Positive electrode plate, battery comprising the positive electrode plate, and electrical device

CA3329498A1Pending Publication Date: 2026-11-05CALB GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CA3329498
Authority / Receiving Office
CA · CA
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-01-16
Filing Date
2025-06-03
Publication Date
2026-11-05

AI Technical Summary

Technical Problem

LMFP batteries exhibit poor electronic and ionic conductivity at high SOC levels, leading to deterioration in fast-charging and high-temperature cycling performance. Furthermore, the continuous consumption of electrolyte prevents the positive electrode active material from fully participating in the electrochemical reaction, resulting in poor cycle performance.

Method used

By compounding lithium manganese iron phosphate with ternary cathode materials in the cathode electrode sheet and adjusting the Ni content and longitudinal wettability in the cathode active material layer, a specific relationship is achieved to promote the balance of lithium-ion and electron transport rates, thereby improving the battery's fast-charging performance and high-temperature cycle performance.

Benefits of technology

It significantly shortens the charging time during the high-voltage phase of the battery, improves the lithium-ion and electron transport rate, and enhances the battery's fast-charging performance and high-temperature cycling performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Provided is a positive electrode plate, a battery comprising the positive electrode plate, and an electrical device, and belongs to the technical field of batteries. The positive electrode plate of the present disclosure includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode active material layer contains a positive electrode active material, and the positive electrode active material includes lithium manganese iron phosphate (LMFP) and a ternary positive electrode material, and the positive electrode plate satisfies: 0.09 ≤ a / b ≤ 5.1, wherein a is the mass percentage content of the Ni element in the positive electrode active material layer, and the unit is %; and b is the longitudinal wettability of the positive electrode plate, and the unit is %. In the present disclosure, by compounding the LMFP with the ternary positive electrode material and reasonably controlling the content of the Ni element in the positive electrode active material layer and the longitudinal wettability of the positive electrode plate, after the positive electrode plate is applied to the battery, the charging time of the battery at a high-voltage stage can be significantly shortened, while the lithium ion transport rate and the electron transport rate of the positive electrode plate in the longitudinal direction are balanced, thereby effectively improving the fast charging performance and high-temperature cycling performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Positive electrode, battery containing the positive electrode, and electrical device

[0001] This application is based on and claims priority to Chinese applications CN202411966433.2, filed on December 30, 2024, and CN202510071144.4, filed on January 16, 2025. The disclosures of the above two Chinese applications are again incorporated into this application as a whole. Technical Field

[0002] This application relates to the field of battery technology, and more particularly to a positive electrode, a battery comprising the positive electrode, and an electrical device. Background Technology

[0003] Lithium manganese iron phosphate (LMFP) has a high voltage platform, large theoretical specific capacity, wide availability, and is environmentally friendly, making it a promising positive electrode active material for lithium-ion batteries.

[0004] During the charging process of LMFP batteries, they are first charged to the cutoff voltage using constant current charging, and then charged to the cutoff current using constant voltage charging. However, when the battery is charged to a high SOC, the electronic and ionic conductivity of the LMFP itself and its interface is relatively poor, leading to a deterioration in the battery's fast charging performance. At the same time, under high SOC, both the LMFP and the electrolyte are continuously charged at high voltage and low current. The positive electrode and the electrolyte continuously undergo chemical reactions, and the effective solvent in the electrolyte is continuously consumed. The battery DCR continues to increase, and the polarization of the LMFP charge and discharge electrodes continues to increase. Before the charge and discharge voltage is cut off, the positive electrode active material does not have time to participate in the electrochemical reaction, and the released active lithium continues to decrease, resulting in poor cycle performance.

[0005] Therefore, it is necessary to improve the fast charging performance and high-temperature cycling performance of LMFP batteries. Summary of the Invention

[0006] The purpose of this application is to overcome the shortcomings of the prior art and provide a positive electrode, a battery containing the positive electrode, and an electrical device to improve the fast charging performance and high-temperature cycle performance of LMFP batteries.

[0007] To achieve the above objectives, in a first aspect, this application provides a positive electrode sheet, comprising a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector, wherein the positive active material layer comprises a positive active material, and the positive active material comprises lithium manganese iron phosphate and a ternary positive electrode material, and the positive electrode sheet satisfies the following:

[0008] 0.09≤a / b≤5.1

[0009] Where a is the mass percentage of Ni element in the positive electrode active material layer, in %;

[0010] b represents the longitudinal wettability of the positive electrode sheet, expressed as a percentage.

[0011] Furthermore, the above positive electrode sheet satisfies: 0.17≤a / b≤2.4.

[0012] Furthermore, the range of 'a' above is 0.9% to 47%.

[0013] Furthermore, the range of 'a' above is 2% to 42%.

[0014] Furthermore, the range of b above is 5% to 40%.

[0015] Furthermore, the range of b above is 10% to 35%.

[0016] Furthermore, in the aforementioned lithium manganese iron phosphate, the molar content of manganese, excluding lithium, ranges from 0.6 to 0.8 based on the total molar number of metal elements; and in the aforementioned ternary cathode material, the molar content of nickel, excluding lithium, ranges from 0.1 to 0.92 based on the total molar number of metal elements.

[0017] Furthermore, in the aforementioned lithium manganese iron phosphate, when the molar content of manganese is ≥0.75 based on the total number of moles of metal elements other than lithium, the aforementioned b ≥10%.

[0018] Furthermore, in the aforementioned lithium manganese iron phosphate, when the molar content of manganese is ≥0.75 based on the total molar number of metal elements other than lithium, the aforementioned ternary cathode material is polycrystalline.

[0019] Secondly, this application provides a battery including the aforementioned positive electrode plate.

[0020] Thirdly, this application provides an electrical device including the aforementioned battery.

[0021] Compared with existing technologies, the beneficial effects of this application of ternary materials are as follows: By compounding LMFP with ternary cathode materials and adjusting the content of Ni element in the cathode active material layer and the longitudinal wettability of the cathode sheet to meet a specific relationship, the cathode sheet can significantly shorten the charging time of the battery in the high-voltage stage after being applied to the battery. At the same time, it achieves a balance between the lithium-ion transport rate and electron transport rate of the cathode sheet in the longitudinal direction, effectively improving the fast charging performance and high-temperature cycle performance of the battery. Detailed Implementation

[0022] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0023] In this application, the technical features described in an open-ended manner include both closed technical solutions consisting of the listed features and open technical solutions that include the listed features.

[0024] In this application, numerical ranges are referred to as continuous unless otherwise specified, and include the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values ​​of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.

[0025] In this application, there are no particular restrictions on the specific dispersion and mixing methods.

[0026] Unless otherwise specified, all reagents or instruments used in this application are commercially available products.

[0027] In this application, terms such as "first time" and "second time" are not used to limit the number of times.

[0028] Positive electrode sheet

[0029] This application provides a positive electrode sheet, comprising a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector, wherein the positive active material layer comprises a positive active material, the positive active material comprising lithium manganese iron phosphate and a ternary positive electrode material, and the positive electrode sheet satisfies the following:

[0030] 0.09≤a / b≤5.1

[0031] Where a is the mass percentage of Ni element in the positive electrode active material layer, in %;

[0032] b represents the longitudinal wettability of the positive electrode sheet, expressed as a percentage.

