Double emulsification of alkenyl succinic anidride for melhorar o performance ea estabilidade da colagem
The double emulsification of ASA with cationic polymer and starch stabilizes emulsions, addressing inefficiencies in high-ash papermaking by reducing starch usage and enhancing sizing performance.
Patent Information
- Application Number
- BR112025020736
- Authority / Receiving Office
- BR · BR
- Patent Type
- Applications
- Publication Date
- 2026-11-17
AI Technical Summary
Existing ASA emulsification methods for papermaking are inefficient and unstable, particularly in high-ash materials, leading to increased starch usage, reduced water retention, and decreased productivity due to the instability of natural and synthetic polymer emulsions, which are often created on-site and affected by process water chemistry.
A double emulsification technique using a cationic polymer as the primary emulsifying agent and cationic starch as the secondary emulsifying agent to stabilize ASA emulsions, reducing overall starch usage and improving sizing performance in high-ash papermaking.
The method achieves superior emulsion stability and enhanced sizing performance with reduced starch consumption, improving the efficiency and productivity of paper manufacturing processes.
Smart Images

Figure 00000000_0000_ABST
Description
1 / 52 Double emulsification of alkenyl succinic anhydride to improve performance and stability of COLLAGE RELATED ORDERS
[0001] This application claims the benefit of priority over U.S. Provisional Application No. 63 / 456265, filed March 31, 2023, and Finnish Application No. 20236040, filed September 20, 2023, the contents of which are incorporated by reference in their entirety. FIELD OF THE INVENTION
[0002] The present invention relates generally to compositions and methods for preparing an alkenyl succinic anhydride (ASA) sizing emulsion for use in paper and cardboard manufacturing. In particular, the disclosure provides methods for dual emulsification of ASA using a cationic polymer as the primary emulsifying agent and cationic starch as the secondary emulsifying agent to impart superior emulsion stability and improve sizing performance in woodless papermaking systems, generally containing high ash content, with considerable reduction in overall starch utilization compared to conventional natural polymer ASA emulsification applications. BACKGROUND OF THE INVENTION
[0003] In paper manufacturing and finishing, a sizing agent is often used to provide the desired characteristics sought in the final product. Sizing, or sizing property, is a measure of the resistance of a manufactured paper or cardboard product to penetration or wetting by an aqueous liquid, water or ink.
[0004] Sizing agents are generally internal additives in Petition 870260109050, dated 10 / 23 / 2026, page 6 / 63 2 / 52 sizing agents are applied during papermaking or external surface additives used on the finished sheet or web that increase this strength. Sizing agents can be various substances used to enhance liquid resistance, which may include, but are not limited to, water, ink, or other media, as protection for a paper surface. These substances are typically used to prevent fluids from being absorbed by the paper.
[0005] Alkenyl succinic anhydride (ASA) is a common internal sizing agent for papermaking. ASA sizing agents tend to be hydrophobic and are generally intended for use in aqueous papermaking systems.
[0006] ASA is typically emulsified in a natural polymer, usually modified cationic starch, or a synthetic cationic polymer before being introduced into the wet end of the paper machine. Because ASA emulsions made with natural or synthetic polymer are not stable, they are typically created on-site at the mill in situ with equipment that provides sufficient shear to create an effective emulsion to be applied directly to the machine or within a few hours of manufacture. While there are clear benefits to using (high) starch for ASA emulsification with respect to emulsion quality, sizing retention, and overall sizing efficiency, high starch use in the wet end of the papermaking process will increase paper web water retention with increasing starch levels and, conversely, will reduce paper web water retention with decreasing starch levels in the wet end.Increased water retention reduces the pressing efficiency of the paper web, decreasing the amount of web solids exiting the pressing section. This will increase the energy demand for drying the web and may decrease the overall productivity and operability of the paper machine. Petition 870260109050, dated 10 / 23 / 2026, page 7 / 63 3 / 52
[0007] Considerable effort is required to obtain a uniform and stable ASA emulsion suitable for papermaking. The chemistry of the process water, along with the various components of the supplied material, can negatively affect the efficiency of ASA sizing. The efficiency of ASA emulsified with synthetic polymer is often impractical for this reason when applied in isolation, in materials with significant levels of ash, frequently observed in alkaline printing and writing grades and some packaging grades where calcium carbonate pigments and various kaolin pigments are used, or when there is a significant level of free calcium ions present in the wet side. Generally, [Ca++] > 150 ppm as calcium or 400 ppm as calcium carbonate are considered high.
[0008] Currently, the availability of starch for commercial applications is severely limited due to supply chain shortages. The present invention seeks to utilize a double emulsification technique using a cationic solution polymer in the primary emulsification step, followed by secondary emulsification in low-dose starch under shear. The present invention also seeks to form a low-starch ASA sizing emulsion suitable for use in high-ash materials for the preparation of ink- and water-resistant writing and printing paper and cardboard. Double emulsification confers superior emulsion stability and improves sizing performance in the manufacture of high-ash paper, with a considerable reduction in overall starch usage compared to conventional natural ASA polymer emulsification applications. SUMMARY OF THE INVENTION
[0009] The present invention relates generally to composition Petition 870260109050, dated 10 / 23 / 2026, page 8 / 63 4 / 52 tions and methods for preparing an alkenyl succinic anhydride (ASA) sizing emulsion for use in paper and cardboard manufacturing. In particular, the disclosure provides methods for double emulsification of ASA using a cationic polymer as the primary emulsifying agent and cationic starch as the secondary emulsifying agent to impart superior emulsion stability and improve sizing performance in high-ash papermaking, with considerable reduction in overall starch utilization compared to conventional natural polymer ASA emulsification applications.
[0010] In one aspect, the present invention provides a method for preparing a stable alkenyl succinic anhydride (ASA) sizing emulsion that is suitable for use in the manufacture of paper and cardboard, the method comprising: (a) to obtain or produce an alkenyl succinic anhydride (ASA) binding agent; (b) combine said ASA binding agent with a primary emulsifying agent and emulsify to form a primary emulsion; and (c) after step (b), add a secondary emulsifying agent and emulsify to form said ASA sizing emulsion, and (d) optionally, after steps (a) to (c), add the resulting stable ASA sizing emulsion to a papermaking pulp, pulp or fiber stock, optionally a high-ash paper pulp.
[0011] In some exemplary embodiments, the method also includes, after step (c): (a) add said ASA sizing emulsion to said pulp for the manufacture of paper, pulp or fiber stock; or Petition 870260109050, dated 10 / 23 / 2026, p. 9 / 63 5 / 52 (b) add said ASA sizing emulsion to said high-ash paper pulp comprising selected ashes from the group consisting of calcium carbonate, TiO2, kaolin clay, silicates, carbonate-based pigments, kaolin-based pigments or any combination thereof, wherein said high-ash paper pulp comprises an ash percent content of 1-35%, 2-30%, 5-25% or 10-20% by mass, preferably 5%-25% ash by mass.
[0012] In some exemplary embodiments, the ASA liaison agent comprises: (a) an ASA solid, a waxy ASA solid, a waxy ASA liquid, an ASA liquid, or a mixture thereof; and (b) a single ASA binding agent or a mixture of ASA binding agent molecules and / or isomers.
[0013] In some exemplary embodiments of the method (i) said primary emulsifying agent comprises an aqueous polymer solution comprising one or more cationic polymers and water; and (ii) said secondary emulsifying agent comprises one or more cationic starches.
[0014] In some exemplary embodiments, the aqueous polymer solution comprises a weight solids percentage of one or more cationic polymers ranging from 1-70%, 2-50% or 5-30%.
[0015] In some exemplary embodiments, the aforementioned one or more cationic polymers comprise: (a) one or more synthetic copolymers, terpolymers or tetrapolymers comprising acrylamide and one or more cationic monomers selected from the group consisting of (i) diallyldialkylammonium halides, including, but not limited to, diallyldimethylammonium chloride (“DADMAC”) and diallyldiethylammonium chloride; Petition 870260109050, dated 10 / 23 / 2026, page 10 / 63 6 / 52 (ii) N,N-dialkylaminoalkyl acrylates, N,N-dialkylaminoalkyl (meth)acrylates and acid addition salts and / or quaternary ammonium salts thereof, including, but not limited to, acryloyloxyethyltrimethylammonium chloride (“AETAC”), methacryloyloxyethyltrimethylammonium chloride (“MAETAC”), dimethylaminoethyl acrylate (“DMAEA”) and acid addition salts thereof, dimethylaminoethyl methacrylate (“DMAEMA”) and acid addition salts thereof, quaternary methyl sulfate salt of dimethylaminoethyl acrylate, quaternary benzyl chloride salt of dimethylaminoethyl acrylate, sulfuric acid salt of dimethylaminoethyl acrylate, hydrochloric acid salt of dimethylaminoethyl acrylate, diethylaminoethyl acrylate, quaternary chloride salt of methyl methacrylate quaternary salt, methyl sulfate quaternary salt, benzyl chloride quaternary salt, dimethylaminoethyl methacrylate sulfuric acid saltdimethylaminoethyl methacrylate hydrochloride salt, dimethylaminoethyl methacrylate hydrochloride salt; (iii) N,N-dialkylaminoalkylacrylamides and N,N-dialkylaminoalkyl(meth)acrylamides and acid addition salts or quaternary ammonium salts thereof, including, but not limited to, acrylamidopropyltrimethylammonium chloride (“APTAC”), methacrylamidopropyltrimethylammonium chloride (“MAPTAC”), quaternary methyl sulfate salt of dimethylaminopropyl acrylamide, sulfuric acid salt of dimethylaminopropyl acrylamide, hydrochloric acid salt of dimethylaminopropyl acrylamide, quaternary methyl sulfate salt of dimethylaminopropylmethacrylamide, sulfuric acid salt of dimethylaminopropylmethacrylamide, hydrochloric acid salt of dimethylaminopropylmethacrylamide, diethylaminoethylacrylate, diethylaminoethylmethacrylate; or (iv) any combination of (i)-(iii); (b) said one or more synthetic copolymers, terpolymers or tetrapolymers of (a), optionally containing: Petition 870260109050, dated 10 / 23 / 2026, p. 11 / 63 7 / 52 (i) one or more additional nonionic monomers selected from the group consisting of methacrylamide; N-alkylacrylamides, including but not limited to N-methylacrylamide, N-ethylacrylamide, N-propylacrylamide and N-butylacrylamide; N,N-dialkylacrylamides, including but not limited to N,N-dimethylacrylamide and N,N-diethylacrylamide; N-alkyl methacrylamides; alkyl acrylates; hydroxyalkyl acrylates and methacrylates, including but not limited to hydroxymethyl acrylate, 2-hydroxyethyl acrylate, 3-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, hydroxymethyl methacrylate, 2-hydroxyethyl methacrylate, 3-hydroxypropyl methacrylate and 4-hydroxybutyl methacrylate; Dihydroxyalkyl acrylates and methacrylates, including, but not limited to, 2,3-dihydroxypropyl acrylate, 3,4-dihydroxybutyl acrylate, 2,3-dihydroxypropyl methacrylate (DHPMA) and 3,4-dihydroxybutyl methacrylate;Alkyl acrylates, including but not limited to methyl methacrylate; acrylonitrile; N-vinylmethylacetamide, N-vinylmethylformamide; N-vinyl acetate, glyoxalated acrylamides and vinylpyrrolidone; (ii) one or more additional anionic monomers selected from the group consisting of acrylic acid, methacrylic acid, sulfonic acids, phosphonic acids and alkali metal salts, alkaline earth metal salts and ammonium salts thereof, including, but not limited to, acrylic acid, methacrylic acid, maleic acid, itaconic acid, vinyl sulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid (AMPS), acrylamidomethanesulfonic acid, acrylamidoethanesulfonic acid, 2-hydroxy-3-acrylamidepropanesulfonic acid, styrenesulfonic acid and vinylphosphonic acid; or (iii) any combination of (i)-(ii): (c) one or more cationic glyoxalated polyacrylamide (GPAM) polymers obtained by reacting glyoxal with one or more synthetic copolymers, terpolymers or tetrapolymers of (a), one or more copo- Petition 870260109050, dated 10 / 23 / 2026, p. 12 / 63 8 / 52 synthetic limers, terpolymers or tetrapolymers of (b), or a combination thereof. (d) one or more semisynthetic polymers comprising one or more synthetic copolymers, terpolymers or tetrapolymers of (a) or (b) optionally grafted onto one or more natural polymers, including, but not limited to, starch, chitin, chitosan and natural polysaccharides; or (e) any combination of (a)-(d), wherein said one or more cationic polymers have a weight-average molecular weight ranging from 10,000-3,000,000 Da, 10,000-2,000,000 Da, 10,000-1,000,000 Da, 10,000-500,000 Da, 10,000-200,000 Da, 10,000-100,000 Da or 10,000-50,000 Da.
