Rubber composition for steel cord bonding and conveyor belt
By using components such as polybutadiene rubber and cobalt borate neodecanoate in the rubber composition, the problems of cold resistance and water adhesion of the conveyor belt in cold regions are solved, achieving excellent cold resistance and durability.
Patent Information
- Application Number
- CN202010101142.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-02-27
- Filing Date
- 2020-02-19
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2040-02-19
AI Technical Summary
Existing rubber compositions have poor cold resistance when used in cold regions, making it difficult to balance durability and water-resistant adhesion.
A rubber composition containing polybutadiene rubber and cobalt borate neodecanoate is used, along with carbon black, vulcanization accelerator, sulfur, and other components, to optimize the formulation of the rubber composition and improve its cold resistance and water resistance adhesion.
It achieves excellent cold resistance, durability and water-resistant adhesion of rubber compositions in cold regions, making it suitable for the manufacture of conveyor belts.
Smart Images

Figure CN111621066B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to a rubber composition for bonding steel cords and a conveyor belt. Background Technology
[0002] In the past, various rubber compositions have been proposed to improve the adhesion performance of steel cords.
[0003] For example, Patent Document 1 discloses a rubber composition comprising 40-80 parts by weight of carbon black, cobalt neodecanoate borate, phenolic resin, and a curing agent in 100 parts by weight of a diene rubber containing natural rubber. The carbon black has a DBP oil absorption of 50 × 10⁻⁶. -5 ~80×10 -5 m 3 / kg, iodine adsorption capacity is 100-150g / kg, and the dynamic storage modulus (E') at 2% dynamic strain and 20℃ is above 8MPa, the loss tangent (tanδ) at 60℃ is below 0.20, and the number of repetitions until failure in constant strain fatigue test at 60% strain and 400rpm is above 45,000.
[0004] Furthermore, Patent Document 2 discloses a method for bonding galvanized steel cord to rubber using a rubber composition that exhibits excellent moisture resistance and initial adhesion to galvanized steel cord, and a steel cord conveyor belt manufactured using this bonding method. The method involves bonding a rubber composition to galvanized steel cord, wherein the rubber composition, relative to 100 parts by weight of sulfur-curable rubber, contains: 3 to 15 parts by weight of rosin or rosin derivatives, 0.2 to 1.0 parts by weight of an organocobalt salt (based on cobalt content), and 3 to 50 parts by weight of an organochlorine compound.
[0005] Existing technical documents
[0006] Patent documents
[0007] Patent Document 1: Japanese Patent Application Publication No. 2018-131522
[0008] Patent Document 2: Japanese Patent No. 4449941 Summary of the Invention
[0009] The problem the invention aims to solve
[0010] On the other hand, when a conveyor belt with built-in steel cords is used in a cold region, the rubber composition used for the coated rubber layer (buffer rubber) of the steel cords in the aforementioned conveyor belt is required to have cold resistance in addition to adhesion to the steel cords.
[0011] Against this backdrop, the inventors prepared and evaluated rubber compositions with reference to Patent Document 1, etc., and the results clearly showed that such compositions had poor cold resistance and were difficult to balance durability and water-resistant adhesion (Comparative Examples 2-4).
[0012] Therefore, the object of the present invention is to provide a rubber composition for bonding steel cords that exhibits excellent cold resistance, durability, and water-resistant adhesion. It should be noted that, in the present invention, water-resistant adhesion includes moisture-resistant adhesion.
[0013] Furthermore, the present invention aims to provide a conveyor belt with excellent cold resistance, durability, and water-resistant adhesion.
[0014] Technical solution
[0015] In order to solve the above-mentioned problems, the inventors conducted in-depth research and discovered the following facts, thereby completing the present invention, namely, that the desired effect can be obtained when the rubber composition contains at least a rubber component including polybutadiene rubber and cobalt neodecanoate borate.
[0016] The present invention is based on the above-mentioned insights, and specifically, the above-mentioned problems are solved by the following configuration.
[0017] [1] A rubber composition for bonding steel cords, comprising at least a rubber component including polybutadiene rubber and cobalt neodecanoate borate.
[0018] [2] The rubber composition for bonding steel cords according to [1], wherein the rubber component further comprises natural rubber and / or styrene-butadiene copolymer rubber.
[0019] [3] The rubber composition for bonding steel cords according to [1] or [2], wherein the content of the polybutadiene rubber is 15 to 60 parts by mass relative to 100 parts by mass of the rubber component.
[0020] [4] The rubber composition for bonding steel cords according to any one of [1] to [3] further contains carbon black, wherein the content of carbon black is 35 to 75 parts by mass relative to 100 parts by mass of the rubber composition.
