MÉTODO DE FABRICAÇÃO DE AÇO
The electric furnace with a hydrogen-based burner and powdered auxiliary material addresses high costs and emissions by enhancing heat transfer and preventing slag solidification, achieving efficient and sustainable steel production.
Patent Information
- Application Number
- BR112023022801
- Authority / Receiving Office
- BR · BR
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-05-07
- Filing Date
- 2022-04-08
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-04-08
AI Technical Summary
Conventional steelmaking methods using electric furnaces face challenges such as high investment and maintenance costs due to complex installations, slag solidification issues, and increased CO2 emissions, particularly when using hydrogen gas as a fuel with high combustion rates and flame temperatures.
An electric furnace with a burner that jets hydrogen gas or a hydrogen-enriched gaseous fuel, accompanied by a powdered auxiliary material, such as lime, to form a burner flame that heats the cold iron source efficiently, reducing electrical energy consumption and CO2 emissions.
The method enhances heat transfer efficiency, reduces electrical energy use, prevents slag solidification, and lowers CO2 emissions while maintaining furnace durability, thus improving operational stability and environmental impact.
Abstract
Description
1 / 23 STEEL MANUFACTURING METHOD TECHNICAL FIELD
[001] The present invention relates to a technique for melting a cold iron source using a heat source with reduced CO2 emissions to decrease greenhouse gas emissions in the production of iron and steel products. TECHNICAL BACKGROUND
[002] From the perspective of preventing global warming, techniques have recently been developed in the iron and steel industry to reduce CO2 emissions by decreasing the amount of fossil fuel consumption. In existing integrated steel mills, molten pig iron is produced by reducing iron ore with carbon. The production of this molten pig iron requires approximately 500 kg of a carbon source per 1 t of molten pig iron to reduce the iron ore or similar materials. In contrast, when producing cast steel with a cold iron source, such as scrap iron, as raw material, the carbon source needed to reduce the iron ore is not required, while only energy with a sufficient amount of heat to melt the cold iron source is required. Consequently, CO2 emissions can be substantially reduced.
[003] For an operation with a high content of a cold iron source, an electric furnace, such as an arc furnace or an induction melting furnace, is frequently used, in which most of the heat to melt the cold iron source is supplied by electrical power. To reduce the consumption of electrical power units, the arc furnace is operated by adopting the following techniques: (1) an auxiliary burner is provided in the furnace wall or in the slag removal door to promote the melting of the cold iron source at a cold point and the like; (2) a so-called oxygen-enriched operation to provide Petition 870260090227, dated 02 / 09 / 2026, page 10 / 35 2 / 23 Oxidation heat to iron is achieved by feeding oxygen through an oxygen gas feed lance; and (3) the heat transfer efficiency from an arc to the molten steel is improved by feeding oxygen and carbon powder from an oxygen gas feed lance and a carbon injection lance, respectively, causing slag foaming to cover the arc.
[004] However, oxygen-enriched operation has the problem of a decrease in yield accompanied by the loss of iron oxidation. Furthermore, most auxiliary burners use hydrocarbons as a fuel. Slag frothing operation generates CO2 gas by blowing carbon dust into the slag. These techniques can decrease unit consumption of electrical energy, but have a small effect on reducing CO2 emissions. Firstly, when the electrical energy used is obtained from a fossil fuel, CO2 will also be emitted from the use of electrical energy. Therefore, to further reduce CO2 emissions, it is desirable to improve heat efficiency and increase the use of energy sources with reduced CO2 emissions.
[005] Even if we can obtain electrical energy with reduced CO2 emissions and replace the electrical energy we use with it in the future, the need for techniques to reduce unit consumption of electrical energy will remain unchanged. Thus, these techniques also need to aim at reducing CO2 emissions. For example, hydrogen gas produced from renewable energy or other sources can be used as a fuel for an auxiliary burner or similar; however, hydrogen gas has a higher combustion rate and a higher flame temperature compared to hydrocarbon gas and other gases, which presents a problem. Below are some known techniques to solve this problem. Petition 870260090227, dated 02 / 09 / 2026, page 11 / 35 3 / 23
[006] For example, both Patent Literature 1 and Patent Literature 2 propose a technique for lowering the flame temperature by providing an additional combustion space upstream of a main combustion space to reduce the oxygen concentration therein. Additionally, Patent Literature 3 proposes a method for lowering the flame temperature by maintaining a distance between a hydrogen gas feed flow path and a combustion air feed flow path, thus preventing hydrogen gas from mixing with combustion air to decrease the combustion rate.