[0016] In some exemplary embodiments, the aforementioned one or more cationic starches; (a) comprise one or more modified or unmodified cationic starches selected from the group of starches consisting of maize starch, waxy maize starch, potato starch, tapioca starch, wheat starch, rice starch, barley starch, pea starch, sweet potato starch and any combination thereof; and (b) have a percentage nitrogen content (%N) ranging from 0.2-2%, 0.2-1.75%, 0.2-1.5%, 0.2-1.25%, 0.2-1% or 0.25-0.45% by mass, preferably 0.35-1.45% by mass.
[0017] In some exemplary embodiments, the aforementioned one or more cationic starches are formulated prior to the addition of the aforementioned ASA binding agent by a method comprising: (a) Dissolve a dry cationic starch in water; cook by a method including, but not limited to, jet cooking, steaming or pan cooking; and cool to a temperature ranging from 20-80 °C, 20-60 °C, 20-40 °C or 20-25 °C, preferably Petition 870260109050, dated 10 / 23 / 2026, page 13 / 63 9 / 52 at 20-40 °C to obtain a cooked starch solution with a solids percentage ranging from 1-10%, 2-8% or 3-6% by mass; or (b) obtain a pre-gelatinized cationic starch with a solids percentage ranging from 20% to 40% by mass and dilute with water to obtain a pre-gelatinized starch solution with a solids percentage ranging from 1-10%, 2-8% or 3-6% by mass.
[0018] In some exemplary embodiments of the method, (i) the aforementioned one or more cationic polymers are selected from the group consisting of acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride copolymer (AMD / MAETAC), acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride / 2-hydroxyethyl methacrylate terpolymers (AMD / MAETAC / HEMA), acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride / 2-hydroxyethyl methacrylate / acrylic acid tetrapolymers (AMD / MAETAC / HEMA / AA), and acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride / 2,3-dihydroxypropyl methacrylate terpolymer (AMD / MAETAC / DHPMA) and (ii) said one or more cationic starches comprise maize starch, waxy maize starch, potato starch, tapioca starch, wheat starch or pea starch.
[0019] In some exemplary embodiments, the method comprises one or more of the following: (a) add said primary emulsifying agent to said alkenyl succinic anhydride (ASA) sizing agent to obtain a ratio of grams of active cationic polymer to grams of ASA of 0.05:1 to 0.6:1, 0.1:1 to 0.5:1, 0.15:1 to 0.4:1 or 0.2:1 to 0.25:1; and (b) add said secondary emulsifying agent to said primary emulsion to obtain a mass ratio of dry starch to ASA of 0.25:1 to 2:1, 0.3:1 to 1.6:1, 0.4:1 to 1.2:1 or 0.5:1 to 1:1.
[0020] In some exemplary embodiments, the method comprises: Petition 870260109050, dated 10 / 23 / 2026, p. 14 / 63 10 / 52 (a) add said primary emulsifying agent to said ASA binding agent at room temperature and emulsify by stirring with sufficient energy to achieve an average ASA particle size ranging from 0.5-3 µm, 0.5-2 µm or 0.5-1 µm in diameter; (b) add the secondary emulsifying agent to the primary emulsion at a temperature ranging from 20-80 °C, 20-60 °C, 20-40 °C or 20-25 °C, preferably 20-40 °C and emulsify by stirring with sufficient energy to achieve an average ASA particle size ranging from 0.5-3 µm, 0.5-2 µm or 0.5-1 µm in diameter.
[0021] In some exemplary embodiments, the aforementioned ASA bonding emulsion, in its final form: (a) comprises an average particle size ranging from 0.5-1 pm, 0.6-0.9 pm or 0.7-0.8 pm in diameter; (b) comprises a viscosity ranging from 10-100 cP, 20-90 cP, 30-80 cP, 40-70 cP or 50-60 cP, when measured by a Brookfield viscometer with a 62 spindle at 60 rpm and 20 °C; (c) has a stability of 1-4 min, 1-10 min, 1 min-1 h, 16 h, 1-12 h, 1-24 h or 1-48 h, wherein said stability is determined by the retention of the ASA bonding emulsion of (1) an average particle size of 0.5-3 µm, 0.5-2 µm, 0.5-1 µm, 0.6-0.9 µm or 0.7-0.8 µm in diameter, preferably less than 1 µm in diameter; and / or (2) a viscosity ranging from 10-100 cP, 20-90 cP, 30-80 cP, 40-70 cP or 50-60 cP, preferably less than 100 cP, when measured by a Brookfield viscometer with a 62 spindle at 60 rpm and 20 °C; (d) is immediately added to a papermaking pulp, pulp or fiber stock, optionally a high-ash paper pulp, or is stored in a storage tank or holding facility for a storage time. Petition 870260109050, dated 10 / 23 / 2026, p. 15 / 63 11 / 52 of 1-4 min, 1-10 min, 1 min-1 h, 1-6 h, 1-12 h, 1-24 h or 1-48 h before adding said ASA sizing emulsion to a papermaking pulp, pulp or fiber stock, optionally a high-ash paper pulp; (e) comprises a reduced final mass ratio of dry starch to ASA compared to an ASA sizing emulsion prepared by a single or double emulsification method using one or more emulsifying agents comprising one or more cationic starches; or (f) any combination of (a)-(e).
[0022] In some exemplary embodiments of the method, when stable alkenyl succinic anhydride (ASA) sizing emulsion is used as a sizing agent during the manufacture of paper or cardboard, it results in a sheet-like product selected from the group consisting of a high-ash paper or cardboard, a printing or writing grade paper or cardboard, an alkaline printing or writing grade paper or cardboard, a bleached paper or cardboard, a packaging grade paper or cardboard, and a partially recycled or 100% recycled paper or cardboard, wherein the sheet-like product comprises optimal sizing performance as measured by industry standardized tests, including but not limited to HST, Cobb, water drop test, contact angle, edge wilt, or water penetration,wherein the ideal bonding performance is determined in relation to a sheet-like equivalent product comprising an ASA bonding emulsion prepared by a single or double emulsification method using one or more emulsifying agents comprising one or more cationic starches.
[0023] In another aspect, the present invention provides a double emulsification method for preparing a bonding emulsion. Petition 870260109050, dated 10 / 23 / 2026, page 16 / 63 12 / 52 of alkenyl succinic anhydride (ASA) for use in the manufacture of paper and cardboard, the method comprising: (a) to obtain or produce an alkenyl succinic anhydride (ASA) sizing agent; (b) combine said ASA bonding agent with a primary emulsifying agent and emulsify at room temperature and stir with sufficient energy to achieve an average ASA particle size ranging from 0.5-3 µm, 0.5-2 µm or 0.5-1 µm in diameter, thereby forming a primary emulsion; (c) after step (b), add a secondary emulsifying agent and emulsify at a temperature ranging from 20-80 °C, 20-60 °C, 20-40 °C or 20-25 °C, preferably 20-40 °C and stir with sufficient energy to achieve an average ASA particle size ranging from 0.5-3 µm, 0.5-2 µm or 0.5-1 µm in diameter, thus forming said ASA sizing emulsion, and (d) optionally, after step (c), add said ASA sizing emulsion to a high-ash papermaking pulp,wherein (i) the said primary emulsifying agent comprises an aqueous polymeric solution comprising cationic acrylamide copolymers selected from the group consisting of acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride copolymer (AMD / MAETAC), acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride / 2-hydroxyethyl methacrylate (AMD / MAETAC / HEMA) terpolymers, acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride / 2-hydroxyethyl methacrylate / acrylic acid tetrapolymers (AMD / MAE-, TAC / HEMA / AA) and acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride / 2,3-dihydroxypropyl methacrylate terpolymer (AMD / MAETAC / DHPMA); (ii) the aforementioned secondary emulsifying agent comprises Petition 870260109050, dated 10 / 23 / 2026, page 17 / 63 13 / 52 one or more modified or unmodified cationic starches; selected from the group of starches consisting of corn starch, waxy corn starch, potato starch, tapioca starch, wheat starch, pea starch and a mixture thereof; (iii) said high-ash papermaking pulp comprises selected ash from the group consisting of calcium carbonate, TiO2, kaolin clay, silicates, carbonate-based pigments, kaolin-based pigments or any combination thereof; (iv) the said high-ash papermaking material comprises an ash percentage of 1-35%, 2-30%, 5-25% or 10-20% by mass, preferably 5-25% ash by mass; (v) said primary emulsifying agent is added to said alkenyl succinic anhydride (ASA) sizing agent to obtain a ratio of grams of active cationic polymer to grams of ASA of 0.05:1 to 0.6:1, 0.1:1 to 0.5:1, 0.15:1 to 0.4:1 or 0.2:1 to 0.25:1; and (vi) said secondary emulsifying agent is added to said primary emulsion to obtain a mass ratio of dry starch to ASA of 0.25:1 to 2:1, 0.3:1 to 1.6:1, 0.4:1 to 1.2:1 or 0.5:1 to 1:1.
[0024] In another aspect, the present invention provides an ASA sizing emulsion composition or a pulp for making paper, pulp or fiber stock, optionally a high-ash paper pulp, comprising said ASA sizing emulsion composition, obtained by a method according to any of the foregoing.
[0025] In another aspect, the present invention provides a process for the production of paper or cardboard, the process comprising Petition 870260109050, dated 10 / 23 / 2026, page 18 / 63 14 / 52 Obtaining a high-ash content paper pulp comprising wood pulp, optionally a fiber stock comprising a high content of recycled fibers and / or production waste fibers, optionally a concentrated fiber stock, optionally a bleached fiber stock, optionally containing process water from the production of pulp, paper or cardboard and treating said fiber stock at the wet end of a paper machine with an ASA sizing emulsion according to any of the preceding claims, wherein: (a) said high-ash paper pulp comprises selected ash from the group consisting of calcium carbonate, TiO2, kaolin clay, silicates, carbonate-based pigments, kaolin-based pigments or any combination thereof; and (b) said high-ash paper pulp comprises an ash percentage of 1-35%, 2-30%, 5-25% or 10-20% by mass, preferably 5%-25% by mass. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The invention will be described in more detail with reference to the accompanying drawings, described in detail below.
[0027] Figure 1 provides an exemplary flowchart for conventional ASA emulsification (Conventional) and the inventive double emulsification method (Novel Two-Step Approach) according to Example 1.
[0028] Figure 2 shows an exemplary table of primary, secondary and control ASA emulsion compositions, particle sizes and viscosity measurements according to Example 1.
[0029] Figure 3 shows an exemplary variability plot of Cobb values indicating the amount of water absorption in hand sheets prepared with inventive double-emulsified ASA bonding emulsions and control ASA bonding emulsions. Petition 870260109050, dated 10 / 23 / 2026, page 19 / 63 15 / 52 according to Example 2.
[0030] Figure 4 shows an exemplary variability plot of the Hercules size test (HST) indicating the amount of ink penetration on hand sheets prepared with inventive double-emulsified ASA bonding emulsions and control ASA bonding emulsions according to Example 2.
[0031] Figure 5 shows an exemplary bar graph of HST values indicating the deficiency of starch only or synthetic polymer only, when used as emulsifying agents for ASA sizing emulsions for high-ash paper sizing according to Example 3.
[0032] Figure 6 shows an exemplary bar graph of Cobb values indicating similar bonding performance for ASA emulsions prepared using the inventive double emulsification method (red bars) compared with starch alone (blue bars) according to Example 3. DETAILED DESCRIPTION OF THE INVENTION
[0033] Before describing the invention, the following definitions are provided. Unless otherwise indicated, all terms should be interpreted as they would be by a person skilled in the art. DEFINITIONS
[0034] As used in this document, the singular forms “a / an”, “and” and “the” include plural referents, unless the context clearly indicates otherwise.
[0035] As used herein, the terms “percentage of N content” and “% of N content” refer to the molar percentage of nitrogen substitution of cationic starch.