[0021] [5] A rubber composition for bonding steel cords according to any one of [1] to [4], wherein the content of cobalt borate neodecanoate is 1.2 to 3.5 parts by mass relative to 100 parts by mass of the rubber component.
[0022] [6] The rubber composition for bonding steel cords according to any one of [1] to [5] further comprises a vulcanization accelerator, wherein the vulcanization accelerator is a thiazole-based vulcanization accelerator.
[0023] [7] The rubber composition for bonding steel cords according to [6], wherein the content of the vulcanization accelerator is 0.3 to 1.2 parts by mass relative to 100 parts by mass of the rubber component.
[0024] [8] A rubber composition for bonding steel cords according to any one of [1] to [7], wherein sulfur is further contained in a content of 2.1 to 5.0 parts by weight relative to 100 parts by weight of the rubber composition.
[0025] [9] A rubber composition for bonding steel cords according to any one of [1] to [8], wherein it further comprises at least one selected from the group consisting of rosin, rosin derivatives, phenolic resin and chlorinated paraffin.
[0026]
[10] A rubber composition for bonding steel cords according to any one of [1] to [9], wherein zinc oxide is further contained in a content of 5.0 parts by mass or more relative to 100 parts by mass of the rubber composition.
[0027]
[11] The rubber composition for bonding steel cords according to any one of [1] to
[10] further comprises oil, wherein the content of the oil is 2.0 parts by mass or more relative to 100 parts by mass of the rubber composition.
[0028]
[12] The rubber composition for bonding steel cords according to any one of [1] to
[11] is used to bond galvanized steel cords.
[0029]
[13] A conveyor belt formed using any one of the steel cord bonding rubber compositions described in [1] to
[12] .
[0030] Beneficial effects
[0031] The rubber composition for bonding steel cords of the present invention exhibits excellent cold resistance, durability, and water-resistant bonding properties.
[0032] Furthermore, the conveyor belt of the present invention exhibits excellent cold resistance, durability, and water-resistant adhesion. Attached Figure Description
[0033] Figure 1 This is a cross-sectional perspective view schematically illustrating an example of a conveyor belt according to the present invention. Detailed Implementation
[0034] The present invention will now be described in detail.
[0035] The numerical range indicated by “~” in this specification refers to the range of values recorded before and after “~” as the lower and upper limits.
[0036] In this specification, unless otherwise specified, each component may be used alone or in combination of two or more substances that conform to this component. When a component contains two or more substances, the content of the component refers to the total content of the two or more substances.
[0037] Unless otherwise specified in this specification, there are no particular limitations on the manufacturing methods of the components. For example, conventionally known methods can be listed.
[0038] In this specification, the superiority of at least one of cold resistance, durability, and water-resistant adhesion is sometimes referred to as the superiority of the present invention.
[0039] [Rubber composition for bonding steel cords]
[0040] The rubber composition for bonding steel cords of the present invention (the composition of the present invention) is a rubber composition for bonding steel cords containing at least a rubber component comprising polybutadiene rubber and cobalt neodecanoate borate.
[0041] It can be assumed that the composition of the present invention adopts such a configuration, thus achieving the desired effect. Although the reason is not yet clear, it is roughly speculated as follows.
[0042] The composition of the present invention contains polybutadiene rubber as a rubber component, thereby enabling the embrittlement temperature to be set within a preferred range and exhibiting excellent cold resistance.
[0043] Furthermore, the inventors have discovered that when using cobalt naphthenate as an organic cobalt salt, there is a problem that the elongation at break (EB) of the rubber in the over-vulcanized state is low, which reduces the durability of the conveyor belt.
[0044] Here, over-vulcanization refers to the further vulcanization of rubber after the usual vulcanization time required during product manufacturing (after initial vulcanization). Specifically, examples of this further vulcanization include: vulcanization times longer than usual when vulcanizing unvulcanized rubber; further vulcanization of vulcanized rubber or conveyor belts during repairs; and cyclization of vulcanized rubber through further vulcanization.
[0045] Regarding the above-mentioned problems, the inventors have discovered that when using cobalt neodecanoate borate as an organic cobalt salt, water-resistant adhesion can be maintained or improved, and the durability of the conveyor belt can be enhanced.
[0046] The inventors hypothesize that, when the amount of cobalt contained in cobalt neodecanoate borate or cobalt naphthenate is set to be equal, cobalt neodecanoate borate has less organic acid content than cobalt naphthenate, thus reducing the decrease in elongation at break (EB) after oversulfurization.
[0047] Thus, the composition of the present invention contains cobalt neodecanoate borate, thereby achieving an excellent balance between durability and water-resistant adhesion.
[0048] As described above, the compositions of the present invention exhibit excellent cold resistance, durability, and water-resistant adhesion.
[0049] The components contained in the composition of the present invention will be described in detail below.