[007] Additionally, as a source of cold iron to be smelted, not only scrap iron but also reduced solid iron, which is produced using a reducing agent with reduced CO2 emissions, is expected to be used in greater quantities. LIST OF QUOTES PATENTARY LITERATURE
[008] Patent Literature 1: JP-A-2020-46098 Patent Literature 2: JP-A-2021-25713 Patent Literature 3: JP-A-2020-46099 SUMMARY OF THE INVENTION TECHNICAL PROBLEM
[009] Conventional techniques have the following problems.
[010] The methods described in Patent Literatures 1 to 3 have a complicated and large installation structure, which brings a problem of increased investment costs for facilities and maintenance costs if applied to an electric steelmaking furnace. Furthermore, reduced solid iron typically contains gangue components, such as SiO2, Al2O3, derived from iron ore being its raw material. Therefore, a Petition 870260090227, dated 02 / 09 / 2026, p. 12 / 35 4 / 23 A large amount of slag can be produced during the melting process, causing operational difficulties, such as slag solidification in a furnace.
[011] The present invention is made in view of such background and aims to provide an electric furnace that can obtain cast iron by melting a cold iron source using electrical energy and a heat source with reduced CO2 emissions. The invention also proposes a steelmaking method that uses an electric furnace and a heat source with reduced CO2 emissions to melt a cold iron source. The present invention further proposes a steelmaking method that can stably melt reduced solid iron as the cold iron source. SOLUTION TO THE PROBLEM
[012] An electric furnace of the present invention can advantageously solve the aforementioned problems and obtain cast iron by melting a cold iron source using electrical energy. The electric furnace is characterized in that: the electric furnace is provided with a burner directed towards the furnace contents; the burner comprises a powder feed tube, a jet hole for jetting a fuel and a jet hole for jetting combustion support gas; a burner flame is formed by jetting hydrogen gas or a hydrogen-enriched gaseous fuel as the fuel; and an auxiliary material that is in powder form or is processed in powder form is jetted through the powder feed tube, so that the auxiliary material passes through an interior of the burner flame.
[013] Additionally, the electric furnace of the present invention is preferably a DC arc furnace, an AC arc furnace or an induction melting furnace to solve the above problems. Petition 870260090227, dated 02 / 09 / 2026, p. 13 / 35 5 / 23
[014] A steelmaking method of the present invention can advantageously solve the aforementioned problems and obtain cast iron by melting a cold iron source using electrical energy in an electric furnace. The steelmaking method is characterized in that: the electric furnace is provided with a burner comprising a jet hole for jetting a fuel and a jet hole for jetting combustion support gas and which jets a flame through the jet holes towards an interior of the electric furnace; and for at least part of the duration of operation of an electric furnace run, hydrogen gas or a hydrogen-enriched gaseous fuel is used as the burner fuel, and an auxiliary material that is in a powder form or is processed into a powder form is blown through an interior of the flame formed by the burner.
[015] The steel manufacturing method of the present invention can provide more preferable solutions to the following problems: (1) The cold iron source comprises reduced solid iron; (2) The raw material that is in powder form or is processed in powder form is powdered lime; and (3) the electric furnace is a DC arc furnace, an AC arc furnace or an induction melting furnace. ADVANTAGEOUS EFFECTS OF THE INVENTION
[016] According to the present invention, the powdered material is heated in the burner flame because it is fed through the burner flame and serves as a heat transfer medium. Therefore, the combustion heat from the burner can be used to heat the cold iron source in the electric furnace with high efficiency, decreasing the amount of electrical energy used. Furthermore, using hydrogen gas as fuel can reduce CO2 emissions. Additionally, the flame temperature is lowered because the sensible heat of Petition 870260090227, dated 02 / 09 / 2026, page 14 / 35 6 / 23 of the burner's combustion gas is consumed to heat the powdered material in the burner flame, ensuring the durability of a burner nozzle and preventing wear on the refractory lining of the electric furnace body.