[0036] As used herein, the term “retention” refers to the efficiency with which small particles or chemical additives remain on the paper during its formation, rather than remaining in the white water. Petition 870260109050, dated 10 / 23 / 2026, page 20 / 63 16 / 52
[0037] As used in this document, the terms “papermaking process” and “papermaking application” generally refer to any process in which any form of paper and / or cardboard product can be produced. For example, such processes include the manufacture of paper products from pulp, such as methods comprising the formation of an aqueous feedstock for the manufacture of cellulosic paper, the draining of the feedstock to form a sheet, and the drying of the sheet. The papermaking feedstock formation, draining, and drying steps may be carried out in any conventional manner generally known in the art. In some cases, papermaking processes and applications may comprise the use of one or more sizing agents, which are added to the pulp for papermaking.
[0038] As used in this document, the term “fiber” refers to the basic structural unit of paper or cardboard.
[0039] As used in this document, the terms “recycled fiber” and “recovered fiber” refer to paper, cardboard, and fibrous waste from retail stores, office buildings, homes, factories, and so forth, after they have passed through their end-use as a consumer item. Manufacturing waste includes: dry paper and cardboard waste generated after the completion of the papermaking process, including, by way of example: envelope trimmings, binding trimmings, and other paper and cardboard waste resulting from printing, cutting, forming, and other converting operations; waste from the manufacture of bags, boxes, and packages; factory packaging and rejected unused water and fiber mixtures; and finished paper and cardboard pulped again from obsolete papers from paper and cardboard manufacturers, traders, wholesalers, retailers, im Petition 870260109050, dated 10 / 23 / 2026, page 21 / 63 17 / 52 presses, converters or others. In particular, the term “recycled fibers” includes recycled fibers derived from the processing of paper and other consumer cellulosic materials, for example, paper, old corrugated cardboard boxes (OCC), mixed office waste (MOW), old magazines (OMG), unbleached kraft pulp, neutral sulfite semi-chemical pulp (NCCS) and / or mechanical pulp. Source materials for recycled fibers may be selected from old corrugated cardboard boxes, mixed office waste, old newsprint, old magazines, double-lined kraft paper and any mixtures thereof. Mixed waste (MXW) denotes a recycled mixture of recycled cardboard, such as OCC, white-lined chipboard and / or folding cardboard boxes, and recycled paper, such as old newsprint, old magazines and / or office waste paper.Mixed office waste denotes recycled fiber material containing mainly copy paper, printer paper, and offset paper. Double-lined kraft denotes recycled fiber material comprising cleanly sorted, unprinted corrugated cardboard packages, boxes, sheets, or cuts, for example, of kraft or jute lining. White-lined corrugated board (WLC) denotes multi-layer board comprising detinned fiber material and / or unintinned recycled fiber material originating, for example, from OCC, mixed office waste, or old newspapers (ONP) in one or more of the layers. The presence of any of these recycled fiber materials in the fiber suspension generally decreases the drainage and strength of the paper and provides a substantial load of starch, hydrophobic, and colloidal substances to the process.
[0040] As used in this document, the term “OCC” refers to old corrugated cardboard and / or cardboard boxes. Corrugated refers to boxes in which the materials are made of three separate layers of paper, two liners and a corrugated or wavy layer sandwiched between them. Brown paper bags are commonly accepted by OCC for Petition 870260109050, dated 10 / 23 / 2026, p. 22 / 63 18 / 52 recycling. The term OCC denotes recycled fiber material that has test, jute or kraft linings, and may also include double-grade corrugated cardboard (DS OCC).
[0041] As used in this document, the terms “waste” or “production waste” refer to paper that, during the papermaking process, becomes suitable only for repulping, for example, cuts or paper that is out of specification. Waste forms the reused material that never left the factory and is not considered recycled or recovered. Waste forms a valuable source of fiber and is recycled internally at the factory.
[0042] As used in this document, the term “fiber suspension” is understood to mean an aqueous suspension comprising fibers, preferably recycled fibers and, optionally, fillers. For example, the fiber suspension may comprise at least 5%, 10-30%, 11-19% mineral filler, preferably 5%-25% by mass for woodless communication and specialty papers. The mineral filler may be any filler conventionally used in the manufacture of paper and board, such as ground calcium carbonate, precipitated calcium carbonate, clay, talc, gypsum, titanium dioxide, synthetic silicate, aluminum trihydrate, barium sulfate, magnesium oxide or any mixture thereof.
[0043] As used in this document, the terms “paper pulp” or “paper pulp for papermaking” generally refer to a mixture of cellulosic fibers, pulp, optional fillers, dyes and water from which paper or cardboard is made.
[0044] As used in this document, the term “concentrated stock” generally refers to a mixture of paper pulp and other materials with a consistency of about 1 to 5%.
[0045] As used in this document, the term “diluted stock” generally refers to a pulp mixture for papermaking. Petition 870260109050, dated 10 / 23 / 2026, page 23 / 63 19 / 52 and other materials, after being diluted to a consistency below 1% with white water or other process water in a fan pump.
[0046] As used herein, the term “high-ash coating material” refers to supplied materials comprising ash components, including, but not limited to, calcium carbonate, TiO2, kaolin clay, silicates, carbonate-based pigments, kaolin-based pigments, or any combination thereof. High-ash papermaking materials are considered to contain an ash percentage of 1-35%, 2-30%, 5-25%, or 10-20% by mass, preferably 5%-25% by mass for woodless communication papers and specialty papers. These materials are typically used in papermaking applications for the production of alkaline writing or printing grade paper and packaging materials.
[0047] As used herein, the term “bonding agent” generally refers to various substances, typically hydrophobic, that are used to facilitate the water-resistant protection of a material surface (e.g., paper, cardboard, textile, or composite material). These substances are normally used to prevent the absorption of liquids into the paper.
[0048] As used herein, the term “glue performance” or “ideal glue performance” can be determined by industry-standardized tests, including but not limited to: HST, Cobb, water drop test, contact angle, edge wilt, or water penetration. Neither HST nor Cobb are exclusive to ink and water resistance, respectively. Both tests are used depending on the size level required based on the end use. The gluing requirement for printing (office) paper is not demanding, so the HST test is usually a good and more automated option. Petition 870260109050, dated 10 / 23 / 2026, p. 24 / 63 20 / 52 For higher bonding demands, the Cobb test is frequently used and can be run for 1 or 2 minutes, but up to 30 minutes for some packaging types. Other bonding tests, such as water droplet, edge wick, ink float, and contact angle, can also be used. The media for HST and ink float is typically a 1% formic acid solution dyed green, while the other tests usually use water, except for the edge wick test, which may use different media than those mentioned here.
[0049] As used in this document, the terms “fixation”, “fixing” and “fixing” mean that a substance is associated with or attached to the fibers, at least temporarily or permanently.
[0050] As used in this document, the terms “polymer” or “polymer additives” and similar terms are used in their common sense, as understood by someone skilled in the art, and therefore may be used in this document to refer to or describe a large molecule (or group of such molecules) that may comprise recurring units. Polymers may be formed in various ways, including by the polymerization of monomers and / or by the chemical modification of one or more recurring units of a precursor polymer. Unless otherwise specified, a polymer may comprise a “homopolymer” that may comprise substantially identical recurring units that may be formed, for example, by the polymerization of a specific monomer.Unless otherwise specified, a polymer may also comprise a copolymer comprising two or more different recurring units which may be formed, for example, by the copolymerization of two or more different monomers and / or by the chemical modification of one or more recurring units of a precursor polymer. Unless otherwise specified, a polymer or copolymer may also comprise a copolymer comprising two or more different recurring units which may be formed, for example, by the copolymerization of two or more different monomers and / or by the chemical modification of one or more recurring units of a precursor polymer. Petition 870260109050, dated 10 / 23 / 2026, page 25 / 63 21 / 52 A polymer may also comprise a “terpolymer” or a “tetrapolymer,” which generally refer to polymers comprising three, four, or more different recurring monomeric units. Any one or more of the polymers discussed here may be used in any applicable process, for example, as a primary emulsifying agent to form ASA bonding emulsions.
[0051] As used in this document, the term monomer generally refers to nonionic monomers, anionic monomers, cationic monomers, zwitterionic monomers, betaine monomers, and amphoteric ion pair monomers.
[0052] As used in this document, the term anionic monomers may refer to anionic monomers that are substantially anionic in whole or (at equilibrium) in part, at a pH in the range of about 4.0 to about 9.0. “Anionic monomers” may be neutral at low pH (from a pH of about 2 to about 6) or anionic monomers that are anionic at low pH.
[0053] As used in this document, the term cationic monomer generally refers to a monomer that has a positive charge or a monomer that is positively charged at a pH within the normal operating range of paper machine processes.
[0054] As used in this document, the term “water-soluble” generally refers to polymeric products that are completely miscible with water. When mixed with excess water, the cationic emulsion polymer in the polymeric product is preferably completely dissolved and the resulting polymeric solution is preferably free of discrete polymer particles or granules.
[0055] As used in this document, the term “aqueous solution” or “solution” generally refers to a mixture of water and a water-soluble solute or solutes that are completely dissolved. The solution may be homogeneous. When mixed with excess Petition 870260109050, dated 10 / 23 / 2026, page 26 / 63 22 / 52 water, the cationic emulsion polymer in the polymeric product is preferably completely dissolved and the resulting polymeric solution is preferably free of discrete polymer particles or granules.
[0056] As used in this document, the terms “wet end of a paper machine” or “wet end” generally refer to the parts of a papermaking process between pulping (or bleaching) and wet pressing of the paper.
[0057] The terms “total solids” or “total suspended solids” are used interchangeably herein and generally refer to the total amount or weight of suspended solids, such as cellulosic fiber, cellulose fibers, and mineral pigments contained in aqueous media. “Total solids” or “total suspended solids” generally do not include dissolved solids.
[0058] As used in this document, the terms “lbs / ton” or “# / T” denote pounds of dry mass of added material (e.g., additive, solute, and / or particle) per ton of suspended solids (e.g., ASA weight per total dry ton of suspended solids).
[0059] As used in this document, the phrases “% by weight” denote pounds of dry mass of additive per dry mass of solids in the formulation, solution or fluid paste, multiplied by 100%.
[0060] The term “alkenyl succinic anhydride” or “ASA” generally refers to alkenyl succinic anhydride compounds composed of monounsaturated hydrocarbon chains containing pendant succinic anhydride groups. Alkenyl succinic anhydride compounds are generally liquids and may be derived from maleic anhydride and suitable olefins. Alkenyl succinic anhydride compounds may also be solids.
[0061] The ASA glues useful in the subject matter of this invention are generally described by the following structural formula: Petition 870260109050, dated 10 / 23 / 2026, page 27 / 63 23 / 52 O °YR-R1 ο where R represents a dimethylene or trimethylene radical, and where R is a hydrophobic group containing more than 5 carbon atoms that can be selected from the group consisting of alkyl, alkenyl, aralkyl or aralkenyl groups.
[0062] In general, alkenyl succinic anhydride compounds can be made by reacting an isomerized C14-C20 monoolefin, preferably an excess of an internal olefin, with maleic anhydride, at a temperature and for a time sufficient to form the alkenyl succinic anhydride compound.
[0063] If the olefin to be used in the preparation of alkenyl succinic anhydride compounds is not an internal olefin, as is the case, for example, with α-olefins, it may be preferable to first isomerize the olefins to provide internal olefins. The olefins that can be used in the preparation of alkenyl succinic anhydride compounds may be linear or branched. Preferably, the olefins may contain at least about 14 carbon atoms. Typical structures of alkenyl succinic anhydride compounds are disclosed, for example, in U.S. Patent No. 4,040,900, incorporated herein by reference in its entirety. Alkenyl succinic anhydride compounds and methods for their preparation are described, for example, in CE Farley and RB Wasser, The Sizing of Paper, Second Edition, edited by WF Reynolds, TAPPI Press, 1989, pages 51-62, the disclosures of which are incorporated herein by reference in their entirety.
[0064] The alkenyl succinic anhydride component may contain some hydrolyzed alkenyl succinic anhydride. The amount of hydrolyzed alkenyl succinic anhydride may vary from about 1 to about Petition 870260109050, dated 10 / 23 / 2026, p. 28 / 63 24 / 52 99% by weight, based on the total weight of the alkenyl succinic anhydride component. The alkenyl succinic anhydride component is generally present in the emulsion in an amount that is at least about 0.01% by weight, or from about 0.1% to about 20% by weight, or from about 0.3% by weight to about 15% by weight, based on the total weight of the emulsion. In another embodiment, the alkenyl succinic anhydride component is present in the emulsion in an amount that is about 20% to about 40% by weight.