[0033] LMFP itself has relatively poor electronic and ionic conductivity, while ternary cathode materials have better electronic and ionic conductivity. This is because ternary cathode materials are layered oxides, and their layered structure makes Li... +The transport path is shorter, and the elements Co and Ni it contains are more beneficial to the electronic conductivity of the material. Doping ternary cathode materials into LMFP can promote further lithium insertion / extraction in LMFP at high SOC, reduce the time for lithium insertion / extraction in the constant voltage stage, thereby reducing the proportion of the constant voltage stage during charging and reducing the high voltage charging time. At the same time, doping with ternary cathode materials can also compensate for the electronic conductivity required for electrochemical reactions in LMFP at high SOC before the potential cutoff, promoting the release of more active lithium from LMFP and improving cycle performance. In addition, ternary cathode materials are mainly composed of large particles with a stronger physical structure, while LMFP is mainly composed of small particles with a looser physical structure. After rolling, the two materials complement each other through their physical structural characteristics, stress is released, and the compaction density is improved. However, this also makes it more difficult for the electrolyte to wet the cathode sheet, increasing the resistance to lithium-ion transport.

[0034] It should be noted that in this application, SOC is an abbreviation for "State of Charge", which represents the state of charge of the battery. It is the ratio of the remaining battery capacity to the rated capacity of the battery, and is usually expressed as a percentage.

[0035] The longitudinal wettability (b) of the positive electrode refers to the degree of electrolyte wetting of the positive electrode in the direction perpendicular to the positive current collector (i.e., along the thickness direction of the positive current collector). It is calculated based on the mass change of the positive electrode before and after electrolyte wetting. During fast charging, high current density requires efficient transport of electrolyte ions in a short time. Insufficient longitudinal wettability will lead to an increase in the electrolyte concentration gradient in the deeper layers of the electrode, thus limiting ion transport. When the electrode thickness is large, and in high-rate fast charging designs, the requirements for longitudinal wettability are even more stringent, directly affecting the utilization rate of deep active materials. It is essential to ensure uniform electrolyte distribution throughout the entire electrode thickness to avoid forming "dead zones" for ion transport. The impact of insufficient overall wettability is mostly uneven reaction in the surface area, while insufficient longitudinal wettability directly "fails" or reduces the reaction rate of active materials in the deeper areas. The degradation problem in the deeper areas is more insidious and difficult to detect in time through ordinary detection methods. Long-term accumulated degradation will lead to irreversible performance degradation of the battery. Improving the longitudinal wettability of the positive electrode, i.e., enhancing the longitudinal wetting effect, helps improve the lithium-ion transport rate in the positive electrode's longitudinal direction, thus enhancing the battery's fast-charging performance. However, excessively high longitudinal wettability means that the structure of the positive electrode active material layer is too loose in the longitudinal direction. This leads to poor electron contact and conductivity in the positive electrode active material in the longitudinal direction, and during cycling, the electrolyte is more likely to undergo side reactions with the positive electrode active material, resulting in increased impedance. Conversely, excessively low longitudinal wettability of the positive electrode will also result in poor longitudinal wetting effect, low lithium-ion transport rate, and insufficient electrolyte wetting between the positive electrode active material particles, leading to rapid degradation of battery cycle performance.

[0036] The value of the longitudinal wettability (b) of the positive electrode sheet can be adjusted by changing the type of ternary positive electrode material and / or LMFP (e.g., choosing single crystal or polycrystalline for ternary positive electrode material, and single crystal or polycrystalline for LMFP), the content of the conductive agent, or adjusting the pressure during the rolling process. Specifically, single crystal of ternary positive electrode material refers to the primary particles of the ternary positive electrode material; polycrystalline of ternary positive electrode material refers to the secondary particles of the ternary positive electrode material, composed of multiple primary particles; single crystal of LMFP refers to non-agglomerated primary particles, or secondary particles with a low degree of agglomeration (two or three primary particles clustered together); polycrystalline LMFP refers to LMFP agglomerates, which are secondary particles formed by the aggregation of more than three (i.e., four or more) primary particles, exhibiting an agglomerated state.

[0037] This application does not limit the method for detecting the longitudinal wettability (b) of the positive electrode sheet. Those skilled in the art can detect the longitudinal wettability (b) of the positive electrode sheet using conventional techniques. For example, the longitudinal wettability (b) of the positive electrode sheet can be detected using the following method:

[0038] Take the de-energized positive electrode sheet, soak it in dimethyl carbonate for 2 hours, dry it at 80℃, and cut it into 1.5×1.5cm pieces. Weigh the electrode sheet mass M0 (in g), and then hot-press it together with a polymer film containing a circular hole with a radius r = 0.5cm. After hot pressing, the surface of the positive electrode sheet is covered with a polymer film, with the circular hole located at the center of the polymer film. Place it flat on a horizontal table, and add the prepared electrolyte (solvents are EC and EMC, with a mass ratio of EC:EMC = 3:7, containing 1mol / L lithium salt, lithium hexafluorophosphate) to the circular hole of the polymer film on the surface of the electrode sheet at a dropping rate of 0.5mL / min. The amount of electrolyte added is 2mL. After the electrolyte diffuses for 2 minutes, measure the mass M1 (in g) of the electrode sheet at this time. Calculate the longitudinal wettability (b) of the positive electrode sheet according to the following formula: b = (M1-M0) / M0×100%.

[0039] Among them, the material of the polymer membrane can be any polymer membrane material that is impermeable to the electrolyte and does not react with the electrolyte at room temperature and high temperature, such as PET-based-EVA hot melt adhesive composite film.

[0040] The mass percentage of Ni in the positive electrode active material layer (a) affects the battery's fast-charging performance, cycle performance, and safety performance. When the mass percentage of Ni in the positive electrode active material layer is too high, the proportion of ternary positive electrode material is too high, increasing its high reactivity with the electrolyte, causing the battery's DCR (DC resistance) to increase too quickly, and all aspects of cycle performance, fast-charging performance, and safety performance will decline. When the mass percentage of Ni in the positive electrode active material layer is too low, the proportion of ternary positive electrode material in the positive electrode active material is too low, which cannot effectively improve the ionic conductivity and electronic conductivity of the positive electrode active material, resulting in poor cycle performance and fast-charging performance of the battery.

[0041] The mass percentage (a) of Ni element in the positive electrode active material layer can be adjusted by changing the ratio of LMFP to ternary positive electrode material and the molar ratio of nickel element in the ternary positive electrode material structure.

[0042] This application does not limit the method for detecting the mass percentage (a) of Ni element in the positive electrode active material layer. Those skilled in the art can detect the Ni element content in the positive electrode active material layer using conventional techniques. For example, the mass percentage (a) of Ni element in the positive electrode active material layer can be detected using the following method:

[0043] Disassemble the empty lithium-ion battery to obtain the positive electrode sheet. Soak the positive electrode sheet in DMC (dimethyl carbonate) at room temperature (25℃, the same below) for 60 minutes to remove residual electrolyte and by-products on the surface of the electrode sheet. Take it out and dry it at room temperature with humidity ≤15%. Scrape off the positive active material layer on the surface of the current collector and calcine it at 400℃ for 3 hours to remove binders, etc. Then gently tap the electrode sheet to obtain positive active material powder.