[0050] <Rubber Composition>
[0051] The compositions of the present invention contain a rubber component comprising at least polybutadiene rubber.
[0052] <Polybutadiene rubber>
[0053] There are no particular limitations on the polybutadiene rubber (butadiene rubber, also known as "BR") contained in the compositions of the present invention, as long as it is a homopolymer of butadiene. It should be noted that the above-mentioned polybutadiene rubber can also be modified.
[0054] (Weight-average molecular weight of polybutadiene rubber)
[0055] From the viewpoint that the present invention has better effects and higher extraction force (the force required to extract the steel cord from the rubber), the weight-average molecular weight of polybutadiene rubber is preferably 400,000 to 1,000,000, more preferably 450,000 to 800,000.
[0056] In this invention, the weight-average molecular weight of polybutadiene rubber is a standard polystyrene conversion value based on the measurement obtained by gel permeation chromatography (GPC) using cyclohexane as a solvent.
[0057] (Glass transition temperature of polybutadiene rubber)
[0058] From the viewpoint of achieving better results (especially cold resistance) of the present invention, the glass transition temperature of polybutadiene rubber is preferably below -50°C, and more preferably -150 to -80°C.
[0059] In this invention, the glass transition temperature can be set as follows: the value obtained by reading the inflection point from the curve obtained by measuring the change in heat flow rate at a heating temperature of 20°C / min using a differential thermal analysis device according to JIS K7121:2012.
[0060] From the viewpoint that the present invention has superior effects (especially cold resistance), that the rubber after initial vulcanization is further cross-linked due to over-vulcanization so that the rubber does not become too hard, and that the embrittlement temperature can be set within an appropriate range, the content of the above-mentioned polybutadiene rubber is preferably 15 to 60 parts by mass relative to 100 parts by mass of the above-mentioned rubber component, more preferably 20 to 50 parts by mass, even more preferably more than 20 parts by mass and less than 50 parts by mass, and particularly preferably 25 to 45 parts by mass.
[0061] (Rubber other than BR)
[0062] In addition to BR, the above-mentioned rubber components may also include other rubbers.
[0063] Other types of rubbers besides BR include, for example, natural rubber, isoprene rubber (IR), aromatic vinyl-conjugated diene copolymer rubber (e.g., styrene-butadiene copolymer rubber), acrylonitrile-butadiene rubber (NBR), butyl rubber (IIR), halogenated butyl rubber, chloroprene rubber (CR), and other diene-based rubbers.
[0064] From the viewpoint of achieving better results with the present invention, the above-mentioned rubber component preferably further includes natural rubber and / or styrene-butadiene copolymer rubber, and more preferably includes natural rubber and styrene-butadiene copolymer rubber.
[0065] Natural rubber
[0066] There are no particular limitations on the aforementioned natural rubber (NR). For example, previously known natural rubbers can be listed.
[0067] Styrene-butadiene copolymer rubber
[0068] There are no particular restrictions on the above-mentioned styrene-butadiene copolymer rubber as long as it is a copolymer of styrene and butadiene.
[0069] (The amount of styrene bound in styrene-butadiene copolymer rubber)
[0070] From the viewpoint that the effects of the present invention (especially cold resistance) are superior and the glass transition temperature of the styrene-butadiene copolymer rubber described later is lower, the amount of styrene bound in the styrene-butadiene copolymer rubber is preferably 5 to 40% by mass, more preferably 10 to 30% by mass, relative to the total amount of the styrene-butadiene copolymer rubber.
[0071] (Vinyl content of styrene-butadiene copolymer rubber)
[0072] From the viewpoint that the effects of the present invention (especially cold resistance) are superior and the glass transition temperature of the styrene-butadiene copolymer rubber described later is lower, the vinyl content of butadiene (1,2-vinyl binding content) of the styrene-butadiene copolymer rubber is preferably 5 to 30% by mass, more preferably 5 to 20% by mass, relative to the total amount of repeating butadiene units in the styrene-butadiene copolymer rubber.
[0073] In this invention, the aforementioned amount of bound styrene and vinyl content in the styrene-butadiene copolymer rubber can be determined by... 1 The measurements were performed using H-NMR.
[0074] (Glass transition temperature of styrene-butadiene copolymer rubber)
[0075] From the viewpoint of superior performance of the present invention (especially cold resistance), the glass transition temperature of the above-mentioned styrene-butadiene copolymer rubber is preferably below -50°C.
[0076] The lower limit of the glass transition temperature of the above-mentioned styrene-butadiene copolymer rubber can be set, for example, above -100°C.
[0077] The method for determining the glass transition temperature of the styrene-butadiene copolymer rubber is the same as described above.
[0078] (Weight-average molecular weight of styrene-butadiene copolymer rubber)
[0079] There are no particular limitations on the weight-average molecular weight of styrene-butadiene copolymer rubber. For example, it can be set to 200,000 to 3,000,000.
