Polymeric composition, film, coated article, process for fabricação do coated artigo and use of itself
A polymeric composition combining a C2C3 heterophasic copolymer and propylene homopolymer addresses the limitations of existing polypropylene coatings by enhancing molten material strength, sealing properties, and reducing hexane extractables, resulting in improved films and coated articles for packaging.
Patent Information
- Application Number
- BR112023020128
- Authority / Receiving Office
- BR · BR
- Patent Type
- Patents
- Current Assignee / Owner
- Publication Date
- 2026-11-17
AI Technical Summary
Existing polypropylene compositions for extrusion coating lack a combination of high molten material strength, excellent sealing properties, low seal onset temperature, and low opacity, while also having a high content of hexane extractables, which are not adequately addressed by prior art.
A polymeric composition comprising 30.0 to 80.0% by weight of a C2C3 heterophasic copolymer produced by a single-site catalyst and 20.0 to 70.0% by weight of a propylene homopolymer, with specific properties such as melting point, MFR2, and soluble fraction, to achieve enhanced molten material strength, low opacity, and reduced hexane extractables.
The composition provides films and coated articles with improved molten material strength, low seal onset temperature, and low opacity, along with a reduced content of hexane extractables, suitable for packaging applications.
Description
POLYMER COMPOSITION, FILM, COATED ARTICLE, PROCESS FOR MANUFACTURING THE COATED ARTICLE AND ITS USE
[001] The present invention relates to a polymeric composition comprising a specific C2C3 heterophasic copolymer and a specific propylene homopolymer and to films and coated articles comprising a layer comprising said polymeric composition.
[002] Polypropylene compositions suitable for coating, especially for extrusion coating, are already known in the art.
[003] US patent 3,418,396 A refers to a polyolefin composition for extrusion, coating and molding of various articles, comprising a predominant portion of a mixture of about 40% to 99% by weight of a polypropylene having a flow rate of about 12 dg / min to 120 dg / min and about 1% to 60% of a polyethylene having a melt index of about 1 dg / min to 15 dg / min, a density greater than about 0.912 g / cc and a melt index recovery greater than 50%.
[004] US patent 4,378,451 A refers to blends containing degraded crystalline polypropylene or propylene-containing copolymers useful as extrusion coating compositions. These coated substrates can be used in the manufacture of bags and other packaging applications. In particular, these coatings are a blend of degraded crystalline polypropylene or Petition 870250099583, dated 10 / 30 / 2025, p. 25 / 109 2 / 41 copolymer containing propylene and low-density polyethylene.
[005] Document EP 1 638 695 A1 refers to an extrusion-coated substrate having a coating comprising a polyethylene produced by single-site catalyst-catalyzed polymerization and comprising ethylene and at least two C412 alpha olefins as comonomers.
[006] US patent 2014 / 031462 A1 refers to a process for extruding a blend of a first irradiated propylene polymer and a second non-irradiated propylene polymer, wherein the first propylene polymer comprises a non-phenolic stabilizer. Irradiation of the first extruded propylene polymer product is conducted in an oxygen-reducing environment, and the first irradiated propylene polymer and the second non-irradiated propylene polymer are combined at a temperature below their respective melting points. The blend has a viscosity retention of 20 to 35%.
[007] Document EP2 492 293 A1 refers to a polypropylene composition suitable for extrusion coating or extrusion foaming onto a wide variety of substrates having high melt strength and stampability, excellent processability, low gel content, and being able to withstand high temperatures, a process for providing such polypropylene compositions Petition 870250099583, dated 10 / 30 / 2025, page 26 / 109 3 / 41 and articles coated by extrusion or extrusion foam. The polypropylene composition comprises a polypropylene base resin such that the polypropylene base resin has an MFR2 (2.16 kg, 230°C, ISO 1133) of 5 to 35 g / 10 min and an optical gel index of 1000 or less, measured with an OCS gel counting apparatus on melt thin films with a film thickness of 70 μm that were produced with a cooling roll temperature of 40°C, such that the polypropylene base resin has a strain hardening factor (SHF) of 2.3 to 7.0 when measured at a strain rate of 3.0 s-1 and a Hencky strain of 2.5.The process for producing such a polypropylene composition is distinguished from a single-site catalyst-derived polypropylene intermediate base resin having an MFR2 (2.16 kg, 230°C, ISO 1133) of 6.0 g / 10 min or less being mixed with a peroxide masterbatch composition and an oligomeric diene masterbatch composition to form a premixed material; and the premixed material is melt-mixed in a melt-mixing device at a barrel temperature in the range of 180 to 300°C.
[008] EP 2 877 535 A1 refers to a process for providing a polypropylene composition comprising a branched polypropylene in which a polypropylene with a melt flow ratio MFR2 (230°C) of more than 1.0 g / 10 min is reacted with a free radical forming agent in Petition 870250099583, dated 10 / 30 / 2025, page 27 / 109 4 / 41 thermal decomposition and optionally with a bifunctionally unsaturated monomer, thus obtaining branched polypropylene, in which the polypropylene composition has a molten material strength F30 of more than 5.8 cN and a molten material extensibility v30 of more than 200 mm / s.
[009] For film and coating applications, high molten material strength and, for many applications, an excellent balance of sealing and optical properties are required. Additionally, for food applications, a low content of hexane extractable materials is a requirement. Known prior art compositions do not offer this combination of properties and / or have a high content of hexane extractables. In general, compositions offering low opacity and low seal onset temperature (SIT) are preferred.
[0010] Therefore, it was an objective of the present invention to provide a polymeric composition having a high molten material strength and exhibiting an excellent combination of sealing properties, especially a low SIT, and optical properties, especially a low opacity. Additionally, it was an objective of the present invention to provide compositions that allow the production of coated films and articles having a low content of hexane extractables.
[0011] These objectives were solved by Petition 870250099583, dated 10 / 30 / 2025, page 28 / 109 5 / 41 polymeric composition, according to claim 1, comprising at least the following components: 30.0 to 80.0% by weight based on the total weight of the polymer composition of a C2C3 heterophasic copolymer produced by a single-site catalyst (HECO); wherein said copolymer has a melting point in the range of 150 to 162°C determined by differential scanning calorimetry according to ISO 11357-3; an MFR2 (230°C, 2.16 kg) determined according to ISO 1133 in the range of 5.0 to 40.0 g / 10 min; and a total C2 content in the range of 1 to 10% by weight based on the total weight of component (A); and a soluble fraction (SF) based on the total weight of component (A) in the range of 10 to 50% by weight determined according to CRYSTEX QC, Polymer Char as described in the description; 20.0 to 70.0% by weight based on the total weight of the polymeric composition of a propylene homopolymer; such that said propylene homopolymer has: an MFR2 (230°C, 2.16 kg) determined according to ISO 1133 in the range of 1.0 to 20.0 g / 10 min; and a molten material strength F30 determined according to ISO 16790 of at least 10 cN; provided that the weight proportions of components A) and B) add up to 100% by weight.