[0044] Accurately weigh 0.5g of positive electrode active material powder, disperse it in 20mL of water, then add 10mL of nitric acid (HNO3 mass percentage of 65%–68%), disperse and heat until the positive electrode active material powder is completely dissolved, and dilute to 100mL with water to obtain the test solution; perform ICP testing on the test solution. Before the test, a standard solution needs to be prepared. Dilute the standard solution with a Ni element concentration of 1000mg / L (the standard solution can be prepared by dissolving metallic nickel in nitric acid) with deionized water to different concentrations (generally 0, 1mg / 100mL, 2mg / 100mL, and 3mg / 100mL, respectively). Test and calculate the relationship between the Ni element concentration and the peak area of ​​the standard sample. The linear correlation coefficient of this relationship should be above 0.999 to be used as a normal standard sample. Then, calculate the Ni element content 'a' in the positive electrode active material layer based on this relationship and the corresponding peak area of ​​the test sample. The ICP instrument operating conditions were set as follows: gas flow rate 0.5 L / min, power 1150 W, element selected for Ni testing, wavelength 231.604 nm.

[0045] The mass percentage of Ni in the positive electrode active material layer and the longitudinal wettability of the positive electrode sheet both affect the fast-charging performance and high-temperature cycling performance of the battery to varying degrees, and they also have a certain degree of mutual influence. Controlling a single variable makes it difficult to achieve both good fast-charging performance and high-temperature cycling performance in the battery. This application combines LMFP with ternary positive electrode materials and adjusts the mass percentage of Ni in the positive electrode active material layer and the longitudinal wettability of the positive electrode sheet to satisfy the above-mentioned specific relationship. This significantly shortens the charging time of the battery containing this positive electrode sheet in the high-voltage stage, while achieving a balance between the lithium-ion transport rate and electron transport rate of the positive electrode sheet in the longitudinal direction, effectively improving the fast-charging performance and high-temperature cycling performance of the battery.

[0046] For example, the value of a / b can be selected as 0.09, 0.1, 0.3, 0.5, 0.8, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.1 or any range formed by any two of the above values.

[0047] In one preferred embodiment, the positive electrode sheet satisfies: 0.17 ≤ a / b ≤ 2.4. Controlling the value of a / b within the range of 0.17 to 2.4 improves the battery's fast-charging performance and high-temperature cycle performance.

[0048] In some embodiments, the mass percentage (a) of Ni element in the positive electrode active material layer ranges from 0.9% to 47%, such as 0.9%, 1.5%, 2%, 5%, 10%, 20%, 30%, 40%, 43%, 47%, or any range formed by any two of the above values.

[0049] In one preferred embodiment, the mass percentage (a) of Ni element in the positive electrode active material layer ranges from 2% to 42%.

[0050] The mass percentage (a) of Ni element in the positive electrode active material layer includes, but is not limited to, the ranges mentioned above. When the mass percentage (a) of Ni element in the positive electrode active material layer is in the range of 0.9% to 47%, especially in the range of 2% to 42%, it has better fast charging performance and high temperature cycling performance while having good safety performance.

[0051] In some embodiments, the longitudinal wettability (b) of the positive electrode sheet ranges from 5% to 40%. For example, b is 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, or a range formed by any two of the above values.

[0052] In one preferred embodiment, the longitudinal wettability (b) of the positive electrode sheet ranges from 10% to 35%.

[0053] The longitudinal wettability (b) of the positive electrode sheet includes, but is not limited to, the ranges mentioned above. When the longitudinal wettability (b) of the positive electrode sheet is in the range of 5% to 40%, especially in the range of 10% to 35%, the structural density of the positive electrode active material layer is suitable. Not only does the positive electrode active material have good electronic contact and conductivity in the longitudinal direction, but there are also fewer side reactions between the electrolyte and the positive electrode active material during cycling, resulting in low impedance. At the same time, the longitudinal wettability of the positive electrode sheet is better, the lithium-ion transport rate in the longitudinal direction of the positive electrode sheet is higher, and the battery cycle performance is better, thereby improving the fast charging performance and high-temperature cycle performance of the battery.

[0054] In some embodiments, the ternary cathode material in the positive electrode active material has a mass percentage content of 3% to 93%, and the lithium manganese iron phosphate has a mass percentage content of 7% to 97%. For example, the mass percentage content of the ternary cathode material in the positive electrode active material is 3%, 5%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 93%, or any range formed by any two of the above values; the mass percentage content of the lithium manganese iron phosphate in the positive electrode active material is 7%, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 90%, 97%, or any range formed by any two of the above values.

[0055] When the mass percentages of the ternary cathode material and the lithium manganese iron phosphate in the cathode active material are within the above-mentioned range, the electronic and ionic conductivity of the cathode active material is relatively good, resulting in a shorter lithium insertion / extraction time in the constant voltage section under high SOC, a smaller proportion of the constant voltage section during charging, and better promotion of LMFP release of active lithium under high SOC. At the same time, the compaction density of the cathode sheet is appropriate, the electrolyte wets the cathode sheet well, and the lithium-ion transport resistance is low, which helps to improve the fast charging performance and high-temperature cycle performance of the battery.

[0056] In some embodiments, the manganese iron phosphate battery has a manganese content of 0.5 to 0.99 moles of manganese, based on the total moles of metal elements other than lithium. For example, it can be 0.5, 0.6, 0.7, 0.8, 0.9, 0.95, 0.99, or any two of these ranges. Compared to other ranges, when the manganese content in the lithium iron phosphate battery is 0.6 to 0.8 moles of manganese, based on the total moles of metal elements other than lithium, it is beneficial for the battery to achieve a balance between high energy density, fast charging performance, and cycle performance.

[0057] In some embodiments, the lithium manganese iron phosphate has the chemical formula LiMn. d Fe e Q fn PO4, where 0 < d < 1, 0 < e < 1, 0 ≤ f < 1, Q refers to a doping element, n refers to the valence of the doping element, and it satisfies: 2(d + e) + n·f = 2. Among them, d can be selected as 0.5, 0.6, 0.7, 0.8, 0.9, 0.95, 0.99 or the range formed by any two of the above values; e can be selected as 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5 or the range formed by any two of the above values. The lithium iron phosphate manganese can either contain no doping element or contain a doping element. This application places no limitation on the type of Q element. For example, Q includes but is not limited to at least one of V, W, Ti, and Mg. In one of the embodiments, part or all of the surface of the lithium iron phosphate manganese is coated with a carbon layer.

