretation of the CY model and derived parameters can be found in: CA Hieber and HH Chiang, Rheol. Acta, 28, 321 (1989); CA Hieber and HH Chiang, Polym. Eng. Sci., 32, 931 (1992); and RB Bird, RC Armstrong, and O. Hasseger, Dynamics of Polymeric Liquids, Volume 1, Fluid Mechanics, 2nd Edition, John Wiley & Sons (1987); each of which is incorporated herein by reference in its entirety. An alignment adjustment was used to extend the low-frequency range of rheological characterization to 10-4s-1, as described in US Patent No. 9,169,337, incorporated herein by reference in its entirety.

[116] Polymer viscosities at 0.1 s-1, at 100 s-1, and in HLMI were determined from the Carreau-Yasuda model at 190 °C with alignment adjustment, described above in this document.

[117] Long chain branches (LCBs) per 1000000 total carbon atoms of the overall polymer were calculated using the Janzen method. Petition 870240096702, dated 12 / 11 / 2024, p. 52 / 192 42 / 68 and Colby (J. Mol. Struct., 485 / 486, 569-584 (1999), incorporated herein by reference in its entirety), from zero shear viscosity values, in (determined from the Carreau-Yasuda model with alignment adjustment, described above in this document) and measured Mw values ​​obtained using a Dawn EOS multi-angle light scattering detector (Wyatt).

[118] LCB content and LCB distribution were determined using the method established by Yu, et al (Yu, DesLauriers, Rohlfing, Polymer, 2015, 46, 5165-5192, incorporated herein by reference in its entirety). Briefly, in the SEC-MALS system, a DAWN EOS photometer (Wyatt Technology, Santa Barbara, CA) was attached to a Waters 150-CV plus GPC system (Milford, MA) or a PL-210 GPC system (Polymer Labs, an Agilent company) via a controlled hot transfer line at 145 °C. Degassed 1,2,4-trichlorobenzene (TCB) mobile phase containing 0.5 wt% BHT (butylated hydroxytoluene) was pumped through an in-line filter before passing through a SEC column bank. Polymer solutions injected into the system were placed downstream of the columns by the mobile phase for fractionation.The fractionated polymers first eluted through the MALS photometer where the light scattering signals were recorded before passing through the differential refractive index (DRI) detector or an IR4 detector (Polymer Characterization SA, Spain) where their concentrations were quantified.

[119] The DAWN EOS system was calibrated with pure toluene at room temperature to convert the measured voltage into scattered light intensity. During calibration, toluene was filtered with a 0.02 µm filter (Whatman) and passed directly through the flow cell of the EOS system. At room temperature, the Rayleigh ratio is given by 1.406 x 10⁻⁵ cm⁻¹. A narrow polystyrene (PS) standard (American Polymer Standards) with a MW of 30000 g / mol at a concentration of approximately 5-10 mg / ml in TCB was used to normalize the system at 145 °C. Under the given chromatographic conditions, the radius of gyration (Rg) of polystyrene (PS) was estimated at 5.6 nm. The differential refractive index (DRI) detector was calibrated with a known quantity of PE standard. By averaging the total chromatographic areas of recorded chromatograms to Petition 870240096702, dated 12 / 11 / 2024, page 53 / 192 43 / 68 at least five injections, the DRI constant (aRi) was obtained using the equation below (equation 1): ( dn jTaRI = \~T IcIRI Equation 1 where I ri is the DRI detector intensity, c is the polymer concentration, and dn / dc is the increase in the refractive index of PE in TCB at the measurement temperature.

[120] At a defined flow rate of 0.7 ml / min, the mobile phase was eluted through three mixed A columns (3) 7.5 mm x 300 mm 20 µm (Polymer Labs, an Agilent company). PE solutions with nominal concentrations of 1.5 mg / ml were prepared at 150 °C for 4 h. In each chromatographic slice, both the absolute molecular weight (M) and the root mean square radius (RMS), also known as the radius of gyration, Rg, were obtained from Debye plots. The linear PE control employed was CPChem Marlex™HiD9640, a high-density PE with a wide MWD. ​​The refractive index increment dn / dc used in this study was 0.097 ml / g for PE dissolved in TCB at 135 °C.

[121] The Zimm-Stockmayer approach (Zimm, Stockmayer, J. Chem. Phys. 1949, 17, 1301, incorporated herein by reference in its entirety) was employed to determine the amount of LCB in polyethylene resins. In SEC-MALS, both M and Rg were measured simultaneously on each slice of a chromatogram. At the same molecular weight, Rg of a branched polymer is smaller than that of a linear polymer. The branching index factor (gm) is defined as the ratio of the mean square radius of gyration of the branched polymer to that of the linear polymer at the same molecular weight using equation 2, Sm =rSl'MEquation 2 where the subscripts bel represent the branched and linear polymer, respectively.

[122] The average weighted LCB per molecule (B3w) was calculated using Equation 3 which uses internal software, Petition 870240096702, dated 12 / 11 / 2024, page 54 / 192 44 / 68 gM 6B3 wi „ >1 / i r2-B3w i / 22I B3 w J ln (2 + B3 w )+(B3 w ) (2 + B3 w )^2 -(B3 w )2. ( 3) _____ _ λ, . . . ____. . . . .

[123] LCB frequency (Mi, number of LCB per 1000 total carbons) was calculated using equation 4 which uses the value of B 3w obtained from equation 3, λM{-1,000 x M0 X B3w / Mi where M0 is the molecular weight unit of polyethylene, Mi is the molecular weight of the i-th slice.

[124] Since the presence of SCB in a polymer can affect its R g-MW relationship, the effect of SCB was corrected before using equations 3 and 4 for LCB and calculating the LCB distribution for PE copolymers. To correct the effect of SCB on the branching index through MWD, two relationships are needed: one is the relationship between the branching index correction factor (Δ gm) and the SCB content (xscb), and the other is the relationship between SCB content and molecular weight, both of which were determined experimentally. Mathematically, the product of these two relationships generates the branching index correction factor (ΔρM) as a function of MW, as shown in equation 5, d (ΔSm ) = d (xscb ) χ d (ΔSm ) d (M) d (M) d (xScb ) (5) where x scb is the SCB content (i.e., number of SCB per 1000 total carbons) of the copolymer in question.

[125] To establish the relationship between Δgm and xscb, PE standards that meet the following criteria were used: the standards contain essentially no LCB and have a flat SCB distribution and known SCB contents. At least five SCB standards were used for SCB effect correction. The SCB content for these SCB standards was in the range of 0 to 34 SCB / 1000 total carbon atoms.