[0065] As used herein, the terms “starch” and “cationic starch” generally refer to cationic agents, various cationic starch derivatives, including primary, secondary, tertiary or quaternary amine starch derivatives and other starch derivatives substituted with cationic nitrogen, as well as sulfonium and phosphonium cationic starch derivatives. Such derivatives, as stated by the patent holder, may be prepared from all types of starches, including corn starch, waxy corn starch, potato starch, tapioca starch, wheat starch, rice starch, barley starch, pea starch, sweet potato starch and any combination thereof.
[0066] Cationic starches can be formulated before use in a papermaking process by a method such as dissolving a dry cationic starch in water; cooking by a method including, but not limited to, jet cooking, steam cooking or pan cooking; and cooling to a temperature ranging from 20-80 °C, 20-60 °C, 20-40 °C or 20-25 °C, preferably 20-40 °C to obtain a cooked starch solution with a solids percentage ranging from 1-10%, 2-8% or 3-6% by mass; or obtaining a pre-gelatinized cationic starch with a solids percentage ranging from 20% to 40% by mass and diluting with water to obtain a pre-gelatinized starch solution with a solids percentage ranging from 1-10%, 2-8% or 3-6% by mass. Any one or more of the starches discussed here can Petition 870260109050, dated 10 / 23 / 2026, page 29 / 63 25 / 52 can be used in any applicable process, for example, as a secondary emulsifying agent to form ASA bonding emulsions.
[0067] The methods used to measure the molecular weight of polymers include the light scattering method, the osmotic pressure method, and the viscosity method. They allow obtaining average molecular weight values. However, many polymers consist of molecules with not just one molecular weight, but rather a set of molecules with many different molecular weights.
[0068] As used herein, the terms “molecular weight” or “weight-average molecular weight” or “MW” refer to the weight fraction of molecules in a polymer sample. The MW of a polymer can be determined by gel permeation chromatography (GPC), which is a type of size exclusion chromatography (SEC). It is primarily used to measure the molecular weight of polymeric compounds based on retention time on a size exclusion column under standardized conditions. Other methods used to determine the weight-average molecular weight of polymers include light scattering and ultracentrifugation methods.
[0069] As used herein, the phrase “stir with sufficient energy” or “emulsify by stirring with sufficient energy” generally refers to high shear agitation of the ASA to provide an emulsion and achieve proper mixing results. The stirring and mixing devices used to mix the ASA emulsion ingredients must achieve emulsion formation with sufficient stability (e.g., 1 to 2 hours, 1 to 20 hours, 1 to 24 hours, or 1 to 48 hours), sufficient average particle size (e.g., not more than 3, 2, or 1 µm in diameter), sufficient particle size distribution (e.g., 95% of particles with a diameter not greater than 3 µm), and sufficient intrinsic viscosity (e.g., not more than 100 cP). Petition 870260109050, dated 10 / 23 / 2026, page 30 / 63 26 / 52 when measured by a Brookfield viscometer with a 62-axis at 60 rpm and 20 °C) for use as a sizing emulsion on the wet end of a paper machine. Before adding the inventive ASA emulsions to a paper machine, it is common to expose the emulsion ingredients to a mixing pump that performs the mixing of the relevant ingredients of these emulsions. The mixing can be performed in various ways (e.g., static mixing, pump mixing, in-line mixing, or any mixing method known in the art). The ingredients of the inventive ASA sizing emulsions can be added to the feed side of a pump capable of forming emulsions. The discharge from this pump can be split so that a portion of the discharge goes to the paper machine while another portion of the discharge is fed back to the pump feed point.By controlling the percentage of output from this type of pump that is recirculated back to the pump feed point, it is possible to control the amount of energy to which the emulsion components are exposed and thus control the quality of the emulsion formed by the ASA bonding emulsion ingredients. Using sufficient energy, controlled by the output recycling rates, can control the particle size of the ASA bonding emulsion within the ranges described above. By controlling the ratio between the output and feedback of the emulsifying pump, it is possible to control the particle size of the emulsion to achieve the desired physical characteristics of these ASA emulsion sizes. Alternatively, the emulsifying pump can be operated so that no discharge is recycled to the feed point. To obtain adequate emulsion quality, it is preferable that the pump be operated at pressures exceeding atmospheric pressure. DESCRIPTION OF THE INVENTION.
[0070] The present invention relates generally to composition Petition 870260109050, dated 10 / 23 / 2026, page 31 / 63 27 / 52 tions and methods for preparing an alkenyl succinic anhydride (ASA) sizing emulsion for use in paper and cardboard manufacturing. In particular, the disclosure provides methods for double emulsification of ASA using a cationic polymer as the primary emulsifying agent and cationic starch as the secondary emulsifying agent to impart superior emulsion stability and improve sizing performance in high-ash papermaking, with considerable reduction in overall starch utilization compared to conventional natural polymer ASA emulsification applications.
[0071] Sizing is a process that reduces the extent to which dry paper or cardboard absorbs fluids. Sizing paper or cardboard improves water resistance, reduces fluid permeability, and prevents ink and printing from smudging. Two commonly used methods are internal sizing and surface sizing. Internal sizing is widely used on a wide variety of papers, while surface sizing is generally used for the production of higher quality papers.
[0072] Internal sizing involves treating the pulp with sizing agents so that the paper resists fluid absorption. Internal sizing agents are added to the fibers in the wet end of the papermaking process and generally form a strong bond with the fibers. Desirable characteristics of internal sizing agents include high hydrophobicity, a high degree of retention on the fibers, and uniform distribution throughout the fiber. Alkylsuccinic anhydride (ASA) is a commonly used internal sizing agent that reacts with hydroxyl groups on cellulose fibers through esterification reactions, thus anchoring itself to the fibers. The alkyl or alkenyl side chains of ASA impart hydrophobicity to the cellulosic material. Highly effective internal sizing agents reduce the amount Petition 870260109050, dated 10 / 23 / 2026, page 32 / 63 28 / 52 of fluid absorbed by the paper, measured by, but not limited to, the Cobb test, Hercules size test, edge wick test, water droplet test, ink float test, or any combination thereof.
[0073] ASA sizing agents tend to be hydrophobic and are generally intended for use in aqueous papermaking systems. Considerable effort is required to obtain a uniform and stable ASA emulsion suitable for papermaking. The formulation of ASA sizing agents of the type described above has presented serious problems for the application of the sizing agents to paper or cellulose prior to their formation into sheets or other useful forms. Part of the problem is that ASA sizing materials are not water-soluble and therefore must be uniformly suspended in the pulp so that the sizing agent can make proper contact with the cellulose fibers and thus create the desired effect in the final product.
[0074] Additives that will serve to emulsify or disperse the glue of ASA in the pulp and allow for size retention in the fiber. Cationic agents (e.g., various starch derivatives), along with other emulsifiers, have been successfully used as emulsifying agents to form ASA emulsions with stability, viscosity, and particle size characteristics suitable for use in papermaking.
[0075] Currently, the availability of starch for commercial applications is severely limited due to shortages in the supply chain. The present invention utilizes a double emulsification technique using a cationic solution polymer in the primary emulsification step, followed by secondary emulsification in low-dose starch under shear. Double emulsification confers superior emulsion stability and improves sizing performance in high-ash paper manufacturing, with a considerable reduction in overall utilization. Petition 870260109050, dated 10 / 23 / 2026, page 33 / 63 29 / 52 of starch compared to conventional natural polymer ASA emulsification applications.
[0076] In one aspect, the present invention provides a method for preparing a stable alkenyl succinic anhydride (ASA) sizing emulsion that is suitable for use in the manufacture of paper and cardboard, the method comprising: (a) to obtain or produce an alkenyl succinic anhydride (ASA) sizing agent; (b) combine said ASA sizing agent with a primary emulsifying agent and emulsify to form a primary emulsion; and (c) after step (b), add a secondary emulsifying agent and emulsify to form said ASA sizing emulsion, and (d) optionally, after steps (a) to (c), add the resulting stable ASA sizing emulsion to a papermaking pulp, pulp or fiber stock, optionally a high-ash paper pulp.
[0077] In some exemplary embodiments, the method also includes, after step (c): (a) adding said ASA sizing emulsion to said pulp for papermaking, pulp or fiber stock; or (b) adding said ASA sizing emulsion to said high-ash paper pulp comprising selected ashes from the group consisting of calcium carbonate, TiO2, kaolin clay, silicates, carbonate-based pigments, kaolin-based pigments or any combination thereof, wherein said high-ash paper pulp comprises an ash content percentage of 1-35%, 2-30%, 5-25% or 10-20% by mass, preferably 5-25% ash by mass. Generally, the ideal range Petition 870260109050, dated 10 / 23 / 2026, pp. 34 / 63 30 / 52 ash content is 5% to 25% for communication papers and specialty papers without wood.
[0078] In some exemplary embodiments, the ASA bonding agent comprises: (a) an ASA solid, a waxy ASA solid, a waxy ASA liquid, an ASA liquid, or a mixture thereof; and (b) a single ASA bonding agent or a mixture of ASA bonding agent molecules and / or isomers.
[0079] In some exemplary embodiments of the method (i) said primary emulsifying agent comprises an aqueous polymeric solution comprising one or more cationic polymers and water; and (ii) said secondary emulsifying agent comprises one or more cationic starches.
[0080] In some exemplary embodiments, the aqueous polymer solution comprises a weight solids percentage of one or more cationic polymers ranging from 1-70%, 2-50% or 5-30%.
[0081] In some exemplary embodiments, the aforementioned one or more cationic polymers comprise: (a) one or more synthetic copolymers, terpolymers or tetrapolymers comprising acrylamide and one or more cationic monomers selected from the group consisting of (i) diallyldialkylammonium halides, including, but not limited to, diallyldimethylammonium chloride (“DADMAC”) and diallyldiethylammonium chloride; (ii) N,N-dialkylaminoalkyl acrylates, N,N-dialkylaminoalkyl (meth)acrylates and acid addition salts and / or quaternary ammonium salts thereof, including, but not limited to, acryloyloxyethyltrimethylammonium chloride (“AETAC”), methacryloyloxyethyltrimethylammonium chloride (“MAETAC”), dimethylaminoethyl acrylate (“DMAEA”) and salts of Petition 870260109050, dated 10 / 23 / 2026, page 35 / 63 31 / 52 Acid addition of the same, dimethylaminoethyl methacrylate (“DMAEMA”) and acid addition salts thereof, quaternary methyl sulfate salt of dimethylaminoethyl acrylate, quaternary benzyl chloride salt of dimethylaminoethyl acrylate, sulfuric acid salt of dimethylaminoethyl acrylate, hydrochloric acid salt of dimethylaminoethyl acrylate, diethylaminoethyl acrylate, quaternary methyl chloride salt, quaternary dimethylaminoethyl methacrylate salt, , quaternary methyl sulfate salt, , quaternary benzyl chloride salt, sulfuric acid salt of dimethylaminoethyl methacrylate, hydrochloric acid salt of dimethylaminoethyl methacrylate, hydrochloride salt of dimethylaminoethyl methacrylate; (iii) N,N-dialkylaminoalkylacrylamides and N,N-dialkylaminoalkyl(meth)acrylamides and acid addition salts or quaternary ammonium salts thereof, including, but not limited to, acrylamidopropyltrimethylammonium chloride (“APTAC”), methacrylamidopropyltrimethylammonium chloride (“MAPTAC”), quaternary methyl sulfate salt of dimethylaminopropyl acrylamide, sulfuric acid salt of dimethylaminopropyl acrylamide, hydrochloric acid salt of dimethylaminopropyl acrylamide, quaternary methyl sulfate salt of dimethylaminopropylmethacrylamide, sulfuric acid salt of dimethylaminopropylmethacrylamide, hydrochloric acid salt of dimethylaminopropylmethacrylamide, diethylaminoethylacrylate, diethylaminoethylmethacrylate; or (iv) any combination of (i)-(iii); (b) referring to one or more synthetic copolymers, terpolymers or tetrapolymers of (a), optionally containing (i) one or more additional nonionic monomers selected from the group consisting of methacrylamide; N-alkylacrylamides, including but not limited to N-methylacrylamide, N-ethylacrylamide, N-propylacrylamide and N-butylacrylamide; N,N-dialkylacrylamides, including but not limited to N,N-dimethylacrylamide and N,N-diethylacrylamide; N-alkyl Petition 870260109050, dated 10 / 23 / 2026, pp. 36 / 63 32 / 52 methacrylamides; alkyl acrylates; hydroxyalkyl acrylates and methacrylates, including, but not limited to, hydroxymethyl acrylate, 2-hydroxyethyl acrylate, 3-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, hydroxymethyl methacrylate, 2-hydroxyethyl methacrylate, 3-hydroxypropyl methacrylate and 4-hydroxybutyl methacrylate; dihydroxyalkyl acrylates and methacrylates, including, but not limited to, 2,3-dihydroxypropyl acrylate, 3,4-dihydroxybutyl acrylate, 2,3-dihydroxypropyl methacrylate (DHPMA) and 3,4-dihydroxybutyl methacrylate; alkyl acrylates, including, but not limited to, methyl methacrylate; acrylonitrile; N-vinylmethylacetamide, N-vinylmethylformamide; N-vinyl acetate, glyoxalated acrylamides and vinylpyrrolidone; (ii) one or more additional anionic monomers selected from the group consisting of acrylic acid, methacrylic acid, sulfonic acids, phosphonic acids and alkali metal salts, alkaline earth metal salts and ammonium salts thereof, including, but not limited to, acrylic acid, methacrylic acid, maleic acid, itaconic acid, vinyl sulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid (AMPS), acrylamidomethanesulfonic acid, acrylamidoethanesulfonic acid, 2-hydroxy-3-acrylamidepropanesulfonic acid, styrenesulfonic acid and vinylphosphonic acid; or (iii) any combination of (i)-(ii); (c) one or more cationic glyoxalated polyacrylamide (GPAM) polymers obtained by reacting glyoxal with one or more synthetic copolymers, terpolymers or tetrapolymers of (a), one or more synthetic copolymers, terpolymers or tetrapolymers of (b), or a combination thereof; (d) one or more semi-synthetic polymers comprising one or more synthetic copolymers, terpolymers or tetrapolymers of (a) or (b) optionally grafted onto one or more natural polymers, Petition 870260109050, dated 10 / 23 / 2026, pp. 37 / 63 33 / 52 including, but not limited to, starch, chitin, chitosan and natural polysaccharides; or (e) any combination of (a)-(d), wherein said one or more cationic polymers have a weight-average molecular weight ranging from 10,000-3,000,000 Da, 10,000-2,000,000 Da, 10,000-1,000,000 Da, 10,000-500,000 Da, 10,000-200,000 Da, 10,000-100,000 Da or 10,000-50,000 Da.
