Capacitor components and their manufacturing methods

By introducing silicon into the dielectric layer and using high dielectric constant materials, the problem of the dielectric constant of the capacitor element decreasing when the withstand voltage is increased is solved, achieving both high capacitance density and high withstand voltage, and improving the performance of the capacitor element. Overall performance.

CN110164850BActive Publication Date: 2024-10-11PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201811579957.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-02-15
Filing Date
2018-12-24
Publication Date
2024-10-11
Estimated Expiration
2038-12-24

AI Technical Summary

Technical Problem

When the film thickness of existing capacitive elements is increased to increase the withstand voltage, the dielectric constant decreases, resulting in a decrease in the withstand electric field strength, making it difficult to achieve both high capacitance density and high withstand voltage.

Method used

By introducing silicon into the dielectric layer, a concentration distribution containing cross-interface convexities is formed, defects within the dielectric layer are interpolated, the withstand voltage of the capacitive element is improved, and high dielectric constant materials such as hafnium oxide and zirconium oxide are used to achieve high capacitance.

Benefits of technology

A capacitive element with excellent withstand voltage characteristics has been realized, taking into account high capacitance density and high withstand voltage, and improving the withstand voltage characteristics of image sensors and memory devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110164850B_ABST
    Figure CN110164850B_ABST
Patent Text Reader

Abstract

A capacitor element according to one embodiment of the present invention comprises: a first electrode; a second electrode facing the first electrode; and a dielectric layer located between the first electrode and the second electrode and in contact with the first electrode. A first portion of the first electrode in contact with an interface between the first electrode and the dielectric layer and a second portion of the dielectric layer in contact with the interface contain silicon. A concentration distribution of the silicon along the thickness direction of the first portion and the second portion includes a convex portion that crosses the interface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a capacitor element and a method for manufacturing the capacitor element. Background Art

[0002] In the past, in order to improve the integration of semiconductor integrated circuits, the capacitance density per unit area of ​​the capacitor element possessed by the semiconductor integrated circuit has been studied. As one of the countermeasures to improve the capacitance density, the insulating film of the capacitor element formed by the material with high dielectric constant has been studied. For example, Soon-Wook Kim, "Effects of electrical stress on the leakage current characteristics of multilayer capacitor structures", Appl. Phys. Lett. 96, 262904, 2010 (hereinafter referred to as non-patent document 1) and TS Boscke, "Ferroelectricity in Hafnium Oxide: CMOS compatible Ferroelectric Field Effect Transistors" IEEE, IEDM, 11, 547-550, 2011, etc. disclose a capacitor element, which has an insulating film formed by using hafnium oxide (HfO2) with a dielectric constant higher than that of silicon dioxide (SiO2) commonly used in the past. Summary of the invention

[0003] A capacitor element of a non-limiting exemplary embodiment of the present invention comprises: a first electrode; a second electrode, the second electrode facing the first electrode; and a dielectric layer, the dielectric layer being located between the first electrode and the second electrode and in contact with the first electrode. A first portion of the first electrode in contact with an interface between the first electrode and the dielectric layer, and a second portion of the dielectric layer in contact with the interface contain silicon. A concentration distribution of the silicon along the thickness direction of the first portion and the second portion includes a convex portion that crosses the interface.

[0004] In addition, a method for manufacturing a capacitor element according to a non-limiting exemplary embodiment of the present invention includes the following steps: a step of forming a first electrode; a step of exposing the first electrode to a gas containing a silicon compound so that the first electrode contains silicon; and a step of forming a dielectric layer on the first electrode. The step of containing silicon is performed before the step of forming the dielectric layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0005] Figure 11 is a cross-sectional view showing an example of a cross-sectional structure of a capacitor element according to an embodiment.

[0006] Figure 2 2 is a cross-sectional view showing another example of the cross-sectional structure of the capacitor element according to the embodiment.

[0007] Figure 3A The diagram is a cross-sectional view showing each step of the method for manufacturing the capacitor element according to the embodiment.

[0008] Figure 3B It is a cross-sectional view showing one step of the method for manufacturing the capacitor element according to the embodiment.

[0009] Figure 3C It is a cross-sectional view showing one step of the method for manufacturing the capacitor element according to the embodiment.

[0010] Figure 3D It is a cross-sectional view showing one step of the method for manufacturing the capacitor element according to the embodiment.

[0011] Figure 4 It is a diagram showing the results of SIMS analysis of TiN in the capacitor element according to the embodiment.

[0012] Figure 5 It is a diagram showing the results of SIMS analysis of HfO in the capacitor element according to the embodiment.

[0013] Figure 6 FIG. 1 is a diagram showing the concentration distribution of silicon (Si) in the depth direction of the capacitor according to the embodiment.

[0014] Figure 7 It is a diagram showing the concentration distribution of carbon (C) in the depth direction of the capacitor element according to the embodiment.

[0015] Figure 8 This is a diagram showing an example of the voltage-current characteristics of the capacitor element according to the embodiment.

[0016] Fig. 9 It is a cross-sectional view showing a cross-sectional structure of an image sensor including a capacitive element according to an embodiment.

[0017] Fig.10 It is a cross-sectional view showing a cross-sectional structure of a memory device including a capacitor according to an embodiment.

[0018] Explanation of symbols

[0019] 10, 20 Capacitor elements

[0020] 11, 21 Lower electrode

[0021] 12, 22 Dielectric layer

[0022] 13, 23 Upper electrode

[0023] 90 bulge

[0024] 91 Vertex

[0025] 92 Top

[0026] 93 Lower end

[0027] 100 Image Sensor

[0028] 110, 210 substrate

[0029] 120 Multilayer Wiring Structure

[0030] 130 Photoelectric conversion element

[0031] 131 pixel electrode

[0032] 132 Photoelectric conversion film

[0033] 133 Transparent Electrode

[0034] 200 Storage Devices

[0035] 201 DRAM formation area

[0036] 202 Logic circuit formation area

[0037] 220 storage units

[0038] 230 Wiring Layer

[0039] 231, 232 Contact plug

[0040] 240, 241, 242 Insulation film DETAILED DESCRIPTION

[0041] (Knowledge that is the basis of the present invention)

[0042] As for the electrostatic capacitance C of the capacitor element, when the dielectric constant of the dielectric layer sandwiched between the electrodes is set to ε, the dielectric constant of the vacuum is set to ε0, the film thickness of the dielectric layer is set to t, and the area of ​​the electrode is set to S, it is expressed by C = ε × ε0 × S / t. Therefore, the countermeasures for improving the capacitance density include not only increasing the dielectric constant ε of the dielectric layer, but also reducing the film thickness t of the dielectric layer.

