Reactivated hydroprocessing catalysts for use in sulfur abatement
Patent Information
- Application Number
- CA3138356
- Authority / Receiving Office
- CA · CA
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-05-22
- Filing Date
- 2020-05-22
- Publication Date
- 2026-10-13
- Estimated Expiration
- 2040-05-22
AI Technical Summary
Spent hydroprocessing catalysts from hydrocarbon streams are typically discarded as hazardous waste, leading to environmental and economic inefficiencies, and there is a need for effective sulfur abatement in tailgas treatment processes.
Reactivating spent hydroprocessing catalysts by regeneration or rejuvenation processes, followed by resizing, reshaping, and reformulating, to utilize them in tailgas treatment processes for converting sulfur-containing species to hydrogen sulfide, thereby reducing waste and enhancing catalyst performance.
The reactivated catalysts demonstrate superior performance in sulfur conversion, reducing hazardous waste generation and providing an economically attractive source for high-performance catalysts in tailgas treatment, achieving high sulfur recovery efficiency and lowering environmental impact.
Abstract
Description
<DP=1>²WO 2020 / 237200 ² PCT / US2020 / 034353²Reactivated Hydroprocessing Catalysts for Use in Sulfur²Abatement²FIELD OF THE TECHNOLOGY²100011 The present application relates to catalysts and processes for tailgas ²treatment in a ²hydrocarbon treating process. More specifically, the application relates to ²reactivating a ²catalyst used in a hydroprocessing process and using the reactivated catalyst ²for tailgas ²treatment.²BACKGROUND²100021 The necessity of removing sulfur from hydrocarbon streams, such as oil ²and natural gas ²derivative streams, for pollution control is well known. If sulfur is not ²removed from ²hydrocarbon compounds, then, upon combustion, sulfur dioxide and sulfur ²trioxide will be ²formed. These compounds can react with moisture in the atmosphere to form ²sulfuric acid, a ²contributor to the phenomenon known as acid rain. For this reason, in most ²jurisdictions, it is ²required by law to minimize sulfur emissions to the environment.²100031 Sulfur is commonly removed from natural gas and other refined petroleum ²products by ²a catalytic process known as hydrodesulfurization (HDS), also commonly ²referred to as ²hydrotreating (HDT) or hydroprocessing (HDP). In this process, the hydrocarbon ²stream is ²mixed with hydrogen gas, heated, and passed over a fixed catalyst bed at ²elevated temperature ²and pressure. Commonly used catalysts for hydroprocessing comprise one or more ²Group ²VIIIB metals, such as cobalt (Co) or nickel (Ni) and one or more Group VIB ²metals, such as ²molybdenum (Mo) or tungsten (W) supported on a carrier material, such as ²alumina (A1203), ²silica alumina, zeolite, or combinations thereof When a hydrotreating catalyst ²is used in a ²hydrotreating process, the activity of the catalyst decreases over time, due ²to the accumulation ²of carbon-containing deposits, referred to as coke, on the catalyst and / or by ²the presence of ²deactivating inorganic materials, such as silicon (Si), arsenic (As), and ²vanadium (V). Some ²of these catalysts may be reactivated by regeneration or rejuvenation and ²reused as HDS ²catalysts, but more often the spent catalysts are not recovered and, instead, ²are treated as ²hazardous waste. Thus, environmental and economic incentives exist for ²developing further ²uses for catalysts recovered from hydrocarbon processes such as HDS treatment.²1²CA 03138356 2021- 11- 16²<DP=2>²WO 2020 / 237200 ² PCT / US2020 / 034353²SUMMARY²100041 Disclosed herein is a method of treating a gas stream in a tailgas ²treating process, the ²method comprising: contacting the gas stream with a catalyst that was ²previously used in a ²hydrotreating process and that has been reactivated by a reactivation process ²prior to contacting ²the gas stream in the tailgas treating process, wherein the gas stream ²comprises one or more ²sulfur-containing species selected from the group consisting of elemental ²sulfur (Sx), sulfur ²dioxide (S02), carbonyl sulfide (COS), and carbon disulfide (CS2), and wherein ²contacting the ²gas stream with the reactivated catalyst in the presence of hydrogen (H2) ²converts the one or ²more sulfur-containing species to hydrogen sulfide (H2S). According to some ²embodiments, ²the hydrotreating process is selected from the group consisting of petroleum ²hydrotreating ²processes, hydrodesulfiirization (HDS), hydrodenitrogenation (HDN), ²hydrogenation, ²hydrodemetallization (HDM), naphtha hydrotreating (NHT), diesel hydrotreating ²(DHT), ²kerosene hydrotreating (ICHT), jet fuel hydrotreating (JHT), atmospheric gas ²oil hydrotreating, ²vacuum gas oil (VGO) hydrotreating, and fluid catalytic cracker (FCC) feed ²hydrotreating. ²According to some embodiments, the catalyst comprises one or more Group VII1B ²metals and ²one or more Group VIB metals supported on an inorganic oxide carrier material. ²According ²to some embodiments, the catalyst comprises cobalt and molybdenum supported on ²aluminum ²oxide. According to some embodiments, the catalyst comprises nickel and ²molybdenum ²supported on aluminum oxide. According to some embodiments, the reactivation ²process ²comprises regeneration. According to some embodiments, the regeneration ²comprises heating ²the catalyst in an oxygen-containing atmosphere at a temperature of 300 to 500 ² C for a time ²of 30 minutes or more. According to some embodiments, prior to the ²regeneration treatment, ²hydrocarbons are removed from the catalyst by solvent extraction or by ²contacting the catalyst ²with steam, natural gas combustion products, hydrogen or nitrogen at a ²temperature of 150 to ²550 C. According to some embodiments, the reactivation process comprises ²rejuvenation. ²According to some embodiments, the rejuvenation comprises impregnating the ²catalyst with a ²solution containing a chelating agent and drying the catalyst at a temperature ²of 50 C to 300 C. ²According to some embodiments, the chelating agent is an organic acid. ²According to some ²embodiments, the reactivated catalyst is pre-sulfurized prior to contacting ²the gas stream in the ²tailgas treating process. According to some embodiments, the reactivated ²catalyst is pre-²sulfided prior to contacting the gas stream in the tailgas treating process. ²According to some ²embodiments, the reactivated catalyst is resized, reshaped, and / or ²reformulated prior to ²contacting the gas stream in the tailgas treating process_ According to some ²embodiments, the ²reactivated catalyst is resized by length grading the catalyst. According to ²some embodiments,²2²CA 03138356 2021- 11- 16²<DP=3>²WO 2020 / 237200 ² PCT / US2020 / 034353²the resizing, reshaping, and / or reformulating comprises milling the ²reactivated catalyst to a fine ²powder and then reforming the reactivated catalyst. According to some ²embodiments, the ²reactivated catalyst is resized from having a diameter of 1.3 to 2.5 mm to ²having a diameter of ²3 to 5 mm. According to some embodiments, contacting the gas stream with the ²reactivated ²catalyst comprises combining the reactivated catalyst with a second catalyst, ²wherein the ²second catalyst provides a lower pressure drop than the reactivated catalyst. ²According to some ²embodiments, contacting the gas stream with the reactivated catalyst comprises ²short loading ²the reactivated catalyst. According to some embodiments, the reactivated ²catalyst exhibits a ²pressure drop of 0_05 to 0.20 psi / ft, when sock-loaded and tested at 100 ²ft / rnin superficial ²velocity in ambient air.²100051 Also disclosed herein is a method of forming a reactivated catalyst for ²a tailgas treating ²process, the method comprising: obtaining a spent catalyst from a ²hydrotreating process, and ²reactivating the catalyst to form the reactivated catalyst, wherein the ²reactivated catalyst, when ²contacted with a gas stream comprising one or more sulfur-containing species ²selected from ²the group consisting of elemental sulfur (S), sulfur dioxide (S02), carbonyl ²sulfide (COS), and ²carbon disulfide (CS2), is capable of catalyzing the conversion of the one or ²more sulfur-²containing species to hydrogen sulfide (H2S) in the presence of hydrogen (Hz). ²According to ²some embodiments, the hydrotreating process is selected from the group ²consisting of ²petroleum hydrotreating processes, hydrodesulfurization (HDS), ²hydrodenitrogenation (HDN), ²hydrogenation, hydrodemetallization (HDM), naphtha hydrotreating (NHT), diesel ²²hydrotreating (DHT), kerosene hydrotreating (KHT), jet fuel hydrotreating ²(JHT), atmospheric ²gas oil hydrotreating, vacuum gas oil (VGO) hydrotreating, and fluid catalytic ²cracker (FCC) ²feed hydrotreating. According to some embodiments, the spent catalyst ²comprises: an ²inorganic oxide support material having a surface area of 20 to 600 m2 / g, one ²or more Group ²VIIIB metals, and one or more Group VIB metals supported on the inorganic ²oxide support ²material. According to some embodiments, the catalyst comprises cobalt and ²molybdenum ²supported on aluminum oxide. According to some embodiments, the catalyst ²comprises nickel ²and molybdenum supported on aluminum oxide. According to some embodiments, the ²²reactivating comprises regeneration. According to some embodiments, the ²regeneration ²comprises heating the catalyst in an oxygen-containing atmosphere at a ²temperature of 300 to ²500 C for a time of 30 minutes or more. According to some embodiments, prior ²to the ²regeneration, removing hydrocarbons from the catalyst by solvent extraction or ²by contacting ²the catalyst with steam, natural gas combustion products, hydrogen or nitrogen ²at a temperature ²of 150 to 550 'C. According to some embodiments, the reactivating comprises ²rejuvenation.