[126] Short chain branching content and short chain branching distribution (SCBD) through molecular weight distribution were determined by means of an IR5-detected GPC (IR5-GPC) system using the method Petition 870240096702, dated 12 / 11 / 2024, page 55 / 192 45 / 68 established by Yu (Y. Yu, Macromolecular Symposium, 2020, 390, 1900014), in which the GPC system was a GPC / SEC PL220 system (Polymer Labs, an Agilent company) equipped with three Styragel HMW-6E columns (Waters, MA) for polymer separation. A thermoelectrically cooled IR5 MCT detector (IR5) (Polymer Characterisation SA, Spain) was connected to the GPC columns via a hot transfer line. Chromatographic data were obtained from two output ports of the IR5 detector. First, the analog signal goes from the analog output port to a digitizer before connecting to Computer “A” for molecular weight determinations using Cirrus software (Polymer Labs, now an Agilent company) and the integral calibration method using a Marlex™ BHB5003 HDPE resin (Chevron Phillips Chemical) as the molecular weight standard.The digital signals, on the other hand, are transmitted via a USB cable directly to Computer “B” where they are collected by LabView data acquisition software provided by Polymer Char. Chromatographic conditions were defined as follows: column oven temperature of 145 °C; flow rate of 1 ml / min; injection volume of 0.4 ml; and polymer concentration of approximately 2 mg / ml, depending on the sample molecular weight. The temperatures for both the hot transfer line and the IR5 detector sample cell were set at 150 °C, while the temperature of the IR5 detector electronics was set at 60 °C. The short-chain branching content was determined using an internal method with the CH3 intensity ratio (Ich3) to CH2 (Ich2) coupled to a calibration curve. The calibration curve was a plot of SCB content (xscb) as a function of the Ich3 / Ich2 intensity ratio.To obtain a calibration curve, a group of polyethylene resins (not less than 5) with SCB levels ranging from zero to approximately 32 SCB / 1000 total carbons (SCB Standards) was used. All these SCB Standards have known SCB levels and predetermined flat SCBD profiles obtained separately by NMR and solvent gradient fractionation coupled to NMR (SGFRMN) methods. Using the SCB calibration curves thus established, short-chain branching distribution profiles across the molecular weight distribution were obtained for resins fractionated by the IR5-GPC system under 5-weight distribution. Petition 870240096702, dated 12 / 11 / 2024, page 56 / 192 46 / 68 exactly the same chromatographic conditions as these SCB standards. A relationship between the intensity ratio and the elution volume was converted into an SCB distribution as a function of MWD using a predetermined SCB calibration curve (i.e., Ich3 / Ich2 intensity ratio relative to SCB content) and MW calibration curve (i.e., molecular weight relative to elution time) to convert the ICH3 / ICH2 intensity ratio and elution time into SCB content and molecular weight, respectively.

[127] Extension viscosity was measured on a rotating rheometer (Physica MCR-500, Anton Paar) using the extension viscosity attachment, a Sentimanat Extension Rheometer (SER-3 model universal test platform, Xpansion Instruments). The SER attachment makes it possible to easily measure transient extension viscosity as a function of time.

[128] Test samples were prepared by compression molding at 182 °C. The pellet samples were allowed to melt at a relatively low pressure for 1 min and then subjected to a high molding pressure for a further 2 min. Then the hot pressing was switched off for slow cooling. The cooled plate was retrieved from the press the following day. Rectangular strips with dimensions of 12.77 x 18 mm were cut from the molded plate and the thickness of the sample was measured.

[129] The SER test platform has two drums that rotate in opposite directions (ML Sentmanat, “Miniature universal test platform: from extensional melt rheology to solid-state deformation behavior”, Rheol. Acta 43, 657 (2004); ML Sentmanat, BN Wang, GH McKinley, “Measuring the transient extensional rheology of polyethylene melts using the SER universal testing platform”, J. Rheol. 49, 585 (2005); both incorporated herein by reference in their entirety). The rectangular samples were tested by cutting into the two posts of the accessory, then closing the furnace to heat up to 150 °C, where they were annealed at 150 °C for 30 s to allow the temperature to reach equilibrium. The sample was then elongated at constant Hencky strain rates / ?„ between 0.03 and 25 s⁻¹ at 150 °C. The torque M resulting from the tangential elongation force of the sample between the rotating drums F was recorded by the rotating rheometer: Petition 870240096702, dated 12 / 11 / 2024, p. 57 / 192 47 / 68 M(t) = 2 RF (t) (A) where the drum radius R = 5.155 mm. The Hencky strain rate έ„ ..... . ~ . . SH at constant drum rotation speed Ω is 2Ω R έ „ =---HL(B) where the length of the elongation zone between the rotating drums L = 12.72 mm. The transient extension viscosity ηE(t) was obtained for a given Hencky strain rate as η + (t) = °2H = F(' ' έE A(t, T)έE(C) where A(t, T) is the cross-sectional area of ​​the sample that expands thermally upon casting and decreases exponentially with elongation: \2 / 3A(tT) =Ao expl-έEt)| -7=7 eu 1P(T) J (D) where Ao and ps are the initial cross-sectional area and the sample density measured at room temperature in the solid state. The casting density p(T) is given by p(T) = p0 - Δρ(T-273.15)T. Therefore, the viscosity of the transient extension ηE(t) as a function of time was calculated at each extension rate as M-M- f TH Ί2 / 3 2RέeA0exp^Et) ^ PsJ (E) where Moffset is a predefined torque that can be applied before the actual test. To compare the extension response with the linear viscoelastic limit (LVE), the LVE envelope 3 η+( t) was obtained from the relaxation spectrum of the dynamic frequency sweep data measured at 150 °C as Λ η(t) = ΣGÀI1-exp(-t / Ài)]i=1 (F) where the set of Gi and Ài defines the relaxation spectrum of the material.

[130] In general, it was observed that when long-chain branching exists in the polymer, the transient extension viscosity deviates from the LVE. Petition 870240096702, dated 12 / 11 / 2024, page 58 / 192 48 / 68 drastically increasing the slope just before breakage. This behavior is called stress hardening. On the other hand, for linear resins, the transient extension viscosity growth curves do not show any stress hardening as they continue to follow the LVE (3 η+( t)) envelope according to Trouton's rule.

[131] Metal content, such as the amount of catalyst residue in the ethylene polymer or in the manufacturing article (in ppm), can be determined by ICP analysis on a PerkinElmer Optima 8300 instrument. Polymer samples can be turned to ash in a Thermolyne furnace with sulfuric acid overnight, followed by acid digestion in a HotBlock with HCl and HNO3 (3:1 v:v).

[132] Fluorinated silica-coated alumina activating supports (FSCA) used in Examples 1-2 were prepared as follows. Boehmite was obtained by WR Grace & Company under the designation “Alumina A” and has a surface area of ​​300 m2 / g, a pore volume of 1.3 ml / g and an average particle size of 100 microns. The alumina was first calcined in dry air at about 600 °C for approximately 6 hours, cooled to room temperature and then contacted with tetraethyl orthosilicate in isopropanol to equalize 25 wt% SO2. After drying, the silica-consolidated alumina was calcined at 600 °C for 3 hours. Fluoridated silica-coated alumina (7 wt% F) was prepared by impregnating calcined silica-coated alumina with a solution of ammonium bifluoride in methanol, drying it, and then calcining it for 3 hours at 600 °C in dry air.After that, the fluorinated silica-coated alumina (FSCA) was collected and stored under dry nitrogen and used without exposure to the atmosphere.