[0058] In this application, no limitation is placed on the preparation method of the lithium iron phosphate manganese. Those skilled in the art can obtain the lithium iron phosphate manganese according to conventional technical means. Exemplarily, the preparation method of the lithium iron phosphate manganese includes the following steps:

[0059] Mix a manganese source, an iron source, a phosphorus source, a lithium source, and a first carbon source, and obtain a lithium iron phosphate manganese precursor through first grinding, first spray drying, and first sintering;

[0060] Mix the obtained lithium iron phosphate manganese precursor and a second carbon source, and obtain lithium iron phosphate manganese through second grinding, second spray drying, second sintering, and iron removal by sieving.

[0061] Exemplarily, in the process of preparing the lithium iron phosphate manganese precursor, the manganese source used includes but is not limited to at least one of manganese tetraoxide, manganese nitrate, manganese carbonate, manganese oxalate, manganese sulfate, manganese chloride, and manganese acetate;

[0062] and / or, the iron source used includes but is not limited to at least one of iron phosphate, ferrous phosphate, iron hydroxide, ferrous hydroxide, iron carbonate, ferrous carbonate, iron acetate, ferrous acetate, iron oxide, iron tetroxide, ferrous oxalate, and iron oxalate;

[0063] and / or, the phosphorus source used includes but is not limited to at least one of lithium dihydrogen phosphate, lithium phosphate, diammonium hydrogen phosphate, and ammonium phosphate;

[0064] and / or, the lithium source used includes but is not limited to at least one of lithium dihydrogen phosphate, lithium phosphate, lithium hydroxide, lithium carbonate, lithium nitrate, lithium oxalate, lithium citrate, and lithium acetate;

[0065] And / or, the first carbon source used includes, but is not limited to, at least one of glucose (GLC), sucrose, polyethylene glycol (PEG), and polyvinyl alcohol. Additionally, during the preparation of LMFPs, a certain amount of a dopant element source (if any) can be mixed with a manganese source, iron source, phosphorus source, and lithium source, such as a vanadium source (e.g., vanadium pentoxide), a tungsten source (e.g., ammonium metatungstate), a titanium source (e.g., titanium oxide), or a magnesium source (e.g., magnesium carbonate), to obtain an LMFP containing a certain amount of dopant element.

[0066] In some embodiments, during the preparation of the lithium manganese iron phosphate precursor, the amounts of manganese, iron, phosphorus, and lithium sources used can be selected to satisfy the following ratio: molar amount of Li: sum of molar amounts of Mn and Fe: molar amount of P = (1~1.04):1:(1~1.02) (e.g., 1:1:1, 1:1:1.02, 1.04:1:1, or any range formed by any two of the above values), and the molar amount of Mn is more than 50% of the sum of molar amounts of Mn and Fe, such as 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, or any range formed by any two of the above values. In one preferred embodiment, the molar amount of Mn is 65% to 80% of the sum of molar amounts of Mn and Fe.

[0067] In some embodiments, the residual carbon content in the lithium manganese iron phosphate precursor is 0.1 wt.% to 0.5 wt.%, for example, 0.1 wt.%, 0.2 wt.%, 0.3 wt.%, 0.4 wt.%, 0.5 wt.%, or any range formed by two of the above values. In some embodiments, a dispersant may also be added during the first grinding process, wherein the dispersant may be selected from at least one of water and ethanol.

[0068] In some embodiments, the first grinding may be performed using ball milling, wherein the grinding beads may be made of zirconium oxide or the like. In one embodiment, the first grinding meets the following requirements: grinding time 0–48 h, and grinding cycles 1–6 times.

[0069] In one embodiment, the pressure for the first spray drying can be selected as 0.1-1.2 MPa, for example 0.1 MPa, 0.3 MPa, 0.5 MPa, 0.8 MPa, 1 MPa, 1.2 MPa, or any range formed by any two of the above values.

[0070] In one embodiment, the sintering atmosphere for the first sintering is an inert atmosphere, such as a nitrogen atmosphere.

[0071] In one embodiment, the temperature of the first sintering can be selected as 300 to 680°C, for example 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 680°C or any range formed by two of the above values.

[0072] In one embodiment, the first sintering time can be selected as 2 to 18 hours, for example, 2 hours, 4 hours, 6 hours, 8 hours, 10 hours, 12 hours, 14 hours, 16 hours, 18 hours or any range formed by any two of the above values.

[0073] For example, the second carbon source includes, but is not limited to, at least one of glucose (GLC), sucrose, polyethylene glycol (PEG), and polyvinyl alcohol.

[0074] In some embodiments, the residual carbon content in the lithium manganese iron phosphate can be selected to be 1.4 wt.% to 2.6 wt.%, for example, 1.4 wt.%, 1.8 wt.%, 2.0 wt.%, 2.2 wt.%, 2.4 wt.%, 2.6 wt.%, or any range formed by any two of the above values.

[0075] In some embodiments, the second grinding may be performed using ball milling, wherein the grinding beads may be made of zirconium oxide or the like. In one embodiment, the second grinding satisfies the following conditions: grinding time 0–48 h, and grinding cycles 1–6 times.

[0076] In one embodiment, the pressure for the second spray drying can be selected as 0.1-1.5 MPa, for example 0.1 MPa, 0.3 MPa, 0.5 MPa, 0.8 MPa, 1 MPa, 1.2 MPa, 1.5 MPa or any range formed by any two of the above values.

[0077] In one embodiment, the sintering atmosphere for the second sintering is an inert atmosphere, such as a nitrogen atmosphere.

[0078] In one embodiment, the temperature of the second sintering can be selected as 400 to 800°C, for example 400°C, 450°C, 500°C, 550°C, 600°C, 620°C, 640°C, 660°C, 680°C, 700°C, 720°C, 750°C, 800°C or any range formed by any two of the above values.

[0079] In one embodiment, the second sintering time can be selected as 3 to 18 hours, for example, 3 hours, 5 hours, 7 hours, 10 hours, 12 hours, 15 hours, 18 hours or any range formed by any two of the above values.

[0080] In the preparation of lithium manganese iron phosphate, the carbon source can be added in two steps as described above, or the carbon source can be added only in the preparation of lithium manganese iron phosphate using the lithium manganese iron phosphate precursor, without adding a carbon source in the preparation of the lithium manganese iron phosphate precursor.

[0081] To obtain single crystals of lithium manganese iron phosphate, a centrifugal spraying device can be used during the second spray drying, and an air-crushing process is required after the second calcination. The type of spraying equipment used in the first spray drying is not limited; either a centrifugal spraying device or a two-fluid spraying device can be used. To obtain polycrystalline lithium manganese iron phosphate, a two-fluid spraying device can be used during the second spray drying. The type of spraying equipment used in the first spray drying is not limited; either a centrifugal spraying device or a two-fluid spraying device can be used.

[0082] In some embodiments, the molar content of nickel in the ternary cathode material, based on the total molar number of metal elements other than lithium, ranges from 0.1 to 0.92. For example, the molar content of nickel in the ternary cathode material, based on the total molar number of metal elements other than lithium, ranges from 0.1 to 0.92, such as 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, 0.63, 0.65, 0.67, 0.70, 0.73, 0.75, 0.77, 0.80, 0.83, 0.85, 0.87, 0.90, 0.92, or any range formed by two of the above values. Compared to other ranges, when the molar content of nickel in the ternary cathode material, based on the total molar number of metal elements other than lithium, is 0.6 or higher, the ternary cathode material is a high-nickel material, which is beneficial for the battery to achieve higher energy density.