[017] In the present invention, powdered lime heated by a burner flame is blown over the slag resulting from the melting of reduced solid iron to heat the slag and lower its melting point. This can improve slag formation and prevent malfunctions caused by slag solidification. In particular, when using an induction melting furnace such as an electric furnace, the slag is not directly heated because no induction current is generated in it, and thus slag solidification is easily caused. The present invention significantly improves this problem. BRIEF DESCRIPTION OF THE DRAWINGS
[018] FIG. 1 is a schematic vertical cross-sectional view showing a schematic configuration of an AC arc furnace, as an electric furnace according to an embodiment of the present invention.
[019] FIG. 2 is a schematic vertical cross-sectional view showing a schematic configuration of an induction melting furnace, such as an electric furnace according to another embodiment of the present invention.
[020] FIG. 3 is a schematic vertical cross-sectional view of a burner lance tip end portion used in the above embodiments. DESCRIPTION OF THE MODALITIES
[021] Embodiments of the present invention will be described in detail below. The drawings are schematic and may differ from reality. Furthermore, the embodiments below illustrate examples of devices and methods for incorporating technical concepts of the present invention and are not intended to be... Petition 870260090227, dated 02 / 09 / 2026, page 15 / 35 7 / 23 specify configurations of those described below. In other words, the technical concepts of the present invention can be modified in various ways within the technical scope set forth in the claims.
[022] FIG. 1 is a schematic vertical cross-sectional view showing a configuration of an AC 101 arc furnace, as an electric furnace according to an embodiment of the present invention and indicates a mode of operation using the AC electric arc furnace. In the present embodiment, a burner lance 1 is inserted through a burner lance insertion hole provided in a furnace lid so as to move up and down. Although FIG. 1 shows an example in which the burner lance 1 is inserted through the furnace lid so as to move up and down perpendicularly, possible embodiments are not limited to this example. The burner lance 1 may be inserted diagonally from the top of a furnace wall towards a furnace interior.Additionally, the burner is not limited to one type of lance that can move up and down and may have a configuration such that the nozzle part is fixed to the furnace lid or a furnace wall. Furthermore, in addition to the burner, for example, an oxygen blowing lance inserted from a slag removal door may be provided. The burner may have an oxygen blowing function so that oxygen is blown from the burner. The burner lance 1 blasts a burner flame 7 towards the surface of the furnace contents, such as a cold iron source 2 or molten iron 3 housed in a furnace body 9. The AC 101 arc furnace shown in the drawing has three graphite electrodes 5. Agitation can be performed by blowing gas from the bottom of the furnace. Additionally, the furnace body 9 has a vent hole. The furnace lid has an exhaust gas duct (not shown) installed in it. FIG. 1 shows one state. Petition 870260090227, dated 02 / 09 / 2026, p. 16 / 35 8 / 23 in which the reduced solid iron, in which it was loaded as cold iron source 2, is being melted by the application of an electric current. At this moment, an auxiliary powder material 8 is blown from the burner lance 1 through the burner flame 7, so as to promote the melting of the cold iron source 2. This operation preferably uses a fuel composed mainly of hydrogen gas that is produced with renewable energy, such as solar energy, wind energy or hydropower. The fuel containing hydrogen gas composed mainly of hydrogen gas denotes hydrogen gas or a hydrogen-enriched gaseous fuel. The hydrogen-enriched gaseous fuel may use a gas mixture in which hydrogen gas is mixed with methane gas, natural gas or petroleum gas. From the point of view of CO2 reduction, it is desirable that the gas mixture contain hydrogen gas at 50% by volume or more.
[023] The above embodiment uses an AC 101 arc furnace having three electrodes as an electric furnace and can also use a DC arc furnace having an upper electrode and a lower electrode. When using the AC 101 arc furnace, which has electrodes 5 and an arc in a central part of the furnace body 9, as an electric furnace, the possible installation positions of the burner lance 1 are limited. As described later, the burner of the present embodiment can lower the temperature of the burner flame 7 by adequately blowing the powdered auxiliary material 8, even when using fuel whose main component is hydrogen gas, achieving operation without wear on the water cooling panel on the furnace wall, refractories on the furnace floor, etc.
