Method for synthesizing bioenzyme / mof composite functional material by pressure

MOF composite materials prepared by axial pressure self-assembly and solvent treatment have solved the problem of insufficient enzyme stability, achieved high loading rate and synergistic effect, and expanded the application range.

CN109913440BActive Publication Date: 2026-11-20NANJING TECH UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN201910241925.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-03-27
Publication Date
2026-11-20
Estimated Expiration
2039-03-27

AI Technical Summary

Technical Problem

Free enzymes are easily deactivated, and the pores of MOF materials cannot directly encapsulate nanoscale biological enzymes, resulting in insufficient stability and activity.

Method used

MOFs are self-assembled with biological enzymes under axial pressure to form a composite material, which is then treated in solvent vapor to prepare a metal-organic framework composite material with an egg yolk and eggshell structure.

Benefits of technology

It improves the loading rate and stability of biological enzymes, expands the application range, realizes the synergistic effect of enzymes and MOFs, and enhances catalytic and sensing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN109913440B_ABST
    Figure CN109913440B_ABST
Patent Text Reader

Abstract

The application discloses a method for synthesizing a bioenzyme / MOFs composite functional material through pressure, comprising the following steps: mixing MOFs and bioenzymes, and then obtaining a self-assembled composite material of MOFs particles and bioenzymes through axial pressure; placing the self-assembled composite material in a solvent or steam containing the solvent; increasing the temperature of the solvent or the steam containing the solvent to 25-50 DEG C, and keeping the temperature for 5-120 h, and then performing post-processing to obtain the dye / MOFs composite functional material. In the composite functional material obtained by the method, the bioenzyme has a high loading rate in the MOFs material, the method is simple and easy to implement, the activity of the bioenzyme can be fully exerted, and the bioenzyme can also be protected.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of multifunctional coordination polymer composite materials, and more specifically to a method for synthesizing bioenzyme / MOF composite functional materials by pressure. Background Technology

[0002] Enzymes are proteins or RNA produced by living cells and possess high specificity and catalytic efficiency towards their substrates. The catalytic activity of enzymes mainly depends on the integrity of the primary and spatial structures of the enzyme molecule. Denaturation or subunit depolymerization of the enzyme molecule can lead to loss of enzyme activity. Therefore, despite their high efficiency, specificity, and adjustability, their instability is one of the problems that urgently needs to be addressed. The glucose oxidase (GOx) we selected can remove oxygen from food and containers, effectively preventing food spoilage. Therefore, it can be used in the packaging of tea, ice cream, milk powder, beer, fruit wine, and other beverage products. It also plays an important role in medical diagnosis, animal husbandry, and disease prevention. Horseradish peroxidase (HRP), on the other hand, is a commonly used enzyme in clinical laboratory reagents, possessing significant advantages such as high specific activity, small molecular weight, and ease of preparation.

[0003] To address the issue of free enzymes being easily inactivated, current methods utilize materials such as MOFs for immobilization to enhance their stability and activity. Immobilized glucose oxidase / horseradish peroxidase exhibits better stability, is less prone to inactivation, can be reused, and is easier to separate from the product after the reaction.

[0004] However, while biological enzymes are generally in the nanometer range, MOF materials, such as ZIF-8, have pores that are... Bioenzymes cannot be directly encapsulated in ZIF-8. Summary of the Invention

[0005] The purpose of this invention is to provide a metal-organic framework composite material with an egg yolk and eggshell structure and its preparation method, thereby solving one or more of the problems in the prior art.

[0006] This invention provides a method for synthesizing bioenzyme / MOF composite functional materials under pressure, comprising the following steps:

[0007] α1. After mixing MOFs with bio-enzymes, a self-assembled composite material of MOF particles and bio-enzymes is obtained by applying axial pressure.

[0008] α2. Place the above self-assembled composite material in a solvent or vapor containing the solvent;

[0009] α3. Raise the temperature of the above solvent or vapor containing the solvent to 25-50°C and keep it at that temperature for 5-120 hours. After post-processing, the dye / MOFs composite functional material is obtained.

[0010] In some implementations, the MOFs are ZIF-8 or ZIF-67.

[0011] In some embodiments, the bioenzyme is at least one of glucose oxidase or catalase.

[0012] In some embodiments, the solvent is at least one of methanol, ethanol, propanol, butanol, N,N-dimethylformamide, N,N-dimethylhexamamide, or dimethyl sulfoxide.