²3²CA 03138356 2021- 11- 16²<DP=4>²WO 2020 / 237200 ² PCT / US2020 / 034353²According to some embodiments, the rejuvenation comprises impregnating the ²catalyst with a ²solution containing a chelating agent and drying the catalyst at a temperature ²of 50 C to 300 C. ²According to some embodiments, the chelating agent is an organic acid. ²According to some ²embodiments, the method further comprises pre-sulfurizing the reactivated ²catalyst. According ²to some embodiments, the method further comprises pre-sulfiding the ²reactivated catalyst. ²According to some embodiments, the method further comprises resizing, ²reshaping, and / or ²reformulating the reactivated catalyst. According to some embodiments, the ²method further ²comprises milling the reactivated catalyst to a fine powder and then reforming ²the reactivated ²catalyst. According to some embodiments, the spent catalyst, prior to ²reactivating, has a ²diameter of 1.3 to 2.5 mm and the reformed reactivated catalyst has a diameter ²of 3 to 5 mm. ²According to some embodiments, the spent catalyst, as used in the ²hydrotreating process, ²exhibits a pressure drop of 0.20 to 0.80 psi / ft, and wherein the method ²further comprises ²resizing, reshaping, and / or reformulating the reactivated catalyst so that the ²reactivated catalyst ²exhibits a pressure drop of 0.05 to 0.20 psi / fl, when sock-loaded and tested ²at 100 ft / min ²superficial velocity in ambient air.²BRIEF DESCRIPTION OF THE DRAWINGS²100061 Figure 1 shows a process for treating a sour hydrocarbon feed, wherein ²the process²includes a hydroprocessing step and a sulfur treatment step.²100071 Figure 2 is a table showing analysis of regenerated, hot nitrogen ²stripped, and solvent²extracted catalysts.²100081 Figure 3 is a table showing performance of fresh, regenerated, ²rejuvenated, hot nitrogen²stripped, and solvent extracted catalysts for tailgas treatment at 1,200 GHSV.²100091 Figure 4 shows an equation used to calculate overall sulfur conversion ²and a²comparison of overall sulfur conversion using the different catalysts.²100101 Figure 5 is a table showing performance of regenerated and rejuvenated ²catalysts for²tailgas treatment at 3,000 GHSV.²1001111 Figure 6 shows a comparison of sulfur dioxide conversion at 3000 GHSV ²using²different catalysts.²100121 Figure 7 shows a comparison of carbon disulfide conversion at 3000 GHSV ²using²different catalysts.²100131 Figure 8 shows a comparison of carbonyl sulfide conversion at 3000 GHSV ²using²different catalysts.²4²CA 03138356 2021- 11- 16²<DP=5>²WO 2020 / 237200 ² PCT / US2020 / 034353²
[0014] Figure 9 shows a comparison of overall sulfur conversion at 3000 GHSV ²using different²catalysts.²
[0015] Figure 10 shows a process for reactivating a catalyst for use in ²tailgas treatment.²DETAILED DESCRIPTION²100161 Figure 1 illustrates aspects of a hydrocarbon processing plant such as ²a natural gas ²processing facility or a petroleum refinery. As mentioned above, such ²facilities may include ²one or more hydrodesulfurization (HDS) reactors 102. A sour hydrocarbon feed ²(La, a ²hydrocarbon feed containing orgario-sulfur compounds) is provided to the fiDS ²reactor 102. ²As mentioned above, the hydrocarbon stream is heated, mixed with hydrogen gas, ²and passed ²over a catalyst at elevated temperature and pressure. As also mentioned above, ²catalysts for ²hydroprocessing typically comprise one or more Group VIER metals, such as ²cobalt (Co) or ²nickel (Ni) and one or more Group VIB metals, such as molybdenum (Mo) or ²tungsten (W) ²supported on a carrier material, such as alumina (A1203), silica alumina, ²zeolite, or ²combinations thereof The reaction that takes place, hydrogenolysis, is ²characterized by ²cleavage of a C-S chemical bond and formation of C-H and H-S chemical bonds. ²In this way, ²the reaction of the hydrocarbon compounds (containing the embedded sulfur) ²with hydrogen ²allows liberation of the sulfur by formation of hydrogen sulfide gas (}12S).²100171 The effluent of the fixed bed reactor is cooled, and the gas and liquid ²are separated. The ²gas contains hydrogen and hydrogen sulfide, among other components. The gas is ²fed to an ²amine system 104. The amine system 104 includes an amine absorption system ²(not ²specifically illustrated) where the hydrogen sulfide is selectively absorbed ²into an amine ²absorbent. The gas is purified of hydrogen sulfide in this way and the ²remaining hydrogen rich ²gas stream is primarily recycled to be combined with fresh makeup hydrogen and ²fed once ²more to the hydrodesulfurization reactor 102. Within the amine system 104 the ²"rich" H2S-²laden amine solution is sent to an amine regenerator (not specifically ²illustrated). The ²hydrocarbon liquid from the hydrotreater effluent gas separator is routed to a ²stripper 106, ²where the hydrogen sulfide is stripped from the hydrocarbon liquid. This ²purifies the liquid ²hydrocarbon stream of hydrogen sulfide for further refining The stripped ²hydrogen sulfide ²containing gas stream is then routed to an amine system 108 (similar to amine ²system 104), ²where the amine absorbent is used to remove the hydrogen sulfide from the rest ²of the gas ²stream. Upon regeneration of the rich hydrogen sulfide laden amine absorbent, ²a hydrogen ²sulfide rich gas stream is obtained. Most typically, the hydrogen sulfide ²streams are sent to a ²sulfur recovery system, which may comprise a modified Claus process coupled ²with a tail gas² CA 03138356 2021- 11- 16²<DP=6>²WO 2020 / 237200 ² PCT / US2020 / 034353²cleanup process, for further processing and conversion to elemental sulfur. In ²some cases, ²though less common, the hydrogen sulfide containing streams can be convened ²instead to ²sulfutic acid in a wet sulfuric acid (WSA) plant.²100181 Still referring to Figure 1 the illustrated sulfur recovery system 110 ²includes a modified ²Claus process 112 that converts hydrogen sulfide to elemental sulfur. This ²process includes a ²thermal stage, typically a reaction furnace, followed by two or more catalytic ²stages. In the ²thermal stage, one-third of the hydrogen sulfide in the feed stream is ²combusted to yield sulfur ²dioxide, according to reaction 1. The sulfur dioxide reacts with hydrogen ²sulfide to produce ²elemental sulfur according to the Claus reaction, reaction 2. Thus, the ²overall reaction can be ²expressed according to reaction 3.²1125 + -32 02 <-4 SO2 +1120 Reaction ²1: H2S Combustion²2 1 / 25 + 502 e IS8 + 2 1120 Reaction ²2: Claus Reaction²2 ²_______________________________________________________________________________²__________________________________________ ²3 1 / 25 'O2 e + 3 1120 Reaction ²3: Overall Reaction²2²100191 The hydrogen sulfide-containing feed stream(s) are combusted, and the ²amount of air ²is controlled to achieve the desired level of sulfur dioxide, as well as to ²convert any ammonia ²and hydrocarbons present. Typically, about 60-70% of the sulfur entering the ²modified Claus ²process is convened to elemental sulfur in the thermal stage. -Hie gas from ²the thermal stage ²is then processed in each of the consecutive catalytic stages. Each catalytic ²stage consists of ²three process steps: reheat, catalytic conversion, and condensation. In the ²reheat step, the gas ²stream is heated to the desired temperature for the subsequent catalytic ²conversion stage. In the ²catalytic conversion step, additional Claus conversion according to reaction 2 ²is realized with ²a Claus catalyst, which is typically titania or alumina based. The last step ²is condensation of ²the gaseous sulfur formed in the upstream catalytic converter to liquid ²sulfur, which is then ²separated and recovered. Typically, greater than 97% sulfur recovery ²efficiency cannot be ²achieved by the modified Claus process alone. For greater sulfur recovery, for ²example in the ²98-99.9% range, which is required in many jurisdictions, a tailgas cleanup ²process is required. ²100201 Thus, the illustrated sulfur recovery system 110 also includes a ²tailgas cleanup process ²114. A common sulfur recovery tailgas cleanup system 114 includes a ²hydrogenation / amine ²treatment, which may provide 99.8+% sulfur recovery efficiency. Stringent ²environmental ²regulations, imposing mandatory low emissions and high recovery limits, have ²forced many ²sour gas processors to adopt such hydrogenation / amine-type tailgas treatment ²processes.²6²CA 03138356 2021- 11- 16²<DP=7>²WO 2020 / 237200 ² PCT / US2020 / 034353²
[0021] One of the most common hydrogenation / amine treatment processes is the ²Shell Claus ²Offgas Treating (SCOT) process. In the SCOT process, the sulfur dioxide and ²other convertible ²sulfur compounds in Claus tailgas are catalytically convened to hydrogen ²sulfide. First the ²Claus tailgas is heated and mixed with a reducing gas stream containing ²hydrogen and carbon ²monoxide. The reducing gas is commonly generated by a reducing gas generator ²(RGG) 116 ²operating at sub-stoichiometric combustion conditions to partially oxidize the ²fuel into carbon ²monoxide and hydrogen. The resulting gas stream obtained by mixing of the ²Claus tailgas and ²reducing gas, which contains species including sulfur dioxide (SO2), carbonyl ²sulfide (COS), ²and carbon disulfide (CS2), elemental sulfur (Sx), and carbon monoxide (CO), ²is then passed ²over a hydrogenation catalyst in a hydrogenation reactor 118. The ²hydrogenation catalyst most ²typically contains cobalt and molybdenum on an alumina support. The catalyst ²facilitates the ²hydrogenation of residual sulfur dioxide (reaction 4), hydrolysis of carbonyl ²sulfide (reaction ²5), hydrolysis of carbon disulfide (reaction 6), and hydrogenation of ²elemental sulfur (reaction ²7), all back to H2S.²SO2 +3112 -> H25 +21120 Reaction ²4: SO2 Reduction²COS + H20 1125 + CO2 Reaction ²5: COS Hydrolysis²CS2 + 2 1120 -fr 2 HS + CO2 Reaction ²6: CS2 Hydrolysis²-S8 + H2 -> H2S Reaction ²7: Sulfur Reduction²100221 The catalyst also facilitates a water-gas shift reaction, where carbon ²monoxide and ²water react to form hydrogen and carbon dioxide, per reaction 8.