[0012] The advantageous forms of composition Petition 870250099583, dated 10 / 30 / 2025, page 29 / 109 6 / 41 polymeric compositions according to the present invention are specified in dependent claims 2 to 7. Claim 8 of the present invention relates to a film comprising at least one layer comprising the polymeric composition according to the invention, and claims 8 to 11 relate to preferred embodiments of said film. Claims 12 to 13 relate to a coated article comprising at least one layer comprising said polymeric composition, claim 14 relates to a process for producing said article, and claim 15 relates to the use of the coating for specific end applications. DEFINITIONS Quantity Indications
[0013] The polymeric composition according to the present invention necessarily comprises components (A) and (B) and optionally additives (C). The requirement applies such that components (A) and (B) and, if present, additives (C) add up to 100% by weight in the sum. The fixed ranges of quantity indications for the individual components (A) and (B) and, optionally, additives (C) should be understood such that an arbitrary quantity for each of the individual components may be selected within the specified ranges provided that a strict standard is satisfied that the sum of all components (A), (B) and, optionally, additives (C) adds up to 100% by weight. Petition 870250099583, dated 10 / 30 / 2025, page 30 / 109 7 / 41 REGIO-DEFECTS
[0014] The region defects of propylene polymers can be of three different types, namely, 2,1-erythro (2,1e), 2,1-threo (2,1it) and 3,1 defects. A detailed description of the structure and mechanism of formation of regiodefects in polypropylene can be found in Chemical Reviews 2000, 100(4), pages 1316 to 1327. These defects are measured using 13C NMR as described in more detail below.
[0015] The term 2,1 regio-defects as used in the present invention defines the sum of 2,1-erythro regio-defects and 2,1-threo regio-defects. Random propylene copolymers or polypropylene homopolymers having multiple regio-defects as required in the propylene composition of the invention are usually and preferably prepared in the presence of a single-site catalyst.
[0016] The catalyst particularly influences the polymer microstructure. Consequently, polypropylenes prepared using a single-site metallocene catalyst provide a different microstructure compared to those prepared using Ziegler-Natta (ZN) catalysts. The most significant difference is the presence of regio-defects in metallocene-based polypropylenes, which is not the case for polypropylenes made with Ziegler-Natta (ZN) catalysts.
[0017] A polymer “produced by the site catalyst Petition 870250099583, dated 10 / 30 / 2025, page 31 / 109 "8 / 41 single" is a polymer that was produced in the presence of a single-site catalyst.
[0018] Where the term comprising is used in the present description and claims, it does not exclude other unspecified elements of greater or lesser functional importance. For the purposes of the present invention, the term consisting of is considered to be a preferred embodiment of the term comprised of. If a group is defined herein as comprising at least a certain number of embodiments, this shall also be understood as disclosing a group which preferably consists only of those embodiments.
[0019] Whenever the terms including or having are used, these terms are intended to be equivalent to comprising as defined above.
[0020] Where an indefinite or definite article is used when referring to a singular noun, for example, a, an or the, it includes a plural of that noun unless something else is specifically specified. Component (A)
[0021] The polymeric composition according to the present invention comprises as component (A) 30.0 to 80.0% by weight based on the total weight of the polymeric composition of a C2C3 heterophasic copolymer produced by a single-site catalyst (HECO); wherein said copolymer has a melting point in the range of 150 to 162°C determined by Petition 870250099583, dated 10 / 30 / 2025, page 32 / 109 9 / 41 differential scanning calorimetry according to ISO 11357-3; an MFR2 (230°C, 2.16 kg) determined according to ISO 1133 in the range of 5.0 to 40.0 g / 10 min; a total C2 content in the range of 1 to 10% by weight based on the total weight of component (A); and a soluble fraction (SF) based on the total weight of component (A) in the range of 10 to 50% by weight determined according to CRYSTEX QC, Polymer Char as described in the experimental section.
[0022] The preferred modalities of component (A) will be discussed below.
[0023] A preferred embodiment of the present invention stipulates that component (A) has a melting point determined by differential scanning calorimetry according to ISO 11357-3 in the range of 151 to 160°C, preferably in the range of 151 to 155°C and preferably in the range of 151 to 154°C.
[0024] According to another preferred embodiment according to the present invention, component (A) has an MFR2 (230°C, 2.16 kg) determined according to ISO 1133 in the range of 10.0 to 30.0 g / 10 min, preferably in the range of 15.0 to 25.0 g / 10 min and most preferably in the range of 20.0 to 23.0 g / 10 min.
[0025] Yet another preferred embodiment according to the present invention stipulates that component (A) has a total C2 content in the range of 1.0 to 8.0% by weight, preferably in the range of 1.5 to 6% by weight and in a way Petition 870250099583, dated 10 / 30 / 2025, p. 33 / 109 10 / 41 most preferred in the range of 2.5 to 4.0% by weight based on the total weight of the component (A).
[0026] In another preferred embodiment of the present invention, component (A) has a soluble fraction (SF) based on the total weight of component (A) in the range of 15 to 40% by weight, preferably in the range of 20 to 30% by weight and most preferably in the range of 24 to 28% by weight determined according to CRYSTEX QC, Polymer Char as described in the experimental section.
[0027] According to a further embodiment of the present invention, component (A) has a C2 content of the soluble fraction (SF) based on the total weight of the soluble fraction in the range of 5 to 40% by weight, preferably in the range of 8 to 30% by weight, more preferably in the range of 8 to 25% by weight and even more preferably in the range of 9 to 12% by weight determined according to CRYSTEX QC, Polymer Char as described in the experimental section.
[0028] Yet another preferred embodiment according to the present invention stipulates that component (A) has a C2 content of the crystalline fraction (CF) based on the total weight of the crystalline fraction that is below 4% by weight, preferably below 2% by weight, more preferably in the range of 0 to 1% by weight and even more preferably is 0% by weight determined according to CRYSTEX QC, Polymer Char as described in the experimental section.
[0029] According to another preferred modality of Petition 870250099583, dated 10 / 30 / 2025, p. 34 / 109 11 / 41 According to the present invention, component (A) has an intrinsic viscosity (IV) of the soluble fraction (SF) that is in the range of 1.0 to 5.0 dl / g, preferably in the range of 2.0 to 4.0 dl / g, more preferably in the range of 2.2 to 3.4 dl / g and even more preferably in the range of 3.0 to 3.3 dl / g determined according to CRYSTEX QC, Polymer Char as described in the experimental section.
[0030] Yet another preferred embodiment according to the present invention stipulates that component (A) has an intrinsic viscosity (IV) of the crystalline fraction (CF) that is in the range of 0.5 to 4.0 dl / g, preferably in the range of 0.8 to 2.0 dl / g and more preferably in the range of 1.0 to 1.2 dl / g determined according to CRYSTEX QC, Polymer Char as described in the experimental section.
[0031] According to another preferred embodiment agreed with the present invention, component (A) has a Tg1 determined by dynamic mechanical analysis (DMA) according to ISO 6721-7 in the range of -10 to 10°C, preferably in the range of -5 to 5°C and most preferably in the range of -2 to 2°C.
[0032] According to another preferred embodiment agreed with the present invention, component (A) has a Tg2 determined by dynamic mechanical analysis (DMA) according to ISO 6721-7 in the range of -70 to -10°C, preferably in the range of -45 to -20°C and most preferably in the range of -26 to -22°C. Petition 870250099583, dated 10 / 30 / 2025, page 35 / 109 12 / 41
[0033] Yet another preferred embodiment according to the present invention stipulates that component (A) has a storage module G' determined by dynamic mechanical analysis (DMA) according to ISO 6721-7 in the range of 250 to 600 MPa, preferably in the range of 300 to 550 MPa and most preferably in the range of 420 to 470 MPa.
[0034] The glass transition temperature Tg and the storage modulus G'(23°C) were determined by dynamic mechanical analysis (DMA) according to ISO 6721-7.