[024] FIG. 2 is a schematic vertical cross-sectional view showing a configuration of an induction melting furnace 102 as an electric furnace according to another embodiment of the present invention and indicates Petition 870260090227, dated 02 / 09 / 2026, p. 17 / 35 9 / 23 A mode of operation using the induction melting furnace. The burner lance 1 of the present embodiment is inserted through a burner lance insertion hole provided in a furnace lid so as to move up and down. The burner is not limited to one type of lance that can move up and down and may have a configuration such that the nozzle part is fixed to the furnace lid or to a furnace wall. The burner lance 1 sprays the burner flame 7 towards the surface of the cold iron source 2 or the molten iron 3 housed in the furnace body 9. The induction melting furnace 102 shown in the drawing has a coil 6 for induction heating, for example. Agitation can be performed by blowing gas from the bottom of the furnace. The furnace body 9 has a vent door. FIG.Figure 2 shows a state in which reduced solid iron, which has been charged as cold iron source 2, is being melted by induction heating using an electric current. At this point, a powdered auxiliary material is blown from burner lance 1 through the burner flame to promote the melting of the cold iron source 2 and improve the slag composition. Specifically, powdered lime is blown onto the slag as powdered auxiliary material 8 from the burner to dilute SiO2 and AkOs contained in the reduced solid iron, lowering the melting point of the slag. It is also desirable to use a fuel composed mainly of hydrogen gas that is produced with renewable energy in this operation as described above.
[025] FIG. 3 is a schematic view of a tip end portion 10 as an example of an embodiment of the burner lance 1 used in the aforementioned embodiment. A powder feed tube 11 having a jet hole is disposed in the center, and a fuel feed tube 12 and a combustion support gas feed tube 13, each having Petition 870260090227, dated 02 / 09 / 2026, page 18 / 35 10 / 23 a jet hole, are arranged sequentially around the powder feed tube 11. An outer casing 15 comprising a cooling water passage 14 is provided on the outside thereof. The burner flame 7 is formed by feeding hydrogen gas or a hydrogen-enriched gaseous fuel as fuel gas 16 and feeding combustion support gas 17, through the jet holes provided in an outer circumferential part of the powder feed tube 11. The powder auxiliary material 8 jetted through the powder feed tube 11 is heated in the burner flame 7. The burner flame 7 is formed by feeding hydrogen gas or a hydrogen-enriched gaseous fuel serving as fuel gas 16 and combustion support gas 17, through the jet holes provided in an outer circumferential part of the powder feed tube 11.Additionally, the powdered auxiliary material 8 sprayed through the powder feed tube 11 is heated in the burner flame 7. This causes the powdered auxiliary material 8 to act as a heat transfer medium, increasing the heat transfer efficiency from the flame to the furnace contents, such as the cold iron source 2 and the cast iron 3. This can reduce the amount of electrical energy required. The combustion support gas 17 can use, in addition to pure oxygen, a gaseous mixture of oxygen with CO2 or inert gas, air, or oxygen-enriched air. Additionally, the gas carrying the powdered material 8 can be an inert gas or a combustion support gas.
[026] The above embodiment is a fully formed burner lance configured with the powder feed tube in the center and disposing of the jet hole for spraying fuel and the jet hole for spraying a combustion support gas around the powder feed tube; however, the possible forms of the burner lance are not limited to this. Petition 870260090227, dated 02 / 09 / 2026, page 19 / 35 11 / 23 example. In other words, the burner according to the present invention may be provided with a powder feed tube, a jet hole for spraying fuel, and a jet hole for spraying a combustion support gas, wherein hydrogen gas or a hydrogen-enriched gaseous fuel is sprayed as the fuel to form a burner, so that an auxiliary material sprayed through the powder feed tube passes through the interior of the burner flame. For example, it is acceptable to provide a lance integrally formed with a jet hole for spraying fuel and a jet hole for spraying combustion support gas and to separately provide a powder feed tube to be positioned adjacent to the lance, so that the auxiliary material sprayed through the powder feed tube passes through the interior of the burner flame.