[0082] In some exemplary embodiments, the aforementioned one or more cationic starches; (a) comprise one or more modified or unmodified cationic starches selected from the group of starches consisting of maize starch, waxy maize starch, potato starch, tapioca starch, wheat starch, rice starch, barley starch, pea starch, sweet potato starch and any combination thereof; and (b) have a percentage nitrogen content (%N) ranging from 0.2-2%, 0.2-1.75%, 0.2-1.5%, 0.2-1.25%, 0.2-1% or 0.25-0.45% by mass, preferably 0.35-1.45% by mass.
[0083] In some exemplary embodiments, said one or more cationic starches are formulated prior to the addition of said ASA binding agent by a method comprising: (a) Dissolve a dry cationic starch in water; cook by a method including, but not limited to, jet cooking, steam cooking or pan cooking; and cool to a temperature ranging from 20-80 °C, 20-60 °C, 20-40 °C or 20-25 °C, preferably 20-40 °C to obtain a cooked starch solution with a solids percentage ranging from 1-10%, 2-8% or 3-6% by mass; or (b) obtain a pre-gelatinized cationic starch with a solids percentage ranging from 20% to 40% by mass and dilute with water to obtain a pre-gelatinized starch solution with a solids percentage ranging from 1-10%, 2-8% or 3-6% by mass. Petition 870260109050, dated 10 / 23 / 2026, pp. 38 / 63 34 / 52
[0084] In some exemplary embodiments of the method, (i) the aforementioned one or more cationic polymers are selected from the group consisting of acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride copolymer (AMD / MAETAC), acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride / 2-hydroxyethyl methacrylate terpolymers (AMD / MAETAC / HEMA), acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride / 2-hydroxyethyl methacrylate / acrylic acid tetrapolymers (AMD / MAETAC / HEMA / AA), and acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride / 2,3-dihydroxypropyl methacrylate terpolymer (AMD / MAETAC / DHPMA) and (ii) said one or more cationic starches comprise maize starch, waxy maize starch, potato starch, tapioca starch, wheat starch or pea starch.
[0085] In some exemplary embodiments, the method comprises one or more of the following: (a) add said primary emulsifying agent to said alkenyl succinic anhydride (ASA) sizing agent to obtain a ratio of grams of active cationic polymer to grams of ASA of 0.05:1 to 0.6:1, 0.1:1 to 0.5:1, 0.15:1 to 0.4:1 or 0.2:1 to 0.25:1; and (b) add said secondary emulsifying agent to said primary emulsion to obtain a mass ratio of dry starch to ASA of 0.25:1 to 2:1, 0.3:1 to 1.6:1, 0.4:1 to 1.2:1 or 0.5:1 to 1:1.
[0086] In some exemplary modalities, the method comprises: (a) add said primary emulsifying agent to said ASA binding agent at room temperature and emulsify by stirring with sufficient energy to achieve an average ASA particle size ranging from 0.5-3 µm, 0.5-2 µm or 0.5-1 µm in diameter; and / or (b) add the secondary emulsifying agent to the primary emulsion at a temperature ranging from 20-80 °C, 20-60 °C, 20-40 °C Petition 870260109050, dated 10 / 23 / 2026, pp. 39 / 63 35 / 52 or 20-25 °C, preferably 20-40 °C, and emulsify by stirring with sufficient energy to achieve an average ASA particle size ranging from 0.5-3 µm, 0.5-2 µm or 0.5-1 µm in diameter.
[0087] In some exemplary embodiments, the aforementioned ASA bonding emulsion, in its final form: (a) comprises an average particle size ranging from 0.5-1 pm, 0.6-0.9 pm or 0.7-0.8 pm in diameter; (b) comprises a viscosity ranging from 10-100 cP, 20-90 cP, 30-80 cP, 40-70 cP or 50-60 cP, when measured by a Brookfield viscometer with a 62 spindle at 60 rpm and 20 °C; (c) has a stability of 1-4 min, 1-10 min, 1 min-1 h, 16 h, 1-12 h, 1-24 h or 1-48 h, wherein said stability is determined by the retention of the ASA bonding emulsion (i) an average particle size of 0.5-3 µm, 0.5-2 µm, 0.5-1 µm, 0.6-0.9 µm or 0.7-0.8 µm in diameter, preferably less than 1 µm in diameter; (ii) a viscosity ranging from 10-100 cP, 20-90 cP, 30-80 cP, 40-70 cP or 50-60 cP, preferably less than 100 cP, when measured by a Brookfield viscometer with a 62 spindle at 60 rpm and 20 °C; (d) is immediately added to a papermaking pulp, pulp or fiber stock, optionally a high-ash paper pulp or is stored in a storage tank or holding facility for a storage time of 1-4 min, 1-10 min, 1 min-1 h, 1-6 h, 1-12 h, 1-24 h or 1-48 h before the addition of said ASA sizing emulsion to a papermaking pulp, pulp or fiber stock, optionally a high-ash paper pulp; (e) comprises a reduced final mass ratio of dry starch to ASA compared to an ASA sizing emulsion prepared by a single or double emulsification method. Petition 870260109050, dated 10 / 23 / 2026, pp. 40 / 63 36 / 52 using one or more emulsifying agents comprising one or more cationic starches; or (f) any combination of (a)-(e).
[0088] In some exemplary embodiments of the method, when stable alkenyl succinic anhydride (ASA) sizing emulsion is used as a sizing agent during the manufacture of paper or cardboard, it results in a sheet-like product selected from the group consisting of a high-ash paper or cardboard, a printing or writing grade paper or cardboard, an alkaline printing or writing grade paper or cardboard, a bleached paper or cardboard, a packaging grade paper or cardboard, and a partially recycled or 100% recycled paper or cardboard, wherein the sheet-like product comprises optimal sizing performance as measured by industry standardized tests, including but not limited to HST, Cobb, water drop test, contact angle, edge wilt, or water penetration,wherein the ideal bonding performance is determined in relation to a sheet-like equivalent product comprising an ASA bonding emulsion prepared by a single or double emulsification method using one or more emulsifying agents comprising one or more cationic starches.
[0089] In another aspect, the present invention provides a double emulsification method for preparing an alkenyl succinic anhydride (ASA) sizing emulsion for use in the manufacture of paper and cardboard, the method comprising: (a) to obtain or produce an alkenyl succinic anhydride (ASA) sizing agent; (b) combine the said ASA bonding agent with a primary emulsifying agent and emulsify at room temperature and Petition 870260109050, dated 10 / 23 / 2026, pp. 41 / 63 37 / 52 Stir with sufficient energy to achieve an average ASA particle size ranging from 0.5-3 µm, 0.5-2 µm or 0.5-1 µm in diameter, thus forming a primary emulsion; (c) after step (b), add a secondary emulsifying agent and emulsify at a temperature ranging from 20-80 °C, 20-60 °C, 20-40 °C or 20-25 °C, preferably 20-40 °C and stir with sufficient energy to achieve an average ASA particle size ranging from 0.5-3 µm, 0.5-2 µm or 0.5-1 µm in diameter, thus forming said ASA sizing emulsion, and (d) optionally, after step (c), add said ASA sizing emulsion to a high-ash papermaking pulp, wherein (i) said primary emulsifying agent comprises an aqueous polymer solution comprising cationic acrylamide copolymers selected from the group consisting of acrylamide / [2-(methyl-acryloyloxy)ethyl]trimethylammonium chloride copolymer (AMD / MAETAC),acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride / 2-hydroxyethyl methacrylate (AMD / MAETAC / HEMA) terpolymers, acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride / 2-hydroxyethyl methacrylate / acrylic acid (AMD / MAE-) tetrapolymers TAC / HEMA / AA) and acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride / 2,3-dihydroxypropyl methacrylate terpolymer (AMD / MAETAC / DHPMA); (ii) the said secondary emulsifying agent comprises one or more modified or unmodified cationic starches; selected from the group of starches consisting of corn starch, waxy corn starch, potato starch, tapioca starch, wheat starch, pea starch and a mixture thereof; (iii) the said pulp for the manufacture of high-content paper Petition 870260109050, dated 10 / 23 / 2026, pp. 42 / 63 38 / 52 of ash comprises ash selected from the group consisting of calcium carbonate, TiO2, kaolin clay, silicates, carbonate-based pigments, kaolin-based pigments or any combination thereof; (iv) the said material for the manufacture of high-ash paper comprises an ash percentage of 1-35%, 2-30%, 5-25% or 10-20% by mass, preferably 5%-25% ash by mass; (v) said primary emulsifying agent is added to said alkenyl succinic anhydride (ASA) sizing agent to obtain a ratio of grams of active cationic polymer to grams of ASA of 0.05:1 to 0.6:1, 0.1:1 to 0.5:1, 0.15:1 to 0.4:1 or 0.2:1 to 0.25:1; and (vi) said secondary emulsifying agent is added to said primary emulsion to obtain a mass ratio of dry starch to ASA of 0.25:1 to 2:1, 0.3:1 to 1.6:1, 0.4:1 to 1.2:1 or 0.5:1 to 1:1.
[0090] In another aspect, the present invention provides an ASA sizing emulsion composition or a pulp for making paper, pulp or fiber stock, optionally a high-ash paper pulp, comprising said ASA sizing emulsion composition, obtained by a method according to any of the foregoing.
[0091] In another aspect, the present invention provides a process for the production of paper or cardboard, the process comprising obtaining a high-ash paper pulp comprising wood pulp, optionally a fiber stock comprising a high content of recycled fibers and / or production waste fibers, optionally a concentrated fiber stock, optionally a bleached fiber stock, optionally containing process water from the production of pulp, paper or cardboard and treating the Petition 870260109050, dated 10 / 23 / 2026, pp. 43 / 63 39 / 52 referred to as fiber stock at the wet end of a paper machine with an ASA sizing emulsion according to any of the preceding claims, wherein: (a) said high-ash paper pulp comprises ash selected from the group consisting of calcium carbonate, TiO2, kaolin clay, silicates, carbonate-based pigments, kaolin-based pigments or any combination thereof; and (b) said high-ash paper pulp comprises an ash content percentage of 1-35%, 2-30%, 5-25% or 10-20% by mass, preferably 5-25% ash by mass.