[0035] In another preferred embodiment according to the present invention, component (A) was produced in the presence of a single-site catalyst of a metallocene catalyst.
[0036] A preferred metallocene catalyst has Formula (I), as shown below. R2Si MtX2 X-R3r <R3(I) em que Mt is Hf or Zr; Each X is a sigma ligand, each R1 * * * * * * is independently the same or may be different and is a CH2-R7 group, with R7 being either a linear or branched C3-6 alkyl group, or a C3-8 cycloalkyl group. Petition 870250099583, dated 10 / 30 / 2025, p. 36 / 109 13 / 41 C6-10 aryl, each R2 is independently a -CH=, -CY=, -CH2-, -CHY- or -CY2- group, wherein Y is a C1-10 hydrocarbyl group and where n is 2-6, each R3 and R4 are independently the same or may be different and are hydrogen, a linear or branched C1-C6-alkyl group, an OY group or a C7-20 arylalkyl, C7-20 alkylaryl group or C6-20 aryl group, such that at least one R3 per phenyl group and at least one R4 is not hydrogen and, optionally, two adjacent R3 or R4 groups may be part of a ring including the phenyl carbons to which they are attached, R5 is a linear or branched C1-C6-alkyl group, C7-20 arylalkyl group, C7-20 alkylaryl group or C6-C20aryl group, R6 is a C(R8)3 group, with R8 being a linear or branched C1-C6 alkyl group, each R independently being a C1-C20-hydrocarbyl, C6C20-aryl, C7-C20-arylalkyl or C7-C20-alkylaryl.
[0037] According to another preferred embodiment, the metallocene catalyst has formula (II) as shown below.(II) (II)
[0038] Preferably, component (A) is Petition 870250099583, dated 10 / 30 / 2025, page 37 / 109 14 / 41 prepared in a sequential polymerization process comprising at least two polymerization reactors (R1) and (R2), such that in the first polymerization reactor (R1) a first polymer fraction a1) is produced, which is subsequently transferred to the second polymerization reactor (R2). In the second polymerization reactor (R2), a second polymer fraction a2) is then produced in the presence of the first polymer fraction a1).
[0039] The polymerization processes that are suitable for producing component (A) generally comprise at least two polymerization stages and each stage can be carried out in solution, flow paste, fluidized bed, bulk or gas phase.
[0040] A preferred multi-stage process for manufacturing component (A) is a circulating gas phase process, as developed by Borealis (known as BORSTAR® technology) which is described, for example, in patent literature, such as in document EP 0 887 379 A1, WO 92 / 12182 A1, WO 2004 / 000899 A1, WO 2004 / 111095 A1, WO 99 / 24478 A1, WO 99 / 24479 A1 or in document WO 00 / 68315 A1. An additional suitable gas-phase fluidized slurry process is the Basell Spheripol® process. Component (B)
[0041] The polymeric composition according to the present invention comprises component (B) from 20.0 to 70.0% by weight based on the total weight of the polymeric composition of a Petition 870250099583, dated 10 / 30 / 2025, p. 38 / 109 15 / 41 propylene homopolymer; whereby said propylene homopolymer has an MFR2 (230°C, 2.16 kg) determined in accordance with ISO 1133 in the range of 1.0 to 20.0 g / 10 min; and an F30 determined in accordance with ISO 16790 of at least 10 cN.
[0042] The preferred modalities of component (B) will be discussed below.
[0043] According to a preferred embodiment of the present invention, component (B) has an MFR2 (230°C, 2.16 kg) determined according to ISO 1133 in the range of 1.0 to 15.0 g / 10 min, preferably in the range of 3.0 to 15.0 g / 10 min, more preferably in the range of 6.0 to 14.0 g / 10 min and even more preferably in the range of 8.0 to 12.0 g / 10 min.
[0044] Yet another preferred embodiment according to the present invention stipulates that component (B) has an F30 determined according to ISO 16790 of at least 20 cN, preferably of at least 30 cN and most preferably in the range of 30 to 60 cN.
[0045] In a preferred additional embodiment of the present invention, component (B) has a molten material extensibility V30 determined in accordance with ISO 16790 of at least 200 mm / s, preferably at least 250 mm / s and more preferably in the range of 250 to 300 mm / s.
[0046] Yet another preferred additional mode of Petition 870250099583, dated 10 / 30 / 2025, p. 39 / 109 16 / 41 according to the present invention stipulates that component (B) has a density determined according to ISO1183 in the range of 895 to 920 kg / m3, preferably in the range of 900 to 910 kg / m3 and more preferably in the range of 904 to 906 kg / m3. Polymer Composition
[0047] According to a preferred embodiment of the present invention, the polymer composition has an MFR2 (230°C, 2.16 kg) determined according to ISO 1133 in the range of 4.0 to 30.0 g / 10 min, preferably in the range of 8.0 to 20.0 g / 10 min and most preferably in the range of 12.0 to 16.0 g / 10 min.
[0048] Another preferred embodiment stipulates that the polymer composition has an F30 determined according to ISO 16790 of at least 2 cN, preferably of at least 3 cN and most preferably in the range of 3 to 5 cN.
[0049] Yet another preferred embodiment according to the present invention stipulates that the polymer composition has a molten material extensibility V30 determined according to ISO 16790 of at least 200 mm / s, preferably at least 230 mm / s, more preferably in the range of 240 to 300 mm / s and even more preferably in the range of 240 to 260 mm / s.
[0050] According to a preferred additional embodiment according to the present invention, the polymeric composition has an MFR2 (230°C, 2.16 kg) determined according to ISO Petition 870250099583, dated 10 / 30 / 2025, p. 40 / 109 17 / 41 1133 in the range of 12.0 to 16.0 g / 10 min and an F30 determined according to ISO 16790 in the range of 3 to 5 cN.
[0051] An additional embodiment according to the present invention stipulates that the polymeric composition has a soluble xylene fraction (XCS) determined according to ISO 16152 in the range of 10 to 20% by weight, preferably in the range of 12 to 18% by weight and most preferably in the range of 14 to 16% by weight.
[0052] According to a preferred additional embodiment according to the present invention, the polymer composition has a flexural modulus determined according to ISO 178 in the range of 1000 to 1600 MPa, preferably in the range of 1100 to 1400 MPa and most preferably in the range of 1200 to 1300 MPa.
[0053] Yet another preferred embodiment according to the present invention stipulates that the polymeric composition has an intrinsic viscosity of XCS measured according to DIN ISO 1628 / 1 and / 3 in the range of 2.5 to 3.6 dl / g, preferably in the range of 2.7 to 3.3 dl / g and more preferably in the range of 3.05 to 3.15 dl / g.
[0054] According to a preferred additional embodiment according to the present invention, the polymeric composition has a Charpy notch impact resistance determined according to ISO 179 1eA at 23°C in the range of 4 to 20 kJ / m2, preferably in the range of 4.5 to 8 kJ / m2 and more preferably in the range of 5 to 6 kJ / m2. Petition 870250099583, dated 10 / 30 / 2025, p. 41 / 109 18 / 41
[0055] Yet another preferred embodiment according to the present invention stipulates that the polymeric composition has a determined opacity in a test specimen having a thickness of 1 mm as described in the experimental section in the range of 5 to below 60%, preferably in the range of 40 to 55% and most preferably in the range of 45 to 51%.