[133] Pilot plant polymerizations were conducted in a 136 L (30 gallon) fluid paste cycle reactor at a production rate of approximately 13 kilograms (30 pounds) of polymer per hour. Polymerization runs were conducted under continuous particle formation process conditions in a cycle reactor (also termed a fluid paste process) by contacting separate metallocene solutions, an organoaluminum solution (triisobutylaluminum, TIBA), and an activator support. Petition 870240096702, dated 12 / 11 / 2024, page 59 / 192 49 / 68 (fluorinated silica-coated alumina, FSCA) in a 1 L stirred autoclave (30 min residence time) with outlet to the cycle reactor.

[134] Ethylene used was polymerization grade ethylene that was purified via an AZ 300 column (activated at 148–260 °C (300–500 °F) in nitrogen). 1-Hexene was polymerization grade 1-hexene (obtained from Chevron Phillips Chemical Company) that was purified by nitrogen purification and stored in AZ 300 activated at 148–260 °C (300–500 °F) in nitrogen. Liquid isobutane was used as the diluent.

[135] Certain polymerization conditions for Examples 1-2 are given in Table I below (mol% of ethylene and ppm by weight of isobutylaluminum (TIBA) are based on isobutane diluent). The polymerization conditions also included a reactor pressure of 4 MPa (590 psig), a polymerization temperature of 97 °C, a feed rate of 13.6 kg / h (30 lb / h) of ethylene, and 2.5-3.5 ppm total of MET 1 and MET 2 (based on isobutane diluent weight). The structures for MET 1 and MET 2, used in Examples 1-2, are shown below: Example 1 - Hexene H2 Weight Ratio C2H4 TIBA (kg / h (lb / h)) (kg / h (lb / h)) MET 1 / MET 2 % mol PPm 1 0.07 (0.16) 0.0009 (0.0021) 1.88 11.73 143 2 0.06 (0.15) 0.0009 (0.0020) 2.01 12.22 144

[136] 4.5 litre (1 gallon) blow molded containers were produced under suitable conditions on a blow molding machine. Petition 870240096702, dated 12 / 11 / 2024, page 60 / 192 50 / 68 reciprocal Uniloy. The parison was extruded using a 6.3 centimetre (2.5”) divergent die and then blown into a mold to produce 4.5 liter (1 gallon) containers weighing approximately 105 g under the following process control settings: extruder temperature 182 °C (360 °F); shot size 2.1-2.2; 160 g total parison weight; screw speed 45 rpm; back pressure of 1.3 (± 0.1) MPa (200 (± 15) psig). Drop impact testing was performed on 4.5 liter (1 gallon) containers that were blow molded from the polymers of Examples 1-3, generally in accordance with ASTM D2463. EXAMPLES 1-4

[137] Comparative Example 3 was a commercially available chromium-catalyzed ethylene / 1hexene copolymer resin from Chevron-Phillips Chemical Company LP, and Comparative Example 4 was a linear double metallocene blow molding resin (without long chain branching).

[138] For the polymers of Examples 1-3, Table II summarizes various properties of molecular weight, LCB (Janzen-Colby), rheology, melt index, density, ESCR and blow-molded bottle, while Table III summarizes a comparison of extrusion and blow molding processing and Figure 1 illustrates the molecular weight distribution curves (amount of polymer relative to the logarithm of molecular weight) for the polymers of Examples 1-3. Compared with the chromium-based Example 3, the ethylene / 1hexene copolymers of Examples 1-2 had fewer LCBs per million total carbon atoms (by Janzen-Colby), shorter relaxation times, higher CY-a parameters and significantly better ESCR properties.

[139] Using the chromium polymer from Example 3 as a reference, Table III shows that the polymers from Examples 1-2 unexpectedly had lower extrusion pressure (psi) and equivalent partial weights, cycle times, layflats, and output rates (measured at 100 rpm with a die gap of 0.05 centimeters (0.022”). Processing similarities are also shown by the relatively small rheological differences between Examples 2-3 and Comparative Example 1 in Figure 10.

[140] Figure 2 illustrates the short-chain branching distributions for the polymers in Examples 1-2. Surprisingly, these polymers have a Petition 870240096702, dated 12 / 11 / 2024, p. 61 / 192 51 / 68 SCBD is substantially flat, in which the SCB content is generally constant with increasing molecular weight.

[141] Figure 3 illustrates a plot of the molecular weight distribution and long-chain branching distribution of the polymer of Example 1, while Figure 4 illustrates a plot of the molecular weight distribution and long-chain branching distribution of the polymer of Example 2. The concentration of long-chain branching content in the molecular weight range ~300000-900000 g / mol (but not in the very high molecular weight fraction) of the inventive polymers of Examples 1-2 is illustrated in these Figures. Furthermore, Figure 5 illustrates a plot of the radius of gyration relative to molecular weight for a linear standard and the polymers of Examples 1-2 and demonstrates the deviation of the polymers of Examples 1-2 from the linear standard, due to the presence of LCB in the range of ~300000-900000 g / mol. Based on Figures 3-4, Table IV summarizes the LCB content of the respective ethylene polymers in certain molecular weight ranges.

[142] As an example, the numerical mean number of LCBs per 1000000 total carbon atoms of the respective polymers in Figures 3-4 in the molecular weight range of 300000 to 900000 g / mol and in the molecular weight range of 1000000 to 2000000 g / mol can be calculated based on Equations I and II, respectively, and are summarized in Table IV. v-,MW = 9Qüfca / mol / dw λΣ2λ = 3QQ kg / molÁ <Xd(Log M)),(d(Lo3M))í mMW = 9QQkg / mol / dw λ ,,z, ^'M / / = 3QQ kg / mol[d(Log M))i(d(Í0^M))imMV= = 2QQQkg / mol.( dw \ ^W = 1QQQkg / molÁi[d(Log M)).(-d(.Lo3M')')i mMW = 2QQQkg / mol( dw λ ,,z,ΣMW = 1QQQkg / mol(d(Log M))(d(Lo3M')')i Equation I Equation II ^^^B where λ is the number of numerically average LCBs in the respective molecular weight range and λι is LCB in slice i. As shown in Table IV, the numerically average number of LCBs per 1,000,000 total carbon atoms of the polymers in Figures 3-4 in the molecular weight range of 300,000 to 900,000 g / mol (or 400,000 to 600,000 g / mol) is significantly – and unexpectedly – ​​greater than that in the molecular weight range of 1,000,000 to 2,000,000 g / mol.