[027] In a steelmaking method according to another embodiment of the present invention, for example, the cold iron source 2, such as scrap iron or reduced solid iron, is first loaded from a bucket (not shown) into an electric furnace, such as the AC 101 arc furnace shown in FIG. 1 or the induction melting furnace 102 shown in FIG. 2. After the cold iron source 2 is first loaded, an electric current is applied. The burner lance 1 installed on an upper part of the furnace is inserted into the electric furnace to heat the cold iron source 2 with electrical energy and with the burner flame 7. When the first additionally loaded cold iron source 2 melts and reaches a flat bath state, a state in which an unmelted portion, even if it exists, of the cold iron source 2 is embedded in the molten iron 3, the slag can be removed through the slag removal door as required.Then, the power and the burner can be switched off, and the oven door can be opened to charge the cold iron 2 for the second time. After the second charge... Petition 870260090227, dated 02 / 09 / 2026, page 20 / 35 12 / 23 Cold Iron Source 2, it is desirable to reapply the electric current and perform the burner heating operation in the same way after the first charge. Cold Iron Source 2 can be charged three or more times.
[028] The present inventors examined the heat transfer efficiency to the furnace contents and the durability of the burner lance nozzle using the electric furnace shown in FIG. 1 or FIG. 2 and varying the fuel gas flow rate and the powder material feed rate. As a result, we found that the heat transfer efficiency to the furnace contents can be increased and the combustion flame temperature can be decreased by feeding powder material 8 in a sufficient quantity relative to a heat-generating quantity of fuel gas 16.When the ratio of powder material to fuel gas expressed as “powder material feed rate” / amount of fuel gas heat generation is 0.41 (kg / MJ) or more, the flame temperature is approximately 1500 °C or lower, which can reduce the thermal loads on the water cooling panel in the furnace wall, on the refractories in the furnace floor, and on the burner lance nozzle.
[029] The powdered material may use: a slag-forming agent which is the powder or powdered auxiliary material 8; dust; or the like. Efficient heating of the powdered material in the burner flame involves increasing the specific surface area and therefore the particle size is preferably approximately 100 µm or less. Auxiliary material with a larger particle size is preferably processed to have a particle size of approximately 100 µm or less. In this case, the particle size is expressed by the 50% volume pass rate.
[030] Cold iron source 2 preferentially uses scrap iron and / or solid iron reduced by using a reducing agent with lower emissions of Petition 870260090227, dated 02 / 09 / 2026, page 21 / 35 13 / 23 CÜ2. Some reduced solid iron contains S1O2 and Al2O3 in approximately 10 to 20% by mass as gangue components derived from iron ore, depending on its grade. When reduced solid iron is melted, these substances form slag 4, which appears on the bath surface of the molten iron 3. Slag has a high melting point composition and therefore would easily solidify and adhere to the furnace wall, which can interfere with operation. Especially when using the induction melting furnace 102, the slag is not heated by induction, which can cause slag solidification.
[031] It is preferable to use lime as an auxiliary powder material 8 to be heated by the burner and fed, because it can control the basicity (i.e., the CaO / SiO2 ratio by mass) of the slag to be approximately 1.0. Thus, the melting point of the slag can be lowered to prevent slag solidification. The slag is heated by the heated powder material, which achieves the advantageous effect of promoting slag formation. After slag formation, the slag can be removed or dumped during melting or before flow by tilting the arc furnace body or induction melting furnace.
[032] Additionally, any type of electric furnace is applicable, provided it can melt the cold iron source with electrical energy to obtain molten iron. For example, electric furnaces include, in addition to AC or DC arc furnaces, a submerged arc furnace that applies heat by submerging a Soederberg self-cooking electrode or similar into the slag; an indirect type resistance furnace that heats an object to be heated by radiation from a heat-generating body supplied in the furnace, convection in the furnace and / or conductive heat transfer; and a plasma arc melting furnace.