[0056] According to a preferred additional embodiment of the present invention, the polymeric composition has a content of hot soluble hexane (C6 FDA, % by weight) determined according to FDA section 177.1520 below 2.1% by weight, preferably in the range of 0.5 to 2.0% by weight, more preferably in the range of 0.5 to 1.8% by weight and even more preferably in the range of 1.2 to 1.6% by weight. It is further preferred that the C6 FDA / XCS ratio is below 0.20 and more preferably below 0.10.
[0057] Another preferred embodiment of the present invention stipulates that the polymer composition comprises at least one additive C), preferably selected from the group consisting of slip agents, acid scavengers, UV stabilizers, pigments, antioxidants, additive carriers, nucleating agents and mixtures thereof, such that these additives are preferably present in 0.1 to 5.0% by weight and more preferably in 0.1 to 4.0% by weight based on the total weight of the polymer composition. Petition 870250099583, dated 10 / 30 / 2025, p. 42 / 109 19 / 41 Film
[0058] The present invention also relates to a film comprising the polymeric composition according to the present invention and, according to a preferred embodiment, said film consists of the polymeric composition.
[0059] Yet another preferred embodiment of the present invention stipulates that the film has a modulus of elasticity determined in accordance with ISO 527-3 at 23°C in a fused film having a thickness of 50 µm in the machine direction as well as in the transverse direction in the range of 200 to 1000 MPa, preferably in the range of 300 to 700 MPa and most preferably in the range of 400 to 500 MPa.
[0060] According to another preferred embodiment of the present invention, the film has a sealing start temperature determined as described in the experimental section in a fused film having a thickness of 50 µm in the range of 100°C down to below 140°C, preferably in the range of 120°C to 135°C, more preferably in the range of 120°C to 132°C and even more preferably in the range of 128 to 130°C.
[0061] In a preferred additional embodiment of the present invention, the film has an opacity determined according to ASTM D1003-00 in a fused film having a thickness of 50 µm in the range of 5 to below 20%, preferably in the range of 8 to 16%, and more Petition 870250099583, dated 10 / 30 / 2025, p. 43 / 109 20 / 41 preferred in the 10-15% range.
[0062] All aspects and preferred embodiments as described above for the composition will also be valid for the film according to the present invention. Coated Article
[0063] The present invention also relates to a coated article comprising at least one layer comprising the polymeric composition according to the present invention and, preferably, said layer consists of this polymeric composition.
[0064] According to a preferred embodiment of the present invention, the coated article is an extrusion-coated article. Said article can be produced by each process comprising an extrusion coating step.
[0065] The extrusion coating process can be carried out using conventional extrusion coating techniques. Consequently, the composition according to the present invention can be fed, typically in pellet form, to an extrusion device. From the extruder, the molten polymer is preferably passed through a flat die to the substrate to be coated. The coated substrate is cooled on a cooling roll, after which it is passed to edge trimmers and rolled.
[0066] The width of the matrix typically depends on Petition 870250099583, dated 10 / 30 / 2025, p. 44 / 109 21 / 41 extruder size used. Thus, with 90 mm extruders the width can suitably be within the range of 600 to 1,200 mm, with 115 mm extruders from 900 to 2,500 mm, with 150 mm extruders from 1,000 to 4,000 mm and with 200 mm extruders from 3,000 to 5,000 mm. The line speed (draft speed) is preferably 75 m / min or more, more preferably at least 100 m / min. In most commercially operating machines, the line speed is preferably more than 300 m / min or more than 500 m / min. Modern machines are designed to operate at line speeds of up to 1,000 m / min, for example, 300 to 800 m / min.
[0067] The molten polymer temperature is typically between 240 and 330°C. The polypropylene composition of the invention can be extruded onto the substrate as a single-layer coating or as one or more layers in a co-extrusion process, preferably as an outer layer. In a multi-layer extrusion coating, a polymer layer structure as defined above and, optionally, the other polymer layers can be co-extruded. Additional ozone and / or corona treatment in a known manner is possible if desired or necessary.
[0068] All aspects and preferred embodiments as described above for the composition will also be valid for the coated article according to the present invention. Petition 870250099583, dated 10 / 30 / 2025, page 45 / 109 22 / 41 Use
[0069] The present invention also relates to the use of the polymeric composition, film or coated article according to the present invention as packaging material, preferably as a temperature-resistant packaging material for food and / or medical products.
[0070] The invention will now be described with reference to the following non-limiting examples. Experimental Part A. Measurement Methods
[0071] The following definitions of terms and methods of determination apply to the general description of the invention above as well as to the examples below unless defined otherwise. Flow Ratio
[0072] The melt flow ratio (MFR) was determined in accordance with ISO 1133 - Determination of the melt mass flow rate (MFR) and melt volume flow rate (MVR) of thermoplastics -- Part 1: Standard method and is indicated in g / 10 min. The MFR is an indication of the fluidity and, consequently, the processability of the polymer. The higher the melt flow ratio, the lower the viscosity of the polymer. The MFR2 of polypropylene is determined at a temperature of 230°C and a load of 2.16 kg. Microstructure Quantification by NMR Spectroscopy (Comonomer Content & Regiodefects) Petition 870250099583, dated 10 / 30 / 2025, page 46 / 109 23 / 41
[0073] Quantitative nuclear magnetic resonance (NMR) spectroscopy was additionally used to quantify comonomer content and comonomer sequence distribution of the polymers. Quantitative 13C{1H} NMR spectra were recorded in solution state using a Bruker Advance III 400 NMR spectrometer operating at 400.15 and 100.62 MHz for 1H and 13C, respectively. All spectra were recorded using a 10 mm³ extended temperature probe head optimized at 125°C using nitrogen gas for all pneumatic systems. Approximately 200 mg of material were dissolved in 3 ml of 1,2-tetrachloroethane-d2 (TCE-d2) together with chromium(III)-acetylacetonate (Cr(acac)3) resulting in a 65 mM relaxing agent solution in solvent (Singh, G., Kothari, A., Gupta, V., Polymer Testing 28 5 (2009), 475).To ensure a homogeneous solution, after initial sample preparation in a heat block, the NMR tube was further heated in a rotary oven for at least 1 hour. Upon insertion into the magnet, the tube was rotated at 10 Hz. This configuration was chosen primarily for the high resolution and quantitative requirements necessary for the accurate quantification of ethylene content. Standard single-pulse excitation was employed without NOE, using an optimized tip angle, a recycle delay of 1, and a two-level WALTZ16 decoupling scheme (Zhou, Z., Kuemmerle, R., Qiu, X., Redwine, D., Cong, R., Taha, A., Baugh, D.). Petition 870250099583, dated 10 / 30 / 2025, page 47 / 109 24 / 41 Winniford, B., J. Mag. Reson. 187 (2007) 225; Busico, V., Carbonniere, P., Cipullo, R., Pellecchia, R., Severn, J., Talarico, G., Macromol. Rapid Commun. 2007, 28, 1128). A total of 6144 (6 k) transients were acquired by the spectra.
[0074] The quantitative 13C{1H} NMR spectra were processed, integrated quantitative properties and relevant properties determined from the integrals using proprietary computer programs. All chemical shifts were indirectly referenced to the central methylene group of the ethylene block (EEE) at 30.00 ppm using solvent chemical shift. This approach allowed comparable referencing even when this structural unit was not present. Characteristic signals, corresponding to the incorporation of ethylene, were observed (Cheng, HN, Macromolecules 17 (1984), 1950).