[0083] In some embodiments, the ternary cathode material has the chemical formula LiNi. x Co y Mn (1-x-y) O2, where,

[0084] x is 0.1 to 0.92, such as 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, 0.63, 0.65, 0.67, 0.70, 0.73, 0.75, 0.77, 0.80, 0.83, 0.85, 0.87, 0.90, 0.92, or any two of the above values ​​forming an interval.

[0085] y is 0.05 to 0.35, such as 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.20, 0.22, 0.24, 0.26, 0.28, 0.3, 0.32, 0.35, or any two of the above values ​​forming an interval.

[0086] Compared to other ranges, when the molar content of manganese in the lithium manganese iron phosphate is ≥0.75 (e.g., 0.75, 0.77, 0.80, 0.83, 0.85, 0.87, 0.90, 0.92 or any two of the above values) based on the total molar number of metal elements other than lithium, then b ≥10% (e.g., 10%, 15%, 20%, 25%, 30%, 35%, 40 or any two of the above values) to better balance the kinetic performance of the ternary cathode material itself and the wetting effect of the electrolyte on the cathode sheet, resulting in better fast charging performance and cycle performance of the battery.

[0087] Compared to other ranges, when the molar content of manganese in the lithium manganese iron phosphate is ≥0.75 (e.g., 0.75, 0.77, 0.80, 0.83, 0.85, 0.87, 0.90, 0.92 or any two of the above values) based on the total molar number of metal elements other than lithium, it is preferable that the ternary cathode material is polycrystalline to improve the wetting effect of the electrolyte on the cathode sheet and enhance fast charging performance and cycle performance.

[0088] The ternary cathode material may be free of dopant elements or contain dopant element M. This application does not limit the type of dopant element M; for example, it may be at least one of niobium, titanium, tantalum, tin, or lanthanide metals.

[0089] This application does not limit the preparation method of the ternary cathode material; those skilled in the art can prepare the ternary cathode material using conventional techniques. For example, the preparation method of the ternary cathode material includes the following steps:

[0090] The ternary cathode material precursor and lithium source are mixed and sintered to obtain the ternary cathode material.

[0091] The ternary cathode material precursor contains Ni, Co, and Mn in a target stoichiometric ratio. The ternary cathode material precursor is one or more of the oxides, hydroxides, and carbonates of Ni, Co, and Mn, for example, the ternary cathode material precursor is a hydroxide of Ni, Co, and Mn.

[0092] The ternary cathode material precursor can be obtained by methods known in the art, such as co-precipitation, gelation, or solid-state methods. As an example, the preparation method of the ternary cathode material precursor includes the following steps:

[0093] Ni source, Co source and Mn source are dispersed in solvent to obtain a mixed solution;

[0094] The mixed solution, strong alkali solution, and complexing agent solution are simultaneously pumped into a stirred reactor. The pH of the reaction solution is controlled at 10–13, and the temperature inside the reactor is controlled at 25°C–90°C. An inert gas is used for protection during the reaction. After the reaction is completed, the mixture is aged, filtered, washed, and vacuum dried to obtain hydroxides containing Ni, Co, and Mn, which is the precursor of the ternary cathode material.

[0095] In the process of preparing the ternary cathode material precursor, the Ni source used includes, but is not limited to, at least one of nickel sulfate, nickel nitrate, nickel chloride, nickel oxalate, and nickel acetate;

[0096] And / or, the Co source used includes, but is not limited to, at least one of cobalt sulfate, cobalt nitrate, cobalt chloride, cobalt oxalate, and cobalt acetate;

[0097] And / or, the Mn source used includes, but is not limited to, at least one of manganese sulfate, manganese nitrate, manganese chloride, manganese oxalate, and manganese acetate;

[0098] And / or, the base used in the strong base solution includes at least one of sodium hydroxide and potassium hydroxide;

[0099] And / or, the complexing agent in the complexing agent solution used includes ammonia.

[0100] In the preparation of the ternary cathode material precursor, the amounts of Ni, Co, and Mn sources used can be selected to satisfy the following ratio: molar amount of Ni, molar amount of Co, and molar amount of Mn = (92-10):(5-35):(3-80). By adjusting the proportion of Ni molar amount in the Ni source within the total molar amounts of Ni, Co, and Mn in the Ni, Co, and Mn sources, the molar proportion of nickel in the ternary cathode material structure can be controlled. Compared to other ranges, limiting the molar ratio of Ni, Co, and Mn within the above range is beneficial for improving the conductivity of the cathode, increasing the lithium-ion transport rate, and thus improving the fast-charging performance of the battery. Furthermore, it is beneficial for the structural stability of the ternary material.

[0101] In the process of preparing the ternary cathode material, the Li source used includes, but is not limited to, at least one of lithium oxide (Li2O), lithium phosphate (Li3PO4), lithium dihydrogen phosphate (LiH2PO4), lithium acetate (CH3COOLi), lithium hydroxide (LiOH), lithium carbonate (Li2CO3), and lithium nitrate (LiNO3).

[0102] In the process of preparing the ternary cathode material, the amounts of the ternary cathode material precursor and the lithium source satisfy the following ratio: molar amount of Li element: sum of molar amounts of Ni, Co and Mn elements = (0.99~1.09):(0.99~1.02).

[0103] Ball mills or high-speed mixers can be used for mixing and sintering in an oxygen-containing atmosphere, such as air or oxygen. In the process of preparing ternary cathode materials using ternary cathode material precursors, the ternary cathode material precursors and lithium source can be mixed using ball mills or high-speed mixers; the sintering atmosphere is oxygen-containing, such as air or oxygen. To obtain single crystals of ternary cathode materials, the sintering temperature is 850–1100℃, and an air-crushing process is required after sintering. To obtain polycrystalline ternary cathode materials, the sintering temperature is 700–850℃.

[0104] In addition, when preparing ternary cathode materials, a certain amount of dopant source (if any) can be dispersed together with Ni source, Co source and Mn source in solvent to prepare ternary cathode material precursor. Dopant source, such as niobium source, titanium source, tantalum source, tin source, lanthanide metal element source, etc., to obtain ternary cathode material containing a certain amount of dopant element.

[0105] In addition, a coating process can be applied to the ternary cathode material precursor. Specifically, a dry coating method (high-temperature solid-state method) is used to coat the surface of the cathode active material with a coating material, so that the surface of the cathode active material is partially or completely coated with the coating layer formed by the coating material. The coating layer contains at least one element selected from the following (hereinafter referred to as the "coating element"): aluminum (Al), titanium (Ti), tungsten (W), boron (B), phosphorus (P), cobalt (Co), yttrium (Y), or silicon (Si).

[0106] In some embodiments, the mass percentage of the positive electrode active material in the positive electrode active material layer is 94% to 97.5%, such as 94%, 94.5%, 95%, 95.5%, 96%, 96.5%, 97%, 97.5%, or any range formed by any two of the above values.