[0080] In this invention, the weight-average molecular weight of the styrene-butadiene copolymer rubber is a standard polystyrene conversion value based on the measurement obtained by gel permeation chromatography (GPC) using tetrahydrofuran as a solvent.
[0081] In the case where the rubber component includes the natural rubber and the styrene-butadiene copolymer rubber in addition to BR (all three are used together), from the viewpoint of achieving better results in this invention and setting the embrittlement temperature to an appropriate range, the content of the natural rubber is preferably 20 to 42.5 parts by mass, more preferably 25 to 40 parts by mass, relative to 100 parts by mass of the rubber component.
[0082] Furthermore, when the above three are used together, from the viewpoint of achieving better results for the present invention and setting the embrittlement temperature within an appropriate range, the content of the above-mentioned styrene-butadiene copolymer rubber is preferably 20 to 42.5 parts by mass, more preferably 25 to 40 parts by mass, relative to 100 parts by mass of the above-mentioned rubber component.
[0083] <Cobalt neodecanoate borate>
[0084] The composition of the present invention contains cobalt neodecanoate borate, which is a compound represented by the following formula (1).
[0085] The composition of the present invention contains cobalt neodecanoate borate, thereby exhibiting excellent adhesion to steel cord.
[0086] [Chemical Formula 1]
[0087]
[0088] (Content of cobalt borate in neodecanoate)
[0089] From the viewpoint that the present invention has better effects, better adhesion to steel cord, and that the rubber will not be too hard due to further cross-linking after initial vulcanization, the content of the above-mentioned cobalt borate neodecanoate is preferably 1.2 to 3.5 parts by mass relative to 100 parts by mass of the above-mentioned rubber component, more preferably more than 1.5 parts by mass and less than 2.5 parts by mass.
[0090] (Carbon black)
[0091] The compositions of the present invention may also contain carbon black.
[0092] There are no special restrictions on the carbon black mentioned above.
[0093] From the viewpoint of achieving better results in this invention, the carbon black is preferably HAF grade carbon black, ISAF grade carbon black, and more preferably HAF grade carbon black.
[0094] (Nitrogen adsorption specific surface area of carbon black)
[0095] From the viewpoint of achieving better results with the present invention, the nitrogen adsorption specific surface area (N2SA) of the above-mentioned carbon black is preferably 60 to 120 m². 2 / g, more preferably 65-95m 2 / g.
[0096] For the nitrogen adsorption specific surface area of carbon black, the amount of nitrogen adsorbed on the carbon black surface can be determined according to JIS K 6217-2:2017 "Part II: Methods for solving specific surface area - Nitrogen adsorption method - Single point method".
[0097] (Carbon black content)
[0098] From the viewpoint of achieving better results with the present invention, the content of carbon black is preferably 35 to 75 parts by mass relative to 100 parts by mass of the rubber component, and more preferably 40 to 70 parts by mass.
[0099] (Vulcanization accelerator)
[0100] The compositions of the present invention may also contain a vulcanization accelerator.
[0101] There are no particular limitations on the above-mentioned vulcanization accelerators. For example, thiazole-based, guanidine-based, thiuram-based, or sulfenamide-based vulcanization accelerators can be listed.
[0102] From the viewpoint that the present invention has better effects and is less likely to promote further crosslinking of rubber after vulcanization, the above-mentioned vulcanization accelerator is preferably a thiazole-based vulcanization accelerator, and more preferably a dibenzothiazole disulfide.
[0103] (Content of vulcanization accelerator)
[0104] From the viewpoint of achieving better results with the present invention, the content of the vulcanization accelerator is preferably 0.3 to 1.2 parts by mass relative to 100 parts by mass of the rubber component, more preferably 0.3 parts by mass or more and less than 1.0 parts by mass, and even more preferably 0.4 to 0.9 parts by mass.
[0105] (sulfur)
[0106] The compositions of the present invention may also contain sulfur. There are no particular limitations on the sulfur content.
[0107] (Sulfur content)
[0108] From the viewpoint of superior effects of the present invention (especially water-resistant adhesion), the content of sulfur is preferably 2.1 to 5.0 parts by weight, more preferably 2.5 to 4.0 parts by weight, relative to 100 parts by weight of the rubber component.
[0109] It should be noted that, relative to 100 parts by weight of the above-mentioned rubber components, the lower limit of the sulfur content can be set to 2.0 parts by weight or more.
[0110] (Mass ratio of cobalt borate to sulfur)
[0111] When the composition of the present invention also contains sulfur, from the viewpoint of better performance of the present invention and better adhesion to steel cord, the mass ratio of the content of the above-mentioned cobalt borate neodecanoate to the content of the above-mentioned sulfur (cobalt borate neodecanoate / sulfur) is preferably 0.24 (1.2 / 5) to 1.7 (3.5 / 2.1), more preferably more than 0.50 and less than 1.0, and even more preferably 0.55 to 0.80.