²CO +1120 -> H2 CO2 Reaction ²8: Water-Gas Shift²100231 The reactor effluent is typically cooled by a waste heat boiler ²(generating low pressure ²steam) followed by a water quench tower system, which both cools the gases and ²lowers the ²water content from about 30% to 5-10%. The cooled gas from die cool / quench ²equipment 120 ²is then contacted with an amine absorbent in art amine contactor column. in ²the amine ²absorption system 122, the H2S in the tailgas is absorbed into the lean amine, ²making it rich ²(laden with H2S) and purifying the gas stream of142S. The purified off-gas ²stream is then routed ²to an incinerator as the final treatment step before release to the ²atmosphere. The rich amine is ²routed to an amine regenerator where it is heated to drive off the 1128, which ²is recycled back ²to the Claus plant for conversion to elemental sulfur. in this way, the sulfur ²is basically recycled²7²CA 03138356 2021- 11- 16²<DP=8>²WO 2020 / 237200 ² PCT / US2020 / 034353²to extinction. The lean, regenerated amine is fed back to the absorber for ²another I-12S pickup ²csrrcle.²100241 It should be noted that Figure I is intended to provide an overview of ²the SCOT process ²and is not intended to illustrate even' piece of equipment and every variable ²It should also be ²noted that other variants of a tailgas clean system are known in the art For ²example, one ²variant of the original SCOT process is the Low Temperature SCOT process, In ²the ²conventional SCOT process, the tailgas stream is typically directly heated ²using an in-line ²burner (i.e., RUG 116) to about 260-300 C before being fed to the ²hydrogenation reactor 118.. ²In the low temperature SCOT process, the tailgas stream is typically ²indirectly heated using a ²high-pressure steam heater, typically to about 220-230 C. The low temperature ²SCOT proc-ess ²also requires the use of an external hydrogen sourceõ since the reducing gas ²generator is no ²longer a part of the process scheme. Lastly, low temperature units typically ²use a catalyst that ²is specifically designed for higher activity, usually by using higher ²concentrations of active ²metals, to achieve a similar level of conversion as coiwentional temperature ²units.²100251 Another alternative tailgas clean-up process is the Beavon Sulfur ²Removal (BSR) ²process, which also features hydrogenation of the Claus tailgas. In the BSR ²process, Claus ²tailgas is heated by an in-line burner (e.g., a reducing gas generator, RUG) ²at sub-²stoichtometric conditions to partially oxidize the fuel to generate reducing ²gases.. The mixture ²of Claus tailgas and reducing gases are fed to a hydrogenation bed packed with ²cobalt and ²molybdenum on alumina catalyst. The same reactions as listed above for the ²SCOT process (4-²8) occur in the hydrogenation step. After the hydrogenation step, the gas is ²sent to a waste heat ²boiler, which generates low pressure steam, followed by a quench tower system, ²which both ²lowers the temperature and significantly reduces the water content. It is ²common to pair the ²BSR process with another process which aims to either recycle the H2S gas (for ²example ²BSRIMDEA) or convert the H2S gas into elemental sulfur for recovery (for ²example ²BSR / Selectox or BSR / Stretford).²100261 Notice that each of the tailgas clean-up processes described here ²involve a ²hydrogenation reactor that effects the reactions 4-7 described above. Notice ²also that the ²hydrogenation catalysts implemented in the hydrogenation reactors of the ²tailgas clean-up ²process typically comprise one or more Group VIIIB metals, such as cobalt (Co) ²or nickel (Ni) ²and one or more Group VIB metals, such as molybdenum (Mo) or tungsten (W) ²supported on ²a carrier material, such as alumina (A1203), silica alumina, zeolite, or ²combinations thereof²100271 Aspects of the present disclosure involve obtaining catalyst that was ²used in a ²hydro-treating process, and then using the so-obtained catalyst in a tailgas ²treating process. The²8²CA 03138356 2021- 11- 16²<DP=9>²WO 2020 / 237200 ² PCT / US2020 / 034353²applications from which the hydrotreating catalyst originates cart include, ²but are not limited ²to, catalyst used in hydrodesulfurization (HDS), hydrodenitrogenation (HDN), ²hydrodemetallization (HDM), hydrodearomatization (HDA), hydrodeoxygmation ²(HDO), ²aromatic saturation, hydrocracking and other hydrogenation processes. For ²example, the spent ²catalyst may originate from the application of naphtha hydrotreating (NHT)õ ²diesel ²hydro-treating (DHT), kerosene hydrotreating (KHT), jet fuel hydrotreating ²(.IHT), atmospheric ²gas oil hydrotreating, vacuum gas oil (VG0) hydrotreating, fluid catalytic ²cracker (FCC) feed ²hydrotreating, or any other petroleum fraction hydrotreating application. It ²is important to note ²that when referring to a hydrotreating catalyst, this term is not intended to ²include a catalyst ²that was previously used in a Claus tailgas treating process. The catalysts ²typically comprise ²one or more Group -11111.13 metals, such as cobalt (Co) or nickel (Ni) and one ²or more Group ²VIE metals, such as molybdenum (Mo) or tungsten (W) supported on a carrier ²material, such ²as alumina (Al2.03), silica alumina zeolite, or combinations thereof. These ²hydroprocessing ²catalysts cart also have Type I or Type II active sites. The catalyst may also ²include promoters, ²such as boron or phosphorous promoters, among others.²[00281 As used herein, the term "reactivated catalyst: refers to a catalyst ²obtained from the ²hydrotreating process, submitted to a reactivation treatment, and then re-used ²in a tailgas ²treating process. A reactivated catalyst may be regenerated andfor rejuvenated ²(revitalized) ²catalyst²100291 The term "regenerated catalyst" is used herein to refer to a spent ²catalyst that has been ²submitted to in-situ or ex-situ controlled thermal treatment in the presence ²of oxygen to ²remove contaminants such as volatile hydrocarbons, carbon (coke), and sulfur. ²Regeneration ²processes are known to those skilled in the art, and although these processes ²may differ in ²configuration details, they are all aimed at removing hydrocarbons, sulfur, ²and carbon, ²converting substantially all the metals to their oxide form, and recovering as ²much activity as ²possible, all while minimizing breakage to realize the highest yield and ²lowest product length ²loss possible Most catalyst regeneration is performed ex-situ, however in-situ ²regeneration ²can be performed, and the term regenerated as used herein is not intended to ²limit the scope ²to ex-situ regeneration only.. Regeneration processes are commonly used on ²spent ²hy drotreatirtg catalysts to recover a portion of the fresh catalyst activity ²front the spent ²catalyst. Regenerated catalysts are typically re-used in a lower severity ²hydrotreating unit as a ²lower cost alternative to fresh catalyst. Regeneration processes differ from ²rejuvenation ²(revitalization) processes in that they do not feature any process of metals ²re-dispersion to ²reverse th.e activity decline from metals agglomeration.²9²CA 03138356 2021- 11- 16²<DP=10>²WO 2020 / 237200 ² PCT / US2020 / 034353²100301 According to some embodiments, a regenerated catalyst can be prepared ²by obtaining ²a catalyst used in a hydrotreating process, as described above. The obtained ²catalyst can be ²regenerated by heating the catalyst in air to remove contaminants from the ²hydroprocessirig ²process from the catalyst For example, the catalyst may he heated within a ²temperature range ²of about 200 C to about 600'C, more preferably 380 C to about 500 C for 1-24 ²hours, more ²preferably 1-3 hours. One of the key contaminants removed during the ²regeneration process is ²coke. Typically spent catalyst has a coke concentration of greater than 4 wt%. ²After ²regeneration, the coke concentration is typically less than 4 wt.%.²190311 The term "rejuvenated" (or revitalized) catalyst is used herein to ²refer to a spent catalyst ²that has been submitted to an in-situ or ex-situ controlled thermal treatment ²(regeneration) to ²remove volatile hydrocarbons, carbon (coke), and sulfur, followed by an ex-²sin.' application of ²a chelating agent via impregnation to re-disperse active metal sites on the ²support that have ²migrated, causing metal site growth. After a specified aging period, the ²catalyst can be dried to ²the final product form. Rejuvenation processes are known to those skilled in ²the art, and ²although these processes may differ in configuration details, they are all ²aimed at removing ²hydrocarbons, sulfur, and carbon, converting substantially all of the metals ²to their oxide form, ²re-dispersing the active metal sites on the support, recovering as much ²activity as possible,. all ²while minimizing breakage to realize the highest yield and lowest product ²length loss possible. ²Rejuvenation processes often recover enough activity to be close to fresh ²catalyst in terms of ²performance. In some cases, especially with regards to Type I catalysts, ²rejuvenation of spent ²catalyst can provide even higher performance than the original fresh catalyst ²(under ²hydrotreating conditions). Because of the higher degree of activity recovery ²compared to ²regenerated catalyst, a rejuvenated catalyst may be re-used in the same unit ²it was harvested ²from or one of similar severity. It does not necessarily have to be cascaded ²to a lower severity ²unit like regenerated catalyst often is.