[0075] With the characteristic signals corresponding to 2,1 erythro regio-defects observed (as described in L. Resconi, L. Cavallo, A. Fait, F. Piemontesi, Chem. Rev. 2000, 100 (4), 1253, in Cheng, HN, Macromolecules 1984, 17, 1950, and in WJ. Wang and S. Zhu, Macromolecules 2000, 33 1157), correction for the influence of regio-defects on certain properties was required. Characteristic signals corresponding to other types of regio-defects were not observed. Petition 870250099583, dated 10 / 30 / 2025, p. 48 / 109 25 / 41
[0076] The comonomer fraction was quantified using the method of Wang et al. (Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157) by integrating multiple signals across the entire spectral region in the 13C{1H} spectra. This method was chosen for its robust nature and ability to account for the presence of regio-defects when necessary. The integral regions were slightly adjusted to increase applicability across the entire range of comonomer contents found.
[0077] For systems in which only isolated ethylene in PPEPP sequences was observed, the method of Wang et al. was modified to reduce the influence of non-zero integrals from sites known to be absent. This approach reduced the overestimation of ethylene content for such systems and was achieved by reducing the number of sites used to determine the absolute ethylene content to: E = 0.5(S33 + Spy + Sβδ + 0.5(S«3 + Say))
[0078] By using this set of sites, the corresponding integral equation becomes: E = 0.5(Ih +Ig + 0.5(Ic + Id)) Using the same notation used in the article by Wang et al. (Wang, WJ., Zhu, S., Macromolecules 33 (2000), 1157). The equations used for the absolute propylene content were not modified.
[0079] Comonomer incorporation in mole percent Petition 870250099583, dated 10 / 30 / 2025, page 49 / 109 26 / 41 was calculated from the mole fraction: E [% in mol] = 100 * fE
[0080] The comonomer incorporation in weight percent was calculated from the molar fraction: E [weight percent] = 100 * (fE * 28.06) / ((fE * 28.06) + ((1-fE) * 42.08))
[0081] The comonomer sequence distribution at the triad level was determined using the analytical method of Kakugo et al. (Kakugo, M., Naito, Y., Mizunuma, K., Miyatake, T. Macromolecules 15 (1982) 1150). This method was chosen for its robust nature and slightly adjusted integration regions to increase applicability to a wider range of comonomer contents. Xylene Solubles (XCS, % by weight)
[0082] The soluble fraction of xylene (XCS) as defined and described in the present invention was determined according to ISO 16152 as follows: 2.0 g of the polymer were dissolved in 250 ml of p-xylene at 135°C under stirring. After 30 minutes, the solution was allowed to cool for 15 minutes at room temperature and then allowed to settle for 30 minutes at 25 + / - 0.5°C. The solution was filtered with filter paper into two 100 ml flasks. The solution from the first 100 ml flask was evaporated in a nitrogen stream and the residue dried under vacuum at 90°C until constant weight was achieved. The soluble fraction of xylene (percent) can be determined as follows: XCS% = (100*m*V0) / (m0*v) Petition 870250099583, dated 10 / 30 / 2025, page 50 / 109 27 / 41 m0 = initial quantity of polymer (g); m = weight of the residue (g); V0 = initial volume (ml); v = volume of the sample analyzed (ml). DSC Analysis, Melting Temperature (MT) and Crystallization Temperature (CT)
[0083] Data were measured using a TA Instrument Q2000 differential scanning calorimetry (DSC) on samples of 5 to 7 mg. DSC was performed according to ISO 11357 / part 3 / method C2 in a heat / cooling / heat cycle with a scan rate of 10 °C / min in the temperature range of -30 to +225 °C.
[0084] The crystallization temperature (Tc) and enthalpy of crystallization (Hc) were determined from the cooling stage, while the melting temperature (Tm) and enthalpy of fusion (Hm) are determined from the second heating stage. Seal Start Temperature (SIT)
[0085] The method determines the sealing temperature range (sealing range) of polypropylene films, in particular blown films or fused films. The sealing temperature range is the temperature range in which the films can be sealed according to the conditions provided below. The lower limit (thermal sealing start temperature (SIT)) is the sealing temperature at which a seal strength of 5+ / -0.5 N is achieved. The limit Petition 870250099583, dated 10 / 30 / 2025, page 51 / 109 The upper 28 / 41 (final sealing temperature (SET)) is reached when the films adhere to the sealing device. The sealing range was determined on a J&B type 3000 universal sealing machine with a 50 μm thick film produced on a three-layer fused film co-extrusion line as described below with the following additional parameters: Specimen width: 25 mm Sealing pressure: 0.67 N / mm2 Sealing time: 1 s Cooling time: 30 s Peeling speed: 42 mm / s Starting temperature: 80°C Final temperature: 150°C Increments: 5°C
[0086] The specimen is sealed A to A at each seal bar temperature and seal strength (force) is determined at each step. The temperature is determined at which the seal strength reaches 5+ / - 0.5 N. Elasticity Modulus (TM)
[0087] The modulus of elasticity in the machine direction (MD) and transverse direction (TD) was determined according to ISO 527-3 at 23°C in 50 μm cast films produced as described below. The test was performed at a tensile speed of 1 mm / min for the linear modulus range, and at 10 mm / min for larger deformations. Petition 870250099583, dated 10 / 30 / 2025, page 52 / 109 29 / 41 Opacity
[0088] Opacity was determined in accordance with ASTM D1003-00 on cast films produced as described below with a thickness of 50 µm, reported as opacity (film) or on a 1 mm injection molded specimen, reported as opacity (1 mm). The specimen used 60 x 60 x 1 mm3 was prepared in accordance with EN ISO1873-2. Cast Material Strength F30 and Cast Material Extensibility V30
[0089] The test described in this document follows ISO 16790:2005. The strain hardening behavior was determined by the method described in the article “Rheotens-Mastercurves and Drawability of Polymer Melts”, MH Wagner, Polymer Engineering and Science, Vol. 36, pages 925 to 935. The strain hardening behavior of the polymers is analyzed with a Rheotens apparatus (product of Gottfert, Siemensstr.2, 74711 Buchen, Germany) in which a molten wire is elongated by stretching with a defined acceleration. The Rheotens experiment simulates industrial spinning and extrusion processes. In principle, a molten material is pressed or extruded through a round die and the resulting wire is drawn. The stress on the extrudate is recorded as a function of the melt properties and measurement parameters (especially the ratio between the exit velocity and the drawability, practically a measure for the extension rate). For the results presented Petition 870250099583, dated 10 / 30 / 2025, p. 53 / 109 Figures 30 / 41 below show that the materials were extruded using a HAAKE Polilab laboratory extruder system and a gear pump with a cylindrical die (L / D = 6.0 / 2.0 mm). The gear pump was pre-set to a filament extrusion rate of 5 mm / s, and the melting temperature was set to 200°C. The spinline length between the die and the Rheotens wheels was 80 mm. At the start of the experiment, the winding speed of the Rheotens wheels was adjusted to the speed of the extruded polymer filament (zero tensile forces). The experiment then began by slowly increasing the winding speed of the Rheotens wheels until the polymer filament broke. The acceleration of the wheels was small enough so that the tensile forces could be measured under near-stationary conditions. The acceleration of the molten filament pulled downwards is 120 mm / s². Rheotens was operated on in combination with the PC EXTENS program.This is a real-time data acquisition program that displays and stores measured data on tensile forces and draw speed. The results of the Rheotens curve (force versus pulley rotation speed) are taken as the F30 casting strength and formability values. Crystalline and Soluble Fractions, Comonomer Content, and Intrinsic Viscosity