[0107] In addition to the aforementioned positive electrode active material, the positive electrode active material layer also includes a conductive agent and a binder.

[0108] The conductive agent in the positive electrode active material layer is used to provide conductivity. Any conductive agent can be used without particular limitation, as long as it has suitable electronic conductivity and does not significantly cause adverse chemical changes in the battery. For example, the conductive agent in the positive electrode active material layer includes, but is not limited to, at least one of carbon nanotubes, carbon black, graphite, carbon fibers, activated carbon, mesoporous carbon, and fullerenes. Carbon fibers include, for example, carbon nanofibers; carbon black includes, for example, SP (Super P), acetylene black, and Ketjen black.

[0109] In some embodiments, the mass percentage of the conductive agent in the positive electrode active material layer is 1.0% to 2.0%, such as 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, or any range formed by any two of the above values.

[0110] The binder in the positive electrode active material layer is used to improve the adhesion between positive electrode active material particles and the adhesion between the positive electrode active material and the positive electrode current collector. Any binder can be used without particular limitation, as long as it has suitable adhesive properties and does not significantly cause adverse chemical changes in the battery. For example, the binder in the positive electrode active material layer includes, but is not limited to, fluorinated polyolefin binders, including but not limited to polyvinylidene fluoride (PVDF), PVDF copolymers, or their modified derivatives (e.g., modified with carboxylic acids, acrylic acid, acrylonitrile, etc.).

[0111] In some embodiments, the mass percentage of the binder in the positive electrode active material layer is 1% to 4.0%, such as 1%, 1.2%, 1.5%, 1.8%, 2.0%, 2.2%, 2.5%, 2.7%, 3.0%, 3.2%, 3.5%, 3.8%, 4.0%, or any range formed by any two of the above values.

[0112] This application does not impose any particular restrictions on the positive electrode current collector, as long as it is conductive and will not cause adverse chemical changes in the battery, and materials such as aluminum, nickel, titanium, stainless steel, sintered carbon, or aluminum or stainless steel that has undergone a surface treatment of carbon, nickel, titanium, silver, etc. can be used.

[0113] The positive electrode sheet of this application can be prepared according to conventional methods in the art. For example, the positive electrode active material, conductive agent and binder are dispersed in a solvent to obtain a positive electrode slurry, and then the positive electrode slurry is coated on at least one side of the positive electrode current collector. After drying, rolling, cutting and other processes, the positive electrode sheet is obtained. The solvent includes, but is not limited to, at least one of N-methylpyrrolidone (NMP) and deionized water.

[0114] Battery

[0115] The present application also provides a battery, including the positive electrode sheet, the negative electrode sheet and the electrolyte.

[0116] The negative electrode sheet of the present application includes a negative electrode current collector and a negative electrode active material layer provided on at least one surface of the negative electrode current collector, and the negative electrode active material layer contains a negative electrode active material.

[0117] There is no particular limitation on the negative electrode active material in the present application. Exemplarily, the negative electrode active material includes, but is not limited to, natural graphite, artificial graphite, mesocarbon microbeads (MCMB), hard carbon, soft carbon, silicon, SiO f (0 < f < 2, such as f = १), silicon carbide, Li4Ti5O 12 and at least one of them.

[0118] In some embodiments, the mass percentage content of the negative electrode active material in the negative electrode active material layer is 94% - 97.5%. For example, the content of the positive electrode active material in the negative electrode active material layer is 94%, 94.5%, 95%, 95.5%, 96%, 96.5%, 97%, 97.5% or the range formed by any two of the above values.

[0119] The negative electrode active material layer may further contain a conductive agent and / or a binder.

[0120] The conductive agent in the negative electrode active material layer is used to provide conductivity, and any conductive agent can be used without particular limitation as long as it has suitable electron conductivity and does not significantly cause adverse chemical changes in the battery. Exemplarily, the conductive agent in the negative electrode active material layer includes, but is not limited to, at least one of carbon nanotubes, carbon black, graphite, carbon fiber, activated carbon, mesoporous carbon, fullerenes, etc. Among them, the carbon fiber is, for example, carbon nanofiber, etc.; the carbon black is, for example, SP, acetylene black, Ketjen black, etc.

[0121] In some embodiments, the mass percentage content of the conductive agent in the negative electrode active material layer is 0.4% - 2%, such as 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2% or the range formed by any two of the above values.

[0122] The binder in the negative electrode active material layer is used to improve the adhesion between negative electrode active material particles and the adhesion between the negative electrode active material and the negative electrode current collector. Any binder can be used without particular limitation, as long as it has suitable adhesive properties and does not significantly cause adverse chemical changes in the battery. For example, the binder in the negative electrode active material layer includes, but is not limited to, at least one of carboxymethyl cellulose (CMC), styrene-butadiene rubber, polyvinylidene fluoride, polytetrafluoroethylene, polyvinyl butyral, and aqueous acrylic resin.

[0123] In some embodiments, the mass percentage of the binder in the negative electrode active material layer is 1.0% to 4.5%, such as 1.0%, 1.2%, 1.5%, 1.8%, 2.0%, 2.2%, 2.5%, 2.7%, 3.0%, 3.2%, 3.5%, 3.8%, 4.0%, 4.2%, 4.5%, or any range formed by any two of the above values.

[0124] This application does not impose any particular restrictions on the negative electrode current collector, as long as it is conductive and will not cause adverse chemical changes in the battery, and can use, for example: copper, stainless steel, aluminum, nickel, titanium, sintered carbon, copper or stainless steel surface-treated with at least one of carbon, nickel, titanium, silver, etc., or aluminum-cadmium alloy.

[0125] The electrolyte used in this application can be any of the various electrolytes suitable for batteries available in the art. The electrolyte comprises an electrolyte and a solvent, and the electrolyte typically includes a lithium salt.

[0126] For example, the lithium salt includes, but is not limited to, at least one of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalate borate (LiDFOB), lithium dioxalate borate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorodioxalate phosphate (LiDFOP), and lithium tetrafluorooxalate phosphate (LiTFOP). The concentration of the electrolyte in the electrolyte solution can be selected as 0.5–5 mol / L.

[0127] For example, the solvent includes, but is not limited to, at least one selected from ethylene carbonate (EC), methyl ethyl carbonate (EMC), diethyl carbonate (DEC), propylene carbonate (PC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butyl carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS), and diethyl sulfone (ESE). The mass percentage of the solvent in the electrolyte can be selected from 70% to 98%.

[0128] In addition, the electrolyte may also contain additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery performance, such as additives that improve battery high-temperature performance, additives that improve battery overcharge performance, additives that improve battery low-temperature performance, etc.

[0129] The battery may further include a separator located between the positive and negative electrode plates to separate them and prevent short circuits caused by contact. The separator can be any suitable battery separator material in the art. Exemplarily, the separator includes, but is not limited to, at least one of polypropylene and polyethylene.

[0130] Electrical appliances

[0131] This application also provides an electrical device that includes the battery. The battery serves as the power source for the electrical device.