²100321 Mw rejuvenation process known in the art may be used according to the ²instant ²disclosure According to sonic embodiments, a rejuvenated catalyst can be ²prepared by ²obtaining a catalyst used in a hydrotreating process, as described above. ²According to some ²embodiments, the obtained catalyst is first regenerated as described above. ²Following the ²regeneration process, the catalyst can be contacted with one or more reagents ²to rejuvenate the ²catalyst. Examples of reagents that may be used to contact the catalyst ²include one or more ²organic additives such as butanediol, pyruvic aldehyde, glycolic aldehyde, ²ethylene glycol, ²propylene glycol, glycerin, trimethylol ethane, trimethy Tel propane, ²diethylene glycol, ²dipropylene glycol , -trimethyIerie glycol, Methylene glycol, nibutylene ²glycol, tetraethy I ene² CA 03138356 2021- 11- 16²<DP=11>²WO 2020 / 237200 ² PCT / US2020 / 034353²glycol, tetrapentylene glycol, polyethers like polyethylene glycol, ethylene ²glycol monobutyl ²ether, diethvlene glycol monornethyl ether, diethylene glycol morioethid ²ether, diethylene ²glycol monopropyl ether, and diethylene glycol monobtityl ether The catalyst ²may be ²contacted with a solution comprising the organic additive, such as a solution ²of the organic ²additive in an alcohol or an aqueous solution, for example. Alternatively, or ²additionally, the ²catalyst may be contacted with an. acid such as glycolic acid, glyoxylic acid, ²lactic acid, ²diethylene triamine penta acetic acid, ethylene amine tetra acetic acid, ²citric acid, tartaric acid, ²oxalic acid, rnalonic acid, mane acid, or the like. Foilevying contacting, the ²catalyst may be ²aged and / or dried. For example, the catalyst may be aged for a time ranging ²from hours to ²several days, for example, 1 hour to 24 hours, 6 to 24 hours, or for example, ²about 14 hours. ²According to some embodiments, the catalyst may be aged at room temperature. ²As used ²herein, "room temperature" refers to a temperature of about 2O-25'C. According ²to some ²embodiments, a portion of the organic additive may remain in the catalyst even ²after drying. ²100331 Common commercial rejuvenation processes are exemplified by the ²following: ²EXCEL (by Porocel, Houston, TX) described in U.S. Patent No. 9,895,679, ²ENCORE (by ²Criterion, Houston, TX) described in U.S. Patent No. 7,696,120, REACT (by ²Albemarle ²Corporation, Charlotte, NC) described in U.S. Patent No. 7,956,000, and ²REFRESH (by ²Haldor Topsoe, Inc., Houston, TX). The contents of U.S. Patent No. 9,895,679 ²("the '679 ²Patent") are incorporated herein by reference in their entirety_²100341 According to some embodiments, the reactivated (i.e., regenerated or ²rejuvenated) ²catalyst can be either applied "as-is," i.e., in the original size, shape, and ²composition as was ²used in the hydrotreating process. According to other embodiments, the ²catalyst may be re-²sized, re-shaped, reformulated, or any combination of resizing, reshaping, and ²reformulating, ²prior to use in a tailgas treating process. Resizing involves changing the ²size of the catalyst. ²This can be accomplished, for example, by length grading the catalyst, which ²involves ²selectively removing the smallest catalyst particles, effectively increasing ²the average particle ²size of the remaining catalyst. Length grading can be accomplished by ²sieving / screening or by ²other, more specialized methods known to those skilled in the art. Resizing ²can also be ²accomplished by means of milling the catalyst to a fine powder and re-forming ²a different sized ²catalyst. For example, resizing may involve milling a 1.3 mm, 1.6 mm, or 2,5 ²mm catalyst ²extrudate to a fine powder and reforming to produce a 3.0 mm or 3.5 mm ²catalyst extrudate_ ²Re-shaping involves changing the shape of the catalyst. For example, re-²shaping may involve ²milling a tri-lobe or quad-lobe catalyst extrudate to a fine powder and ²reforming to produce a ²cylindrical extrudate, spherical product, or even a ring / hollow cylinder ²product. Resizing and²11²CA 03138356 2021- 11- 16²<DP=12>²WO 2020 / 237200 ² PCT / US2020 / 034353²reshaping may first involve reducing the catalyst from the "as-is" form to a ²powder by a milling ²operation. The forming of the new size or shape can then be accomplished by ²any forming ²method, including but not limited to: extrusion (e.g., screw or piston ²extrusion), tableting, ball ²forming, nodulation, granulation, drop coagulation, etc.²100351 Reformulating involves the incorporation of additional components or ²materials to the ²reactivated catalyst. For example, boehmite / pseudo-boehmite alumina or anatase ²titania ²powder may be added in a certain proportion with milled catalyst powder to ²produce a ²reformulated product. Reformulation may involve the addition of active metals, ²promoters, or ²other ingredients by physical mixing such as co-mulling, admixing, plow ²mixing, paddle ²mixing or ribbon mixing, for example. It may also involve the addition of ²metals, promoters, ²or other ingredients by precipitation or impregnation, for example. ²Alternatively, reformulating ²may involve a combination of physical mixing and impregnation to introduce ²additional ²components to the reactivated catalyst material. Any method in which ²additional components ²are added to the reactivated catalyst in any form constitutes reformulation. ²For example, the ²catalyst may be reformulated by taking the catalyst in its native form and ²wetting the catalyst ²with a solution or a slurry of active phase precursors, for example, soluble ²metal salts of one ²or more Group VIIIB metals, such as cobalt (Co) or nickel (Ni) and one or more ²Group VIII ²metals, such as molybdenum (Mo) or tungsten (W). For example, the catalyst may ²be re-²formulated by wet impregnation with an excess of solution, dry impregnation ²(otherwise ²known as incipient wetness impregnation or pore volume impregnation), or ²precipitation.²100361 Generally, a tailgas catalyst can be installed in one of three states: ²the oxidic state, the ²pre-sulfurized state, or the pre-sulfided (pre-activated) state. The oxidic ²state may be described ²as a state in which nearly all the metals are present in the metal oxide form ²and there is no ²significant amount of sulfur present on the catalyst as well as no significant ²amount of metal ²sulfides. Pre-sulfurizing may be described as a treatment in which elemental ²sulfur and / or ²sulfur containing compounds are added to the catalyst, typically with less ²than 60% of the metal ²oxides converted into metal sulfides. Pre-sulfiding (pre-activation) may be ²described as a ²treatment in which typically greater than 60% of the metal oxides are ²converted to metal ²sulfides. The advantages of pre-sulfurizing or pre-sulfiding (pre-activating) ²treatments (versus ²the oxidic state) are primarily faster and easier reactor startup after ²initial loading. The ²reactivated hydroprocessing catalysts, whether in the native or resized, ²reshaped, and / or ²reformulated state, may be submitted to a pre-sulfurizing or pre-sulfiding ²treatment prior to use ²in the target application. The disclosure and the claims set forth herein is ²not intended to limit²12²CA 03138356 2021- 11- 16²<DP=13>²WO 2020 / 237200 ² PCT / US2020 / 034353²the scope to any specific pre-sulfurizing or pre-sulfiding technology but is ²instead intended to ²apply to them all.²1041371 The inventors have found that, surprisingly, catalyst from a ²hydrotreating application ²may be reactivated to be fit for use in a tail-gas hydrogenation applicafion. ²A beneficial aspect ²of the disclosed methods and systems is that the re-use of spent ²hydroprocessing catalyst ²reduces hazardous waste generation by operators from spent catalyst disposal. ²Ultimately, this ²helps reduce the environmental impact (carbon footprint) of the catalyst life ²cycle. The ²disclosed methods and systems also provide an economically attractive source ²of high-²performance catalyst for tailgas treatment, which benefits the spent catalyst ²generator, the ²catalyst provider, and the catalyst consumer, all through beneficial reuse of ²an otherwise ²hazardous waste.²100381 Persons of skill in the art will appreciate that some aspects of ²catalysts used for tailgas ²treatment (i.e., hydrogenation of tailgas components) may differ from aspects ²of catalysts used ²in non-tailgas treating operations (such as the hydroprocessing and other ²processes described ²above). In other words, even though the catalysts for both types of processes ²may use similar ²group metals supported on similar carrier materials, the catalysts may be ²optimized for one or ²the other types of processes. For example, a common difference between ²catalysts used in ²hydroprocessing applications and those used in taigas treating is size. ²Typically, ²hydroprocessing catalysts are available in smaller sizes, for example, ²diameter sizes of 1.3 mm, ²1.6 nun, or 2.5 mm extrudates are veiy common, while tailgas catalysts are ²available in larger ²sizes, typically with diameters from 3 to 5 mm in various shapes / forms. ²Another distinction ²between the typical hydroprocessing catalyst and the typical tailgas catalyst ²comes in the metals ²used and metals concentrations. Commercial tailgas catalysts on the market ²today are ²predominantly cobalt and molybdenum (CoMo) active metals, with typical ²concentration ²ranges of 2-3.5% Co and 6-11% Mo. Commercial hydrotreating catalysts on the ²market today ²are primarily cobalt and molybdenum (CoMo) or nickel and molybdenum (NiMo) ²active ²metals combinations. For commercial CoMo hydrotreating catalysts, typical ²concentration ²ranges are 3-4.5% Co and 12-17% Mo. For commercial NiMo hydrotreating ²catalysts, typical ²concentration ranges are 2.5-5% Ni and 9-19% Mo. Notice that the active metals ²content is ²typically much higher for hydrotreating catalysts than for taigas catalysts. ²Notice also that it ²is not a common commercial practice, as it is in hydroprocessing service, to ²use Ni and / or W ²containing catalysts in tailgas service. Another distinction between the two ²catalysts is their ²shape. Hydroprocessing catalysts are predominantly multi-lobed extrudates ²whereas tail gas ²catalysts come in a variety of shapes, including multilobed extrudates, ²spherical forms, and²13²CA 03138356 2021- 11- 16²<DP=14>²WO 2020 / 237200 ² PCT / US2020 / 034353²even hollow cylinder extrudaies. Another distinction between the two types of ²catalysts is that ²hydrotreating catalysts almost exclusively comprise extruded gamma / delta / theta ²alumina phase ²catalyst supports whereas tailgas catalysts comprise both spherical ²chi / rho / eta alumina phase ²catalyst supports, and extruded gamma / delta / theta alumina phase catalyst ²supports.