[143] Figures 6-8 illustrate extension viscosity plots, respectively, for the polymers of Example 1, Example 2, and Comparative Example 4. Extension rheology was used as a means to quantify the Petition 870240096702, dated 12 / 11 / 2024, page 62 / 192 52 / 68 quantity of LCBs, since for a Newtonian fluid, the extension viscosity ratio will be equal to 3 times the shear viscosity; the nE / 3n ratio will be equal to 1 for a Newtonian fluid (see the linear polymer of Comparative Example 4 in Figure 8, without long-chain branching). For melt polymers with stress hardening due to the presence of LCBs, the ηΞ / 3η ratio will be greater than 1. Figures 6-7 are extension viscosity plots for the polymers of Examples 1-2, determined using SER. The smaller baseline diffusion occurred due to the limited number of samples for the SER experiments. From Figures 6-7, Figure 9 was prepared to summarize the maximum nE / 3n ratio in extension rates in the range of 0.03 to 10 s-1 for the polymers of Examples 1-2. A higher ratio equates to greater tensile hardening and therefore higher LCB levels.For these inventive polymers, unexpectedly, the maximum nE / 3n ratio at an extension rate of 0.03 s-1 was in the range of 3 to 4 and was in the range of 1.5 to 2.5 at an extension rate of 0.1 s-1.

[144] Although not wishing to be bound by theory, higher LCB levels – and thus higher extension viscosity – can be obtained in the present paper by decreasing the ethylene concentration in the reactor. Additionally or alternatively, increasing comonomer levels (e.g., more 1-hexene) for a given ethylene concentration (the [1-hexene] / [ethylene] ratio) can be used to increase LCB levels in the polymer. LCB levels can also be adjusted by varying the ratio of metallocene compounds in the catalyst system.

[145] Thus, the ethylene copolymers disclosed in this document offer a beneficial combination of density, melt flow, molecular weight, relaxation time, long chain branching and extension rheology properties, resulting in processability comparable to chromium-based polymers, but with improved ESCR and hardness properties. Petition 870240096702, dated 12 / 11 / 2024, page 63 / 192 53 / 68 TABLE II Example Mn / 1000 (g / mol) Mw / 1000 (g / mol) Mz / 1000 (g / mol) Mp / 1000 (g / mol) Mw / Mn Mz / Mw LCB / million carbon atoms 1 18.3 156 783 40.2 8.52 5.02 8.2 2 18.7 149 740 44.5 8.03 4.97 10.9 3 20.7 134 635 52.5 6.47 4.74 37 TABLE II (CONTINUED) Example: 367 2 1.40E+05 1.4 0.26 32780 1165 28.1 401 3 1.43E+06 3.7 0.14 35480 1318 26.9 757 TABLE II (CONTINUED) Petition 870240096702, dated 12 / 11 / 2024, p. 64 / 192 54 / 68 Example HLMI (g / 10 min) MI (g / 10 min) Density (g / cm3) Folded Strip ESCR (h) Yield Strength (MPa (psi)) Bottle ESCR (h) Bottle Top Load (Kg (lb)) Bottle Drop Impact (meters (feet)) 1 45 0.30 0.9583 115 29.3 (4260) 499 79.3 (175) >3.6 (>12) 2 50 0.36 0.9581 79 29.7 (4310) — — — 3 32 0.33 0.9556 <50 29.7 (4310) 165 79.3 (175) 3.6 (11.9) TABLE III Example Casting Temperature (°C (°F)) Weight Definition (%) Die Range (cm (in)) Parison Weight (g) Partial Weight (g) Screw Load (s) Cycle Time (s) Head Pressure (MPa (psi)) Upper Layflat (cm (in)) Lower Layflat (cm (in)) Output (g / min) Melting Capacity (s) 1 210 (411) 1.2 0.03 (0.015) 160.8 105.5 15.3 17.0 30.6 (4450) 13.9 (5.52) 14 (5.79) 1295 14.3 2 207 (405) 0 0.03 (0.013) 161.5 109.6 15.2 16.9 31.7 (4600) 13.8 (5.46) 14.4 (5.70) 1297 14.7 3 213 (416) 1.2 0.03 (0.015) 160.2 105.1 14.6 16.3 34.7 (5040) 13.2 (5.22) 13.9 (5.55) 1302 31.5 Petition 870240096702, dated 12 / 11 / 2024, page 65 / 192 55 / 68 TABLE IV Average LCBs per 1,000,000 total carbon atoms Example 1 Example 2 (a) range 300,000-900,000 g / mol 7.83 6.66 (b) range 1,000,000-2,000,000 g / mol 1.89 2.45 Percentage (a) / (b) 414% 272% (a) range 400,000-600,000 g / mol 8.98 8.32 (b) range 1,000,000-2,000,000 g / mol 1.89 2.45 Percentage (a) / (b) 475% 340% Petition 870240096702, dated 12 / 11 / 2024, page 66 / 192 56 / 68

[146] The invention is described above with reference to various specific aspects and examples. Many variations will be apparent to those skilled in the art in light of the detailed description above. All such obvious variations are encompassed within the intended full scope of the appended claims. Other aspects of the invention may, however, include, without limitation, the following (aspects are described as “comprising”, but alternatively may “essentially consist of” or “consist of”):

[147] Aspect 1. An ethylene polymer that has: a melting point of less than or equal to approximately 1 g / 10 min; a density in a range of about 0.94 to about 0.965 g / cm3; a Mw in a range of about 100,000 to about 250,000 g / mol; a relaxation time of about 0.5 to about 3 s; and an average number of long-chain branches (LCBs) per 1,000,000 total carbon atoms of the polymer in a molecular weight range of 300,000 to 900,000 g / mol that is greater (by any amount disclosed herein, for example, at least 50%, at least 75%, at least 100%, at least 150%, at least 200%, etc.) than that in a molecular weight range of 1,000,000 to 2,000,000 g / mol.

[148] Aspect 2. An ethylene polymer having: a melting point of less than or equal to approximately 1 g / 10 min; a density in a range of about 0.94 to about 0.965 g / cm3; a Mw in a range of about 100,000 to about 250,000 g / mol; a relaxation time of about 0.5 to about 3 seconds; an average number of long-chain branches (LCBs) per 1,000,000 total carbon atoms of the polymer in a molecular weight range of 1,000,000 to 2,000,000 g / mol less than or equal to about 5; and a maximum ηE / 3η ratio at an extension rate of 0.1 s⁻¹ in a range of about 1.2 to about 10.

[149] Aspect 3. The polymer defined in aspect 1 or 2, wherein the ethylene polymer has a melt index (MI) in any range disclosed herein, for example, less than or equal to about 0.7 g / 10 min, less than or equal to about 0.5 g / 10 min, from about 0.1 to about 0.5 g / 10 min, from about 0.2 to Petition 870240096702, dated 12 / 11 / 2024, p. 67 / 192 57 / 68 about 0.4 g / 10 min, etc.