[0043] In order to increase the withstand voltage of a capacitor, the following operations are usually performed: increasing the thickness of the dielectric layer or using a material with a wide band gap and a low dielectric constant. In addition, the withstand voltage refers to the voltage at which the leakage current flowing between electrodes increases significantly.

[0044] However, as shown in Non-Patent Document 1, the withstand electric field strength of hafnium oxide (HfO2) decreases as the film thickness increases. In addition, the withstand electric field strength refers to the electric field strength at which the leakage current increases significantly, and is used in the same meaning as the withstand voltage. Therefore, when a dielectric layer is formed using hafnium oxide, there is a problem that the withstand voltage decreases even if the film thickness of the dielectric layer is increased.

[0045] An outline of one aspect of the present invention is as follows.

[0046] A capacitor element according to one embodiment of the present invention comprises: a first electrode; a second electrode facing the first electrode; and a dielectric layer located between the first electrode and the second electrode and in contact with the first electrode. A first portion of the first electrode in contact with an interface between the first electrode and the dielectric layer and a second portion of the dielectric layer in contact with the interface contain silicon. A concentration distribution of the silicon along the thickness direction of the first portion and the second portion includes a convex portion that crosses the interface.

[0047] Thus, the silicon contained in the dielectric layer fills in the defects in the dielectric layer, thereby suppressing the formation of the current path. Therefore, the withstand voltage of the capacitor element can be improved. Thus, according to this scheme, a capacitor element with excellent withstand voltage characteristics can be realized.

[0048] In the capacitor element according to one aspect of the present invention, for example, the dielectric layer may be composed of at least one selected from the group consisting of hafnium oxide and zirconium oxide.

[0049] Thus, hafnium oxide and zirconium oxide are materials with high dielectric constants, and thus can achieve high capacitance of the capacitor element. Therefore, according to this embodiment, it is possible to achieve both high capacitance and high withstand voltage of the capacitor element.

[0050] In the capacitor element according to one aspect of the present invention, for example, the position where the concentration of the silicon reaches a maximum in the protrusion may be located in the first portion.

[0051] Thus, silicon is distributed in a manner that expands on both sides of the position where the concentration of silicon reaches the maximum in the convex portion, so that a large amount of silicon is contained near the interface with the first electrode in the dielectric layer by positioning the apex in the first electrode. Therefore, defects near the interface in the dielectric layer can be effectively filled, thereby increasing the withstand voltage of the capacitor element.

[0052] In the capacitor element according to one aspect of the present invention, for example, the content of the silicon at a position in the protrusion where the concentration of the silicon reaches a maximum may be 1 atomic % or more and 25 atomic % or less.

[0053] Thus, by having a content of the silicon at the position where the concentration of the silicon in the convex portion reaches the maximum of 1 atom % or more, the dielectric layer also contains a sufficient amount of silicon that can fully fill in the defects. Therefore, the defects in the dielectric layer are filled in, thereby increasing the withstand voltage of the capacitor element. In addition, by having a content of the silicon at the position where the concentration of the silicon in the convex portion reaches the maximum of 25 atom %, the oxide of hafnium or the oxide of zirconium has a high dielectric constant. Therefore, the capacitance of the capacitor element can be increased. In this way, according to this scheme, it is possible to take into account both the high capacitance and the high withstand voltage of the capacitor element.

[0054] In the capacitor element according to one aspect of the present invention, for example, the first electrode may be composed of at least one selected from the group consisting of titanium nitride and tantalum nitride.

[0055] Thus, a metal nitride film such as titanium nitride or tantalum nitride has high affinity with a semiconductor process using a dielectric layer, and thus a capacitor element having excellent withstand voltage characteristics can be easily realized.

[0056] In the capacitor element according to one aspect of the present invention, for example, the position where the concentration of the silicon reaches a maximum in the protrusion may be located within a range of ±10 nm from the interface in the thickness direction.

[0057] Thus, a large amount of silicon is distributed in a range of at least ±10 nm based on the interface, so that a sufficient amount of silicon to fill defects is also contained in the dielectric layer. Therefore, defects in the dielectric layer are filled, and the withstand voltage of the capacitor element can be increased.

[0058] Furthermore, for example, an image sensor according to one aspect of the present invention includes the above-mentioned capacitive element.

[0059] Thus, the image sensor includes a capacitor element having excellent withstand voltage characteristics, and thus the withstand voltage characteristics of the image sensor can be improved.

[0060] Furthermore, for example, a storage device according to one aspect of the present invention includes the above-mentioned capacitor element.

[0061] Thus, the memory device includes a capacitor element having excellent withstand voltage characteristics, and thus the withstand voltage characteristics of the memory device can be improved.

[0062] In addition, for example, a method for manufacturing a capacitor element according to one embodiment of the present invention includes the following steps: a step of forming a first electrode; a step of exposing the first electrode to a gas containing a silicon compound so that the first electrode contains silicon; and a step of forming a dielectric layer on the first electrode. The step of containing silicon is performed before the step of forming the dielectric layer.

[0063] Thus, the first electrode contains silicon, and thus by stacking the dielectric layer on the first electrode, silicon can be efficiently contained in the stacked dielectric layer. Therefore, defects in the dielectric layer are filled with silicon, and the formation of a current path can be suppressed.