²100391 One limitation of using reactivated hydrotreating catalysts in a ²tailgas service is the size ²difference of the catalyst particles. This is perhaps one reason why, to the ²knowledge of the ²inventors, it has never been done. As already mentioned, hydroprocessing ²catalysts are ²typically of a smaller size than tailgas catalysts (1.3-2.5 mm vs. 3-5 mm, ²respectively). ²Catalysts of a smaller size cause higher packed-bed pressure drop per linear ²foot. There are ²many cases where this higher-pressure drop may be unacceptable due to the ²hydraulic capacity ²limitations it would impose on the tailgas unit. Fortunately, the inventors ²have identified ²several ways to circumvent this obstacle. One option is to length grade the ²catalyst. Length ²grading is a commercially established process which separates catalyst ²particles based on their ²size. By doing so, the smallest particles can be effectively removed which ²increases the average ²length of the remaining catalyst extrudate particles. By increasing the ²average particle length ²of the catalyst extrudates and tightening up the particle size distribution, ²the bed void fraction ²also increases. Both of these changes cause a lower pressure drop per linear ²foot. Within certain ²limits, the extent of length grading can be tailored to the desired pressure ²drop profile. Length ²grading can be accomplished by either screening / sieving, or other more ²specialized method. ²Another option is to load a shorter bed of high activity reactivated ²hydroprocessing catalyst ²than would normally be loaded for fresh tailgas catalyst in order to target ²both the desired ²pressure drop and performance profile of a standard fresh tailgas catalyst ²loading configuration. ²This is called "short-loading" and is possible because in some cases, the ²reactivated ²hydroprocessing catalysts have been shown to perform better than competitive ²fresh tailgas ²catalysts being sold in the market today. Another option is to combine a high ²activity and high ²pressure drop reactivated hydroprocessing catalyst with a lower pressure drop ²(larger particle ²size) fresh or reactivated tailgas catalyst in a layered bed configuration in ²order to target the ²desired performance and pressure drop profiles. Another option is to combine a ²high activity ²and high pressure drop reactivated hydroprocessing catalyst with a low ²pressure drop (larger ²particle size) resized, reshaped, and / or reformulated catalyst to target the ²desired performance ²and pressure drop.²100401 Each of these options allow pressure drop limitations to be mitigated ²and a reactivated ²hydrotreating catalyst to be made suitable for application in a tailgas unit. ²According to some ²embodiments, the catalyst, as used in the original hydrotreating process would ²cause a pressure²14²CA 03138356 2021- 11- 16²<DP=15>²WO 2020 / 237200 ² PCT / US2020 / 034353²drop of about 0.20 psi / ft to about 0.80 psi / ft, for example about 0.40 psi / ft ²to about 0.60 psi / ft, ²when sock-loaded and tested at a superficial velocity of 100 ft / min in ambient ²air. After the ²catalyst is resized, reshaped, reformulated, short loaded, and / or combined ²with another lower ²pressure drop catalyst for taigas treatment using one of the methods described ²above, the ²catalyst may cause a pressure drop of about 0.05 psi / ft to about 0.20 psi / ft, ²for example about ²0.10 psi / ft to about 0.15 psi / ft, when sock-loaded and tested at a superficial ²velocity of 100 ²ft / min in ambient air.²100411 One or more of the resizing, reshaping, and reformulating steps ²described above may ²be used to reconfigure a catalyst obtained from a first, non-tailgas treatment ²process to optimize ²the catalyst for tailgas treating. Figure 10 illustrates an embodiment of a ²process 1500 for ²reactivating a catalyst for tailgas treating. First a catalyst is obtained ²from a non-tailgas ²treatment process 1502. The catalyst may be a tri-lobe or quad-lobe catalyst, ²for example, and ²may typically have a size of about 1.3-2.5 mm. As mentioned above, the ²catalyst may comprise ²one or more Group \FMB metals and one or more Group V1B metals supported on a ²carrier ²material, such as alumina (A1203), silica alumina, zeolite, or combinations ²thereof.²100421 The obtained catalyst may be thermally stripped or solvent extracted ²1504, typically to ²remove residual hydrocarbons from the catalyst. For example, the thermal ²stripping process ²may involve contacting the catalyst with hot steam or gas, air, natural gas ²combustion products, ²hydrogen or nitrogen at a temperature from 150 C to 550 C. For example, the ²solvent ²extraction process may involve contacting the catalyst with a non-polar ²solvent. The stripped ²or solvent extracted catalyst may be regenerated 1506, as described above. For ²example, the ²catalyst may be heated at a temperature of about 200 C to about 600 C, more ²preferably 380 C ²to about 500 C for 1-24 hours, inure preferably 1-3 hours. The regenerated ²catalyst may be ²resized 1508, typically by grinding or milling the regenerated catalyst to ²form a powder. The ²powder may be isolated, for example, by screening. The powder may be ²reformulated 1510 in ²one or more aspects. For example, the powder may be combined with additional ²carrier ²material, such as alumina, thereby adjusting the relative loading of the ²active catalyst materials ²(Le., metals). The catalyst may be reshaped 1512, for example, by extruding ²the resized and ²reformulated material into a shape that is the same or different than the ²original catalyst shape_ ²For example, the original catalyst may have been multi-lobed with a Oven ²number of lobes²tri-lobed or quad-lobed) and it may be reshaped to yield a cylindrical or ²spherical shaped ²catalyst. It should be noted that the catalyst may be further reformulated ²after reshaping. For ²example, the reshaped catalyst may be impregnated with further active ²materials (e.g.,. cobalt, ²nickel, and / or molybdenum precursor materials). The catalyst may be ²rejuvenated 1514. For² CA 03138356 2021- 11- 16²<DP=16>²WO 2020 / 237200 ² PCT / US2020 / 034353²example, the newly shaped catalyst may be exposed to one or more rejuvenation ²reagents and ²processes as described above. According to some embodiments, the catalyst is ²impregnated ²using a chelating matenal as described above, aged, and dried. According to ²some ²embodiments, the chelating material can include an organic additive, a portion ²of which ²remains in the catalyst material following the rejuvenation process.²100431 It should be noted that the process 1500 is only exemplary. Some of the ²steps may be ²omitted or the steps may be conducted in a different order. For example, the ²catalyst obtained ²from the original (non-tailgas treatment) process may be regenerated and ²rejuvenated prior to ²resizing and reshaping or even be prepared without any resizing or reshaping. ²Other ²modifications to the process 1500 will be apparent to a person of skill in the ²art based on this ²disclosure.²100441 The following examples are included to demonstrate aspects of the ²disclosed techniques ²and compositions.²100451 Example 1: Realistic Space Velocity (1.200 (JHSV) Testing ²100461 A cylindrical vertically oriented glass reactor with an internal ²diameter of 3.0 cm and a ²height of 51 cm was filled with 70 mL of catalyst for each catalyst tested. ²Each of the fresh, ²regenerated, and Excel rejuvenated catalyst samples (#1-10 and 13 in list ²below) were ²submitted to the same testing protocol, which consisted first of an in-situ ²sulfiding activation ²step, followed by specified performance test conditions. During the in-situ ²sulfiding step, a gas ²of the following molar composition was passed over the catalyst in down-flow ²fashion: 2% ²H2S, 10%142, and 88% N2, The feed gas composition was set using properly ²calibrated mass ²flow controllers for each component and verified by gas chromatography ²initially. The space ²velocity of the gas during the in-situ sulfiding step was 2,000 GI-ISV. The ²temperature was ²evenly ramped from 200 C to 315 C over a period of 16 hours. The effluent gas ²composition ²was measured every 2 hours by gas chromatography. After the 16 hours was ²completed, the ²catalyst was considered to have been fully activated by the in-situ sulfiding ²condition. There ²were two samples tested for which the in-situ sulfiding was not necessary ²because the active ²metals were already in the sulfide state, the solvent extracted, and hot ²nitrogen stripped samples ²(#11 and 12, respectively). An alternative activation startup used for pre-²activated (pre-²sulfided) tailgas catalysts was selected for these tests. For the alternative ²activation startup, a ²gas of the following molar composition was passed over the catalyst in down-²flow fashion: 3% ²112, 3% CO, 9% CO2, 25% H20, and 60% N2. The feed gas composition was set ²using properly ²calibrated mass flow controllers for each component and verified by gas ²chromatography ²initially. The space velocity of the gas during the activation step was 500 ²GHSV. The²16²CA 03138356 2021- 11- 16²<DP=17>²WO 2020 / 237200 ² PCT / US2020 / 034353²temperature was evenly ramped from 200 C to 315 C over a period of 24 hours. ²The effluent ²gas composition was measured every 2 hours by gas chromatography. After the 24 ²hours was ²completed, the catalyst was considered to have been fully activated and ready ²for performance ²testing.²100471 After completion of the startup in-situ sulfiding or activation, the ²catalyst bed was ready ²for the performance test conditions. During the performance test conditions, a ²gas of the ²following molar composition was passed over the catalyst in down-flow fashion: ²70.05% N2, ²25% H20, 233% Hz, 1.20% CO2., 0.59% CO, 0.47% 112S, 0.23% S02, 0.060% COS, and ²²0.061% CS2. The feed gas composition was set using properly calibrated mass ²flow controllers ²for each component and verified by gas chromatography initially. The space ²velocity of the gas ²for the performance test conditions was 1,200 GHSV, equivalent to a residence ²time of 3 ²seconds, and was intended to represent realistic commercial operating space ²velocity. The ²performance tests occurred at four distinct temperature conditions: 220 C, 240 ²C, 280 C, and ²300 C. At each condition, the temperature was held for a time of 12 hours, ²more than enough ²time for performance to reach steady state. Compositional analysis of the ²reactor effluent was ²performed every 2 hours by gas chromatography. From the feed and average gas ²analysis at ²each performance test condition, the conversion of SO2, CS2, and COS were ²determined.²100481 Thirteen different catalyst samples were tested according to the above-²specified testing ²protocol. These are listed below:²1. Regenerated Commercial Hydroprocessing Catalyst A (2.5nun trilobe)²2. Excel Rejuvenated Commercial Hydroprocessing Catalyst A (2.5mm trilobe)²3. Regenerated Commercial Hydroprocessing Catalyst B (2.5 mm quadlobe)²4. Excel Rejuvenated Commercial Hydroprocessing Catalyst B (2.5 mm ²quadlobe)²5. Fresh Commercial Hydroprocessing Catalyst C (2.5 min quadlobe)²6. Regenerated Commercial Hydroprocessing Catalyst C (2.5 mm quadlobe) from ²²Application 1.²7. Regenerated Commercial Hydroprocessing Catalyst C (2.5 mm quadlobe) from ²²Application 2.²8. Regenerated Commercial Hydroprocessing Catalyst D (2.5 mm trilobe)²9. Excel Rejuvenated Commercial Hydroprocessing Catalyst D (2.5 mm ²trilobe)²10. Regenerated Commercial Hydroprocessing Catalyst E (2.5 mm trilobe)²11. Solvent Extracted Commercial Hydroprocessing Catalyst F (2.5 mm ²trilobe)²12. Hot Nitrogen Stripped Commercial Hydroprocessing Catalyst F (2.5 mm ²trilobe), and²13. Fresh Commercial Tailgas Catalyst (3.2 mm trilobe).²17²CA 03138356 2021- 11- 16²<DP=18>²WO 2020 / 237200 ² PCT / US2020 / 034353²