[0013] In some embodiments, step α1, the method for achieving the self-assembly of MOF particles and biological enzymes through axial pressure, includes the following steps:

[0014] The mixed MOFs and bioenzymes are placed in the cavity of an infrared tablet press, and the cavity wall is tapped to make them evenly adhere to the bottom of the infrared tablet press disc. Then, pressure is applied to them, and the pressure is not less than 1364 MPa.

[0015] In some embodiments, in step α1, the MOFs are mixed with the biological enzymes at a mass ratio of 1:1 to 20:1.

[0016] In some embodiments, step α1 further includes: mixing MOFs with a biological enzyme and then grinding them.

[0017] In some embodiments, the post-processing in step α3 includes centrifuging, washing, and finally drying the solution.

[0018] In some embodiments, MOFs are activated by vacuum drying at 100-140°C for 10-14 hours.

[0019] Beneficial effects:

[0020] This invention employs a relatively simple and mild method to construct a dye / MOF composite functional material. This method, on the one hand, improves the loading rate of biological enzymes, and on the other hand, allows biological enzymes larger than the pores of MOFs to be encapsulated within the pores of the MOF material, thus overcoming the pore confinement effect during the synthesis of MOF composite materials and ultimately achieving a synergistic effect between MOFs and biological enzymes. The biological enzymes encapsulated by this method exhibit high loading rates and good stability during catalysis.

[0021] Furthermore, this invention achieves synergistic effects by synthesizing bioenzyme / MOF composite functional materials under pressure, thus expanding the application scope and realizing the functional applications of bioenzyme / MOF materials. For example, it can be applied to catalysis, sensing, biomedicine, and other fields. Attached Figure Description

[0022] Figure 1 TEM image of the recovered bioenzyme / ZIF-8;

[0023] Figure 2 The graph shows the bioenzyme / ZIF-8 enzyme activity data after tableting and recovery in Example 1;

[0024] Figure 3 The graph shows the enzyme activity data of free enzyme after treatment with protease solution and EDTA solution, enzyme / ZIF-8 composite material after tableting, and ZIF-8 composite material after recovery. Detailed Implementation

[0025] The present invention will be further described below with reference to embodiments. The following embodiments are only used to illustrate the performance of the present invention more clearly, and should not be limited to the embodiments described below.

[0026] Example 1

[0027] Preparation of MOF materials (taking ZIF-8 as an example):

[0028] Weigh 22.7 g (0.28 mol) of 2-methylimidazole and dissolve it in 8 ml of water (0.03 mol mL⁻¹). Weigh 1.17 g (3.9 mmol) of Zn(NO₃)₂·6H₂O and dissolve it in 80 ml of water (0.049 mmol mL⁻¹). Sonicate the solutions from turbid to clear. Pour the Zn(NO₃)₂·6H₂O aqueous solution into the 2-methylimidazole aqueous solution; the solution instantly turns into a white emulsion. Stir for 5 minutes at 600 rpm. Then, centrifuge the white emulsion in a centrifuge tube, sonicate for a few minutes, wash three times with water, and then activate it at 120 °C in a vacuum drying oven to obtain ZIF-8 with a dodecahedral size of 100 nm. Preparation of HRP-GOx / ZIF-8 composite material:

[0029] Weigh 90mg of activated ZIF-8 material, then weigh 5mg of glucose oxidase (GOx) and 5mg of horseradish peroxidase (HRP) respectively. Mix them thoroughly and then take 20mg each time and put it into the cavity of the infrared tablet press. Tap the cavity wall to make it evenly adhere to the bottom of the disc. Apply a pressure of 30MPa (gauge pressure, actual pressure is 1364MPa) to it. After 5 minutes, remove the pressure. After demolding, the material can be clearly seen to turn into a reddish-brown disc. Set aside for later use and record it as tableted bioenzyme / ZIF-8.

[0030] A portion of the compressed composite material was placed in methanol vapor, and then the methanol vapor temperature was raised to 25℃ and maintained for 48 hours. This was then stored as the recovered bioenzyme / ZIF-8. The obtained product was processed through... Figure 1 Visible with a transmission electron microscope (TEM).

[0031] Performance testing:

[0032] Take 20 mg of the tableted and recovered ZIF-8 enzymes and place them in 6 mM 2,2'-azido-bis-3-ethylbenzothiazoline-6-sulfonic acid (ABTS) phosphate buffer solution (PBS) at pH 7.4. Then add small amounts of glucose to ensure glucose concentrations of 1 mM, 2 mM, 2.5 mM, 4 mM, and 6 mM, respectively. After diluting the discolored solutions with aqueous solution, the activities of the tableted and recovered ZIF-8 enzymes at different concentrations were compared using UV light and Beer-Lambert law.