[0064] In addition, by exposing the first electrode to the silicon compound, since silicon is added to the first electrode, the amount of silicon added to the first electrode can be made uniform within the surface. In particular, in the case of a non-parallel plate type capacitor element such as a capacitor element having a trench structure, silicon can be uniformly added from the surface exposed to the silicon compound even when the first electrode has a three-dimensional structure. Therefore, the unevenness of silicon can be reduced, defects in the dielectric layer can be uniformly interpolated within the surface, and the formation of a current path can be suppressed.

[0065] As described above, according to the present embodiment, a capacitor element having excellent withstand voltage characteristics can be manufactured.

[0066] In addition, for example, the above-mentioned silicon compound is any one of silane (SiH4), disilane (Si2H6), dichlorosilane (SiH2Cl2), trichlorosilane (SiHCl3), silicon tetrachloride (SiCl4) and silicon tetrafluoride (SiF4).

[0067] Thereby, silicon contained in the silicon compound can be uniformly added to the first electrode.

[0068] Below, the embodiments of the present invention are described in detail with reference to the accompanying drawings. In addition, the embodiments described below all show general or specific examples. The numerical values, shapes, materials, constituent elements, configurations and connection forms of constituent elements, manufacturing processes, the order of manufacturing processes, etc. shown in the following embodiments are only examples, and the main purpose is not to limit the present invention. As long as no contradiction occurs, the various schemes described in this specification can be combined with each other. In addition, for the constituent elements in the following embodiments that are not recorded in the independent claims showing the highest concept, they are described as optional constituent elements.

[0069] In addition, each figure is only a schematic diagram and may not be strictly illustrated. Therefore, for example, the scales in each figure may not be consistent. In addition, in each figure, components having substantially the same function are represented by common reference numerals, and the description is sometimes omitted or simplified.

[0070] In addition, in this specification, the terms "above" and "below" do not refer to the upward direction (vertically above) and the downward direction (vertically below) in absolute spatial recognition, but are used as terms defined by relative positional relationships based on the stacking order in the stacking structure. In addition, the terms "above" and "below" are applicable not only to the case where two components are arranged at a distance from each other and there is another component between the two components, but also to the case where two components are arranged closely to each other and the two components are in contact.

[0071] (Implementation Method)

[0072] [constitute]

[0073] Figure 1 2 is a cross-sectional view showing an example of a cross-sectional structure of the capacitor element 10 according to the embodiment.

[0074] like Figure 1 As shown, the capacitor element 10 includes a lower electrode 11, a dielectric layer 12, and an upper electrode 13. The capacitor element 10 is formed by sequentially stacking the lower electrode 11, the dielectric layer 12, and the upper electrode 13 on a substrate (not shown).

[0075] The lower electrode 11 and the upper electrode 13 are examples of a first electrode and a second electrode disposed to face each other. The dielectric layer 12 is located between the lower electrode 11 and the upper electrode 13 and is in contact with the lower electrode 11 and the upper electrode 13 .

[0076] like Figure 1 As shown, the capacitor element 10 is a parallel plate type capacitor element. Specifically, the lower electrode 11, the dielectric layer 12 and the upper electrode 13 are respectively configured as a plate with a substantially uniform film thickness. The lower electrode 11 and the upper electrode 13 are arranged parallel to each other with the dielectric layer 12 sandwiched therebetween. The upper surface of the lower electrode 11 contacts the lower surface of the dielectric layer 12. The lower surface of the upper electrode 13 contacts the upper surface of the dielectric layer 12.

[0077] In addition, the electrode area of ​​the capacitor element 10 corresponds to the area where the upper electrode 13 and the lower electrode 11 overlap when viewed from above. Viewing from above means observing the capacitor element 10 from the stacking direction. The stacking direction is Figure 1 The opposite direction to the depth direction shown is the direction from bottom to top.

[0078] The lower electrode 11 is an example of a first electrode provided by the capacitor element 10. The lower electrode 11 is formed using a conductive material. As a conductive material, a metal single substance such as titanium (Ti), aluminum (Al), gold (Au) or platinum (Pt) is used. Alternatively, as a conductive material, a conductive metal nitride film such as titanium nitride (TiN), tantalum nitride (TaN) or hafnium nitride (HfN) is used. In addition, as a conductive material, a conductive oxide such as indium tin oxide (ITO: Indium Tin Oxide) or zinc oxide (ZnO) can also be used.

[0079] The lower electrode 11 is formed, for example, by using metal organic chemical vapor deposition (MOCVD), atomic layer deposition (ALD), or sputtering. The lower electrode 11 is formed, for example, by forming a conductive material in a thin film on the substrate. The film thickness of the lower electrode 11 is, for example, 15 nm, but is not limited thereto.

[0080] The upper electrode 13 is an example of a second electrode provided in the capacitor 10. The upper electrode 13 may be formed using the same material as the lower electrode 11, or may be formed using a different material. The upper electrode 13 is formed using the MOCVD method, the ALD method, the sputtering method, or the like, similarly to the lower electrode 11. The upper electrode 13 is formed, for example, by forming a conductive material in a thin film in a region that overlaps with the lower electrode 11 when viewed from above as a region on the dielectric layer 12. The film thickness of the upper electrode 13 is, for example, 200 nm, but is not limited thereto.

[0081] The dielectric layer 12 is formed using a high-k material having a higher dielectric constant than silicon dioxide (SiO2). Specifically, the dielectric layer 12 contains an oxide of hafnium (Hf) or zirconium (Zr) as a main component. The dielectric layer 12 contains more than 50 mol% of the oxide of hafnium or zirconium. The dielectric layer 12 is formed using an ALD method, an MOCVD method, or an EB (Electron Beam) evaporation method. The dielectric layer 12 is formed, for example, by forming a dielectric film composed of an oxide of hafnium or zirconium in a thin film on the lower electrode 11.

[0082] The dielectric layer 12 has a monoclinic crystal structure and is a normal dielectric.

[0083] The film thickness of the dielectric layer 12 can be measured by, for example, a physical film thickness from a photograph taken using a transmission electron microscope. Alternatively, when the area (S) of the capacitor element 10 and the dielectric constant (ε) of the dielectric layer 12 are known, the average film thickness (t) can be calculated from the capacitance value (C) of the capacitor element 10 based on the formula: t = ε × S / C.