[0049] Catalyst A was used in diesel (ULSD) hydrotreating service prior to its ²reactivation. ²Following its use in diesel hydrotreating, Catalyst A was treated by ²regeneration and Excel ²rejuvenation processes, as described in the above-incorporated '679 Patent. ²The regeneration ²process features, in some cases, a fluidized hot air strip to remove ²hydrocarbons and reduce ²coke content, followed by, in all cases, a high residence time, moving belt ²heat soak to remove ²carbon and sulfur embedded deep in the catalyst pores. The Excel rejuvenation ²process ²involves first catalyst regeneration, as just described, followed by ²impregnation with a solution ²of chelating agent into the pores. The impregnated catalyst is allowed to age ²for a specific ²amount of time and then dried. The rejuvenation process helps to reverse ²metals agglomeration ²that occurs while the catalyst is in service and as a result of the ²regeneration process. While ²Porocel's regeneration and Excel rejuvenation processes were used in these ²examples, ²regeneration and rejuvenation processes are well-known to those skilled in the ²art and are ²described, for example, in the above-referenced patents.²
[0050] Catalyst B was used to process vacuum gas oil for fluid catalytic ²cracking feed ²pretreatment prior to its reactivation. Following its use in vacuum gas oil ²treating, Catalyst B ²was treated by regeneration and Excel rejuvenation processes, as described ²above.²
[0051] The fresh sample of commercial hydroprocessing Catalyst C was acquired ²in the ²surplus catalyst market for the purpose of performance testing.²
[0052] Catalyst C from Application 1 was used in gas oil hydrotreating service ²prior to ²regeneration. Following its use in gas oil hydrotreating, Catalyst C was ²treated by a ²regeneration process, as described above.²
[0053] Catalyst C from Application 2 was used in kerosene hydrotreating ²service prior to ²regeneration. Following its use in kerosene hydrotreating, Catalyst C was ²treated by a ²regeneration process, as described above.²
[0054] Catalyst D was used in diesel (ULSD) hydrotreating service prior to ²reactivation. ²Following its use in diesel (ULSD) hydrotreating, Catalyst D was treated by ²regeneration and ²Excel rejuvenation processes, as described above.²
[0055] Catalyst E was used in a hydrotreating service prior to reactivation. ²Following its use ²in the hydrotreating service, Catalyst E was treated by a regeneration ²process.²
[0056] Catalyst F was used in vacuum gas oil (VGO) pretreatment service for ²hydrocracicing ²prior to recovery of the spent sample. Following its use in vacuum gas oil ²(VGO) pretreatment ²service for hydrocracking, Catalyst F was divided into two samples and ²submitted to two ²different treatments. The first treatment was a Soxhlet solvent extraction ²performed with ²toluene for 4 hours before drying for 2 hours at 110 C. The purpose of the ²solvent extraction²18²CA 03138356 2021- 11- 16²<DP=19>²WO 2020 / 237200 ² PCT / US2020 / 034353²was to remove residual hydrocarbons from the spent catalyst. The second ²treatment was a hot ²strip at 370 C in a pure nitrogen sweep for 1 hour in a rotary tube calciner. ²The hot nitrogen ²strip was also intended to remove residual hydrocarbons from the spent ²catalyst sample.²100571 The fresh commercial tailgas catalyst was acquired in the surplus ²catalyst market for ²the purpose of performance testing.²100581 All the hydroprocessing catalysts tested were of the same size and ²shape as used for ²their original service and no reformulation was performed. Catalyst A, B, and ²C were all ²different catalysts made by different manufacturers and used in different ²hydrotreating ²services. Catalyst A and Catalyst D were made by the same manufacturer, were ²in the same ²service, and were even originally used in the same reactor but were different ²catalysts, with ²Catalyst A being CoMo on alumina and Catalyst D being NiMo on alumina Catalyst ²C from ²application 1 and Catalyst C from application 2 were made by the same ²manufacturer and were ²the same type of catalyst but were sourced from different reactors after being ²used in different ²hydrotreating services and both had different contaminant profiles. Catalysts ²A and D-F were ²all made by the same manufacturer but were different catalysts, with different ²types of metals ²and metal concentrations present. Catalysts A-C were all cobalt and molybdenum ²(CoMo) on ²alumina support, whereas Catalyst D-F were nickel and molybdenum (NiMo) on ²alumina ²support. The fresh tailgas catalyst used for competitive evaluation and the ²fresh Catalyst C ²reference sample had seen no prior service and were used in the completely ²fresh form without ²alteration, just as it would be directly from the manufacturer. Select ²analytical data for the ²catalyst samples that were performance tested is shown in Table 1 (Figure 2). ²The Excel* ²rejuvenated samples for each catalyst were from the same source material as ²the regenerated ²samples and are expected to be virtually identical with respect to the ²physical properties in ²Table 1. In the case of Catalyst F, the metals data was acquired by performing ²XRF analysis ²on a lab-scale regenerated sample, while the other analytical data were from ²the solvent ²extracted and hot nitrogen stripped samples in the state they were in before ²performance testing. ²Catalyst A and C were both phosphorous promoted CoMo on alumina catalysts, ²whereas ²Catalyst B was a non-phosphorous promoted CoMo on alumina catalyst. On the ²other hand, ²Catalyst D and F were both phosphorous promoted NiMo on alumina catalysts, ²whereas ²Catalyst E was a non-phosphorous promoted NiMo on alumina catalyst. Catalyst E ²was silicon ²promoted, whereas all other catalysts were not. Overall, the list of catalysts ²tested in Example ²1 and Figure 2 show that a good cross section of the hydroprocessing catalyst ²market was ²tested, from CoMo to NiMo, from phosphorous promoted to non-phosphorous ²promoted, from ²higher to lower active metals loadings, from silicon to non-silicon promoted, ²from fresh to²19²CA 03138356 2021- 11- 16²<DP=20>²WO 2020 / 237200 ² PCT / US2020 / 034353²regenerated and rejuvenated (as well as hot nitrogen stripped and solvent ²extracted), and from ²different catalyst types / products, manufacturers, and hydroprocessing ²applications.²100591 The test results for the above described testing protocol and catalysts ²are listed in Table ²2 (Figure 3). Looking first at SO2 conversion performance, Figure 3 shows that ²out of the 36 ²performance data points generated at each temperature condition for the nine ²regenerated and ²rejuvenated hydroprocessing catalysts in their native form, only four ²performance data points ²fell below the fresh tailgas competitive reference catalyst. The fact that 32 ²out of the 36 ²performance data points indicated superior performance (an outperformance rate ²of almost ²90%) provides strong evidence that the reactivated hydroprocessing catalysts ²can be fit for use ²in Claus tailgas hydrogenation service. Overall, conversion was very high ²(>98%) for all the ²regenerated and rejuvenated hydroprocessing catalysts in their native form ²that were tested. ²High SO2 conversion was also achieved for the solvent extracted and hot ²nitrogen stripped ²versions of Catalyst F, with only three out of eight performance data points ²falling below the ²fresh tailgas competitive reference catalyst. From a practical standpoint, ²since hydrogenation ²of SO2 proceeds much more readily than the hydrolysis of COS and CS2 and, in ²many cases, ²closely approaches 100%, it is often more useful to compare the performance ²for hydrolysis of ²COS and CS2 between the different catalysts for better resolution and ²differentiation of ²performance.²100601 Looking next at CS2 conversion performance, Figure 3 shows that out of ²the 36 ²performance data points generated at each condition for the nine regenerated ²and rejuvenated ²hydroprocessing catalysts in their native form, only one performance data ²point fell below the ²fresh tailgas competitive reference catalyst. The fact that 35 out of the 36 ²performance data ²points indicated superior performance (an outperformance rate of 97%) provides ²compelling ²evidence that the reactivated hydroprocessing catalysts can be fit for the use ²of CS2 hydrolysis ²in Claus tailgas hydrogenation service. One observation worth noting is that ²the ²outperformance of all the hydroprocessing catalysts tested when compared to ²the fresh tailgas ²competitive reference catalyst was much more pronounced at the 240 C, 280 C, ²and 300 C ²temperature conditions. It is only at the 220 C condition that there is a ²significant (>10%) drop ²in performance for three out of the nine regenerated and rejuvenated ²hydroprocessing catalysts ²in their native form. Still, even with this significant drop in performance at ²220 C, all but one ²of the hydroprocessing catalysts still displayed higher CS2 conversion ²activity. The hot nitrogen ²stripped and solvent extracted versions of Catalyst F generally underperformed ²the fresh tailgas ²competitive reference catalyst, with seven out of the eight performance data ²points falling ²below the fresh tailgas competitive reference catalyst. It is worth noting ²that the solvent² CA 03138356 2021- 11- 16²<DP=21>²WO 2020 / 237200 ² PCT / US2020 / 034353²extracted version of Catalyst F displayed nearly equal but slightly lower ²performance than the ²fresh tailgas competitive reference, whereas the hot nitrogen stripped version ²of Catalyst F ²displayed a widening margin of underperformance as temperature decreased.