[0092] The methods and compositions disclosed herein may be appropriately applied in the absence of any element not specifically disclosed herein and / or any element specifically disclosed herein. Examples of embodiments of the invention and their advantages are further disclosed in the following examples. EXAMPLES
[0093] The examples given here are for illustrative purposes so that the invention may be more fully understood. These examples should not be construed as limiting the invention in any way. EXAMPLE 1: DOUBLE EMULSIFICATION METHOD FOR PREPARING ALKENYL SUCCINIC ANHYDRIDE (ASA) BONDING EMULSIONS
[0094] ASA sizing emulsions were prepared to be evaluated as a sizing agent for paper or cardboard. The inventive methods of double emulsification, using a cationic solution polymer as a primary emulsifier in a primary emulsification step followed by a secondary emulsification using cationic starch as a low-dose secondary emulsifier under shear, were Petition 870260109050, dated 10 / 23 / 2026, pp. 44 / 63 40 / 52 compared to conventional emulsification techniques using only starch as a control. An exemplary flowchart for conventional ASA emulsification and the inventive double emulsification method (New Two-Step Approach) are shown in Figure 1. DOUBLE EMULSIFICATION METHOD
[0095] Alkenyl succinic anhydride (ASA) bonding emulsions were prepared in the laboratory by a double emulsification procedure, ensuring that the shear rate and time were kept constant for all emulsions.
[0096] A primary emulsifying agent was prepared from a water-based solution of a cationic acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride / 2-hydroxyethyl methacrylate (AMD / MAETAC / HEMA) terpolymer (Polymer 1).
[0097] A secondary emulsifying agent was prepared by cooking dry cationic modified corn starch in a jet cooker to obtain a liquid starch solution with a working solids content of 3-6% by mass (cooked starch, i.e., wet-end cationic starch cooked in a mill). The starch had a nitrogen content of 0.25-0.45% by mass. Alternatively, pre-gelatinized starch can be obtained with a typical solids content in the range of 20-40% by mass. This pre-gelatinized solution can be diluted with water on site to the desired working solids range of 3-6% by mass.
[0098] The primary emulsifying agent containing an acrylamide-based polymer solution was added to the alkenyl succinic anhydride (ASA) sizing agent at a primary emulsifier to ASA ratio of 0.8:1 or 1:1 by mass, as per Figure 2. Primary emulsification was carried out at room temperature (20 °C) using a high-shear pump until it was completely emulsified to form a primary emulsion.
[0099] After a short period of time (less than 10 minutes), the Petition 870260109050, dated 10 / 23 / 2026, pp. 45 / 63 41 / 52 Secondary emulsifying agent was added to the primary emulsion mixture at a ratio of secondary emulsifier (starch) to ASA of 0.5:1 to 2:1 by mass, and secondary emulsification was carried out at room temperature (20 °C) or elevated temperature (80 °C), as per Figure 2, using a high shear pump until completely emulsified to form a double-emulsified (secondary) ASA bonding emulsion. CONVENTIONAL EMULSIFICATION METHODS (CONTROL)
[0100] Single and double emulsion control emulsions were prepared according to standard techniques using the same cooked starch emulsifying agent described in the double emulsification method.
[0101] For individually emulsified control samples, the cooked starch emulsifying agent was added at room temperature (20 °C) to the alkenyl succinic anhydride (ASA) sizing agent in a primary emulsification step at a 4:1 mass ratio (starch to ASA), as per Figure 2. Emulsification was performed using a high shear pump until fully emulsified.
[0102] For individually emulsified control samples, the cooked starch emulsifying agent was added at room temperature (20 °C) to the alkenyl succinic anhydride (ASA) sizing agent in a primary emulsification step at a ratio of 2:1 or 4:1 by mass (starch to ASA), as per Figure 2. For doubly emulsified control samples, a secondary emulsification was performed by adding the same cooked starch emulsifying agent at room temperature (20 °C) at a ratio of 2:1 by mass (starch to ASA), as per Figure 2. Primary and secondary emulsifications were performed using a high-shear pump until complete emulsification.
[0103] Complete emulsification was determined by the emulsion Petition 870260109050, dated 10 / 23 / 2026, pp. 46 / 63 42 / 52 having an average ASA particle size ranging from 0.5-3 µm, 0.5-2 µm or 0.5-1 µm in diameter and an ASA particle size distribution in which 95% of the ASA particles have a diameter of no more than 3 µm. EVALUATION OF WING EMULSIONS
[0104] Primary, secondary and control ASA emulsions, prepared according to inventive double emulsification methods and conventional (control) emulsification methods, were analyzed for particle size and viscosity.
[0105] Primary, secondary, and control ASA emulsions were analyzed for average particle size (average PS) and maximum particle diameter (95% of diameter) immediately after emulsification. Secondary and control ASA emulsions were also analyzed for initial viscosity immediately after emulsification. To determine the relative stability of the emulsions, the secondary and control ASA emulsions were aged for 2 hours at room temperature (20 °C) and then analyzed for final particle size and final viscosity. The particle size and viscosity results are shown in Figure 2.
[0106] For secondary emulsions before and after aging, an average particle size below 1 micron and 95% diameter below 3 µm was considered desirable for laboratory papermaking applications. The ideal particle size distribution is smaller for field applications due to the shear mechanics of the emulsification equipment, resulting in emulsions with smaller particle sizes.
[0107] The results indicate that the ASA samples from the inventive double emulsification process made with cationic polymer as the primary emulsifier (Polymer 1) and starch as the secondary starch emulsifier exhibit good particle size. All ASA samples of Petition 870260109050, dated 10 / 23 / 2026, pp. 47 / 63 43 / 52 double emulsification samples showed a secondary average particle size below 1 μm before and after 2 hours of retention. The final 95% diameter values were also well below 3 μm for all double emulsification ASA samples. These particle size results indicate that the inventive double emulsification method provides highly desirable particle size distributions that are stable for at least 2 hours.
[0108] The best final particle size results were obtained using a polymer to ASA ratio of 0.8:1 in the primary emulsifier and a starch to ASA ratio of 0.5:1 in the secondary emulsifier. Surprisingly, these particle size results were comparable to or better than control samples prepared using only starch at a much higher starch to ASA ratio (e.g., 4:1 overall).
[0109] Viscosity below 100 cP, when measured by a Brookfield 62-axis viscometer at 60 rpm and 20 °C, after a holding time of 2 hours, was indicative of good emulsion stability and considered desirable for papermaking applications.
[0110] The viscosity results for the inventive double-emulsified ASA samples were highly indicative of good ASA emulsion stability. All double-emulsified ASA samples showed initial viscosity results below 100 cP, and more than 2 / 3 of the samples maintained viscosity below 100 cP after 2 hours of holding, indicating good emulsion stability. Surprisingly, these results were comparable to or better than control samples prepared using only starch at a much higher starch-to-ASA ratio (e.g., 4:1 overall). On the other hand, all control samples showed extremely poor final viscosity results, indicating low stability.
[0111] It was surprisingly observed that the inventive method Petition 870260109050, dated 10 / 23 / 2026, pp. 48 / 63 Double emulsification (44 / 52) was able to reduce the overall starch demand by 75-80%, while achieving equally desirable or improved particle sizes and viscosity-based stability.
[0112] Without limiting ourselves to theory, a mechanistic justification for these surprising results is that the primary emulsification step with polymer as the primary emulsifier results in smaller and narrower particle sizes compared to those formed with cooked starch as the primary emulsifier. The surface area is smaller, so less starch is needed in the secondary step to obtain emulsions with comparable or superior stability. Furthermore, the use of a shear pump during the secondary emulsification step facilitates the incorporation of starch into the particles, further allowing for the use of less starch. Typically, for conventional methods, shear pumping is performed only during the initial emulsification step.
[0113] Normally, during emulsification, ASA hydrolysis is an undesirable side reaction, which follows a first-order rate kinetics. Elevated temperatures increase the rate of hydrolysis. For this reason, starch is normally cooled to room temperature before being added to AAS to retard hydrolysis. It was surprising to find that starch temperatures of 25 °C and 80 °C provided an increase in particle size and stability of the inventive double emulsification technique.
[0114] These results provide a proof of concept that the inventive double emulsification method can be used to prepare double emulsion ASA bonding emulsions with enhanced emulsion properties, using less starch compared to conventional natural polymer ASA emulsification methods. Petition 870260109050, dated 10 / 23 / 2026, pp. 49 / 63 45 / 52 EXAMPLE 2: EVALUATION OF DOUBLE-EMULSIFIED WINGED EMULSIONS FOR HAND-BINDING SHEETS PREPARATION OF HAND-BINDED SHEETS
[0115] Double-emulsified ASA bonding emulsions and a control emulsion (starch only) were prepared according to Example 1 with cationic polymer (Polymer 1) as the primary emulsifying agent and starch as the secondary emulsifying agent using emulsification conditions shown in Table 1. The resulting ASA emulsions were evaluated for emulsion quality based on particle size and viscosity, and then the emulsions were used as bonding for hand-made sheets. The results for particle size and viscosity are shown in Table 1. TABLE 1: WING EMULSIFICATION CONDITIONS, PARTICLE SIZES AND VISCOSITY MEASUREMENTS FOR STUDIES FROM HANDWRITTEN SHEETS. Primary Emulsifier Primary Polymer Ratio (for ASA) Secondary Emulsifier Secondary Starch Ratio (for ASA) Primary Median PS (micron) Primary Diameter 95% (micron) Secondary Median PS (micron) Secondary Diameter 95% (micron) Cationic Starch 4 none 0 0.609 1.48 Polymer 1 1 Cationic Starch (25°C) 2 0.746 1.5 0.959 34.59 Polymer 1 1 Cationic Starch (80°C) 1 0.746 1.5 0.948 29.34 Polymer 1 1 Cationic Starch (25°C) 1 0.873 1.69 0.943 40.5 Polymer 1 1 Cationic Starch (25°C) 0.5 0.873 1.69 0.871 2.513 Polymer 1 0.8 Cationic Starch (25°C) 1 0.851 1.69 1.002 39.76 Polymer 1 0.8 Cationic Starch (25°C) 0.75 0.851 1.69 0.944 2.469
[0116] The hand-rolled sheets were prepared in a Noble and Wood hand-rolled sheet mold. The material was supplied by a paper mill using a mixture of hardwood and softwood with a high content of Petition 870260109050, dated 10 / 23 / 2026, pages 50 / 63 46 / 52 filler (15%) HOPCC. ASA sizing emulsions were incorporated into the supplied material. Efforts were made to simulate the factory retention system to ensure proper retention of the ASA on the handsheets. Handsheets were produced and then paper samples were conditioned for at least one day at 23°C and 50% relative humidity. This follows the TAPPI T 402 om-93 standard conditioning method and test atmospheres for paper, board, pulp, test sheets and related products. EVALUATION OF MANUAL SHEETS
[0117] The Cobb test was performed to determine the mass of water absorbed by the surface of the scaled paper sheets, in g / m2 (gsm) over a period of time. Lower water absorption mass indicates better water resistance. For the manual sheet study, the Cobb test was performed using deionized water at 23 °C with an elapsed time of 2 minutes. The paper sheet preparation conditions (ASA dosage in lbs / ton, primary and secondary agent ratios to ASA, and temperature) and the Cobb results are shown in Figure 3.
[0118] The Hercules size test (HST) was performed to measure the time required for the ink to penetrate the paper sheets. Longer times indicate better ink resistance. For the present hand-paper study, the HST test was performed using 80% reflectance and 1% formic acid ink. The hand-paper preparation conditions (ASA dosage in lbs / ton, primary and secondary agent ratios to ASA, and temperature) and the HST results are shown in Figure 4.
[0119] Cobb's results indicate good bonding performance of the inventive double-emulsification ASA samples made with cationic polymer as primary emulsifier (Polymer 1) and starch as secondary starch emulsifier, compared to Petition 870260109050, dated 10 / 23 / 2026, pp. 51 / 63 47 / 52 starch-only controls and Polymer-only 1 plus controls. A restricted clustering of Cobb values means that the sizing is evenly distributed throughout the sheet, as opposed to uneven distribution between the top and bottom of the sheet.