[0084] The crystal structure of the dielectric layer 12 can be known by performing an analysis using an X-ray diffraction (XRD) method. Alternatively, the crystal structure can also be known by a cross-sectional TEM (Transmission Electron Microscope).

[0085] The lower electrode 11 and the dielectric layer 12 each contain silicon (Si). The concentration distribution of silicon along the thickness direction of the lower electrode 11 and the dielectric layer 12 includes a convex portion crossing the interface between the lower electrode 11 and the dielectric layer 12. The details are described in the examples described later.

[0086] The concentration of silicon contained in the lower electrode 11 and the dielectric layer 12 can be measured using, for example, time-of-flight secondary ion mass spectrometry (ToF-SIMS). The method for measuring the film thickness, crystal structure, and silicon concentration of each layer is not limited to these.

[0087] In addition, the cross-sectional structure of the capacitor element 10 is not limited to Figure 1 That is, the capacitor element 10 may not be a parallel plate capacitor element.

[0088] Figure 2 2 is a cross-sectional view showing a cross-sectional structure of a capacitor element 20 according to another example of the present embodiment. Figure 2 The capacitor element 20 shown is not a parallel plate capacitor element, but a three-dimensional structure capacitor element. Specifically, the capacitor element 20 includes a lower electrode 21, a dielectric layer 22, and an upper electrode 23. Figure 1 Compared with the capacitor element 10 shown, except for the point that its cross-sectional structure is different, the materials constituting each layer and the manufacturing method are the same as those of the capacitor element 10.

[0089] like Figure 2 As shown in FIG. 1 , the interface between the lower electrode 21 and the dielectric layer 22 has a groove shape that is recessed in the direction from the upper electrode 23 to the lower electrode 21, that is, in the depth direction. The dielectric layer 22 is provided along the groove shape with a substantially uniform film thickness. Figure 2In the example shown, the lower electrode 21 is also provided along the groove shape with a substantially uniform film thickness. The upper surface of the upper electrode 23 is substantially flat, and the lower surface is provided along the groove shape.

[0090] As a result, the area where the upper electrode 23 and the lower electrode 21 face each other increases in the side surface of the groove in the groove shape. Figure 1 The capacitor element 10 shown is of the same size, and the surface area of ​​the capacitor element 20 is also increased, and the capacitance is also increased.

[0091] in addition, Figure 2 Although an example of a groove shape having two grooves is shown, the number of grooves may be one or more than three. In addition, the capacitance of the capacitor element 20 can be increased by increasing the number of grooves or making the grooves deeper.

[0092] [Method for manufacturing capacitor element]

[0093] Next, use FIG. 3A to FIG. 3D , a method for manufacturing the capacitor element 10 according to the present embodiment will be described. FIG. 3A to FIG. 3D The diagrams are cross-sectional views showing the respective steps of the method for manufacturing the capacitor element 10 according to the present embodiment.

[0094] The method for manufacturing the capacitor element 10 includes the steps of forming the lower electrode 11, making the lower electrode 11 contain silicon, and stacking the dielectric layer 12 on the lower electrode 11. The step of making the lower electrode 11 contain silicon is performed before the step of stacking the dielectric layer 12.

[0095] Specifically, first, Figure 3A As shown, a lower electrode 11 is formed on a substrate (not shown). For example, a TiN film is formed using an MOCVD method to form the lower electrode 11. The thickness of the TiN film is, for example, 15 nm, but is not limited thereto. The raw materials used in the MOCVD method are, for example, TDMAT (Ti[N(CH3)2]4, tetrakis(dimethylamide)titanium, etc.

[0096] Then, if Figure 3B As shown, the lower electrode 11 is exposed to a gas containing a silicon compound, thereby causing the lower electrode 11 to contain silicon. Specifically, a gas containing a silicon compound is supplied into a chamber in which the lower electrode 11 is disposed, thereby exposing the surface of the lower electrode 11 to the silicon compound. The gas containing the silicon compound is, for example, silane (SiH4) gas, but is not limited thereto. For example, the silicon compound may also be disilane (Si2H6), dichlorosilane (SiH2Cl2), trichlorosilane (SiHCl3), silicon tetrachloride (SiCl4), silicon tetrafluoride (SiF4), etc.

[0097] Then, if Figure 3C As shown in FIG. 1 , a dielectric layer 12 is formed on the lower electrode 11 exposed to the silicon compound using an ALD method. The substrate temperature at this time is, for example, 250° C. or higher and 300° C. or lower. For example, hafnium oxide (HfO x ) is formed on the lower electrode 11, thereby forming a dielectric layer 12.

[0098] The raw material used in the ALD method is TEMAH (Hf[NCH3C2H5]4; tetrakis(ethylmethylamino)hafnium). The raw material gas and O3 gas are alternately introduced into the chamber, thereby forming HfO on the lower electrode 11 after silane exposure. x Film growth. In addition, the raw material may also be TDMAH (Hf[N(CH3)2]4; tetrakis(dimethylamino)hafnium).

[0099] In addition, zirconium oxide (ZrO x ) film. x The film thickness of HfO is, for example, 21 nm, but is not limited thereto. x and ZrO x The subscript x is a positive value, for example, x=2, but not limited thereto.

[0100] Then, if Figure 3D As shown, the upper electrode 13 is formed on the dielectric layer 12. For example, a TiN film is formed on the dielectric layer 12 using the MOCVD method, thereby forming the upper electrode 13. The film thickness of the TiN film is, for example, 70 nm, but is not limited thereto.

[0101] Finally, after forming the upper electrode 13, heat treatment is performed in a nitrogen (N2) atmosphere. Heat treatment in a nitrogen atmosphere is also called nitrogen annealing. Nitrogen annealing is performed at 400° C. for 30 minutes, for example.