[0112] (Rosin, etc.)
[0113] From the viewpoint of superior performance and excellent adhesion to steel cord, the composition of the present invention preferably further contains at least one selected from the group consisting of rosin, rosin derivatives, phenolic resin and chlorinated paraffin, and more preferably, rosin or rosin derivatives, phenolic resin and chlorinated paraffin are used together.
[0114] In this specification, rosin, rosin derivatives, phenolic resins and chlorinated paraffins are sometimes collectively referred to as "rosin, etc."
[0115] The aforementioned rosin and other substances can function as adhesive agents.
[0116] · Rosin, rosin derivatives
[0117] Rosin is a type of natural resin, also known as pine resin.
[0118] Examples of rosin derivatives include gum rosin, wood rosin, tall oil rosin, polymers of these rosins, disproportionated rosin, maleic rosin, aldehyde-modified rosin, hydrogenated rosin, and their processed products.
[0119] Rosin and rosin derivatives can be used as rosin and rosin derivatives that are commonly used as tackifiers.
[0120] Commercially available products can be used as rosin or rosin derivatives. Specifically, examples include: resin rosin or wood rosin manufactured by Arakawa Chemical Industry Co., Ltd., tall oil rosin manufactured by Halima Chemical Group Co., Ltd., and hydrogenated rosin manufactured by Hercules Co., Ltd.
[0121] From the viewpoint of achieving superior effects and excellent adhesion to steel cords, the content of rosin is preferably 3 to 10 parts by weight relative to 100 parts by weight of the rubber component. The content of rosin derivatives is also the same as the content of rosin.
[0122] ·Phenolic resin
[0123] As the phenolic resin, phenolic resins that are typically compatible with rubber compositions can be used. The aforementioned phenolic resin may comprise resins obtained through the reaction of phenols and aldehydes, and their modified forms. Examples of phenols include phenol, cresol, xylenol, or resorcinol. Examples of aldehydes include formaldehyde, acetaldehyde, or furfural.
[0124] It should be noted that, as one of the preferred embodiments, the compositions of the present invention do not contain curing agents of phenolic resins.
[0125] From the viewpoint of achieving better results and superior adhesion to steel cords, the content of the phenolic resin is preferably 2 to 8 parts by mass relative to 100 parts by mass of the rubber component.
[0126] Chlorinated paraffin
[0127] There are no particular restrictions on the chlorinated paraffins mentioned above, as long as they contain chlorine. For example, chain-like saturated hydrocarbon compounds with an average of 26 carbon atoms can be listed, in which all or part of the hydrogen atoms are replaced by chlorine atoms.
[0128] The chlorine content of the chlorinated paraffins is preferably 40 to 80% by mass relative to the total amount of chlorinated paraffins.
[0129] From the viewpoint of achieving better results and superior adhesion to steel cords, the content of the chlorinated paraffin is preferably 3 to 8 parts by mass relative to 100 parts by mass of the rubber component.
[0130] (and the total content under the same conditions)
[0131] When rosin or rosin derivatives, phenolic resin and chlorinated paraffin are used together, from the viewpoint of better performance of the present invention and better adhesion to steel cord, the total content of these components is preferably 8 to 22 parts by mass relative to 100 parts by mass of the above-mentioned rubber components.
[0132] When rosin or rosin derivatives, phenolic resin and chlorinated paraffin are used together, from the viewpoint of better performance of the present invention and better adhesion to steel cord, the content of phenolic resin is preferably 10 to 40% by mass relative to their total content.
[0133] (Zinc oxide)
[0134] The compositions of the present invention may also contain zinc oxide. There are no particular limitations on the zinc oxide content.
[0135] (Zinc oxide content)
[0136] From the viewpoint of achieving better results with the present invention, the content of zinc oxide is preferably 5.0 parts by mass or more relative to 100 parts by mass of the rubber component described above.
[0137] The upper limit of the zinc oxide content can be set to 20 parts by mass or less, relative to 100 parts by mass of the aforementioned rubber component.
[0138] (Oil)
[0139] The compositions of the present invention may also contain oils. There are no particular limitations on the oils mentioned above. Examples include paraffin oils (excluding chlorinated paraffins) and aromatic oils.
[0140] (Oil content)
[0141] From the viewpoint of achieving better results with the present invention, the content of the oil is preferably 2.0 parts by mass or more relative to 100 parts by mass of the rubber component.
[0142] The upper limit of the oil content can be set to less than 10 parts by mass relative to 100 parts by mass of the rubber component mentioned above.