[150] Aspect 4. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has a high charge melt index (HLMI) in any range disclosed herein, for example, from about 10 to about 65 g / 10 min, from about 35 to about 55 g / 10 min, from about 20 to about 60 g / 10 min, from about 40 to about 55 g / 10 min, etc.

[151] Aspect 5. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has an HLMI / MI ratio in any range disclosed in this document, for example, from about 100 to about 200, from about 120 to about 170, from about 130 to about 160, etc.

[152] Aspect 6. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has a density in any range disclosed herein, for example, from about 0.942 to about 0.965 g / cm3, from about 0.94 to about 0.96 g / cm3, from about 0.95 to about 0.965 g / cm3, from about 0.955 to about 0.962 g / cm3, from about 0.955 to about 0.96 g / cm3, etc.

[153] Aspect 7. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has an Mw / Mn ratio in any range disclosed in this document, for example, from about 5 to about 15, from about 6 to about 12, from about 6 to about 10, from about 7 to about 10, etc.

[154] Aspect 8. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has an Mz / Mw ratio in any range disclosed in this document, for example, from about 3.5 to about 10, from about 4 to about 8, from about 4 to about 6, from about 4.5 to about 5.5, etc.

[155] Aspect 9. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has an Mz in any range disclosed in this document, for example, from about 500000 to about 2000000 g / mol, from about 600000 to about 1200000 g / mol, from about 650000 to about 1000000 g / mol, from about 700000 to about 900000 g / mol, etc.

[156] Aspect 10. The polymer defined in any of the aspects Petition 870240096702, dated 12 / 11 / 2024, p. 68 / 192 58 / 68 above, where the ethylene polymer has an Mw in any range disclosed in this document, for example, from about 125000 to about 250000 g / mol, from about 100000 to about 200000 g / mol, from about 110000 to about 190000 g / mol, from about 125000 to about 175000 g / mol, etc.

[157] Aspect 11. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has a Mn in any range disclosed in this document, for example, from about 10000 to about 30000 g / mol, from about 10000 to about 25000 g / mol, from about 15000 to about 25000 g / mol, from about 15000 to about 20000 g / mol, etc.

[158] Aspect 12. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has an average number of long-chain branches (LCBs) per 1,000,000 total carbon atoms of the polymer in a molecular weight range of 300,000 to 900,000 g / mol in any range disclosed in this document, for example, from 3 to about 15, from about 4 to about 10, from about 5 to about 9, from about 6 to about 8, etc.

[159] Aspect 13. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has an average number of long-chain branches (LCBs) per 1,000,000 total carbon atoms of the polymer in a molecular weight range of 400,000 to 600,000 g / mol in any range disclosed in this document, for example, from 4 to about 15, from about 5 to about 12, from about 7 to about 10, from about 8 to about 9, etc.

[160] Aspect 14. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has an average number of long-chain branches (LCBs) per 1000000 total carbon atoms of the polymer in a molecular weight range of 1000000 to 2000000 g / mol in any range disclosed herein, for example, less than or equal to about 5, less than or equal to about 4, less than or equal to about 3.5, less than or equal to about 3, etc.

[161] Aspect 15. The polymer defined in any of the preceding aspects, wherein the ethylene polymer contains from about 5 to about 15 LCBs, from about 6 to about 14 LCBs, from about 8 to about 12 LCBs, etc., per 1,000,000 total carbon atoms.

[162] Aspect 16. The polymer defined in any of the aspects Petition 870240096702, dated 12 / 11 / 2024, p. 69 / 192 59 / 68 above, where the ethylene polymer has a maximum ηE / 3η ratio at an extension rate of 0.1 s-1 in any range disclosed in this document, for example, from about 1.2 to about 10, from about 1.5 to about 8, from about 1.5 to about 5, from about 1.2 to about 4, from about 1.2 to about 3, from about 1.4 to about 3.5, from about 1.4 to about 3, from about 1.5 to about 2.5, etc.

[163] Aspect 17. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has a maximum ηE / 3η ratio at an extension rate of 0.03 s-1 in any range disclosed in this document, for example, from about 1.2 to about 10, from about 1.5 to about 8, from about 2 to about 7, from about 2 to about 5, from about 2.5 to about 4.5, from about 3 to about 4, etc.

[164] Aspect 18. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has a CY-a parameter in any range disclosed in this document, for example, from about 0.15 to about 0.45, from about 0.2 to about 0.4, from about 0.22 to about 0.35, from about 0.22 to about 0.32, etc.

[165] Aspect 19. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has a zero shear viscosity in any range disclosed in this document, for example, from about 1 x 103 to about 1 x 108 Pa-s, from about 1 x 104 to about 1 x 107 Pa-s, from about 1 x 104 to about 1 x 106 Pa-s, etc.

[166] Aspect 20. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has a relaxation time in any range disclosed in this document, for example, from about 0.75 to about 2.5 s, from about 1 to about 2 s, from about 1 to about 1.5 s, etc.

[167] Aspect 21. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has a viscosity at 100 s-1 (eta at 100 or η at 100) in any range disclosed in this document, for example, from about 750 to about 1750, from about 850 to about 1300, from about 1000 to about 1500, from about 1000 to about 1300 Pa-s, etc.

[168] Aspect 22. The polymer defined in any of the aspects Petition 870240096702, dated 12 / 11 / 2024, p. 70 / 192 60 / 68 above, wherein the ethylene polymer has a viscosity in HLMI (eta in HLMI or η in HLMI) in any range disclosed in this document, for example, from about 300 to about 750, from about 300 to about 500, from about 300 to about 450, from about 350 to about 450 Pa-s, etc.

[169] Aspect 23. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has a ratio of η in 0.1 / η in 100 in any range disclosed in this document, for example, from about 20 to about 45, from about 20 to about 35, from about 22 to about 32, from about 25 to about 30, etc.

[170] Aspect 24. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has a substantially constant number of short-chain branches (SCBs) per 1000 total carbon atoms, or a substantially planar SCBD (short-chain branching distribution).

[171] Aspect 25. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has a partial weight in any range disclosed in this document, for example, from about 95 to about 115, from about 100 to about 115, from about 95 to about 110, from about 100 to about 110 g, etc.

[172] Aspect 26. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has a layflat (top) in any range disclosed in the present document, for example, from about 13.2 to about 15.2, from about 12.7 to about 14.4, from about 13.2 to about 14.4 centimeters (from about 5.2 to about 6, from about 5 to about 5.7, from about 5.2 to about 5.7 inches), etc.

[173] Aspect 27. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has a cycle time in any range disclosed in this document, for example, from about 13 to about 20, from about 14 to about 19, from about 15 to about 18, from about 16 to about 17 seconds, etc.