[0102] In the present embodiment, the capacitor element 10 is not subjected to heat treatment at high temperature. Here, high temperature refers to a temperature at which the dielectric layer 12 cannot maintain a normal dielectric range, for example, a temperature above 1000°C. If a heat treatment of 1000°C is performed, the crystal state of the dielectric layer 12 changes from monoclinic to orthorhombic. Due to the change in the crystal state, the dielectric layer 12 becomes a ferroelectric. The dielectric layer 12 that becomes a ferroelectric has hysteresis characteristics. Therefore, when the capacitor element 10 is subjected to heat treatment such as nitrogen annealing, the temperature of the heat treatment is, for example, a temperature below 400°C.

[0103] In addition, the manufacturing method of the capacitor element 20 having a trench structure is FIG. 3A to FIG. 3DThe manufacturing method of the capacitor element 10 shown in FIG. 1 is the same as that of the capacitor element 10 shown in FIG. For example, before forming the lower electrode 21, an insulating film is formed on the upper side of the substrate, and a part of the insulating film is removed to form a concave portion. By forming the lower electrode 21 along the concave portion, the lower electrode 21 having a groove structure is formed. After the lower electrode 21 is formed, FIG. 3B to FIG. 3D Similarly to the manufacturing method shown, exposure to silicon compound, formation of dielectric layer 22, formation of upper electrode 23, and nitrogen annealing are sequentially performed. Thus, the capacitor element 20 having a trench structure is manufactured.

[0104] The following examples are provided for the purpose of illustrating the present invention, and are not intended to limit the present invention.

[0105] The inventors of the present invention produced samples of the capacitor element 10 of the example and samples of the capacitor element of the comparative example described below, and evaluated the characteristics of the produced samples. First, the specific production conditions of each sample will be described.

[0106] [Example]

[0107] First, a TiN film with a thickness of 15 nm was formed on a substrate formed of a Si wafer as the lower electrode 11. Next, an exposure treatment was performed in SiH4 gas for 180 seconds in a furnace set at a high temperature and reduced pressure atmosphere of 350°C and 90 Torr. HfO was formed as the dielectric layer 12. x A film was formed with a thickness of 21 nm. Next, a TiN film was formed with a thickness of 70 nm as the upper electrode 13. After that, a heat treatment was performed at 400° C. for 30 minutes in a nitrogen atmosphere. Thus, the capacitor element 10 of the example was manufactured.

[0108] In addition, HfO constituting the dielectric layer x The film is formed by the ALD method. The raw material used in the ALD method is TEMAH (Hf[NCH3C2H5]4; tetrakis(ethylmethylamino)hafnium). The raw material gas and O3 gas are alternately introduced into the chamber, thereby forming HfO on the lower electrode 11. x Membrane growth.

[0109] The TiN films constituting the lower electrode 11 and the upper electrode 13 are formed by MOCVD. The raw materials used in the MOCVD method are, for example, TDMAT (Ti[N(CH3)2]4, tetrakis(dimethylamide)titanium, and the like.

[0110] In addition, a sample for film analysis was produced under the same manufacturing conditions as those of the capacitor element 10 of the example except that the upper electrode 13 was not formed.

[0111] [Comparative Example]

[0112] The present inventors also fabricated a capacitor element in which the lower electrode 11 was not exposed to the silicon compound as a comparative example. The capacitor element of the comparative example was fabricated under the same conditions as those of the example except that the lower electrode 11 was not exposed to SiH 4 .

[0113] In addition, a sample for film analysis was produced under the same manufacturing conditions as the capacitor element of the comparative example except that the upper electrode was not formed.

[0114] [Comparison of characteristics]

[0115] The following describes the results of analyzing the characteristics of the capacitor elements and film analysis samples produced in Examples and Comparative Examples.

[0116] First, use Figure 4 and Figure 5 , the position of the interface between the lower electrode 11 and the dielectric layer 12 will be described.

[0117] Figure 4 It is a diagram showing the results of SIMS analysis of TiN in the capacitor element of the present embodiment.

[0118] Figure 5 It is a diagram showing the results of SIMS analysis of HfO in the capacitor element according to the embodiment.

[0119] Figure 4 and Figure 5 The results of evaluation of the film analysis samples prepared in the examples and comparative examples using secondary ion mass spectrometry (SIMS) are shown respectively. Figure 4 and Figure 5 In FIG. 1 , the horizontal axis represents the depth from the upper surface of the dielectric layer 12 . Figure 4 The vertical axis represents the intensity of Ti ions. Figure 5 The vertical axis of represents the intensity of Hf ions. The intensity of ions corresponds to the amount (specifically, concentration) of atoms contained in the film to be analyzed at the corresponding depth.

[0120] like Figure 4 As shown in the figure, when the depth exceeds about 17nm, the intensity of Ti ions begins to increase, and the intensity is saturated at a depth of about 26nm. When the depth exceeds about 32nm, the intensity of Ti ions begins to decrease, and Ti ions are basically undetectable at about 58nm.

[0121] On the other hand, Figure 5 As shown in FIG. 1 , the intensity of Hf ions remains approximately constant in the depth direction and slightly increases at a depth of about 20 nm. The intensity of Hf ions reaches a maximum at a depth of about 22 nm and then decreases to about 30 nm.

[0122] In this embodiment, the position of the interface between the lower electrode 11 and the dielectric layer 12 is regarded as the maximum value of the Hf ion intensity, that is, the depth position at which the Hf ion intensity begins to decrease. Figure 5 As shown, the interface is located at a depth of about 22 nm. In the examples and comparative examples, the HfO film was formed under film formation conditions to achieve a thickness of 21 nm, so it is known that the interface exists at a position substantially in accordance with the film formation conditions.

[0123] In addition, in the present embodiment, the position of the upper end of a specific region including the interface (hereinafter referred to as the interface region) is regarded as the position where the intensity of Ti ions begins to increase. Figure 4 As shown, the upper end of the interface region is located at a depth of about 17 nm.

[0124] In addition, the position of the lower end of the interface region is regarded as the position where the intensity of Hf ions stops decreasing. Figure 5 As shown, the lower end of the interface region is located at a depth of about 31 nm.

[0125] In addition, Figure 4 and Figure 5 , the graphs of the embodiment and the comparative example are not shown separately, but they are substantially the same. That is, the crystal structure of HfO and TiN is almost not affected by the exposure treatment using the silicon compound. Therefore, even if the exposure treatment using the silicon compound is performed, the high dielectric property of the dielectric layer 12 and the conductivity of the lower electrode 11 are the same as those in the case where the exposure treatment using the silicon compound is not performed.