[0132] The term "electrical device" refers to any device that can utilize electrical energy and convert it into mechanical energy, thermal energy, light energy, or one or more other energy forms, such as electric motors, electric heaters, and electric light sources. Specifically, it can include, but is not limited to, mobile devices, electric vehicles, electric trains, ships and satellites, and energy storage systems. Mobile devices can include mobile phones, laptops, drones, robot vacuum cleaners, and e-cigarettes; electric vehicles can include pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, and electric trucks.

[0133] The present application is further illustrated below with specific embodiments. It should be noted that, unless otherwise specified, the sintering is carried out in an air atmosphere:

[0134] Example 1

[0135] This embodiment provides a lithium-ion battery, and the specific preparation method is as follows:

[0136] (1) Preparation of positive electrode sheet

[0137] (1.1) Preparation of LMFP materials

[0138] According to LiMn f Fe 1-f The molar ratios of Li, Mn, Fe, and P in the chemical formula of PO4 (f values ​​are shown in Table 1) were determined by adding Mn3O4, FePO4, and LiH2PO4 to a ball mill, followed by glucose and polyethylene glycol. Water was then used as a dispersant, and the raw materials were ground at 2000 rpm for 12 hours. The grinding process was repeated three times, followed by a first spray drying under 1 MPa pressure, and then sintering at 400℃ for 8 hours to obtain the lithium manganese iron phosphate precursor. The ratio of glucose to polyvinyl alcohol was 1:3 (mass ratio), and the total amount of glucose and polyvinyl alcohol was 15 wt.% of the total amount of Mn3O4, FePO4, and LiH2PO4.

[0139] The obtained LMFP precursor was mixed with glucose and polyethylene glycol, and water was used as a dispersant. The raw material was ground at 4000 rpm for 18 hours, and the grinding was repeated three times. Then, a second spray drying was carried out at 1 MPa pressure. The spray drying equipment used is shown in Table 1. Then, it was sintered for 10 hours. The sintering temperature is shown in Table 1. Iron was removed by sieving to obtain LMFP, in which the ratio of sucrose to polyvinyl alcohol was 1:2 (mass ratio), and the total amount of glucose, sucrose and polyvinyl alcohol was 20 wt.% of the total amount of Mn3O4, FePO4 and LiH2PO4.

[0140] (1.2) Preparation of ternary cathode materials

[0141] According to LiNi x Co y Mn (1-x-y) In the chemical formula of O2, the molar proportions of Ni, Co, and Mn were weighed out from nickel sulfate, cobalt sulfate, and manganese sulfate (the values ​​of x and y are shown in Table 1), and dispersed in water to obtain a mixed solution.

[0142] The resulting mixed solution was transported into a reactor and oxygen was introduced as a protective gas. NaOH aqueous solution was added as a precipitant and ammonia water was added as a complexing agent. The concentration and amount of ammonia water added were adjusted to control the pH of the solution (i.e., the pH of the precursor reaction, see Table 1 for details). The temperature inside the reactor was 50℃, and the reaction was carried out for 5 hours. The product was filtered and dried to obtain the ternary cathode material precursor.

[0143] The obtained ternary cathode material precursor and LiOH were mixed and sintered for 8 hours. The sintering temperature is shown in Table 1. A one-time sintered material was obtained. The amounts of ternary cathode material precursor and LiOH were such that the molar amount of Li element: the sum of the molar amounts of Ni, Co and Mn elements = 1.05:1.

[0144] (1.3) Preparation of positive electrode sheet

[0145] The above-mentioned lithium manganese iron phosphate and ternary cathode material were mixed according to the ratio in Table 1 to form the cathode active material. The cathode active material was mixed with binder PVDF, conductive agent SP and conductive agent carbon nanotube at a mass ratio of 97:1:1.7:0.3 and dispersed in NMP to obtain cathode slurry. The cathode slurry was coated on both sides of aluminum foil and then rolled and cut to obtain cathode sheet.

[0146] (2) Preparation of negative electrode sheet

[0147] Artificial graphite, the negative electrode active material, is mixed with conductive agent SP and binder CMC at a mass ratio of 96.4:1:2.6 and dispersed in deionized water to obtain a negative electrode slurry. The negative electrode slurry is coated on both sides of a copper foil, and after drying, rolling and cutting, a negative electrode sheet is obtained.

[0148] (3) Preparation of electrolyte

[0149] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a volume ratio of 1:1:1 to obtain a mixed organic solvent. Then, dried lithium salt LiPF6 was dissolved in the above mixed organic solvent to prepare an electrolyte with a LiPF6 concentration of 1 mol / L.

[0150] (4) Preparation of the separating membrane

[0151] A polyethylene (PE) diaphragm is used.

[0152] (5) Assembly and formation

[0153] The positive electrode, separator, and negative electrode are stacked in sequence, with the separator positioned between the positive and negative electrodes to provide isolation. The resulting cells are then wound to obtain a bare battery cell. The bare battery cell is placed in an outer packaging shell, dried, and then injected with electrolyte. After vacuum sealing, settling, formation, and shaping, a lithium-ion battery is obtained. Examples 2-17 and Comparative Examples 1-2

[0154] These examples and comparative examples all provide a lithium-ion battery, and the preparation method is similar to that of Example 1, except that:

[0155] (a) In step (1.1), the value of f, the equipment used for the second spray drying, and whether gas crushing is performed after sintering are shown in Table 1 (if gas crushing is not specified, it means that gas crushing is not performed);

[0156] (b) In step (1.2), the values ​​of x and y and the sintering temperature are shown in Table 1;

[0157] (c) In step (1.3), the ratio of lithium manganese iron phosphate to ternary cathode material is adjusted, as is the weight ratio of SP in the total weight of cathode active material, PVDF, SP and carbon nanotubes. The weight ratio of cathode active material in the total weight of cathode active material, PVDF, SP and carbon nanotubes is adjusted accordingly. The specific weight ratio of ternary cathode material in cathode active material and the weight ratio of SP in cathode active material layer are shown in Table 1.

[0158] Table 1

[0159] The content of Ni element (a) in the positive electrode active material layer and the longitudinal wettability (b) of the positive electrode sheet in each embodiment and comparative example were detected using the following methods. The test results are shown in Table 2.

[0160] Ni content in the positive electrode active material layer: a) Disassemble a lithium-ion battery to obtain the positive electrode sheet. Immerse the positive electrode sheet in DMC (dimethyl carbonate) at room temperature for 60 minutes, remove it, and air dry it at room temperature with humidity ≤15%. Scrape off the positive electrode active material layer from the current collector surface and calcine it at 400℃ for 3 hours to remove the binder. Then gently tap the electrode sheet to obtain positive electrode active material powder. Accurately weigh 0.5g of positive electrode active material powder, disperse it in 20mL of water, add 10mL of nitric acid (HNO3 content approximately 37wt.%), disperse and heat until the positive electrode active material powder is completely dissolved. Dilute to 100mL with water to obtain the test solution. Perform ICP testing on the test solution to measure... Before the test, a standard solution needs to be prepared. The standard solution with a Ni element concentration of 1000 mg / L is diluted with deionized water to different concentrations (0, 1 mg / 100 mL, 2 mg / 100 mL, and 3 mg / 100 mL, respectively). The relationship between the Ni element concentration and the peak area of ​​the standard sample is tested and calculated. Only when the linear correlation coefficient of this relationship is above 0.999 can it be used as a normal standard sample. Then, the Ni element content 'a' in the positive electrode active material layer is calculated based on this relationship and the corresponding peak area of ​​the sample to be tested. The working conditions of the ICP instrument are set as follows: gas flow rate 0.5 L / min, power 1150 W, element test Ni selected, wavelength 231.604 nm.