[0143] For the compositions of the present invention, in addition to the essential components described above, additives such as stearic acid and anti-aging agents may be included as needed without prejudice to the purpose of the present invention.
[0144] The composition of the present invention can be manufactured by mixing the above-mentioned essential components, such as the carbon black used as needed, using a roll mill or a Banbury mixer.
[0145] The compositions of the present invention can be used, for example, to bond steel cords (specifically, galvanized steel cords).
[0146] When the composition of the present invention is used with steel cord (e.g., galvanized steel cord), for example by vulcanization, a composite having vulcanized rubber and steel cord can be obtained. In the above composite, the vulcanized rubber and steel cord can be bonded together.
[0147] Examples of the aforementioned steel cords include: untreated steel cords; and steel cords that have been galvanized from untreated steel cords.
[0148] From the viewpoint of superior performance and excellent rust prevention of the present invention, the above-mentioned steel cord is preferably galvanized steel cord.
[0149] The diameter of the steel cord, such as the wire diameter or the cord diameter, can be selected appropriately.
[0150] The temperature for vulcanizing the composition of the present invention can be set to, for example, around 140 to 160°C.
[0151] From the viewpoint of superior performance of the present invention (especially cold resistance), the embrittlement temperature of the sulfide obtained by vulcanizing the composition of the present invention is preferably below -50°C, more preferably below -58°C.
[0152] In this invention, the composition of this invention is vulcanized under pressure of 153°C and 2.0 MPa for 20 minutes to obtain vulcanized rubber (sheet with a thickness of 2 mm). Using the above vulcanized rubber, the embrittlement temperature is determined according to JIS K 6261-2:2017 "Vulcanized rubber and thermoplastic rubber - methods for solving low-temperature properties - part 2: low-temperature impact embrittlement test".
[0153] The compositions of the present invention are preferably used, for example, in the manufacture of conveyor belts. When the compositions of the present invention are used in the manufacture of conveyor belts, the compositions of the present invention are preferably formed, for example, into a coated rubber layer (cushioning rubber) of coated steel cords as components constituting the conveyor belt.
[0154] [Conveyor Belt]
[0155] Next, the conveyor belt of the present invention will be described.
[0156] The conveyor belt of the present invention is a conveyor belt formed using the rubber composition for bonding steel cords of the present invention.
[0157] As a preferred embodiment, the conveyor belt of the present invention includes steel cords. From the viewpoint of further enhancing the effects of the present invention, the aforementioned steel cords are preferably galvanized steel cords that have not undergone surface treatment.
[0158] There are no particular limitations on the rubber composition for bonding steel cords used in the conveyor belt of the present invention, as long as it is the same as the rubber composition for bonding steel cords of the present invention.
[0159] From the viewpoint of achieving better results, the composition of the present invention preferably forms a coated rubber layer (buffer rubber) for coating steel cords.
[0160] As one preferred embodiment, the conveyor belt of the present invention also includes a covering rubber layer. There are no particular limitations on the rubber composition capable of forming the aforementioned covering rubber layer.
[0161] The conveyor belt of the present invention will now be described using the accompanying drawings. The conveyor belt of the present invention is not limited to the drawings.
[0162] Figure 1 This is a cross-sectional perspective view schematically illustrating an example of a conveyor belt according to the present invention.
[0163] exist Figure 1 In this embodiment, the conveyor belt 1 has a covering rubber layer 6 on two surfaces, and a steel cord 2 and a coated rubber layer 4 are located between the covering rubber layers 6. The coated rubber layer 4 coats the steel cord 2. The coated rubber layer 4 is preferably formed from the rubber composition for bonding the steel cord according to the present invention.
[0164] [Example]
[0165] The following examples illustrate the present invention in detail. However, the present invention is not limited thereto.
[0166] <Preparation of the Composition>
[0167] Use the components in the first table according to the composition (parts by mass) shown in the first table below.
[0168] First, the components shown in the first table below, except for sulfur and vulcanization accelerator, are mixed using a Banbury mixer. Then, sulfur and vulcanization accelerator are added to the resulting mixture, and they are mixed using a roll to produce the various compositions.
[0169] "evaluate"
[0170] The compositions manufactured as described above were evaluated as follows. The results are shown in Table 1.
[0171] Cold resistance
[0172] Cold resistance was evaluated using embrittlement temperature.
[0173] Evaluation methods
[0174] The above compositions were subjected to pressure vulcanization at 153°C and 2.0 MPa for 20 minutes using a pressure molding machine to obtain vulcanized rubber (sheets with a thickness of 2 mm).