[0120] Little variability in Cobb values was observed for paper sheets made with 5# / ton of ASA. However, a large variability was observed at the ASA dosage of 3# / ton, with the inventive double-emulsified ASA providing the best Cobb values (1st polymer:ASA ratio of 0.8:1 and 2nd starch:ASA ratio of 1:1). This sample provided the lowest Cobb values with the most accurate data clustering, indicating better water resistance and better sizing coverage at the lowest ASA dosage (3# / ton) than the starch control and the polymer control.
[0121] Little variability in HST values was observed for hand sheets made with 5# / ton of ASA. However, a large variability was observed at the ASA dosage of 3# / ton, with the inventive double-emulsified ASA providing the best HST values (1st polymer:ASA ratio of 0.8:1 and 2nd starch:ASA ratio of 1:1). This sample provided the highest HST values with the most rigorous data grouping, indicating better ink resistance and better bonding coverage at the lower ASA dosage (3# / ton) than the starch control and the polymer control.
[0122] These results provide proof of concept that the inventive double emulsification method can be used to prepare double emulsion ASA sizing emulsions with enhanced sizing properties for paper products, using less starch compared to conventional natural polymer ASA emulsification methods. These results also provide proof of concept that the inventive double emulsification ASA samples Petition 870260109050, dated 10 / 23 / 2026, pp. 52 / 63 48 / 52 can be used effectively for sizing in order to improve the water and ink resistance of paper sheets. EXAMPLE 3: EVALUATION OF DOUBLE-EMULSIFIED WING EMULSIONS FOR SIZED PAPER, INTENDED FOR SIZED HIGH-ASH PULP
[0123] Control ASA sizing emulsions were prepared using only starch and only polymer according to Example 1. These ASA sizing emulsions were used to produce paper sheets from high-ash (20% ash) paper pulp, which were evaluated for water resistance (Cobb test) and ink resistance (HST) according to Example 2. The HST results of the starch-emulsified ASA compared to a synthetic polymer-emulsified ASA are shown in Figure 5. The Cobb results of the inventive double-emulsified ASA compared to the starch-emulsified ASA are shown in Figure 6.
[0124] Ash generally refers to calcium carbonate, TiO2, kaolin clay, silicates, and other carbonate- and kaolin-based pigments. Paper with a high ash content is typically used to produce alkaline paper for printing and writing.
[0125] The effectiveness of modified natural polymer (cationic starch) used in high dosages as an emulsifying agent is well documented for ASA sizing applications of materials containing significant ash content (up to 35% ash). When ash is present, the sizing normally bonds rapidly to the ash surface, and if this ash-sizing mixture is not retained on the paper, the sizing will be lost. Therefore, for alkaline printing and paperboard, including packaging materials, it is essential that ASA sizing emulsions are effectively retained on the paper and not lost with the ash. Petition 870260109050, dated 10 / 23 / 2026, pages 53 / 63 49 / 52
[0126] Figure 5 illustrates the effectiveness of an ASA emulsified with starch compared to an ASA emulsified with synthetic polymer in a thin paper blend containing 20% ash content. The deficiency of the synthetic polymer alone in providing water resistance, when used as an emulsifying agent for ASA sizing emulsions for high-ash paper sizing, is apparent.
[0127] Figure 6 shows an exemplary bar graph of Cobb values indicating similar bonding performance for ASA emulsions prepared using the inventive double emulsification method (red bars) compared with starch alone (blue bars). Figure 6 illustrates that the inventive double emulsification for ASA bonding, using synthetic polymer in the primary emulsification followed by a low-dose application of cationic starch for secondary emulsification, allows a significant reduction in starch usage without loss of bonding response.
[0128] These results provide further proof of concept that the inventive double emulsification method can be used as a bonding agent to achieve bonding performance equivalent to or better than starch at high doses, while significantly reducing the total amount of starch used. EXAMPLE 4: EXTENDED STABILITY OF DOUBLE-EMULSIFIED WING BONDING EMULSIONS
[0129] Double-emulsified ASA bonding emulsions were prepared according to Example 1 and maintained for 48 hours for observation and analysis by particle size determination and viscosity measurement. Samples were stored in glass containers at room temperature (20 °C) before analysis. Stability can be assessed based on the average particle size or particle size distribution of the emulsion. Petition 870260109050, dated 10 / 23 / 2026, pages 54 / 63 50 / 52 Specifically, for average particle size, an emulsion can be considered stable when it maintains an average particle size smaller than a specified value for a given period of time after emulsification. For particle size distribution, an emulsion can be considered stable when at least 95% of the particle size is smaller than a specified value for a given period of time after emulsification. The specified value for average particle size or particle size can be [e.g., ranging between 0.5 microns and 3 microns]. The time period provided can be [e.g., ranging between 1 minute and 48 hours]. For example, in a laboratory setting, an emulsion can be considered stable when the average particle size or at least 95% of the particles have a particle size smaller than 3 microns after the completion of the laboratory emulsification process.In an industrial setting, an emulsion is considered stable when the average particle size, or at least 95% of the particles, is smaller than 2 microns after the emulsification process is complete. Typically, emulsions are used in a papermaking process for 1 to 10 minutes, 10 minutes to 1 hour, or 1 to 4 hours after emulsification is complete.
[0130] Extended stability tests were performed to determine the extended stability of the inventive double-emulsified ASA bonding emulsions compared to control ASA emulsions prepared with conventional starch emulsifiers. The results showing the particle size distribution and viscosity measurements over time to reflect emulsion stability are shown in Table 2.
[0131] These extended stability results provide further proof of concept that the inventive double emulsification method can be used to form highly bonding ASA emulsions Petition 870260109050, dated 10 / 23 / 2026, pages 55 / 63 51 / 52 stable materials that can be temporarily stored on-site or off-site in a storage unit or holding tank for up to 48 hours for later use. These results are especially beneficial for recycled cardboard applications. Petition 870260109050, dated 10 / 23 / 2026, pages 56 / 63 52 / 52 Table 2: Particle size and viscosity stability of wing emulsions prepared by the inventive double emulsification technique. Average Particle Size (^m) Primary Emulsifier Primary Emulsifier Ratio (for ASA) Secondary Emulsifier Secondary Emulsifier Ratio (for ASA) Initial 2 h 24 h 48 h Starch 4 None 0 n / a 0.816 2.159 gelled Polymer 1 0.8 None 0 n / a 0.921 1.145 2.44 Polymer 1 0.8 Polymer 1 0.5 0.975 0.901 1.046 1.699 Polymer 1 0.8 Starch 0.5 0.834 0.861 1.293 6.902 Polymer 1 0.8 Starch 1 0.884 0.921 1.302 3.986 Table 2 -continued- 95% particles < ^m) Viscosity (cP) Initial 2 h 24 h 48 h Initial 2 h 24 h 48 hn / a 1.724 21.984 n / an / a gelled 3564 n / an / a 1.882 2.66 8.126 n / a 4 40.5 33.6 2.228 1.953 2.433 5.574 15.9 40.5 44 45.6 1.678 1.456 3.545 18.101 41.1 7 57 69.6 1.867 1.928 3.541 14.542 41.7 96.5 297.5 346.8 Petition 870260109050, dated 10 / 23 / 2026, pp. 57 / 63
Claims
1 / 11 CLAIMS 1. Method for preparing a stable alkenyl succinic anhydride (ASA) sizing emulsion suitable for use in paper and paperboard manufacturing, characterized in that it comprises: (a) obtaining or producing an alkenyl succinic anhydride (ASA) sizing agent; (b) combining said ASA sizing agent with a primary emulsifying agent and emulsifying to form a primary emulsion; and (c) after step (b), adding a secondary emulsifying agent and emulsifying to form said ASA sizing emulsion, and (d) optionally, after steps (a) to (c), adding the resulting stable ASA sizing emulsion to a papermaking pulp, pulp or fiber stock, optionally a high-ash paper pulp.
2. Method according to claim 1, characterized in that it further comprises, after step (c): (a) adding said ASA sizing emulsion to said paper pulp, pulp or fiber stock; or (b) adding said ASA sizing emulsion to said high-ash paper pulp comprising selected ashes from the group consisting of calcium carbonate, TiO2, kaolin clay, silicates, carbonate-based pigments, kaolin-based pigments or any combination thereof, wherein said high-ash paper pulp comprises an ash percentage of 1-35%, 2-30%, 5-25% or 10-20% by mass, preferably 5%-25% ash by mass. Petition 870250087440, dated 09 / 26 / 2025, p. 59 / 85 2 / 11 3. Method according to claim 1 or 2, characterized in that said ASA bonding agent comprises: (a) an ASA solid, a waxy ASA solid, a waxy ASA liquid, an ASA liquid or a mixture thereof; and (b) a single ASA bonding agent or a mixture of ASA bonding agent molecules and / or isomers.
4. Method, according to any one of claims 1 to 3, characterized in that (i) said primary emulsifying agent comprises an aqueous polymeric solution comprising one or more cationic polymers and water; and (ii) said secondary emulsifying agent comprises one or more cationic starches.
5. Method, according to any one of claims 1 to 4, characterized in that said aqueous polymer solution comprises a percentage of solids by weight of said one or more cationic polymers ranging from 1-70%, 2-50% or 5-30%.
6. Method according to any one of claims 1 to 5, characterized in that said one or more cationic polymers comprise: (a) one or more synthetic copolymers, terpolymers or tetrapolymers comprising acrylamide and one or more cationic monomers selected from the group consisting of (i) diallyldialkylammonium halides, including, but not limited to, diallyldimethylammonium chloride (“DADMAC”) and diallyldiethylammonium chloride; (ii) N,N-dialkylaminoalkyl acrylates, N,N-dialkylaminoalkyl (meth)acrylates and acid addition salts and / or quaternary ammonium salts thereof, including, but not limited to, acryloyloxyethyltrimethylammonium chloride (“AETAC”), methacryloyloxyethyltrimethylammonium chloride (“MAETAC”), dimethylaminoethyl acrylate (“DMAEA”) and acid addition salts thereof, dimethylaminoethyl methacrylate (“DMAEMA”) and acid addition salts thereof,quaternary salt of dimethylaminoethyl acrylate methyl sulfate, quaternary salt of dimethylaminoethyl acrylate benzyl chloride, sulfuric acid salt of dimethylaminoethyl acrylate, hydrochloric acid salt of dimethylaminoethyl acrylate, diethylaminoethyl acrylate, quaternary salt of methyl chloride, quaternary salt of dimethylaminoethyl methacrylate methyl chloride, quaternary salt of dimethylaminoethyl methacrylate methyl sulfate, quaternary salt of dimethylaminoethyl methacrylate benzyl chloride, sulfuric acid salt of dimethylaminoethyl methacrylate, hydrochloric acid salt of dimethylaminoethyl methacrylate, hydrochloric acid salt of methacryloyl dimethylaminoethyl; (iii) N,N-dialkylaminoalkylacrylamides and N,N-dialkylaminoalkyl(meth)acrylamides and acid addition salts or quaternary ammonium salts thereof, including, but not limited to, acrylamidopropyltrimethylammonium chloride (“APTAC”),methacrylamide-propyltrimethylammonium chloride (“MAPTAC”), quaternary methyl sulfate salt of dimethylaminopropyl acrylamide, sulfuric acid salt of dimethylaminopropyl acrylamide, hydrochloric acid salt of dimethylaminopropyl acrylamide, quaternary methyl sulfate salt of dimethylaminopropyl methacrylamide, sulfuric acid salt of dimethylaminopropyl methacrylamide, hydrochloric acid salt of dimethylaminopropyl methacrylamide, diethylaminoethyl acrylate, diethylaminoethyl methacrylate; or (iv) any combination of (i)-(iii); (b) said one or more synthetic copolymers, terpolymers or tetrapolymers of (a), optionally containing: (i) one or more additional nonionic monomers selected from the group consisting of methacrylamide; N-alkylacrylamides, including, but not limited to, N-methylacrylamide, N-ethylacrylamide, N-propylacrylamide and N-butylacrylamide; N,N-dialkylacrylamides, including, but not limited to, N,N-dimethylacrylamide and N,N-diethylacrylamide; N-alkyl methacrylamides; alkyl acrylates; hydroxyalkyl acrylates and methacrylates, including, but not limited to, hydroxymethyl acrylate, 2-hydroxyethyl acrylate, 3-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, hydroxymethyl methacrylate, 2-hydroxyethyl methacrylate, 3-hydroxypropyl methacrylate and 4-hydroxybutyl methacrylate; dihydroxyalkyl acrylates and methacrylates, including, but not limited to, 2,3-dihydroxypropyl acrylate, 3,4-dihydroxybutyl acrylate, 2,3-dihydroxypropyl methacrylate (DHPMA) and 3,4-dihydroxybutyl methacrylate; Alkyl acrylates, including, but not limited to, methyl methacrylate; acrylonitrile; N-vinylmethylacetamide, N-vinylmethylformamide; N-vinyl acetate, glyoxalated acrylamides and vinylpyrrolidone; (ii) one or more additional anionic monomers selected from the group consisting of acrylic acid, methacrylic acid, sulfonic acids,phosphonic acids and alkali metal salts, alkaline earth metal salts and ammonium salts thereof, including, but not limited to, acrylic acid, methacrylic acid, maleic acid, itaconic acid, vinyl sulfonic acid, 2-acrylamido-2-methylpropanesulfonic acid (AMPS), acrylamidomethanesulfonic acid, acrylamidoethanesulfonic acid, 2-hydroxy-3-acrylamidepropanesulfonic acid, styrenesulfonic acid and vinyl phosphonic acid; or (iii) any combination of (i)-(ii); (c) one or more cationic glyoxylated polyacrylamide (GPAM) polymers obtained by reacting glyoxal with said one or more synthetic copolymers, terpolymers or tetrapolymers of (a), one or more synthetic copolymers, terpolymers or tetrapolymers of (b), or a combination thereof; (d) one or more semi-synthetic polymers comprising said one or more copolymers, terpolymers or tetrapolymers. Petition 870250087440, dated 26 / 09 / 2025.pg. 62 / 85 5 / 11 synthetics of (a) or (b) optionally grafted onto one or more natural polymers, including, but not limited to, starch, chitin, chitosan and natural polysaccharides; or (e) any combination of (a)-(d), wherein the said one or more cationic polymers have a weight-average molecular weight ranging from 10,000-3,000,000 Da, 10,000-2,000,000 Da, 10,000-1,000,000 Da, 10,000-500,000 Da, 10,000-200,000 Da, 10,000-100,000 Da or 10,000-50,000 Da.