[033] The cast iron 3 cast in the present embodiment has a Petition 870260090227, dated 02 / 09 / 2026, page 22 / 35 14 / 23 composition equivalent to the metallic composition of scrap iron or reduced solid iron as material and generally comprises cast steel with a relatively low C content. To adjust the composition, it is possible, in the same electric furnace where the melting was carried out, to perform other treatments including alloy addition, conducting finishing decarburization treatment and dephosphorization treatment with oxygen blow refining. It is also possible to carry out a secondary refining process comprising desulfurization of the cast steel and vacuum degassing after extraction. Subsequently, a semi-finished product, such as a cast slab, is obtained by ingot casting steps, such as continuous casting and other processes. EXAMPLES Example 1
[034] A cold iron source melting operation test was carried out using the AC 101 arc furnace with the same configuration shown in FIG. 1. Reduced solid iron was used as cold iron source 2 in a total charge of 100 t.
[035] Burner lance 1, which was supplied with a fuel supply line and an oxygen supply line, was installed in the furnace body. The pointed end portion 10 of burner lance 1 had the same multi-tube structure as shown in FIG. 3. Methane gas, hydrogen gas, and a gas mixture of 50% by volume hydrogen and 50% by volume methane were used as burner fuel 16. A comparison was made in the following three cases: a case in which no burner was used; a case in which the furnace contents were heated only by the burner flame, with burner fuel feed but without powder material feed; and a case Petition 870260090227, dated 02 / 09 / 2026, page 23 / 35 15 / 23 in which powdered lime was blown into the burner flame. The extraction temperature was 1650 °C.
[036] After the electric current began to be applied, when the melting of the first source of cold iron loaded progressed to lower the height of the loaded materials in the furnace so that there was space at the top of the furnace, the burner lance 1 was lowered to apply heat also from the burner flame 7. Powdered lime was fed into the electric furnace using argon gas as carrier gas at a feed rate of 100 kg / min. Fuel gas 16 was blasted at different flow rates depending on the type of gas used: 5 Nm3 / min for methane gas, 16 Nm3 / min for hydrogen gas and 10.5 Nm3 / min for hydrogen-methane gas mixture. Oxygen gas was fed as the combustion support gas 17 for the combustion of fuel gas 16 in each case.
[037] When the first additionally charged cold iron source melted and reached a flat bath state, a state in which any unmelted portion of the cold iron source was soaked into the molten metal, the slag was removed through the slag removal door. Then, the electric current and the burner were switched off to open the furnace lid and charge the cold iron source a second time. After the second charge of the cold iron source, the electric current was resumed to perform the operation in the same manner as after the first charge. Thus, molten steel at 1650 °C was eventually obtained and drained into a ladle.
[038] A comparison was made of the burner lance nozzle wear states, electrical energy unit consumption, presence / absence of slag solidification, and CO2 emissions for each treatment condition. Table 1 shows the treatment conditions and results. The nozzle wear factor is an index that indicates a value of Petition 870260090227, dated 02 / 09 / 2026, page 24 / 35 16 / 23 Relative wear when a wear quantity in the case of using methane as fuel gas was defined as 1.0. The unit consumption of electrical energy is an index calculated by dividing the electrical energy consumption under each treatment condition by the electrical energy consumption in treatment No. 1, which represents a conventional example. Slag solidification was observed and determined visually. The CO2 emissions index is an index calculated by dividing the CO2 emissions under each treatment condition by the CO2 emissions in treatment No. 1, which represents a conventional example. In this comparison, the fossil fuels consumed to obtain electrical energy were also taken into account for the calculation of CO2 emissions. Petition 870260090227, dated 02 / 09 / 2026, page 25 / 35
[039] [Table 1] N2. BURNER NOZZLE WEAR INDEX ELECTRICAL ENERGY UNIT CONSUMPTION SLAG SOLIDIFICATION PRESENCE CO2 EMISSION INDEX OBSERVATIONS USED OR NOT USED FUEL TYPE POWDER TYPE 1 NOT USED — — — 1.0 NONE 1.0 CONVENTIONAL EXAMPLE 2 USED METHANE NONE 1.0 1.0 NONE 1.3 COMPARISON EXAMPLE 3 USED HYDROGEN NONE 1.5 1.0 NONE 1.0 COMPARISON EXAMPLE 4 USED 50% HYDROGEN - 50% METHANE NONE 1.4 1.0 NONE 1.2 COMPARISON EXAMPLE 5. Used methane, lime 1.0, 0.7, none, 0.9. Comparison example. 6. Used hydrogen, lime 1.0, 0.7, none, 0.6. Invention example. 7. Used 50% hydrogen - 50% methane, lime 1.0, 0.7, none, 0.7. Invention example. 17 / 23 Petition 870260090227, dated 02 / 09 / 2026, page 26 / 35 18 / 23
[040] Under the conditions (Treatments Nos. 2 to 4) in which the furnace contents were heated only by the burner flame, the burner combustion heat was not effectively transferred, resulting in the electrical energy unit consumption being substantially equal to the conventional example (Treatment 1) in which no burner was used. Under the conditions (Treatments Nos. 3 and 4) in which hydrogen-containing gas was used as the fuel without feeding the powder, the burner lance nozzle was substantially worn. Under the conditions (Treatments Nos. 5 to 7) in which powdered lime was blown through the burner flame, the burner combustion heat was transferred to the furnace contents with high efficiency, significantly reducing the electrical energy unit consumption. Under the conditions (Treatments Nos. 6 and 7) that used hydrogen-containing gas, CO2 emissions were substantially reduced compared to the conditions (Treatment Nos. 7).5) that used methane as the burner fuel, thus avoiding wear on the burner nozzle.