[0126] Next, use Figure 6 , the concentration distribution of silicon (Si) in the depth direction is described.

[0127] Figure 6 : is a diagram showing the concentration distribution of silicon (Si) in the depth direction of the capacitor element of this embodiment. Figure 6 In FIG. 1 , the horizontal axis represents the depth from the upper surface of the dielectric layer 12 , and the vertical axis represents the concentration of silicon.

[0128] like Figure 6 As shown, the concentration of silicon in the interface region is different between the example and the comparative example. Specifically, the concentration of silicon in the sample of the example is higher than the concentration of silicon in the sample of the comparative example in the interface region.

[0129] The concentration distribution of silicon in the sample of the embodiment has a convex portion 90 extending to both sides of the interface between the lower electrode 11 and the dielectric layer 12. The convex portion 90 is a smooth mountain-shaped portion extending from the upper end 92 through the vertex 91 to the lower end 93. In addition, the convex portion 90 may have a plurality of local maximum values ​​between the upper end 92 and the lower end 93.

[0130] The vertex 91 of the convex portion 90 is the portion having the highest concentration of silicon near the interface. That is, the vertex 91 is the maximum value of the silicon concentration in the convex portion 90. Figure 6 As shown, the apex 91 of the protrusion 90 is located inside the lower electrode 11. That is, the apex 91 of the protrusion 90 is located on the lower electrode 11 side relative to the interface. The apex 91 is located at a depth of about 25 nm.

[0131] The silicon content at the vertex 91 is, for example, not less than 1 atomic % and not more than 25 atomic %. The content at the vertex 91 corresponds to the ratio of silicon to all elements at the depth of the vertex 91. Figure 6 As shown, the concentration at vertex 91 is about 2×10 21 Atom / cm 3 , which is 4 atomic % when converted into a content. The concentration of silicon gradually decreases on both sides with the top 91 as a reference in the depth direction. For example, in the shallow depth direction, i.e., HfO x At a position with a side distance of 5 nm, the concentration reaches less than half of the peak 91 .

[0132] The upper end 92 of the convex portion 90 is a portion where the reduction in silicon concentration is moderate when viewed in a shallow direction from the vertex 91. For example, when the slope of silicon concentration reduction is calculated per nm from the vertex 91 in a shallow direction, the position where the slope of reduction is less than half is the upper end 92.

[0133] like Figure 6 As shown, the upper end 92 of the protrusion 90 is located in the dielectric layer 12. Specifically, the upper end 92 is located in the dielectric layer 12 outside the interface region. In addition, the upper end 92 may also be located in the interface region. The upper end 92 is located at a depth of about 15 nm. Figure 6 As shown, the concentration of silicon at the upper end 92 is about 3×10 19 Atom / cm 3 .

[0134] When viewed from the vertex 91 in the depth direction, the lower end 93 of the convex portion 90 is a portion where the reduction in silicon concentration becomes gentler. For example, when the slope of the reduction in silicon concentration is calculated from the vertex 91 per 1 nm in the depth direction, the position where the slope of the reduction becomes less than half is the lower end 93. Figure 6 As shown, the lower end 93 of the protrusion 90 is located inside the lower electrode 11. Specifically, the lower end 93 is located at a position roughly consistent with the lower end of the interface region. In addition, the lower end 93 can be located inside the interface region or inside the lower electrode 11 outside the interface region. The lower end 93 is located at a depth of about 31 nm. Figure 6 As shown, the concentration of silicon at the lower end 93 is about 7×10 19 Atom / cm3 .

[0135] In addition, the upper end 92 and the lower end 93 of the convex portion 90 are not limited to the above examples. For example, the upper end 92 and the lower end 93 may be positions where the decreasing slope becomes 0. Alternatively, the upper end 92 and the lower end 93 may be positions where the concentration of silicon is one digit lower than the concentration of the vertex 91.

[0136] In this embodiment, the vertex 91 of the convex portion 90 is located within a range of ±10 nm based on the interface in the depth direction. In addition, "- (negative)" means shallow depth, and "+ (positive)" means deep depth. That is, the vertex 91 is located within a range from a position 10 nm shallower than the interface to a position 10 nm deeper than the interface.

[0137] like Figure 6 As shown, the vertex 91 is located within the range of +10 nm from the interface in the depth direction. The vertex 91 may also be located within the range of -10 nm from the interface. In addition, the upper end 92 and the lower end 93 are also located within the range of ±10 nm from the interface.

[0138] As described above, it is known that when the lower electrode 11 is exposed to a silicon compound and the dielectric layer 12 is formed, silicon diffuses not only on the lower electrode 11 side based on the interface but also on the dielectric layer 12 side. It is inferred that silicon not only fills the oxygen deficiency in the dielectric layer 12 but also replaces the carbon contained in the lower electrode 11 and the dielectric layer 12. In addition, carbon is a component contained in the raw materials used for forming the lower electrode 11 and the dielectric layer 12.

[0139] Here, use Figure 7 , the concentration distribution of carbon (C) in the depth direction is explained.

[0140] Figure 7 : is a graph showing the concentration distribution of carbon (C) in the depth direction of the capacitor element of this embodiment. Figure 7 In FIG. 1 , the horizontal axis represents the depth from the upper surface of the dielectric layer 12 , and the vertical axis represents the carbon concentration.

[0141] like Figure 7 As shown, the carbon concentration in the interface region is different between the embodiment and the comparative example. Specifically, the carbon concentration in the sample of the embodiment is lower than the carbon concentration in the sample of the comparative example in the interface region. More specifically, the carbon concentration in the sample of the embodiment is lower than the carbon concentration in the sample of the comparative example on the dielectric layer 12 side compared to the interface.

[0142] In this way, after exposing the lower electrode 11 to the silicon compound, the dielectric layer 12 is stacked, thereby reducing the amount of carbon contained as an impurity in the dielectric layer 12. Therefore, the amount of carbon that can become a carrier trap is reduced, so the generation of a current path can be suppressed. As a result, the withstand voltage of the capacitor element 10 is improved.