[0090] The crystalline (CF) and soluble (SF) fractions of polypropylene (PP) compositions as well as the content of Petition 870250099583, dated 10 / 30 / 2025, page 54 / 109 The 31 / 41 comonomer and the intrinsic viscosities (IV) of the respective fractions were analyzed using CRYSTEX QC, Polymer Char (Valencia, Spain). The crystalline and amorphous fractions were separated through temperature cycles of dissolution at 160°C, crystallization at 40°C, and redissolution in 1,2,4-trichlorobenzene (1,2,4-TCB) at 160°C. The quantification of SF and CF and the determination of the ethylene content (C2) were achieved via an infrared detector (IR4) and a 2-capillary online viscometer, which was used for the determination of intrinsic viscosity (IV). The IR4 detector is a multi-wavelength detector that detects IR absorbance in two different bands (CH3 and CH2) for the determination of ethylene concentration and content in ethylene-propylene copolymers.The IR4 detector is calibrated with a series of 8 EP copolymers with known ethylene content ranging from 2% by weight to 69% by weight (determined by 13C-NMR spectroscopy) and various concentrations between 2 and 13 mg / ml for each EP copolymer used for calibration. The amount of soluble fraction (SF) and crystalline fraction (CF) were correlated through XS calibration for the amount of "Soluble Cold Xylene" (XCS) and, respectively, Insoluble Cold Xylene (XCI) fractions, determined according to the standard gravimetric method according to ISO16152. XCS calibration was achieved by testing various EP copolymers with XS content ranging from 2 to 31% by weight. The intrinsic viscosity (IV) of the copolymer. Petition 870250099583, dated 10 / 30 / 2025, page 55 / 109 32 / 41 The original EP and its soluble and crystalline fractions were determined using a 2-capillary online viscometer and correlated to corresponding IVs determined by the standard decalin method according to ISO 1628. Calibration was achieved with various EP-PP copolymers with IV = 2 to 4 dL / g. A sample A of the PP composition to be analyzed was weighed at concentrations of 10 mg / ml to 20 mg / ml. After automated filling of the flask with 1,2,4TCB containing 250 mg / l of 2,6-tert-butyl-4-methylphenol (BHT) as an antioxidant, the sample was dissolved at 160°C until complete dissolution was achieved, usually for 60 min, with constant stirring at 800 rpm. A defined volume of the sample solution was injected into the column filled with inert support where sample crystallization and separation of the soluble fraction from the crystalline part was occurring. This process was repeated twice.During the first injection, the entire sample is measured at high temperature, determining the IV [dl / g] and C2 [% by weight] of the PP composition. During the second injection, the soluble fraction (at low temperature) and the crystalline fraction (at high temperature) with the crystallization cycle are measured (% by weight of SF, % by weight of C2, IV). EP stands for ethylene propylene copolymer. PP stands for polypropylene. Hot Soluble Hexane (C6 FDA, % by weight) FDA Section 177.1520
[0091] 1 g of a 50 gm polymer film of Petition 870250099583, dated 10 / 30 / 2025, pp. 56 / 109 A 33 / 41 thickness, as described in the experimental section, was added to 400 ml of hexane at 50°C for 2 hours during stirring with a reflux chiller. After 2 hours, the mixture was immediately filtered through No. 41 filter paper. The precipitate was collected in an aluminum container and the residual hexane was evaporated in a steam bath under a flow of N2.
[0092] The amount of soluble hexane was determined by the formula below: ((sample weight + crucible weight)-(crucible weight)) / (sample weight)'100. Glass Transition Temperature (TG) and Storage Modulus (G')
[0093] The glass transition temperature Tg and storage modulus G'(23°C) were determined by dynamic mechanical analysis (DMA) according to ISO 6721-7. Measurements were made in torsion mode on compression-molded samples (40 x 10 x 1.0 mm3) between -100°C and +150°C with a heating rate of 2°C / min and a frequency of 1 Hz. Intrinsic Viscosity
[0094] Intrinsic viscosity was measured according to DIN ISO 1628 / 1 and / 3, October 1999 (in Decalina at 135°C). The intrinsic viscosity (IV) value increases with the molecular weight of a polymer. Flexural Module
[0095] The flexural modulus is determined according to ISO 178. The test specimens have dimensions of 80 x 10 Petition 870250099583, dated 10 / 30 / 2025, p. 57 / 109 34 / 41 x 4.0 mm3 (length x width x thickness) and are prepared by injection molding according to EN ISO 1873-2. The extension length between the supports is 64 mm and the test speed is 2 mm / min. Impact Resistance with Charpy Notch
[0096] Charpy notch impact resistance was determined in accordance with ISO 179 1eA at 23°C using 80x10x4 mm3 injection molded test bars in accordance with EN ISO 1873-2. B. Materials Used
[0097] AO is commercially available Irganox® B 215 from BASF (synergistic processing and long-term thermal stabilizing system. It is a blend of Irgafos® 168 and Irganox® 1010).
[0098] CaSt is calcium stearate, commercially available under the trade name CEASIT AV FI from Bärlocher. Reactive Modification for LCB PP (Component B)
[0099] The base polymer used was a polypropylene homopolymer with MFR2 0.23 g / 10 min, produced by Borealis with Advant ZN180M with a single circulation type reactor. The final MFR2 is adjusted by using H2 applying methods well known to those skilled in the art. The typical polymerization configuration used was as follows: reactor temperature 70°C, 125 ppm H2, Teal / C3 180 g / t C3, Teal / donor 6 / 1 wt% / wt%.
[00100] The reactive modification of the polymer powders was Petition 870250099583, dated 10 / 30 / 2025, pp. 58 / 109 35 / 41 performed according to the process description in document EP 2520425. Both butadiene (BD) and peroxide (POX) were premixed with the polymer powder before the melt mixing step in a horizontal mixer with paddle agitator at a temperature of 65°C, maintaining an average residence time of 15 minutes. The premix was transferred under an inert atmosphere to a Theyson TSK60 co-rotational twin-screw extruder, having a barrel diameter of 60 mm and an L / D ratio of 48, equipped with a high-intensity mixing screw having three kneading zones and a two-stage degassing configuration. A melt temperature profile was selected with an initial temperature T1 = 240°C in the feed zone, a maximum temperature T2 = 280°C in the last kneading zone, and a final temperature T3 = 230°C in the die zone, all temperatures being defined as barrel temperatures. The screw speed was set to 350 rpm.The recipe consisted of 0.45% by weight of TRIGONOX BPIC-C75, 0.1% by weight of BD, 0.13% by weight of AO, and 0.1% by weight of CaSt. LCB PP has a density of 905 kg / m³ determined according to ISO 1183, a melt flow rate (230°C / 2.16 kg) of 10 g / 10 min determined according to ISO 1133, an F30 of 31.2 cN, and a V30 of 266 mm / s determined according to ISO 16790.