[041] In the present examples using the arc furnace, slag solidification was not observed under any condition. EXAMPLE 2
[042] A cold iron source melting operation test was carried out using the 102 induction melting furnace with the same configuration shown in FIG. 2. Reduced iron was used as the cold iron source in a charge quantity of 50 t.
[043] Burner lance 1, provided with a fuel supply line and an oxygen supply line, was installed in the furnace body. The pointed end portion 10 of burner lance 1 had a structure similar to the multi-tube structure shown in FIG. 3. The burner fuel was hydrogen gas, methane gas, or a mixture. Petition 870260090227, dated 02 / 09 / 2026, page 27 / 35 19 / 23 gaseous material consisting of 50% hydrogen and 50% methane by volume. Three cases were compared: one in which no burner was used; another in which burner fuel was fed and the furnace contents were heated only by the burner flame, without feeding powdered material; and the last in which powdered lime was blown into the burner flame. The flow temperature was 1650 °C.
[044] After the electric current began to be applied, when the melting of the first source of cold iron loaded progressed to lower the height of the loaded materials in the furnace so that there was space at the top of the furnace, the burner lance 1 was also lowered to apply heat from the burner flame 7. Powdered lime was fed into the electric furnace using argon gas as carrier gas at a feed rate of 100 kg / min. Fuel gas 16 was blasted at different flow rates depending on the type of gas used: 5 Nm3 / min for methane gas, 16 Nm3 / min for hydrogen gas and 10.5 Nm3 / min for hydrogen-methane gas mixture. Oxygen gas was fed as the combustion support gas 17 for the combustion of fuel gas 16 in each case.
[045] When the first additionally charged cold iron source melted and reached a flat bath state, in which any unmelted portion of the cold iron source was soaked into the molten metal, the electric current and the burner were switched off to open the furnace lid and remove the slag by tilting the furnace body. After the slag removal was complete, the furnace body was returned to its original vertical position to charge the cold iron source a second time, and then the application of the electric current was resumed. After the second charging of the cold iron source, the same operation was performed as after the first charging. Thus, molten steel at 1650 °C was eventually obtained and drained into a ladle. Petition 870260090227, dated 02 / 09 / 2026, page 28 / 35 20 / 23
[046] A comparison was made of the wear states of the burner lance nozzle, the electrical energy unit consumption, the presence / absence of slag solidification and CO2 emissions for each treatment condition. Table 2 shows the treatment conditions and results. The evaluation indices used were the same as those used in Example 1. Treatment No. 8 served as a conventional example to be compared. Petition 870260090227, dated 02 / 09 / 2026, page 29 / 35
[047] [Table 2] N2. BURNER NOZZLE WEAR INDEX ELECTRICAL ENERGY UNIT CONSUMPTION SLAG SOLIDIFICATION PRESENCE CO2 EMISSION INDEX OBSERVATIONS USED OR NOT USED FUEL TYPE POWDER TYPE 8 NOT USED — — — 1.0 YES 1.0 CONVENTIONAL EXAMPLE 9 USED METHANE NONE 1.0 1.0 YES 1.3 COMPARISON EXAMPLE 10 USED HYDROGEN NONE 1.5 1.0 YES 1.0 COMPARISON EXAMPLE 11 USED 50% HYDROGEN - 50% METHANE NONE 1.4 1.0 YES 1.2 COMPARISON EXAMPLE 12 USED Methane Lime 1.0 0.7 None 0.9 Comparison Example 13 Used Hydrogen Lime 1.0 0.7 None 0.6 Invention Example 14 Used 50% Hydrogen - 50% Methane Lime 1.0 0.7 None 0.7 Invention Example 21 / 23 Petition 870260090227, dated 02 / 09 / 2026, pages 30 / 35 22 / 23