[0143] also, Figures 4 to 7 Although the analysis results of the sample for film analysis not including the upper electrode 13 are shown, the same also applies to the capacitor element 10 including the upper electrode 13 .

[0144] [Voltage-current characteristics]

[0145] Here, use Figure 8 The voltage-current characteristics of the capacitor elements of the examples and comparative examples will be described.

[0146] Figure 8 is a diagram showing an example of the voltage-current characteristics of the capacitor element of this embodiment. Specifically, Figure 8 The voltage-current characteristics of the above-mentioned embodiment and comparative example are shown. The current value was measured using a semiconductor parameter analyzer 4156C manufactured by Keysight. Specifically, 0V was applied to the lower electrode 11, and the voltage applied to the upper electrode 13 was scanned in the range of 0V to 7V, and the current value of the leakage current flowing between the lower electrode 11 and the upper electrode 13 was measured. The current value exceeded 1×10 9 A / cm 2 When , the capacitor element 10 is regarded as being destroyed, and the voltage at this time is taken as the insulation breakdown voltage.

[0147] The dielectric breakdown voltage of the capacitor element of the comparative example was 4.18 V. On the other hand, the dielectric breakdown voltage of the capacitor element 10 of the example was 4.80 V.

[0148] The above results confirm that after exposing SiH4 or other silicon compounds to the lower electrode 11 made of TiN or the like, HfO x The dielectric layer 12 is formed such that the withstand voltage of the capacitor element 10 is improved.

[0149] In addition, as HfO x The percolation model is being advocated as a failure model. The percolation model is a model in which defects caused by long-term stress form a current path, thereby causing insulation breakdown. The percolation model can also be applied to the capacitor element of this embodiment.

[0150] Therefore, the effect of improving the withstand voltage caused by adding silicon to the dielectric layer 12 can be considered to be due to the ions added to the dielectric layer 12 filling defects and suppressing the formation of current paths; and reducing the amount of impurity carbon contained in the dielectric layer 12 and suppressing the formation of current paths.

[0151] In addition, although TiN film is used as the lower electrode 11 here, the same result can be obtained in the case of other nitride metal films such as TaN film and HfN film. In addition, the same result can be obtained in the case of using conductive oxides such as ITO or metal films as the lower electrode 11. As the dielectric layer 12, instead of HfO x ZrO x The same results can be obtained even when other high-k materials such as silane are used as the silicon compound. In addition, the same results can be obtained even when a material containing silicon other than silane is used as the silicon compound.

[0152] [Image sensor]

[0153] Next, use Fig. 9 An image sensor 100 including the capacitive element 10 according to the present embodiment will be described. Fig. 9 : is a cross-sectional view showing the cross-sectional structure of the image sensor 100 according to the present embodiment.

[0154] The image sensor 100 includes a plurality of pixels arranged in a matrix. Each of the plurality of pixels includes a photoelectric conversion element that generates an electrical signal by photoelectrically converting received light, and a pixel circuit that processes the electrical signal generated by the photoelectric conversion element. Fig. 9 The cross-sectional structure of one pixel of the image sensor 100 is shown.

[0155] like Fig. 9 As shown in FIG. 1 , the image sensor 100 of the present embodiment has a stacked structure in which a photoelectric conversion film 132 is stacked on a pixel circuit. Specifically, the image sensor 100 includes a substrate 110 , a multilayer wiring structure 120 , and a photoelectric conversion element 130 .

[0156] The substrate 110 is a semiconductor substrate, such as a Si substrate.

[0157] The multilayer wiring structure 120 includes a pixel circuit that processes the electrical signal generated by the photoelectric conversion element 130. Specifically, Fig. 9 As shown, the multilayer wiring structure 120 includes a plurality of transistors Tr1, Tr2, and Tr3, a plurality of capacitors Cs and Cc, and a plurality of wirings.

[0158] The plurality of transistors Tr1 , Tr2 and Tr3 are reset transistors and charge readout transistors, respectively. The transistors Tr1 , Tr2 and Tr3 are, for example, MOSFETs. The source region and the drain region of each transistor are formed on the surface area of ​​the substrate 110 .

[0159] The capacitor element Cc is a capacitor element for storing signal charges taken out by the photoelectric conversion element 130. The capacitor element Cs is a capacitor element for removing kTC noise. Each transistor, each capacitor element, and each wiring are separated by an interlayer insulating film or the like formed of an insulating material such as a silicon oxide film.

[0160] The photoelectric conversion element 130 includes a pixel electrode 131, a photoelectric conversion film 132, and a transparent electrode 133. The pixel electrode 131 and the transparent electrode 133 are arranged to face each other with the photoelectric conversion film 132 interposed therebetween. The photoelectric conversion film 132 is in contact with the pixel electrode 131 and the transparent electrode 133 at its surface.

[0161] The pixel electrode 131 is provided separately from each pixel and is formed using a conductive material such as a metal such as aluminum or copper.

[0162] The photoelectric conversion film 132 is formed of an organic material or an inorganic material such as amorphous silicon. When light enters through the transparent electrode 133, the photoelectric conversion film 132 generates signal charges according to the amount of incident light. The signal charges are taken out through the pixel electrode 131 and stored in the capacitor Cc.

[0163] The transparent electrode 133 is formed using a transparent conductive material such as ITO. The transparent electrode 133 and the photoelectric conversion film 132 are provided in common for each pixel, for example.

[0164] The capacitor element 10 of this embodiment is used as a capacitor element Cs, for example. Fig. 9 As shown, the image sensor 100 includes a capacitor 10 as a capacitor Cs for removing kTC noise. The capacitor 10 is provided by sequentially stacking a lower electrode 11, a dielectric layer 12, and an upper electrode 13 above a substrate 110 and inside a multilayer wiring structure 120.

[0165] Furthermore, the capacitor element 10 can also be used as a capacitor element Cc for accumulating signal charges. Thus, even with incident light of high illuminance, overexposure can be achieved, and a pixel with a large number of saturated electrons can be realized.