[00101] Polypropylene (PP HECO1, heterophasic propylene random copolymer) was prepared as follows. Petition 870250099583, dated 10 / 30 / 2025, pp. 59 / 109 36 / 41 Catalytic System for PP HECO1 Catalytic Complex
[00102] The following metallocene complex was used as described in document WO 2019 / 179959 in IE2. Preparation of Silica Support by MAO
[00103] A steel reactor, equipped with a mechanical stirrer and a filter screen, was washed with nitrogen and the reactor temperature was set to 20°C. Then, pre-calcined silica grade DM-L-303 from AGC Si-Tech Co. (5.0 kg) was added from a feed drum followed by careful pressurization and depressurization with nitrogen using manual valves. Next, toluene (22 kg) was added. The mixture was stirred for 15 min. Then, 30% by weight of Lanxess' MAO-in-toluene solution (9.0 kg) was added via the feed line at the top of the reactor within 70 min. The reaction mixture was then heated to 90°C and stirred at that temperature for an additional two hours. The fluid paste was allowed to settle and the mother liquor was filtered. The catalyst was washed twice with toluene (22 kg) at 90°C, followed by settling and filtration. The reactor was cooled to 60°C and the solid was washed with heptane (22.2 kg).Finally, MAO-treated SiO2 was dried at 60°C under a nitrogen stream for 2 hours and then for 5 hours under vacuum (-0.5 barg) with stirring. The MAO-treated support was collected as a free-flowing white powder found to contain 12.2% by weight. Petition 870250099583, dated 10 / 30 / 2025, pp. 60 / 109 37 / 41 weight of Al. Preparation of the Single-Site Catalyst System
[00104] 30% by weight of MAO in toluene (0.7 kg) was added to a nitrogen-covered steel reactor via a burette at 20°C. Toluene (5.4 kg) was then added with stirring. The metallocene complex as described above (93 g) was added from a metal cylinder followed by washing with 1 kg of toluene. The mixture was stirred for 60 minutes at 20°C. Trityl tetrakis(pentafluorophenyl)borate (91 g) was then added from a metal cylinder followed by washing with 1 kg of toluene. The mixture was stirred for 1 h at room temperature. The resulting solution was added to a stirred silica support cake prepared as described above for 1 hour. The cake was left to stand for 12 hours, followed by drying under a stream of nitrogen at 60°C for 2 hours and additionally for 5 hours under vacuum (-0.5 barg) with stirring.
[00105] The polymerization for the preparation of the PPHECO1 invention polymer was carried out in a Borstar pilot plant with a configuration of 3 reactors (circulating gas phase reactor (GPR 1) - gas phase reactor (GPR 2) and a pre-polymerizer), using the catalyst system as described above.
[00106] In Table 1, the polymerization conditions for PP HECO1 and the final resin properties are Petition 870250099583, dated 10 / 30 / 2025, pp. 61 / 109 38 / 41 provided. TABLE 1: Polymerization Conditions for PP HECO1 and the Final Properties. Prepolymerizer Unit GPR2 Unit Temperature °C 20.0 Temperature °C 70 H2 / C3 mol / kmol 0.07 % by weight kg / h Pressure barg 25 Pressure barg 53 C2 / C3 mol / kmol 457 g / h 6.5 H2 / C2 mol / kmol 3.1 Circulation GPR Division % 25 MFR g / 10 min 278.0 Final Powder Temperature °C 75 SF % by weight 26.37 H2 / C3 mol / kmol 0.76 C2 content % by weight 3.32 mol / kmol C2(SF) % by weight 10.5 XS % by weight 1.20 C2(CF) % by weight 0 DSC Tm °C 153 IV(SF) dl / g 3.15 DSC Tcr. °C 117 IV(CF) dl / g 1.08 Matrix division % 42 Tm °C 152 GPR1 MFR g / 10 min 21.6 MFR g / 10 min 172 G' MPa 450 Temperature °C 80 Tg1 °C 0 Pressure barg 22 Tg2 °C -22 H2 / C3 mol / kmol 2.86 XS % by weight 0.80 DSC Tm °C 152 DSC Tcr. °C 115 Matrix division % 33 Petition 870250099583, dated 10 / 30 / 2025, pp. 62 / 109 39 / 41
[00107] Polypropylene (PP HECO2, heterophasic propylene random copolymer) was prepared as described in document WO 2016 / 066453 A2. PP HECO2 is CE2 according to document WO 2016 / 066453 A2 (see page 36 for the catalyst (Ziegler-Natta catalyst) and Table 4 on page 39 for the polymerization conditions). The polymer powders (PP HECO1 and PP HECO2) were processed in a Coperion ZSK 57 co-rotating twin-screw extruder at 220°C using the recipe shown in Table 2. C. Film Manufacturing
[00108] The fused films according to the Invention Example (IE1) and the Comparative Examples (CE1 and CE2) were produced on a Collin 30 fused film line, with a melting temperature of 240°C and a cooling roll temperature of 20°C. The films obtained all had a total thickness of 50 µm. D. Results and Discussion TABLE 2: Compositions, Films and Properties. Component Unit IE1 CE1 CE2 HECO1 (A) % by weight 49.7 1.75* 99.7 HECO2 % by weight - 39.75 - LCB PP (B) % by weight 50 58.20 - AO % by weight 0.25 0.25 0.25 CaSt % by weight 0.05 0.05 0.05 Composition of properties mfr2 g / 10 min 14 10 19 F30 cN 4 4 1 V30 mm / s 247 244 146 xcs % by weight 14.97 13.35 nm IV(XCS) dl / g 3.11 2.48 nm Flexural modulus MPa 1272 1448 730 Petition 870250099583, dated 10 / 30 / 2025, pp. 63 / 109 40 / 41 NIS / 23°C kJ / m2 5.3 7.1 5.8 Opacity (1 mm) % 49.7 93 45.5 C6 FDA % by weight 1.4 2.2 1.1 06 FDA / XCS1 0.09 0.16 na Properties 50 pm Melt film TM (MD) MPa 441 770 146 TM (TD) MPa 456 713 166 SIT °C 129 133 123 Opacity (film) % 14.7 37 43 nm = not measured; na = not available; *used as a vehicle for AO and CaSt.
[00109] 2C6 FDA / XCS is the ratio of C6 FDA to XCS
[00110] As can be seen from Table 2, the polymer composition according to the invention example IE1, produced using a single-site catalyst, has a clear indication of long-chain branching (LCB) expressed by the molten material strength F30 and molten material extensibility V30. Another merit obtained by adding component (B) in the invention example is the stiffness (1272 MPa vs. 730 MPa) of the polymer composition, which is significantly increased with only a small loss of hardness (5.3 kJ / m2 vs. 5.8 kJ / m2), while the polymer composition according to CE1 has a hardness reduction of about 80% (7.1 kJ / m2 vs. 33 kJ / m2, see reference above CE2 in document WO 2016 / 066453 A2) by adding component (B). The polymeric composition according to the IE also has higher purity and significantly fewer extractables. This is reflected by the total extractables (C6 EDA) and also by the C6 EDA to XCS ratio. Furthermore, the film made from the composition... Petition 870250099583, dated 10 / 30 / 2025, pp. 64 / 109 The 41 / 41 polymeric material according to the present invention exhibits very low opacity, a very good sealing start temperature, and an excellent balance between the strength and opacity of the molten material.
Claims
1. Polymer composition characterized in that it comprises at least the following components: A) 30.0 to 80.0% by weight based on the total weight of the polymer composition of a heterophasic C2C3 copolymer produced by a single-site catalyst (HECO); such that said copolymer has: • a melting point in the range of 150 to 162°C determined by differential scanning calorimetry according to ISO 11357-3; • an MFR2 (230°C, 2.16 kg) determined according to ISO 1133 in the range of 5.0 to 40.0 g / 10 min; • a total C2 content in the range of 1.0 to 10.0% by weight based on the total weight of component (A); and • a soluble fraction (SF) based on the total weight of component (A) in the range of 10.0 to 50.0% by weight analyzed by fractionation by crystallization with infrared detection, in accordance with ISO 16152:2022; B) 20.0 to 70.0% by weight based on the total weight of the polymeric composition of a propylene homopolymer;such that the said propylene homopolymer has: • an MFR2 (230°C, 2.16 kg) determined according to ISO 1133 in the range of 1.0 to 20.0 g / 10 min; and • a molten material strength F30 determined according to ISO 16790 of at least 10 cN; Petition 870260086694, dated 25 / 08 / 2026, p. 12 / 26 2 / 7 on the condition that the weight proportions of components A) and B) add up to 100% by weight.