7. Method according to any one of claims 1 to 6, characterized in that said one or more cationic starches: (a) comprise one or more modified or unmodified cationic starches, selected from the group of starches consisting of corn starch, waxy corn starch, potato starch, tapioca starch, wheat starch, rice starch, barley starch, pea starch, sweet potato starch and any combination thereof; and (b) have a percentage nitrogen content (%N) ranging from 0.2-2%, 0.2-1.75%, 0.2-1.5%, 0.2-1.25%, 0.2-1% or 0.25-0.45% by mass, preferably 0.35-1.45% by mass.
8. Method, according to any one of claims 1 to 7, characterized in that said one or more cationic starches are formulated prior to addition to said ASA sizing agent by a method comprising: (a) dissolving a dry cationic starch in water; cooking by a method including, but not limited to, jet cooking, steam cooking or pan cooking; and cooling to a temperature ranging from 20-80°C, 20-60°C, 20-40°C or 20-25°C, preferably 20-40°C to obtain a cooked starch solution with a solids percentage ranging from 1-10%, 2-8% or 3-6% by mass; or Petition 870250087440, dated 09 / 26 / 2025, p. 63 / 85 6 / 11 (b) obtain a pregelatinized cationic starch with a solids percentage ranging from 20% to 40% by mass and dilute with water to obtain a pregelatinized starch solution with a solids percentage ranging from 1-10%, 2-8% or 3-6% by mass.
9. A method according to any one of claims 1 to 8, characterized in that said one or more cationic polymers are selected from the group consisting of acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride copolymer (AMD / MAETAC), acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride / 2-hydroxyethyl methacrylate terpolymers (AMD / MAETAC / HEMA), acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride / 2-hydroxyethyl methacrylate / acrylic acid tetrapolymers (AMD / MAETAC / HEMA / AA), and acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride / 2,3-dihydroxypropyl methacrylate terpolymer (AMD / MAETAC / HEMA / AA). (AMD / MAETAC / DHPMA) and (ii) the aforementioned one or more cationic starches comprise maize starch, waxy maize starch, potato starch, tapioca starch, wheat starch or pea starch.
10. Method, according to any one of claims 1 to 9, characterized in that it comprises one or more of the following: (a) adding said primary emulsifying agent to said alkenyl succinic anhydride (ASA) sizing agent to obtain a ratio of grams of active cationic polymer to grams of ASA of 0.05:1 to 0.6:1, 0.1:1 to 0.5:1, 0.15:1 to 0.4:1 or 0.2:1 to 0.25:1; and (b) adding said secondary emulsifying agent to said primary emulsion to obtain a mass ratio of dry starch to ASA of 0.25:1 to 2:1, 0.3:1 to 1.6:1, 0.4:1 to 1.2:1 or 0.5:1 to 1:
1.
11. Method, according to any one of claims 1 to 10, characterized in that it comprises: Petition 870250087440, dated 09 / 26 / 2025, p. 64 / 85 7 / 11 (a) adding said primary emulsifying agent to said ASA binding agent at room temperature and emulsifying by stirring with sufficient energy to achieve an average ASA particle size ranging from 0.5-3 μm, 0.5-2 μm or 0.5-1 μm in diameter; and / or (b) add said secondary emulsifying agent to the primary emulsion at a temperature ranging from 20-80°C, 20-60°C, 20-40°C or 20-25°C, preferably 20-40°C and emulsify by stirring with sufficient energy to achieve an average ASA particle size ranging from 0.5-3 μm, 0.5-2 μm or 0.5-1 μm in diameter.
12. Method according to any one of claims 1 to 11, characterized in that said ASA bonding emulsion, in the final form: (a) comprises an average particle size ranging from 0.5-1 μm, 0.6-0.9 μm or 0.7-0.8 μm in diameter; (b) comprises a viscosity ranging from 10-100 cP, 2,090 cP, 30-80 cP, 40-70 cP or 50-60 cP, when measured by a Brookfield viscometer with a 62 spindle at 60 rpm and 20 °C; (c) has a stability of 1-4 min, 1-10 min, 1 min-1 h, 16 h, 1-12 h, 1-24 h or 1-48 h, wherein said stability is determined by the retention of the ASA bonding emulsion of (i) an average particle size of 0.5-3 μm, 0.5-2 μm, 0.5-1 μm, 0.6-0.9 μm or 0.7-0.8 μm in diameter, preferably less than 1 μm; (ii) a viscosity ranging from 10-100 cP, 20-90 cP, 30-80 cP, 40-70 cP or 50-60 cP, preferably less than 100 cP, when measured by a Brookfield viscometer with a 62 spindle at 60 rpm and 20°C;(d) is immediately added to a papermaking pulp, pulp or fiber stock, optionally a high-ash paper pulp or is stored in a storage tank or holding facility for a storage time of 1-4 min, 1-10 min, 1 min-1 h, 1-6 h, 1-12 h, 1-24 h or 1-48 h before the addition of said ASA sizing emulsion to a papermaking pulp, pulp or fiber stock, optionally a high-ash paper pulp; (e) comprises a reduced final mass ratio of dry starch to ASA compared to an ASA sizing emulsion prepared by a single or double emulsification method using one or more emulsifying agents comprising one or more cationic starches; or (f) any combination of (a)-(e).; 13. A method according to any one of claims 1 to 12, characterized in that when said stable alkenyl succinic anhydride (ASA) sizing emulsion is used as a sizing agent during the manufacture of paper or cardboard, it results in a sheet-like product selected from the group consisting of a high-ash paper or cardboard, a printing or writing grade paper or cardboard, an alkaline printing or writing grade paper or cardboard, a bleached paper or cardboard, a packaging grade paper or cardboard, and a partially recycled or 100% recycled paper or cardboard, wherein said sheet-like product comprises optimal sizing performance as measured by industry standardized tests, including but not limited to HST, Cobb, water drop test, contact angle, edge wilt or water penetration, or combinations thereof,wherein the said ideal bonding performance is determined in relation to a sheet-like equivalent product comprising an ASA bonding emulsion prepared by a method of Petition 870250087440, dated 09 / 26 / 2025, page 66 / 85 9 / 11, single or double emulsification using one or more emulsifying agents comprising one or more cationic starches.
14. Double emulsification method for preparing an alkenyl succinic anhydride (ASA) sizing emulsion for use in paper and cardboard manufacturing, characterized in that it comprises: (a) obtaining or producing an alkenyl succinic anhydride (ASA) sizing agent; (b) combining said ASA sizing agent with a primary emulsifying agent and emulsifying at room temperature and stirring with sufficient energy to achieve an average ASA particle size ranging from 0.5-3 μm, 0.5-2 μm or 0.5-1 μm in diameter, thereby forming a primary emulsion; (c) after step (b), add a secondary emulsifying agent and emulsify at a temperature ranging from 20-80°C, 20-60°C, 20-40°C or 20-25°C, preferably 20-40°C and stir with sufficient energy to achieve an average ASA particle size ranging from 0.5-3 μm, 0.5-2 μm or 0.5-1 μm in diameter, thus forming said ASA bonding emulsion, and (d) optionally, after step (c),add said ASA sizing emulsion to a high-ash papermaking pulp, wherein (i) said primary emulsifying agent comprises an aqueous polymer solution comprising cationic acrylamide copolymers selected from the group consisting of acrylamide / [2-(methyl-acryloyloxy)ethyl]trimethylammonium chloride copolymer (AMD / MAETAC), acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride / 2-hydroxyethyl methacrylate terpolymers (AMD / MAETAC / HEMA), tetrapolymer Petition 870250087440, dated 09 / 26 / 2025, page. 67 / 85 10 / 11 acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride / 2-hydroxyethyl methacrylate / acrylic acid (AMD / MAETAC / HEMA / AA) terpolymer and acrylamide / [2-(methylacryloyloxy)ethyl]trimethylammonium chloride / 2-hydroxyethyl methacrylate terpolymer3-dihydroxypropyl (AMD / MAETAC / DHPMA); (ii) said secondary emulsifying agent comprises one or more modified or unmodified cationic starches; selected from the group of starches consisting of corn starch, waxy corn starch, potato starch, tapioca starch, wheat starch, pea starch and a mixture thereof; (iii) said high-ash paper pulp comprises ash selected from the group consisting of calcium carbonate, TiO2, kaolin clay, silicates, carbonate-based pigments, kaolin-based pigments or any combination thereof; (iv) said high-ash paper pulp comprises an ash content of 1-35%, 230%, 5-25% or 10-20% by mass,(v) said primary emulsifying agent is added to said alkenyl succinic anhydride (ASA) sizing agent to obtain a ratio of grams of active cationic polymer to grams of ASA of 0.05:1 to 0.6:1, 0.1:1 to 0.5:1, 0.15:1 to 0.4:1 or 0.2:1 to 0.25:1; and (vi) said secondary emulsifying agent is added to said primary emulsion to obtain a mass ratio of dry starch to ASA of 0.25:1 to 2:1, 0.3:1 to 1.6:1, 0.4:1 to 1.2:1 or 0.5:1 to 1:
1.
15. A sizing emulsion composition of ASA or a pulp for making paper, pulp or fiber stock, optionally a high-ash paper pulp, characterized in that it comprises said ASA sizing emulsion composition, obtained by a method as defined in any of the preceding claims.
16. Process for the production of paper or cardboard, characterized in that it comprises obtaining a high-ash paper pulp comprising wood pulp, optionally a fiber stock comprising a high content of recycled fibers and / or production waste fibers, optionally a concentrated fiber stock, optionally a bleached fiber stock, optionally containing process water from the production of pulp, paper or cardboard and treating said fiber stock at the wet end of a paper machine with an ASA sizing emulsion, as defined in any of the preceding claims, wherein: (a) said high-ash paper pulp comprises ashes selected from the group consisting of calcium carbonate, TiO2, kaolin clay, silicates, carbonate-based pigments, kaolin-based pigments or any combination thereof;and (b) said high-ash paper pulp comprises an ash content percentage of 1-35%, 2-30%, 5-25% or 10-20% by mass, preferably 5%-25% ash by mass. Petition 870250087440, dated 09 / 26 / 2025, p. 69 / 85;