²100611 Looking next at COS conversion performance, Figure 3 shows that out of ²the 36 ²performance data points generated at each condition for the nine regenerated ²and rejuvenated ²hydroprocessing catalysts in their native form, ten performance data points ²fell below the fresh ²tailgas competitive reference catalyst. With 26 out of the 36 performance data ²points indicating ²superior performance (an outperformance rate of 72%), evidence is provided ²that these ²reactivated hydroprocessing catalysts can be fit for the use of COS hydrolysis ²in Claus tailgas ²hydrogenation service. It is worth noting that eight out of the ten data ²points that fell below the ²fresh tailgas competitive reference catalyst were for two of the three Excel ²rejuvenated ²catalysts tested. In general, it was observed that Excel rejuvenated ²catalysts showed lower ²COS conversion performance than their regenerated counterparts, a surprising ²finding. Even ²so, the Excel rejuvenated catalysts still displayed quite high levels of COS ²conversion and ²did not significantly underperform the fresh competitive taigas reference. ²Considering only ²the regenerated hydroprocessing catalysts in their native form, the ²outperformance rate ²increases to 22 out of 24, or 92%. Although the data also indicate that in ²general, rejuvenation ²did not contribute to higher COS conversion performance, it did contribute to ²higher CS2 ²conversion performance. Overall the data indicate that both regenerated and ²rejuvenated ²hydroprocessing catalysts in their native form can provide excellent COS ²conversion ²performance relative to the fresh tailgas competitive reference catalyst. The ²solvent extracted ²and hot nitrogen stripped versions of Catalyst F significantly underperformed ²the fresh tailgas ²competitive reference catalyst. In fact, both displayed half or less of the ²COS conversion ²observed for the fresh commercial tailgas reference catalyst at the highest ²temperature (300 C) ²and conversion actually inflected to negative values, or net COS generation, ²at the lowest ²temperature (220 C), indicating these catalysts are highly unsuitable for COS ²conversion.²100621 As can be seen from Figure 3, the regenerated and rejuvenated ²hydroprocessing ²catalysts in their native form compare quite favorably with the fresh tailgas ²competitive ²reference catalyst. To provide a more comprehensive picture of how the ²performance affects ²the sulfur recovery efficiency (SRE) impact by the catalyst, a combined metric ²for overall ²conversion of the sulfur in SO2, CS2, and COS was calculated. The equation ²used to calculate ²this metric is reproduced in Figure 4, which also provides a comparison (Table ²3) of the overall ²sulfur conversion obtained using the thirteen catalysts. All nine of the ²regenerated and ²rejuvenated hydroprocessing catalysts in their native form outperformed the ²fresh tailgas²21²CA 03138356 2021- 11- 16²<DP=22>²WO 2020 / 237200 ² PCT / US2020 / 034353²competitive reference catalyst at 240 C and above. At the low temperature, 220 ²C, six of the ²regenerated and rejuvenated catalysts significantly outperformed the fresh ²tailgas competitive ²reference catalyst, while three were within 1%, a trivial difference. ²Therefore, practically ²speaking, the regenerated and rejuvenated hydroprocessing catalysts in their ²native form ²performed as well or better than the fresh commercial tailgas reference ²catalyst. Overall, this ²comprehensive view of sulfur conversion performance indicates that regenerated ²and ²rejuvenated hydroprocessing catalysts, if applied correctly, can offer an ²excellent alternative to ²very well-established tailgas catalyst products in the market such as the ²fresh tailgas ²competitive reference catalyst tested. The solvent extracted and hot nitrogen ²stripped versions ²of Catalyst F both significantly underperformed the fresh tailgas competitive ²reference catalyst. ²The poor performance results for the solvent extraction and hot nitrogen ²stripped versions of ²Catalyst F can be explained by the fact that the coke deactivation of the ²spent catalyst is not ²eliminated by these treatments as it is with thermal oxidative regeneration. ²Regeneration ²treatment is necessary to substantially remove the coke present on the ²catalyst and enable a ²high performing catalyst for this application.²100631 Example 2¨ "Stress Testing" at High Space Velocity (3,000 GHSV). ²100641 The performance of catalysts 1-4 and 13 described in Example 1 were ²tested using the ²same experimental set-up but under high space velocity conditions. The space ²velocity of the ²gas for the performance test conditions was 3,000 GHSV, equivalent to a ²residence time of 1.2 ²seconds, and was intended to represent a "stress test" to further ²differentiate relative catalyst ²performance vs. the 1,200 GHSV testing. The performance tests occurred at ²three distinct ²temperature conditions: 220 C, 250 C, and 280 C. At each condition, the ²temperature was held ²for a time of 12 hours. Compositional analysis of the reactor effluent was ²performed every 2 ²hours by gas chromatography. From the feed and effluent gas analysis at each ²performance test ²condition, the conversion of S02, CS2, and COS were determined. Table 4 ²(Figure 5) and ²Figures 6-9 show the results of the testing at 3,000 GHSV.²100651 Figure 6 shows SO2 conversion performance at 3000 GHSV using the five ²catalysts. ²Out of the twelve performance data points generated at each condition for the ²four regenerated ²and rejuvenated hydroprocessing catalysts, only three performance data points ²fell below the ²fresh tailgas competitive reference catalyst, with two of the three ²underperforming by less than ²1%. The fact that nine out of the twelve performance data points indicated ²superior ²performance shows that the hydroprocessing catalysts can be fit for the use of ²SO2 ²hydrogenation in Claus tailgas hydrogenation service. Overall, conversion was ²still very high²22²CA 03138356 2021- 11- 16²<DP=23>²WO 2020 / 237200 ² PCT / US2020 / 034353²(>97%) for all samples tested, above 220 C. At 220 C, three out of the four ²hydroprocessing ²catalysts showed higher performance than the fresh tailgas competitive ²reference.²100661 Figure 7 shows CS2 conversion performance at 3000 GHSV using the five ²catalyst& ²Out of the twelve performance data points generated at each condition for the ²five regenerated ²and rejuvenated hydroprocessing catalysts, all of them indicated superior ²performance ²compared to fresh tailgas competitive reference catalyst. The fact that all ²twelve of data points ²indicated superior performance shows that the hydroprocessing catalysts can be ²fit for the use ²of CS2 hydrolysis in Claus tailgas hydrogenation service. Not only did the ²hydroprocessing ²catalysts tested outperform, they did so by a wide margin (>20%) across the ²board, a very ²surprising finding. As with the testing at 1,200 GHSV outlined in Example 1, ²it is important to ²note that these results also suggest that the rejuvenation process enhances ²activity for CS2 ²hydrolysis.²100671 Figure 8 shows COS conversion performance at 3000 GHSV using the five ²catalysts_ ²Out of the twelve performance data points generated at each condition for the ²four regenerated ²and rejuvenated hydroprocessing catalysts, only two performance data points ²fell below those ²of the fresh tailgas competitive reference catalyst. With ten out of the ²twelve performance data ²points indicating superior performance, it is clear that the hydroprocessing ²catalysts can be fit ²for the use of COS hydrolysis in Claus tailgas hydrogenation service. It is ²worth noting that at ²250 C and above, the hydroprocessing catalyst samples tested outperformed the ²fresh tailgas ²competitive reference catalyst by about 20%. Only at the 220 C condition did ²the COS ²conversion for two of the four hydroprocessing catalysts drop below that of ²the fresh tailgas ²competitive reference catalyst. For overall tailgas hydrogenation performance, ²the data indicate ²that both regenerated and rejuvenated forms can provide good performance ²compared to the ²fresh tailgas competitive reference catalyst. One interesting feature to note ²was that the Excel ²Rejuvenated Catalyst A sample displayed a negative conversion, or net ²formation, of COS at ²220 C. This is likely because the COS hydrolysis pathway is kinetically ²limited for this ²catalyst, thus not allowing approach to the calculated equilibrium conversion ²and meaning that ²COS can be formed faster than it is consumed by reaction. This is also ²indicated by the fact ²that conversion was about 62% at 220 C and 1,200 GHSV (see Example 1) but at ²the higher ²space velocity (3000 GHSV) in this example, the conversion decreased to -20%, ²or a net ²formation of 20%.²100681 Overall, the regenerated and rejuvenated hydroprocessing catalysts ²compare favorably ²with the fresh tailgas competitive reference catalyst. Figure 5 and Figure 9 ²shows how these ²catalysts perform with respect to overall sulfur recovery efficiency (SRE, see ²Equation of²23²CA 03138356 2021- 11- 16²<DP=24>²WO 2020 / 237200 ² PCT / US2020 / 034353²Figure 4) at 3000 GHSV. For the overall sulfur conversion performance, all the ²regenerated ²and rejuvenated catalysts that were tested displayed equivalent or better ²performance than the ²fresh tailgas competitive reference catalyst. Except for the Regenerated ²Catalyst A sample at ²220 C, the overall picture was one of substantial outperformance compared to ²fresh tailgas ²competitive reference catalyst. These "stress test" results further confirm ²the findings from the ²realistic 1,200 GHSV testing in Example 1, namely, that regenerated and ²rejuvenated ²hydroprocessing catalysts, when applied correctly, can offer an excellent ²alternative to very ²well-established tailgas catalyst products in the market such as fresh tailgas ²competitive ²reference catalyst_²100691 Example Preparation of Regenerated 3.39wt% Cobalt ¨ 16.57wt% Molybdenum ²- ²Balance Alumina Catalyst ²100701 The following is a preparation procedure for making a catalyst with ²3.39 wt.