[174] Aspect 28. The polymer defined in any of the above aspects, wherein the ethylene polymer has resistance to tensile cracking. Petition 870240096702, dated 12 / 11 / 2024, p. 71 / 192 61 / 68 environmental (ESCR - bottle in 10% Igepal, 60 °C (140 °F), ASTM D2561) in any range disclosed herein, for example, at least 200 hours, at least 250 hours, at least 300 hours, at least 400 hours, at least 500 hours, etc.

[175] Aspect 29. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has an environmental stress crack resistance (ESCR - strip folded in 10% Igepal, 50 °C, 1.9 mm (75 mils), ASTM D1693) in any range disclosed herein, for example, at least 50 hours, at least 60 hours, at least 75 hours, at least 85 hours, at least 100 hours, etc.

[176] Aspect 30. The polymer defined in any of the preceding aspects, wherein the ethylene polymer independently contains less than 0.1 ppm (by weight), less than 0.08 ppm, less than 0.05 ppm, less than 0.03 ppm, etc., of chromium and titanium.

[177] Aspect 31. The polymer defined in any of the preceding aspects, wherein the polymer further comprises any additive disclosed herein, for example, an antioxidant, an acid scavenger, an antiblocking additive, a slip additive, a colorant, a filler, a polymer processing aid, a UV additive, etc., or combinations thereof.

[178] Aspect 32. The polymer defined in any of the preceding aspects, wherein the ethylene polymer has a bimodal molecular weight distribution.

[179] Aspect 33. The polymer defined in any of the preceding aspects, wherein the ethylene polymer is a single reactor product, for example, is not a post-reactor blend of two polymers, for example, having different molecular weight characteristics.

[180] Aspect 34. The polymer defined in any of the preceding aspects, wherein the ethylene polymer comprises an ethylene / αolefin copolymer and / or an ethylene homopolymer.

[181] Aspect 35. The polymer defined in any of the preceding aspects, wherein the ethylene polymer comprises an ethylene / 1 copolymer Petition 870240096702, dated 12 / 11 / 2024, page 72 / 192 62 / 68 butene, an ethylene / 1-hexene copolymer, an ethylene / 1-octene copolymer, an ethylene homopolymer, or any combination thereof.

[182] Aspect 36. The polymer defined in any of the preceding aspects, wherein the ethylene polymer comprises an ethylene / 1-hexene copolymer.

[183] ​​Aspect 37. An article (for example, a blow-molded product) comprising the ethylene polymer defined in any of aspects 136.

[184] Aspect 38. An article comprising the ethylene polymer defined in any of aspects 1-36, wherein the article is an agricultural film, an automobile part, a bottle, a container for chemicals, a drum, a fiber or cloth, a food packaging film or container, a food service article, a fuel tank, a geomembrane, a household container, a liner, a molded product, a medical device or material, an outdoor storage product, outdoor recreational equipment, a pipe, a sheet or tape, a toy or a traffic barrier.

[185] Aspect 39. A catalyst composition comprising: Catalytic component I comprising any single-atom bridge-linked or two-atom bridge-linked metallocene compound disclosed in this document with two indenyl groups; Catalytic component II comprising any single-atom bridge-linked metallocene compound disclosed in this document with a fluorenyl group and a cyclopentadienyl group, and with an alkenyl substituent on the single-atom bridge and / or on the cyclopentadienyl group; any activator disclosed in this document; and optionally, any cocatalyst disclosed in this document.

[186] Aspect 40. The composition defined in aspect 39, wherein the activator comprises an activating support, an aluminoxane compound, an organoboron or organoborate compound, an ionizing ionic compound or any combination thereof.

[187] Aspect 41. The composition defined in aspect 39, wherein the activator comprises an aluminoxane compound. Petition 870240096702, dated 12 / 11 / 2024, p. 73 / 192 63 / 68

[188] Aspect 42. The composition defined in aspect 39, wherein the activator comprises an organoboron or organoborate compound.

[189] Aspect 43. The composition defined in aspect 39, wherein the activator comprises an ionizing ionic compound.

[190] Aspect 44. The composition defined in aspect 39, wherein the activator comprises an activating support, the activating support comprising any solid oxide treated with any electron-withdrawing anion disclosed in this document.

[191] Aspect 45. The composition defined in aspect 39, wherein the activator comprises fluorinated alumina, chlorinated alumina, brominated alumina, sulfated alumina, fluorinated silica and alumina, chlorinated silica and alumina, brominated silica and alumina, sulfated silica and alumina, fluorinated silica and zirconia, chlorinated silica and zirconia, brominated silica and zirconia, sulfated silica and zirconia, fluorinated silica and titania, alumina coated with fluorinated silica, alumina coated with fluorinated and chlorinated silica, alumina coated with sulfated silica, alumina coated with phosphated silica or any combination thereof.

[192] Aspect 46. The composition defined in aspect 39, wherein the activator comprises fluorinated alumina, sulfated alumina, fluorinated silica and alumina, sulfated silica and alumina, alumina coated with fluorinated silica, alumina coated with fluorinated and chlorinated silica, alumina coated with sulfated silica or any combination thereof.

[193] Aspect 47. The composition defined in aspect 39, wherein the activator comprises a fluorinated solid oxide and / or a sulfated solid oxide.

[194] Aspect 48. The composition defined in any of aspects 4447, wherein the activator further comprises any metal or metal ion disclosed herein, for example, zinc, nickel, vanadium, titanium, silver, copper, gallium, tin, tungsten, molybdenum, zirconium or any combination thereof.

[195] Aspect 49. The composition defined in any of aspects 3948, wherein the catalyst composition comprises a cocatalyst, for example, any suitable cocatalyst.

[196] Aspect 50. The composition defined in any of the aspects 39 Petition 870240096702, dated 12 / 11 / 2024, p. 74 / 192 64 / 68 49, wherein the cocatalyst comprises any organoaluminum compound disclosed in this document.

[197] Aspect 51. The composition defined in aspect 50, wherein the organoaluminum compound comprises trimethylaluminum, triethylaluminum, triisobutylaluminum or a combination thereof.

[198] Aspect 52. The composition defined in any of aspects 4451, wherein the catalyst composition comprises catalyst component I, catalyst component II, a solid oxide treated with an electron-withdrawing anion and an organoaluminum compound.

[199] Aspect 53. The composition defined in any of the aspects 3952, wherein catalyst component I has two unsubstituted indenyl groups.

[200] Aspect 54. The composition defined in any of aspects 3953, wherein catalyst component I has a single carbon or silicon bridging atom.

[201] Aspect 55. The composition defined in aspect 54, wherein the carbon or silicon bridging atom has two substituents independently selected from either H or a C18 hydrocarbyl group, for example, a C16 alkyl group.

[202] Aspect 56. The composition defined in any of the aspects 3953, in which the catalyst component I has a bridge of two carbon atoms.