2. Polymer composition, according to claim 1, characterized in that: component (A) has a melting point determined by differential scanning calorimetry according to ISO 11357-3 in the range of 151 to 160°C, preferably in the range of 151 to 155°C and more preferably in the range of 151 to 154°C; and / or component (A) has an MFR2 (230°C, 2.16 kg) determined according to ISO 1133 in the range of 10.0 to 30.0 g / 10 min, preferably in the range of 15.0 to 25.0 g / 10 min and more preferably in the range of 20.0 to 23.0 g / 10 min; and / or component (A) has a total C2 content in the range of 1.0 to 8.0% by weight, preferably in the range of 1.5 to 6.0% by weight and more preferably in the range of 2.5 to 4.0% by weight based on the total weight of component (A);and / or component (A) has a soluble fraction (SF) based on the total weight of component (A) in the range of 15.0 to 40.0% by weight, preferably in the range of 20.0 to 30.0% by weight and most preferably in the range of 24.0 to 28.0% by weight, analyzed by fractionation by crystallization with infrared detection, in accordance with ISO 16152:2022.; 3. Polymer composition, according to claim 1 or 2, characterized in that: Petition 870260086694, dated 08 / 25 / 2026, page 13 / 26 3 / 7 component (A) has a C2 content of the soluble fraction (SF) based on the total weight of the soluble fraction in the range of 5 to 40% by weight, preferably in the range of 8 to 30% by weight, more preferably in the range of 8 to 25% by weight and even more preferably in the range of 9 to 12% by weight, analyzed by fractionation by crystallization with infrared detection, according to ISO 16152:2022; and / or component (A) has a C2 content of the crystalline fraction (CF) based on the total weight of the crystalline fraction that is below 4% by weight, preferably below 2% by weight, more preferably in the range of 0 to 1% by weight and even more preferably is 0% by weight, analyzed by fractionation by crystallization with infrared detection, according to ISO 16152:2022;and / or component (A) has an intrinsic viscosity (IV) of the soluble fraction (SF) that is in the range of 1.0 to 5.0 dl / g, preferably in the range of 2.0 to 4.0 dl / g, more preferably in the range of 2.2 to 3.4 dl / g and even more preferably in the range of 3.0 to 3.3 dl / g, analyzed by fractionation by crystallization with infrared detection, in accordance with ISO 16152:2022; and / or component (A) has an intrinsic viscosity (IV) of the crystalline fraction (CF) that is in the range of 0.5 to 4.0 dl / g, preferably in the range of 0.8 to 2.0 dl / g and more preferably in the range of 1.0 to 1.2 dl / g, analyzed by fractionation by crystallization with infrared detection, in accordance with ISO 16152:2022.
4. Polymer composition, according to any of the preceding claims, characterized in that: component (B) has an MFR2 (230°C, 2.16 kg) determined according to ISO 1133 in the range of 1.0 to 15.0 g / 10 min, preferably in the range of 3.0 to 15.0 g / 10 min, more preferably in the range of 6.0 to 14.0 g / 10 min and even more preferably in the range of 8.0 to 12.0 g / 10 min; and / or component (B) has a melt strength F30 determined according to ISO 16790 of at least 20 cN, preferably of at least 30 cN and more preferably in the range of 30 to 60 cN; and / or component (B) has a molten material extensibility v30 determined in accordance with ISO 16790 of at least 200 mm / s, preferably at least 250 mm / s and more preferably in the range of 250 to 300 mm / s;and / or component (B) has a density determined according to ISO1183 in the range of 895 to 920 kg / m3, preferably in the range of 900 to 910 kg / m3 and most preferably in the range of 904 to 906 kg / m3.; 5. Polymer composition, according to any of the preceding claims, characterized in that: the polymer composition has an MFR2 (230°C, 2.16 kg) Petition 870260086694, dated 08 / 25 / 2026, p.15 / 26 5 / 7 determined according to ISO 1133 in the range of 4.0 to 30.0 g / 10 min, preferably in the range of 8.0 to 20.0 g / 10 min and more preferably in the range of 12.0 to 16.0 g / 10 min; and / or the polymer composition has a melt strength F30 determined according to ISO 16790 of at least 2 cN, preferably of at least 3 cN and more preferably in the range of 3 to 5 cN; and / or the polymer composition has a molten material extensibility v30 determined according to ISO 16790 of at least 200 mm / s, preferably at least 230 mm / s, more preferably in the range of 240 to 300 mm / s and even more preferably in the range of 240 to 260 mm / s; and / or the polymer composition has an MFR2 (230°C, 2.16 kg) determined according to ISO 1133 in the range of 12.0 to 16.0 g / 10 min and an F30 determined according to ISO 16790 in the range of 3 to 5 cN.
6. Polymer composition, according to any of the preceding claims, characterized in that: component (A) was produced in the presence of a metallocene catalyst.
7. Polymer composition, according to any of the preceding claims, characterized in that: Petition 870260086694, dated 08 / 25 / 2026, p. 16 / 26 6 / 7 the polymer composition comprises at least one additive C), preferably selected from the group consisting of slip agents, acid scavengers, UV stabilizers, pigments, antioxidants, additive carriers, nucleating agents and mixtures thereof, such that these additives are preferably present in 0.1 to 5.0% by weight and more preferably in 0.1 to 4.0% by weight based on the total weight of the polymer composition.
8. A film characterized in that it comprises the polymeric composition as defined in any one of claims 1 to 7, and preferably consists of this polymeric composition.
9. Film, according to claim 8, characterized in that: the film has a modulus of elasticity determined according to ISO 527-3 at 23°C in a fused film having a thickness of 50 µm in the machine direction, as well as in the transverse direction in the range of 200 to 1000 MPa, preferably in the range of 300 to 700 MPa and more preferably in the range of 400 to 500 MPa.
10. Film, according to claim 8 or 9, characterized in that: the film has a sealing start temperature in a molten film having a thickness of 50 µm in the range of 100°C to below 140°C, preferably in the range of 120°C to 135°C, more preferably in the range of 120°C to 132°C and even more preferably in the range of 128 to 130°C.
11. Film, according to any one of claims 8 to 10, characterized in that: the film has an opacity determined according to ASTM D1003-00 in a fused film having a thickness of 50 µm in the range of 5 to below 20%, preferably in the range of 8 to 16% and more preferably in the range of 10 to 15%.
12. Coated article characterized in that it comprises at least one layer comprising the polymeric composition, as defined in any one of claims 1 to 7, preferably the layer consisting of this polymeric composition.
13. Coated article, according to claim 12, characterized in that: the article is an extrusion-coated article.
14. Process for manufacturing the coated article, as defined in claim 12, characterized in that it comprises an extrusion coating step.
15. Use of the coated article, as defined in claim 12 or 13, characterized in that it is used as packaging material, preferably as a temperature-resistant packaging material for food and / or medical products.