[0175] According to JIS K 6261-2:2017 "Vulcanized rubber and thermoplastic rubber - Methods for solving low-temperature properties - Part II: Low-temperature impact embrittlement test", test pieces were made from the above-mentioned vulcanized rubbers, and impact bending was applied to the test pieces under specified conditions. When the test pieces were subjected to impact bending, the temperature at which 50% of the total number of test pieces failed was measured, and the temperature measured as described above was set as the "embrittlement temperature".
[0176] Evaluation Criteria
[0177] In this invention, when the embrittlement temperature is below -50°C, the cold resistance is evaluated as excellent.
[0178] When the embrittlement temperature exceeds -50℃, it is evaluated as having poor cold resistance.
[0179] The lower the embrittlement temperature is compared to -50℃, the better the cold resistance is considered.
[0180] <Durability>
[0181] Durability was evaluated using the elongation at break (EB) retention rate.
[0182] Evaluation methods
[0183] The above compositions were subjected to pressure vulcanization at 153°C and 2.0 MPa for 20 minutes using a pressure molding machine to obtain the initial vulcanized rubber.
[0184] In addition, the above-mentioned compositions (the unvulcanized rubber compositions manufactured as described above) were placed at 153°C for 90 minutes to obtain time-cured rubber.
[0185] Initial test pieces (2 mm thick) in the dumbbell shape (JIS No. 3) were punched from each of the initial vulcanized rubbers obtained as described above. Similarly, timed test pieces were obtained from each of the timed vulcanized rubbers.
[0186] According to JIS K6251:2017, tensile tests were conducted on the initial test pieces and the time-exchanged test pieces obtained as described above under the conditions of room temperature and tensile speed of 500 mm / min, and the elongation at break (EB) was determined.
[0187] Substitute the values of the elongation at break of the initial test piece and the time-expired test piece into the following formula to calculate the retention rate of the elongation at break.
[0188] Elongation at break (EB) retention rate (%) = (Elongation at break of the test piece after time) / (Elongation at break of the initial test piece) × 100
[0189] Evaluation Criteria
[0190] In this invention, when the above-mentioned elongation at break retention rate is 45% or more, it is evaluated as having excellent durability.
[0191] If the retention rate is less than 45%, the durability is rated as poor.
[0192] The higher the retention rate is (greater than 45%), the better the durability is rated.
[0193] <Water Resistance and Adhesion>
[0194] Water-resistant adhesion was evaluated using rubber adhesion rate.
[0195] Evaluation methods
[0196] Galvanized steel cord with a diameter of 4.1 mm, stored in a desiccator and treated for dust and moisture protection, was coated with the aforementioned compositions to a thickness of 15 mm, forming composites of the compositions and steel cord (with the steel cord embedded within the compositions). These composites were then pressure-cured for 20 minutes at 153°C and a surface pressure of 2.0 MPa using a pressure molding machine to produce test specimens (rubber / galvanized steel cord composites). In these test specimens, the interface between the rubber and steel cord at the point where the steel cord protrudes from the rubber surface was sealed with beeswax, and the specimens were placed in a constant temperature and humidity chamber at 50°C and 95% relative humidity for one week. Then, a pull-out test was conducted at room temperature to remove the steel cord from each test specimen. The pull-out test was performed according to DIN 22131.
[0197] After the extraction test, the condition of the extracted steel cord was confirmed, and the ratio of the area of rubber coating remaining on the surface of the extracted steel cord to the initial surface area of the steel cord was calculated (rubber coating rate, %). The rubber coating rate calculated as described above is shown as the rubber adhesion rate in the first table.
[0198] Evaluation Criteria
[0199] In this invention, when the rubber adhesion rate (rubber coverage rate) is 65% or more, it is evaluated as having excellent water resistance and adhesion.
[0200] When the rubber adhesion rate is less than 65%, it is evaluated as having poor water resistance and adhesion.
[0201] The higher the rubber adhesion rate is (greater than 65%), the better the water-resistant adhesion is considered.
[0202] [Table 1]
[0203]
[0204] Details of each component shown in the first table are as follows.
[0205] NR: Natural rubber. TSR20
[0206] • SBR: Styrene-butadiene copolymer rubber. NIPOL 1502 (manufactured by ZEON Corporation, Japan). Glass transition temperature -54℃. Weight average molecular weight 490,000, styrene content 24% by mass, vinyl content 16% by mass.
[0207] • BR: Polybutadiene rubber. Nipol BR1220, manufactured by ZEON Corporation, Japan. Weight average molecular weight 500,000, glass transition temperature -105℃
[0208] • HAF grade carbon black: SHOBLACK N330T manufactured by Cabot Japan Co., Ltd. (nitrogen adsorption specific surface area 74m²) 2 / g)
[0209] • Phenolic resins: SUMILITE RESIN PR-175, Sumitomo Durez Co., Ltd.
[0210] • Rosin: Made by China Rosin WW and Arai Chemical Industry Co., Ltd.