[203] Aspect 57. The composition defined in any of the aspects 3952, in which at least one indenyl group is replaced.

[204] Aspect 58. The composition defined in aspect 57, wherein catalyst component I has a single carbon or silicon bridging atom.

[205] Aspect 59. The composition defined in aspect 58, wherein the carbon or silicon bridging atom has two substituents independently selected from either H or a C1 to C18 hydrocarbyl group, for example, a C1 to C6 alkyl group.

[206] Aspect 60. The composition defined in any of the aspects 5759, wherein any substituent on an indenyl group is independently selected from either a C18 hydrocarbyl or a C18 hydrocarbyl group, for example, a C18 hydrocarbyl group. Petition 870240096702, dated 12 / 11 / 2024, p. 75 / 192 65 / 68 C6 alkyl.

[207] Aspect 61. The composition defined in any of the aspects 3960, wherein the catalyst component I contains zirconium.

[208] Aspect 62. The composition defined in any of aspects 3961, wherein catalyst component II has a single carbon or silicon bridging atom.

[209] Aspect 63. The composition defined in aspect 62, wherein the carbon or silicon bridging atom has two substituents independently selected from H or a C18 hydrocarbyl group, for example, a phenyl group.

[210] Aspect 64. The composition defined in any of the aspects 3963, in which the fluorenyl group is substituted.

[211] Aspect 65. The composition defined in any of the aspects 3964, wherein the alkenyl substituent is a C3 to C18 alkenyl group, for example, a terminal C3 to C8 alkenyl group.

[212] Aspect 66. The composition defined in any of the aspects 3965, wherein catalyst component II contains zirconium or hafnium.

[213] Aspect 67. The composition defined in any of aspects 4466, wherein the catalyst composition is substantially free of aluminoxane compounds, organoboron or organoborate compounds, ionizing ionic compounds or combinations thereof.

[214] Aspect 68. The composition defined in any of aspects 3967, wherein a weight ratio of catalyst component I to catalyst component II in the catalyst composition is in any range disclosed herein, for example, from about 10:1 to about 1:10, from about 5:1 to about 1:5, from about 1.2:1 to about 5:1, from about 1.5:1 to about 4:1, from about 1.5:1 to about 2.5:1, etc.

[215] Aspect 69. The composition defined in any of the aspects 3968, wherein the catalyst composition is produced by a process comprising bringing into contact, in any order, catalyst component I, catalyst component II and the activator.

[216] Aspect 70. The composition defined in any of the aspects 39- Petition 870240096702, dated 12 / 11 / 2024, p. 76 / 192 66 / 68 68, in which the catalyst composition is produced through a process that comprises bringing into contact, in any order, catalyst component I, catalyst component II, the activator and the cocatalyst.

[217] Aspect 71. The composition defined in any of aspects 3970, wherein a catalyst activity of the catalyst composition is in any range disclosed herein, for example, from about 500 to about 5000, from about 750 to about 4000, from about 1000 to about 3500 grams, etc., of ethylene polymer per gram of activator support per hour, under flow paste polymerization conditions, with a triisobutylaluminum cocatalyst, using isobutane as a diluent and with a polymerization temperature of 95 °C and a reactor pressure of 4 MPa (590 psig).

[218] Aspect 72. An olefin polymerization process, wherein the process comprises placing the catalyst composition defined in either of aspects 39-71 in contact with an olefin monomer and an optional olefin comonomer in a polymerization reactor system under polymerization conditions to produce an olefin polymer.

[219] Aspect 73. The process defined in aspect 72, wherein the olefin monomer comprises any olefin monomer disclosed herein, for example, any C2-C20 olefin.

[220] Aspect 74. The process defined in aspect 72 or 73, wherein the olefin monomer and the olefin comonomer independently comprise a C2-C20 alpha-olefin.

[221] Aspect 75. The process defined in any of aspects 7274, wherein the olefin monomer comprises ethylene.

[222] Aspect 76. The process defined in any one of aspects 7275, wherein the catalyst composition is in contact with ethylene and an olefin comonomer comprising a C3-C10 alpha-olefin.

[223] Aspect 77. The process defined in any one of aspects 7276, wherein the catalyst composition is in contact with ethylene and an olefin comonomer comprising 1-butene, 1-hexene, 1-octene or a mixture thereof.

[224] Aspect 78. The process defined in any of the aspects 72- Petition 870240096702, dated 12 / 11 / 2024, page 77 / 192 67 / 68 74, wherein the olefin monomer comprises propylene.

[225] Aspect 79. The process defined in any of aspects 7278, wherein the polymerization reactor system comprises a batch reactor, a fluid paste reactor, a gas phase reactor, a solution reactor, a high pressure reactor, a tubular reactor, an autoclave reactor or a combination thereof.

[226] Aspect 80. The process defined in any of aspects 7279, wherein the polymerization reactor system comprises a fluid paste reactor, a gas phase reactor, a solution reactor or a combination thereof.

[227] Aspect 81. The process defined in any of aspects 7280, wherein the polymerization reactor system comprises a cycle fluid paste reactor.

[228] Aspect 82. The process defined in any of the aspects 7281, wherein the polymerization reactor system comprises a single reactor.

[229] Aspect 83. The process defined in any of the aspects 7281, wherein the polymerization reactor system comprises 2 reactors.

[230] Aspect 84. The process defined in any of the aspects 7281, wherein the polymerization reactor system comprises more than 2 reactors.

[231] Aspect 85. The process defined in any of the aspects 7284, wherein the olefin polymer comprises any olefin polymer disclosed herein.

[232] Aspect 86. The process defined in any one of aspects 72-77 and 79-85, wherein the olefin polymer comprises an ethylene homopolymer, an ethylene / 1-butene copolymer, an ethylene / 1-hexene copolymer and / or an ethylene / 1-octene copolymer.

[233] Aspect 87. The process defined in either of aspects 72-77 and 79-85, wherein the olefin polymer comprises an ethylene / 1-hexene copolymer.

[234] Aspect 88. The process defined in either of aspects 72-74 and 78-85, wherein the olefin polymer comprises a polypropylene homopolymer or a propylene-based copolymer. Petition 870240096702, dated 12 / 11 / 2024, p. 78 / 192 68 / 68

[235] Aspect 89. The process defined in any of the aspects 7288, wherein the polymerization conditions comprise a polymerization reaction temperature in a range of about 60 °C to about 120 °C and a reaction pressure in a range of about 200 to about 1000 psig (about 1.4 to about 6.9 MPa).

[236] Aspect 90. The process defined in any of the aspects 7289, in which the polymerization conditions are substantially constant, for example, for a particular grade of polymer.

[237] Aspect 91. The process defined in any of the aspects 7290, in which no hydrogen is added to the polymerization reactor system.

[238] Aspect 92. The process defined in any of the aspects 7290, in which hydrogen is added to the polymerization reactor system.