[0166] The image sensor 100 of the present embodiment includes the capacitor element 10 having a high withstand voltage, and thus can improve reliability. Alternatively, the image sensor 100 may include the capacitor element 20 instead of the capacitor element 10 .

[0167] [Memory Devices]

[0168] Next, use Fig.10 A storage device 200 including the capacitor 20 according to the present embodiment will be described. Fig.10 2 is a cross-sectional view showing a cross-sectional structure of a memory device 200 according to this embodiment.

[0169] The memory device 200 is, for example, an eDRAM (embedded Dynamic Random Access Memory) or other storage device. In addition, the memory device 200 can be any capacitor-based storage device and is not limited to eDRAM.

[0170] like Fig.10 As shown, the memory device 200 of this embodiment includes a DRAM formation region 201 and a logic circuit formation region 202 on a substrate 210. In the DRAM formation region 201, a memory cell 220, a transistor Tr, and a wiring layer 230 are provided.

[0171] In the memory device 200, for example, a plurality of DRAM formation regions 201 and logic circuit formation regions 202 are arranged in a matrix. By writing electric charge into the memory cell 220 included in the DRAM formation region 201, a value can be stored. Fig.10 The cross-sectional structure of one unit region of the memory device 200 is shown.

[0172] The substrate 210 is a semiconductor substrate, such as a Si substrate, and a plurality of insulating films 240 , 241 and 242 are sequentially stacked on the substrate 210 .

[0173] The storage unit 220 is, for example, Figure 2 The capacitor element 20 is shown. The memory cell 220 is provided on an insulating film 241 formed on a substrate 210. Specifically, a through hole is provided in the insulating film 241 to expose the upper surface of the insulating film 240, and the memory cell 220 has a trench structure using the through hole.

[0174] The lower electrode 21 of the memory cell 220 is connected to one of the source and the drain of the transistor Tr via a contact plug 231 that penetrates the insulating film 240. The memory cell 220 accumulates the charge supplied by the transistor Tr.

[0175] The transistor Tr writes or reads the charge of the memory cell 220. The transistor Tr is, for example, a MOSFET. The source and drain of the transistor Tr are formed in the surface area of ​​the substrate 210. The other of the source and drain of the transistor Tr is connected to the wiring layer 230 through a contact plug 231 penetrating the insulating film 240 and a contact plug 232 penetrating the insulating films 241 and 242.

[0176] The wiring layer 230 is a wiring for supplying written charges to the memory cell 220 and for reading charges accumulated in the memory cell 220 .

[0177] The memory cell 220 is not provided in the logic circuit formation region 202. A transistor (not shown) is provided in the logic circuit formation region 202 to form a logic circuit. The logic circuit controls the transistor Tr in the DRAM formation region 201, for example.

[0178] As described above, the memory device 200 of this embodiment includes the capacitor element 20 having a high withstand voltage, and thus can improve reliability. Alternatively, the memory device 200 may include the capacitor element 10 instead of the capacitor element 20 .

[0179] (Other embodiments)

[0180] Above, based on the embodiments, the capacitor element and its manufacturing method, as well as the image sensor and the memory device of one or more schemes are described, but the present invention is not limited to these embodiments. As long as it does not depart from the gist of the present invention, the various deformation modes that can be thought of by those skilled in the art and the modes constructed by combining the constituent elements in different embodiments are also included in the scope of the present invention.

[0181] For example, the silicon content at the apex 91 of the convex portion 90 may be less than 1 atomic % or greater than 25 atomic %. In addition, the apex 91 may not be a single point in the depth direction in the silicon concentration distribution, but may have a width in the depth direction.

[0182] In addition, for example, the apex 91 of the protrusion 90 may be located inside the dielectric layer 12 .

[0183] Furthermore, for example, the concentration distribution of silicon may include convex portions extending over both sides of the interface between the upper electrode 13 and the dielectric layer 12. That is, the upper electrode 13 may be an example of a first electrode, and the lower electrode 11 may be an example of a second electrode.

[0184] In addition, various changes, substitutions, additions, omissions, etc. can be made to the above-mentioned embodiments within the scope of the claims or their equivalents.

Claims

1. A capacitor element, comprising: a first electrode; a second electrode, the second electrode facing the first electrode; and a dielectric layer, the dielectric layer being located between the first electrode and the second electrode and contacting the first electrode, A first portion of the first electrode in contact with an interface between the first electrode and the dielectric layer and a second portion of the dielectric layer in contact with the interface contain silicon. The concentration distribution of the silicon along the thickness direction of the first portion and the second portion includes a convex portion that crosses the interface, The first electrode is composed of at least one selected from the group consisting of titanium, aluminum, gold, platinum, titanium nitride, tantalum nitride, hafnium nitride, indium tin oxide, and zinc oxide.

2. The capacitor element according to claim 1, wherein The dielectric layer is composed of at least one selected from the group consisting of hafnium oxide and zirconium oxide.

3. The capacitor element according to claim 1, wherein The position where the concentration of the silicon reaches the maximum in the protrusion is located in the first portion.

4. The capacitor element according to claim 1, wherein The content of the silicon at a position where the concentration of the silicon in the protrusion is maximum is greater than or equal to 1 atomic % and less than or equal to 25 atomic %.

5. The capacitor element according to claim 1, wherein The first electrode is composed of at least one selected from the group consisting of titanium nitride and tantalum nitride.

6. The capacitor element according to claim 1, wherein The position where the concentration of silicon reaches a maximum in the protrusion is located within a range of ±10 nm from the interface in the thickness direction.

7. A method for manufacturing a capacitor element, comprising the following steps: A step of forming a first electrode; exposing the first electrode to a gas containing a silicon compound, thereby causing the first electrode to contain silicon; and forming a dielectric layer on the first electrode, The step of containing silicon is performed before the step of forming the dielectric layer. The first electrode is composed of at least one selected from the group consisting of titanium, aluminum, gold, platinum, titanium nitride, tantalum nitride, hafnium nitride, indium tin oxide, and zinc oxide.