% cobalt ²(as Co0) and 16.57 wt.% molybdenum (as Moth), with the balance consisting of ²primarily ²alumina (Al2O3). The source of the cobalt and molybdenum metals came from a ²spent 2.5 mm ²trilobe CoMo on alumina hydroprocessing catalyst (See Catalyst C ¨ Application ²1 in Table 1) ²which contained 3.39% cobalt and 16.57% molybdenum as determined by X.RF ²analysis. The ²hydroprocessing catalyst was regenerated by a regeneration process, as ²described above in ²Example 1. In this way, the Regenerated Catalyst C ¨ Application 1 sample ²which was ²performance tested under realistic tailgas conditions (see data in Table 2 and ²3), was prepared. ²100711 While the invention herein disclosed has been described in terms of ²specific ²embodiments and applications thereof, numerous modifications and variations ²could be made ²thereto by those skilled in the art without departing from the scope of the ²invention set forth in ²the claims.²100721 Example 4: Preparation of Rejuvenated 3.50wt% Nickel ¨ 15.86wt4Yo ²Molybdenum - ²Balance Alumina Catalyst ²100731 The following is a preparation procedure for making a catalyst with ²3.50 wt.% nickel ²(as NiO) and 15.86 wt.% molybdenum (as Moth), with the balance consisting of ²primarily ²alumina (Al2O3). The source of the nickel and molybdenum metals came from a ²spent 2.5 nun ²trilobe NiMo on alumina hydroprocessing catalyst which contained 3.50% nickel ²and 15.86% ²molybdenum as determined by XRF analysis. The catalyst was prepared by ²Porocel's Excel* ²rejuvenation process as described in US Patent 9,895,679. In this way, the ²Excel* Rejuvenated ²Commercial Hydroprocessing Catalyst D (25 mm trilobe) sample which was ²performance ²tested under realistic tailgas conditions (see data in Table 2 and 3), was ²prepared.²24²CA 03138356 2021- 11- 16²<DP=25>²WO 2020 / 237200 ² PCT / US2020 / 034353²
[0074] While the invention herein disclosed has been described in terms of ²specific ²embodiments and applications thereof, numerous modifications and variations ²could be made ²thereto by those skilled in the art without departing from the scope of the ²invention set forth in ²the claims.² CA 03138356 2021- 11- 16²
Claims
<DP=1>²WHAT IS CLAIMED IS:²1. A method of treating a gas stream in a tailgas treating process, the ²method ²comprising:²contacting the gas stream with a catalyst that was previously used in a ²hydrotreating ²process and that has been reactivated by a reactivation process prior to ²contacting the gas stream in the tailgas treating process, wherein²the gas stream comprises one or more sulfur-containing species selected from ²the ²group consisting of elemental sulfur (Sx), sulfur dioxide (S02), carbonyl ²sulfide (COS), and carbon disulfide (CS2), and wherein²contacting the gas stream with the reactivated catalyst in the presence of ²hydrogen ²(Hz) converts the one or more sulfur-containing species to hydrogen sulfide ²(H2S).²2. The method of claim 1, wherein the hydrotreating process is selected ²from the group ²consisting of petroleum hydrotreating processes, hydrodesulfurization (HDS), ²hydrodenitrogenation (HDN), hydrogenation, hydrodemetallization (HDM), naphtha ²²hydrotreating (NHT), diesel hydrotreating (DHT), kerosene hydrotreating (KHT), ²jet fuel ²hydrotreating (JFIT), atmospheric gas oil hydrotreating, vacuum gas oil (VGO) ²hydrotreating, ²and fluid catalytic cracker (FCC) feed hydrotreating.²3. The method of claim 1, wherein the catalyst comprises one or rnore Group ²V111B ²metals and one or more Group VIB metals supported on an inorganic oxide ²carrier material.²4. The method of claim 1, wherein the catalyst comprises cobalt and ²molybdenum ²supported on aluminum oxide.²5. The method of claim 1, wherein the catalyst comprises nickel and ²molybdenum ²supported on aluminum oxide.²6. The method of claim 1, wherein the reactivation process comprises ²regeneration.²26²CA 03138356 2021- 11- 16²<DP=2>²7. The method of claim 6, wherein the regeneration comprises heating the ²catalyst in an ²oxygen-containing atmosphere at a temperature of 300 to 500 oiC for a time of ²30 minutes or ²more.²8. The method of claim 6, wherein prior to the regeneration treatment, ²hydrocarbons are ²removed from the catalyst by solvent extraction or by contacting the catalyst ²with steam, ²natural gas combustion products, hydrogen or nitrogen at a temperature of 150 ²to 550 'C.²9. The method of claim 1, wherein the reactivation process comprises ²rejuvenation.²10. The method of claim 9, wherein the rejuvenation comprises impregnating ²the catalyst ²with a solution containing a chelating agent and drying the catalyst at a ²temperature of 50 C ²to 300 C.²11. The method of claim 10, wherein the chelating agent is an organic acid.²12. The method of claim 1, wherein the reactivated catalyst is pre-²sulfurized prior to ²contacting the gas stream in the lailgas treating process.²13. The method of claim 1, wherein the reactivated catalyst is pre-sulfided ²prior to ²contacting the gas stream in the blips treating process.²14. The method of claim 1, wherein the reactivated catalyst is resized, ²reshaped, and / or²reformulated prior to contacting the gas stream in the tailgas treating ²process.²15. The method of claim 14, wherein the reactivated catalyst is resized by ²length grading ²the catalyst.²16. The method of claim 14, wherein the resizing, reshaping, and / or ²reformulating ²comprises milling the reactivated catalyst to a fine powder and then reforming ²the reactivated ²catalyst.²17. The method of claim 14, wherein the reactivated catalyst is resized ²from having a ²diameter of L3 to 2.5 nun to having a diameter of 3 to 5 mm.²27²CA 03138356 2021- 11- 16²<DP=3>²18. The method of claim 1, wherein contacting the gas stream with the ²reactivated ²catalyst comprises combining the reactivated catalyst with a second catalyst, ²wherein the ²second catalyst provides a lower pressure drop than the reactivated catalyst.²19. The method of claim 1, wherein contacting the gas stream with the ²reactivated ²catalyst comprises short loading the reactivated catalyst.²20. The method of claim 1, wherein the reactivated catalyst exhibits a ²pressure drop of ²0.05 to 0.20 psi / ft, when sock-loaded and tested at 100 ft / min superficial ²velocity in ambient ²air.²21. A method of forming a reactivated catalyst for a tailgas treating ²process, the method ²comprising:²obtaining a spent catalyst from a hydrotreating process, and²reactivating the catalyst to form the reactivated catalyst, wherein²the reactivated catalyst, when contacted with a gas stream comprising one or ²more ²sulfur-containing species selected from the group consisting of elemental ²sulfur (Sx), sulfur dioxide (S02), carbonyl sulfide (COS), and carbon ²disulfide ²(CS2), is capable of catalyzing the conversion of the one or more sulfur-²containing species to hydrogen sulfide (H2S) in the presence of hydrogen (H2).²22. The method of claim 21, wherein the hydrotreating process is selected ²from the group ²consisting of petroleum hydrotreating processes, hydrodesulfurization (HDS), ²hydrodenitrogenation (HDN), hydrogenation, hydrodemetallization (HDM), naphtha ²²hydrotreating (NHT), diesel hydrotreating (DHT), kerosene hydrotreating (KHT), ²jet fuel ²hydrotreating (MT), atmospheric gas oil hydrotreating, vacuum gas oil (VGO) ²hydrotreating, ²and fluid catalytic cracker (FCC) feed hydrotreating.²23. The method of claim 21, wherein the spent catalyst comprises: ²an inorganic oxide support material having a surface area of 20 to 600 m2 / g, ²one or²more Group VIIII3 metais, and one or more Group VIB metals supported on ²the inorganic oxide support material.²28²CA 03138356 2021- 11- 16²<DP=4>²24, The method of claim 21, wherein the catalyst comprises cobalt and ²molybdenum²supported on aluminum oxide.²25. The method of claim 21, wherein the catalyst comprises nickel and ²molybdenum ²supported on aluminum oxide.²26. The method of claim 21, wherein the reactivating comprises ²regeneration.²27. The method of claim 26, wherein the regeneration comprises heating the ²catalyst in an ²oxygen-containing atmosphere at a temperature of 300 to 500 C for a time of ²30 minutes or ²more.²28. The method of claim 26, wherein, prior to the regeneration, removing ²hydrocarbons ²from the catalyst by solvent extraction or by contacting the catalyst with ²steam, natural gas²combustion products, hydrogen or nitrogen at a temperature of 150 to 550 oC.²29. The method of claim 21, wherein the reactivating comprises ²rejuvenation.²30. The method of claim 29, wherein the rejuvenation comprises impregnating ²the ²catalyst with a solution containing a chelating agent and drying the catalyst ²at a temperature ²of 50"C to 300 C.²31. The method of claim 30, wherein the chelating agent is an organic acid.²32. The method of claim 21, further comprising pre-sulfurizing the ²reactivated catalyst²33. The method of claim 21, further comprising pre-sulfiding the ²reactivated catalyst.²34. The method of claim 21, further comprising resizing, reshaping, and / or ²reformulating ²the reactivated catalyst.²35, The method of claim 21, thither comprising milling the reactivated ²catalyst to a fine²powder and then reforming the reactivated catalyst.²29²CA 03138356 2021- 11- 16²<DP=5>²36, The method of claim 35, wherein the spent catalyst, prior to ²reactivating, has a²diameter of L3 to 2.5 nun and the reformed reactivated catalyst has a diameter ²of 3 to 5 mm.²37. The method of claim 21, wherein the spent catalyst, as used in the ²hydrotreating²process, exhibits a pressure drop of 0.20 to 0.80 psi / ft, and wherein the ²method further ²comprises resizing, reshaping, and / or reformulating the reactivated catalyst ²so that the ²reactivated catalyst exhibits a pressure drop of 0.05 to 0.20 psi / ft, when ²sock-loaded and ²tested at 100 ft / min superficial velocity in ambient air.² CA 03138356 2021- 11- 16²