[048] Under the conditions (Treatments Nos. 9 to 11) in which the furnace contents were heated only by the burner flame, the burner combustion heat was not effectively transferred, resulting in the electrical energy unit consumption being substantially equal to the conventional example (Treatment 8) in which no burner was used. Under the conditions (Treatments Nos. 10 and 11) in which hydrogen-containing gas was used as the fuel without feeding the dust, the burner lance nozzle was substantially worn. Additionally, operation was hampered by slag solidification in the furnace.
[049] Under the conditions (Treatments Nos. 12 to 14) where powdered lime was added via the burner flame, since the heat of combustion from the burner was transferred to the furnace contents with high efficiency, it was possible to significantly reduce electrical energy consumption rates. Additionally, compared to the level (Treatment No. 12) using methane as the burner fuel, the situations under the conditions (Treatments Nos. 13 and 14) using hydrogen-containing gas were able to significantly reduce CO2 emissions and were also able to prevent burner nozzle wear. Additionally, it was also possible to prevent slag solidification. INDUSTRIAL APPLICABILITY
[050] The electric furnace and steelmaking method of the present invention can increase heat transfer efficiency and melt the cold iron source using a heat source with reduced CO2 emissions. This can reduce electrical energy unit consumption and lessen the environmental impact, which are industrially useful. Additionally, the present invention is applicable to other processes in a refining furnace that require both a heat source with reduced CO2 emissions and the addition of an auxiliary material. Petition 870260090227, dated 02 / 09 / 2026, page 31 / 35 23 / 23 powder. LIST OF REFERENCE SIGNS burner lance cold iron source cast iron slag electrode coil burner flame powder auxiliary material (powdered material) furnace body burner lance tip end (nozzle) powder feed tube fuel feed tube combustion support gas feed tube cooling water passage outer casing fuel gas combustion support gas 101 AC arc furnace 102 induction melting furnace Petition 870260090227, dated 02 / 09 / 2026, pages 32 / 35
Claims
1 / 2 CLAIMS 1. A method of steelmaking that can obtain cast iron (3) by melting a cold iron source (2) using electrical energy in an electric furnace, wherein the electric furnace is provided with a burner comprising a jet hole for jetting a fuel (16) and a jet hole for jetting combustion support gas (17) and which jets a flame through the jet holes towards an interior of the electric furnace, and for at least part of the operating duration of an electric furnace run, hydrogen gas or a hydrogen-enriched gaseous fuel is used as the burner fuel (16), characterized in that an auxiliary material (8) that is in a powder form or is processed into a powder form is blown through an interior of the flame formed by the burner and is blown to the cold iron source (2), cast iron (3) or slag in the cast iron (3) as a heat transfer medium without burning in the burner flame,and that the ratio of powder material to fuel gas expressed as (powder material feed rate) / (fuel gas heat generation quantity) is 0.41 kg / MJ or more.
2. Steelmaking method according to claim 1, characterized in that: the cold iron source (2) includes reduced solid iron.
3. Method of manufacturing steel, according to claim 1 or 2, characterized in that: the auxiliary material (8) which is in powder form or is processed in powder form is powdered lime.
4. Method of manufacturing steel, according to any of claims 1 to 3, characterized in that: the electric furnace is a DC arc furnace, an AC arc furnace (101) or an induction melting furnace (102). Petition 870260090227, dated 02 / 09 / 2026, page 33 / 35 2 / 2