[0033] from Figure 2 Experiments show that under axial pressure, the pressure not only does not inactivate the enzyme, but also allows the enzyme to remain protected by MOFs. Furthermore, most of the enzymes in the restored bio-enzyme / ZIF-8 still maintain high activity. This indicates that restoring the pores of the MOF in steam can increase the mass transfer rate of the composite material, improve the contact sites between reactants and catalysts, and maximize the synergistic effect between the bio-enzyme and MOFs.

[0034] Comparative experiment of enzyme activity of biological enzyme / ZIF-8 after tablet compression and after recovery 24 hours after inhibitor treatment:

[0035] 20 mg of the tableted and recovered ZIF-8 enzymes were treated with 1 mg / ml protease and 1 wt% EDTA for 24 hours, respectively. The solutions were then discarded and placed in 6 mM 2,2'-azido-bis-3-ethylbenzothiazoline-6-sulfonic acid (ABTS) in pH 7.4 phosphate buffered saline (PBS). A small amount of glucose was added to ensure a glucose concentration of 1 mM. The discolored solutions were diluted with aqueous solution, and the activities of the tableted and recovered ZIF-8 enzymes at different concentrations were compared using UV light and Beer-Lambert law.

[0036] from Figure 3It is known that free enzymes lose about 60% of their enzyme activity after being treated with protease, and about 90% after being treated with ethylenediaminetetraacetic acid. However, after being treated with protease and ethylenediaminetetraacetic acid, the tableted bioenzyme / ZIF-8 only lost 10% and 60% of its enzyme activity, respectively. This is because most of the enzyme was embedded in the gaps between the MOF nanoparticles.

[0037] After recovery, the enzyme / ZIF-8 was treated with protease and ethylenediaminetetraacetic acid, and the test results showed that the enzyme activity was almost unaffected. Therefore, the stress-induced recovery process not only maintained the enzyme activity but also protected the enzyme from enzyme inhibitors by utilizing the pores of the MOF.

[0038] The biological enzymes in the embodiments provided by the present invention have a high loading rate in MOF materials, and the method is simple and easy to implement, which can give full play to the activity of biological enzymes, and at the same time play a protective role for enzymes.

[0039] The above description is only a preferred embodiment of the present invention. It should be noted that those skilled in the art can make various modifications and improvements without departing from the inventive concept of the present invention, and these should also be considered within the scope of protection of the present invention.

Claims

1. A method for synthesizing bioenzyme / MOF composite functional materials under pressure, characterized in that, Includes the following steps: α1. Dissolve 0.28 mol of 2-methylimidazole in 8 ml of water, and dissolve 3.9 mmol of Zn(NO3)2•6H2O in 80 ml of water. Sonicate the solutions separately until they become clear and transparent. Pour the Zn(NO3)2•6H2O aqueous solution into the 2-methylimidazole aqueous solution. The solution instantly turns into a white emulsion. Stir for 5 minutes at 600 rpm. Then, centrifuge the white emulsion in a centrifuge tube, sonicate, wash with water 3 times, and then activate it in a vacuum drying oven at 120℃ to obtain ZIF-8 with a dodecahedral size of 100 nm. α2. Weigh 90 mg of activated ZIF-8 material, then weigh 5 mg of glucose oxidase (GOx) and 5 mg of horseradish peroxidase (HRP) respectively. Mix them thoroughly and then take 20 mg each time and put it into the cavity of the infrared tablet press. Tap the cavity wall to make it evenly adhere to the bottom of the disc. Apply an actual pressure of 1364 MPa to it. After 5 minutes, remove the pressure. After demolding, the material can be clearly seen to turn into a reddish-brown disc. α3. Take a portion of the tableted composite material and place it in methanol vapor. Then raise the temperature of the methanol vapor to 25°C and maintain it for 48 h to obtain HRP-GOx / ZIF-8.

Citation Information

Patent Citations

  • Method for preparing nanometer material@metal organic framework material

    CN106117593A

  • Enzyme@ZIF-8@Fe3O4 magnetic nanoenzyme reactor and preparation method thereof

    CN107267494A

  • Protein and metal organic skeleton compound composite material and preparation method thereof

    CN104087572A