[0161] Longitudinal wettability b of the positive electrode: Take the de-energized positive electrode, soak it in dimethyl carbonate for 2 hours, dry it at 80℃, cut it into 1.5×1.5cm pieces, weigh the electrode mass M0 (in g), and then hot-press it together with a polymer film (PET-based-EVA hot melt adhesive composite film) containing a circular hole with a radius r = 0.5cm. The surface of the positive electrode is covered with the polymer film, and the circular hole is located in the center of the polymer film. Place it flat on a horizontal table, and add the prepared electrolyte (solvents are EC and EMC, with a mass ratio of EC:EMC = 3:7, containing 1mol / L lithium salt, lithium hexafluorophosphate) to the circular hole of the polymer film on the surface of the electrode at a dropping rate of 0.5mL / min. The amount of electrolyte added is 2mL. After the electrolyte has diffused for 2 minutes, measure the mass M1 (in g) of the electrode at this time, and calculate the longitudinal wettability (b) of the positive electrode according to the following formula.

[0162] b = (M1 - M0) / M0 × 100%.

[0163] The performance of the positive electrode sheets or lithium-ion batteries obtained in each embodiment and comparative example was tested. The test results are shown in Table 2. The specific test methods are as follows:

[0164] Fast charging test method: The above-mentioned positive electrode sheet and lithium metal were used to form a half-cell. The electrolyte used was the same as in Example 1. At 25°C, the battery was charged at a constant current of 0.33C to the upper limit voltage of 4.25V, and then charged at a constant voltage until the current was less than or equal to 0.05C. Then, it was discharged at 0.33C to 2.5V. This was one cycle. After two cycles of charge and discharge, the discharge capacity of the second cycle was taken as the battery capacity. Then, a double charge test was performed at 1C / 2C / 6C rates. The discharge rate, charging cutoff conditions, and discharging cutoff conditions were the same as described above. The constant current ratio under the 2C double charge test was used to evaluate the fast charging performance. The 2C constant current ratio = 2C constant current charging capacity / 2C total charging capacity × 100%. The higher the constant current ratio, the better the fast charging performance.

[0165] High-temperature cycle performance test: After the battery is formed and capacitated, it is first left to stand for 2 hours at 45℃, then discharged to 2.5V at 0.33C, left to stand for 10 minutes, and then charged to 4.25V at 1C constant current. The charging cutoff current at 4.25V constant voltage is 0.05C. After standing for 10 minutes, it is discharged to 2.5V at 1C. The discharge capacity of the first 1C cycle is taken as the initial discharge capacity of the first cycle. The ratio of the discharge capacity after 500 1C charge-discharge cycles to the initial discharge capacity of the first cycle is taken as the discharge capacity retention rate of the battery at high temperature. The cutoff conditions of 1C charge-discharge cycle are the same as above: charge to the upper limit voltage of 4.25V, and discharge to 2.5V with a cutoff current of less than or equal to 0.05C.

[0166] Table 2

[0167] For the batteries prepared in each embodiment of this application, the 2C constant current ratio is ≥66%, and the capacity retention rate after 45°C, 1C, and 500 cycles is ≥66.5%. It can be seen that the batteries containing the positive electrode sheet of this application have excellent fast charging performance and high temperature cycling performance.

[0168] As can be seen from the comparison of Examples 1-5 with Examples 6-10, and Examples 11-12 with Example 13, when the mass percentage of Ni element in the positive electrode active material layer and the longitudinal wettability of the positive electrode sheet meet the preferred range described in this application, the fast charging performance and high-temperature cycle performance of the battery are relatively better.

[0169] Comparing Examples 1-5 with Examples 11-12, it can be seen that when the positive electrode sheet satisfies 0.31≤a / b≤3.9, the battery's fast charging performance and high-temperature cycle performance are relatively better.

[0170] According to Comparative Examples 1 and 2, even if the mass percentage of Ni in the positive electrode active material layer and the longitudinal wettability of the positive electrode sheet are within a suitable range, the fast charging performance and high-temperature cycle performance of the battery are relatively poor when the value of a / b exceeds the range of 0.14 to 5.82.

[0171] As can be seen from the comparison of Example 4 with Examples 16-17, when the molar content of manganese in lithium iron phosphate is ≥0.75 based on the total molar number of metal elements other than lithium, b≥10% will make the battery's fast charging performance and high temperature cycle performance relatively better.

[0172] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this article and are not intended to limit the scope of protection of this article. Although this application has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of this article without departing from the essence and scope of the technical solutions of this article.

Claims

1. A positive electrode plate, characterized in that, The device includes a positive current collector and a positive active material layer disposed on at least one surface of the positive current collector. The positive active material layer contains a positive active material, including lithium manganese iron phosphate and ternary positive electrode materials. The positive electrode sheet satisfies the following condition: 0.09 ≤ a / b ≤ 5.

1. Where a is the mass percentage of Ni element in the positive electrode active material layer, in %; b represents the longitudinal wettability of the positive electrode sheet, expressed as a percentage.

2. The positive electrode sheet as described in claim 1, characterized in that, The positive electrode sheet satisfies: 0.17≤a / b≤2.

4.

3. The positive electrode sheet as described in claim 1, characterized in that, The range of a is 0.9% to 47%.

4. The positive electrode sheet as described in claim 3, characterized in that, The range of a is 2% to 42%.

5. The positive electrode sheet as described in claim 1, characterized in that, The range of b is 5% to 40%.

6. The positive electrode sheet as described in claim 5, characterized in that, The range of b is 10% to 35%.

7. The positive electrode sheet as described in claim 1, characterized in that, In the lithium manganese iron phosphate, the molar content of manganese, excluding lithium, ranges from 0.6 to 0.8 based on the total molar number of metal elements; in the ternary cathode material, the molar content of nickel, excluding lithium, ranges from 0.1 to 0.92 based on the total molar number of metal elements.

8. The positive electrode sheet as described in claim 7, characterized in that, In the lithium manganese iron phosphate, when the molar content of manganese is ≥0.75 based on the total molar number of metal elements other than lithium, the b ≥10%.

9. The positive electrode sheet as described in claim 7 or 8, characterized in that, In the lithium manganese iron phosphate, when the molar content of manganese is ≥0.75 based on the total molar number of metal elements other than lithium, the ternary cathode material is polycrystalline.

10. A battery, characterized in that, Includes the positive electrode sheet as described in any one of claims 1 to 9.

11. An electrical appliance, characterized in that, Includes the battery as described in claim 10.