[239] Aspect 93. The process defined in any one of aspects 7292, wherein the olefin polymer produced is defined in any one of aspects 1-36.

[240] Aspect 94. An olefin polymer produced by the olefin polymerization process defined in either of aspects 72-92.

[241] Aspect 95. An ethylene polymer defined in any of aspects 1-36 produced by the process defined in any of aspects 7292.

[242] Aspect 96. An article comprising the polymer defined in any of aspects 94-95.

[243] Aspect 97. A method for forming or preparing a manufactured article comprising an olefin polymer, wherein the method comprises (i) carrying out the olefin polymerization process defined in any of aspects 72-92 to produce an olefin polymer (for example, the ethylene polymer of any of aspects 1-36) and (ii) forming the manufactured article comprising the olefin polymer, for example, by means of any technique disclosed herein.

Claims

CLAIMS 1. Ethylene polymer characterized in that it has: a melting index less than or equal to 1 g / 10 min; a density in the range of 0.94 to 0.965 g / cm3; a Mw in the range of 100,000 to 250,000 g / mol; a relaxation time of 0.5 to 3 s; and an average number of long-chain branches (LCBs) per 1,000,000 total carbon atoms of the ethylene polymer in a molecular weight range of 300,000 to 900,000 g / mol that is greater than that in a molecular weight range of 1,000,000 to 2,000,000 g / mol.

2. A manufactured article characterized in that it comprises the ethylene polymer, as defined in claim 1.

3. Ethylene polymer, according to claim 1, characterized in that: the melting index is in a range of 0.1 to 0.5 g / 10 min; the density is in a range of 0.94 to 0.96 g / cm3; the average number of LCBs per 1,000,000 total carbon atoms of the polymer in the molecular weight range of 300,000 to 900,000 g / mol is at least 100% greater than that in the molecular weight range of 1,000,000 to 2,000,000 g / mol; and the ethylene polymer comprises an ethylene / 1-butene copolymer, an ethylene / 1-hexene copolymer, an ethylene / 1-octene copolymer or a combination thereof.

4. Blow-molded product characterized in that it comprises the ethylene polymer, as defined in claim 3.

5. Ethylene polymer, according to claim 3, characterized in that it has: a CY-a parameter in a range of 0.2 to 0.4; and a relaxation time in a range of 0.75 to 2.5 s.

6. Ethylene polymer according to claim 3, characterized in that it has: an environmental stress crack resistance (ESCR, ASTM D2561) of at least 200 hours; and an environmental stress crack resistance (ESCR, ASTM D1693) of at least 50 hours.

7. Ethylene polymer according to claim 1, characterized in that it has: an average number of 3 to 15 LCBs per 1,000,000 total carbon atoms of the ethylene polymer in the molecular weight range of 300,000 to 900,000 g / mol; and / or an average number of 4 to 15 LCBs per 1,000,000 total carbon atoms of the ethylene polymer in a molecular weight range of 400,000 to 600,000 g / mol.

8. Ethylene polymer according to claim 7, characterized in that it comprises an ethylene / 1-butene copolymer, an ethylene / 1-hexene copolymer, an ethylene / 1-octene copolymer, or a combination thereof.

9. Ethylene polymer according to claim 8, characterized in that the Mw is in a range of 110,000 to 190,000 g / mol.

10. Ethylene polymer according to claim 8, characterized in that it has: an Mw / Mn ratio in the range of 6 to 12; and an Mz / Mw ratio in the range of 4 to 8.

11. Ethylene polymer characterized in that it has: a melting index less than or equal to 1 g / 10 min; a density in a range of 0.94 to 0.965 g / cm3; a Mw in a range of 100,000 to 250,000 g / mol; a relaxation time of 0.5 to 3 s; an average number of long-chain branches (LCBs) per 1,000,000 total carbon atoms of the ethylene polymer in a molecular weight range of 1,000,000 to 2,000,000 g / mol less than or equal to 5; and a maximum extension viscosity ratio of three times the shear viscosity ηE / 3η at an extension rate of 0.1 s-1 in a range of 1.2 to 10.

12. Article of manufacture characterized in that it comprises the polymer, as defined in claim 11.

13. Ethylene polymer, according to claim 11, characterized in that: the average number of LCBs per 1,000,000 total carbon atoms of the ethylene polymer in the molecular weight range of 1,000,000 to 2,000,000 g / mol is less than or equal to 3.5; and the maximum nE / 3n ratio at the extension rate of 0.1 s-1 is in the range of 1.5 to 5.

14. Ethylene polymer, according to claim 11, characterized in that: the melting index is in a range of 0.1 to 0.5 g / 10 min; the density is in a range of 0.94 to 0.96 g / cm3; and the ethylene polymer comprises an ethylene / 1-butene copolymer, an ethylene / 1-hexene copolymer, an ethylene / 1-octene copolymer or a combination thereof.

15. Blow-molded product characterized in that it comprises the ethylene polymer, as defined in claim 14.

16. Ethylene polymer, according to claim 14, characterized in that it has: a CY-a parameter in a range of 0.2 to 0.4; and a relaxation time in a range of 0.75 to 2.5 s.

17. Ethylene polymer according to claim 14, characterized in that it has: an environmental stress crack resistance (ESCR, ASTM D2561) of at least 200 hours; and an environmental stress crack resistance (ESCR, ASTM D1693) of at least 50 hours.

18. Ethylene polymer, according to claim 14, characterized in that it contains 5 to 15 LCBs per 1,000,000 total carbon atoms.

19. Ethylene polymer, according to claim 14, characterized in that it has a maximum nE / 3n ratio at an extension rate of 0.03 s-1 in a range of 1.5 to 8. Petition 870240096702, dated 12 / 11 / 2024, pp. 150 / 192 4 / 4 20. Olefin polymerization process, wherein the process comprises placing a catalyst composition in contact with ethylene and an olefin comonomer in a polymerization reactor system under polymerization conditions to produce an ethylene polymer, wherein: the catalyst composition comprises: catalyst component I comprising a metallocene compound bridged to a single atom or bridged to two atoms with two indenyl groups; catalyst component II comprising a metallocene compound bridged to a single atom with a fluorenyl group and a cyclopentadienyl group, and with an alkenyl substituent on the single atom bridge and / or on the cyclopentadienyl group; an activator; and optionally, a cocatalyst; and wherein the ethylene polymer is characterized in that: a melting index less than or equal to 1 g / 10 min; a density in a range of 0.94 to 0.965 g / cm3; a Mw in a range of 100,000 to 250.000 g / mol; a relaxation time of 0.5 to 3 s; and an average number of LCBs per 1,000,000 total carbon atoms of the polymer in a molecular weight range of 300,000 to 900,000 g / mol that is greater than that in a molecular weight range of 1,000,000 to 2,000,000 g / mol.