[0211] • Chlorinated paraffin (70% chlorine content): Chlorinated paraffin (70% chlorine content by mass). Trade name: EMPRA 70S, manufactured by Ajinomoto Fine-Techno.
[0212] • (Comparison) Cobalt naphthenate (10% cobalt content): Cobalt naphthenate. Cobalt content 10% by mass. Cobalt naphthenate 10%, manufactured by DICCORPORATION.
[0213] • Cobalt neodecanoate borate: Cobalt neodecanoate borate as shown in formula (1) below. DICNATE NBC-II (22.2% by mass) manufactured by DIC CORPORATION
[0214] [Chemical Formula 2]
[0215]
[0216] • Zinc oxide: JIS#3 zinc oxide manufactured by Zhengtong Chemical Industry Company
[0217] • Stearic acid: Stearic acid YR (manufactured by Nippon Oil Company)
[0218] • Paraffin oil: Engine oil 22 (Made by Showa Shell Oil Co., Ltd.)
[0219] • DM vulcanization accelerator: A thiazole-based vulcanization accelerator. Dibenzothiazole disulfide. (Trade names: SANCELER DM-PO, Sanshin Chemical Industry Co., Ltd.)
[0220] • Sulfur: Jinhua brand oil-containing powdered sulfur (manufactured by Tsurumi Chemical Industry Co., Ltd.)
[0221] As can be clearly seen from the results shown in Table 1, Comparative Example 1, which does not contain cobalt neodecanoate borate but instead contains cobalt naphthenate, has lower durability.
[0222] Comparative Example 2, which contains no polybutadiene rubber and whose rubber components are all natural rubber, has poor water resistance and adhesion.
[0223] The cold resistance and durability of the comparative example 3, which does not contain polybutadiene rubber, has all natural rubber components, and contains more cobalt borate and neodecanoate than comparative example 2, are poor.
[0224] Comparative Example 4, which does not contain polybutadiene rubber and cobalt neodecanoate borate, contains natural rubber and SBR instead of polybutadiene rubber, and contains cobalt naphthenate instead of cobalt neodecanoate borate, exhibits poor durability.
[0225] In contrast, the composition of the present invention exhibits superior cold resistance, durability, and water-resistant adhesion.
[0226] Symbol Explanation
[0227] 1 Conveyor Belt
[0228] 2. Steel cord
[0229] 4. Apply rubber layer
[0230] 6. Cover with a rubber layer.
Claims
1. A rubber composition for bonding steel cords, comprising rubber components, cobalt neodecanoate and borate, a vulcanization accelerator, and sulfur. The rubber component comprises: Polybutadiene rubber, and Natural rubber and styrene-butadiene copolymer rubber The vulcanization accelerator is a thiazole-based vulcanization accelerator. Relative to 100 parts by weight of the rubber component, the content of cobalt borate neodecanoate is 1.8 to 2.0 parts by weight. The content of polybutadiene rubber is 25 to 50 parts by weight relative to 100 parts by weight of the rubber component. Relative to 100 parts by weight of the rubber component, the content of the natural rubber is 25 to 42.5 parts by weight. Relative to 100 parts by weight of the rubber component, the content of the styrene-butadiene copolymer rubber is 25 to 42.5 parts by weight. The content of the vulcanization accelerator is 0.3 to 1.2 parts by weight relative to 100 parts by weight of the rubber component. The sulfur content is 2.1 to 5.0 parts by weight relative to 100 parts by weight of the rubber component.
2. The rubber composition for bonding steel cords according to claim 1, wherein, It also contains carbon black. The carbon black content is 35 to 75 parts by mass relative to 100 parts by mass of the rubber component.
3. The rubber composition for bonding steel cords according to claim 1 or 2, wherein, It also contains at least one selected from the group consisting of rosin, rosin derivatives, phenolic resins and chlorinated paraffins.
4. The rubber composition for bonding steel cords according to claim 1 or 2, wherein, It also contains zinc oxide. The content of zinc oxide is 5.0 parts by mass or more relative to 100 parts by mass of the rubber component.
5. The rubber composition for bonding steel cords according to claim 1 or 2, wherein, It also contains oil. The oil content is 2.0 parts by mass or more relative to 100 parts by mass of the rubber component.
6. The rubber composition for bonding steel cords according to claim 1 or 2, used for bonding galvanized steel cords.
7. A conveyor belt formed using a rubber composition for bonding steel cords according to any one of claims 1 to 6.
Citation Information
Patent Citations
Rubber composition for coating cord
CN101045840A
Rubber composition for conveyor belt, and conveyor belt
CN102449053A
Rubber composition for conveyor belt, and conveyor belt
CN102459449A
Rubber composition and conveyor belt
CN104837911A
Rubber composition
CN108884274A