Silicon seal for high-performance battery anode materials
Patent Information
- Application Number
- CN201980021485.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-03-30
- Filing Date
- 2019-03-18
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2039-03-18
AI Technical Summary
Existing nanostructured silicon anodes suffer from poor mechanical stability, low Coulombic efficiency, and easy collapse during the rolling process when manufacturing high-area capacity battery electrodes, resulting in poor volumetric energy density and cycle stability.
Using a porous silicon microstructure precursor, a dense silicon shell coating is deposited, and a graphene coating is encapsulated on the silicon shell to form a graphene-encapsulated silicon shell protective structure to improve mechanical stability and Coulomb efficiency while providing The void space accommodates volume expansion.
The mechanical stability and Coulomb efficiency are significantly improved, the voltage resistance and cycle stability of the electrode are enhanced, and high capacity density and long cycle life are achieved.
Smart Images

Figure CN112204766B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority to U.S. Provisional Patent Application No. 62 / 650,576, filed on March 30, 2018, which is incorporated herein by reference.
[0003] Statement of Government Funding Support
[0004] This invention was made with government support under Contract DE-AC02-76SF00515 awarded by the U.S. Department of Energy. The government has certain rights in this invention. Technical Field
[0005] The present invention generally relates to battery electrodes. More specifically, the present invention relates to silicon hollow structure battery electrodes protected by a graphene-encapsulated silicon shell. Background Art
[0006] Nanostructured silicon shows great potential in solving the volume expansion of silicon anodes during cycling. However, there are new challenges regarding excessive surface area and poor Coulombic efficiency. Using nanounits to construct microstructures can solve these problems to a certain extent. Unfortunately, the Coulombic efficiency is still unsatisfactory, and the constructed microstructures often suffer from poor mechanical stability and easily collapse during the calendering process, limiting their application in the manufacture of high areal capacity anodes.
[0007] For example, over the past decade, research on high-capacity silicon anodes through nanostructure design has created exciting hopes for high-energy batteries. Many challenging issues associated with the 300% volume change of silicon anodes have been addressed through structures including nanowires, core-shell, yolk-shell tubes, hollow and porous spheres, pomegranate particles, and new binders. The basic concept of these most promising nanostructured silicon anodes is the pre-reserved hollow space to accommodate large volume changes to reduce damage to the electrode. However, challenges remain, namely that voids such as gaps between carbon shells and silicon microparticles and / or the entire nanostructure cannot withstand large mechanical pressure during the calendaring process of battery electrode manufacturing.
[0008] The calendaring process is an extremely important step in the manufacture of battery electrodes, which densely packs electrode materials to increase the energy density per unit volume, improve the electrical contact between particles, and increase the adhesion between particles and the current collector. The mechanical pressure during the calendaring process can be as high as 80 MPa, at which pressure most hollow nanostructures will break. To date, many nanostructured electrode processing can only be done without or with a gentle calendaring process, resulting in lower volumetric energy density, poor electrical contact, and lower areal capacity loading.
[0009] In another example, high-capacity Si suffers from rapid capacity decay due to large volume expansion, which causes mechanical cracking, electrical contact loss, and unstable solid electrolyte interface (SEI). In the past decade, nanostructures have been shown to effectively solve these problems. However, new problems of high processing cost and poor Coulombic efficiency remain to be solved.
[0010] Si is widely considered to be one of the most promising anode materials for next-generation lithium-ion batteries (LIBs) with high energy density and long cycle life due to its naturally abundant properties and theoretical specific capacity that is 10 times that of commercially available graphite anodes. However, Si suffers from rapid capacity decay due to large volume expansion (~300%) during battery operation, which leads to mechanical fracture, unstable solid electrolyte interface (SEI), and loss of inter-particle electrical contact.
[0011] Attempts have been made to address these issues using concepts from Si materials. For example, various nanostructures such as core-shell Si nanowires, porous Si, and Si / C composites have been developed, considering that fracture toughness is greatly improved when the material size is reduced to the nanoscale. In addition, the design of internal void space to accommodate volume expansion has been demonstrated in hollow particles and tubes, and further demonstrated by yolk-shell Si@void@C and pomegranate structures. Although these two concepts have achieved impressive improvements, new challenges have been introduced: the high cost of synthesized nanostructured Si for stable cycling, and low Coulombic efficiency in the first and / or late cycles. Recent work on non-filled C-Si structures showed higher late cycle Coulombic efficiency, but still suffered from low initial Coulombic efficiency (ICE). The low ICE is caused by severe electrode / electrolyte interface side reactions, which are caused by the large available surface area and irreversible capture of lithium by dangling bonds of the amorphous carbon coating.
[0012] A pressure-tolerant silicon structure is needed that can significantly improve mechanical stability while providing void space to accommodate volume expansion and greatly enhance Coulombic efficiency. Summary of the invention
[0013] In order to meet the needs of the art, the present invention provides a battery electrode, which includes: a porous silicon microstructure precursor, a silicon shell coating deposited on the silicon microstructure precursor, and a graphene coating deposited on the silicon shell coating, wherein the graphene coating encapsulates the silicon shell coating to form a porous silicon microstructure precursor battery electrode protected by a graphene-encapsulated silicon shell.
[0014] According to one aspect of the present invention, the porous silicon microstructure precursor includes Si mesoporous particles or Si nanoparticle clusters.
[0015] In another aspect of the present invention, the porous silicon microstructure precursor comprises an annealed porous silicon microstructure precursor.
[0016] In another aspect of the present invention, the density of the silicon shell coating is higher than the density of the porous silicon microstructure precursor.
[0017] In yet another aspect of the present invention, the silicon shell coating has a sealing structure, wherein the sealing structure is configured to prevent the electrolyte from diffusing into the porous silicon microstructure precursor and to limit the formation of a solid electrolyte interface on the surface of the porous silicon microstructure precursor.
[0018] According to one aspect of the present invention, the silicon shell coating comprises a sealing structure configured to withstand the pressure of a calendaring process, wherein the mechanical strength of the silicon shell coating is greater than the mechanical strength of the porous silicon microstructure precursor. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figures 1A-1C The fabrication and advantages of shell-protected secondary silicon nanostructures are shown, including: (1A) Schematic diagram of the fabrication process; (1B-1C) Comparison of SEI formation and calendering tests between uncoated and Si shell-coated Si NP clusters; (1B) Uncoated Si NP clusters: electrolyte can diffuse into the internal pores, leading to excessive SEI formation; the structure can easily collapse during the calendering process, resulting in electrical contact loss; (1C) After Si shell coating: electrolyte is prevented from leaking into the internal space, thereby limiting SEI formation to the outer surface; More impressively, according to an embodiment of the present invention, the structure becomes highly pressure-resistant and remains intact below 100 MPa.
[0020] Figure 2A-2O Morphological and structural features, including schematic (2A, 2F, 2K), SEM (2B, 2C, 2G, 2H, 2L, 2M), FIB-SEM (2D, 2I, 2N), and TEM (2E, 2J, 2O) images of Si NP clusters (2A-2E), Si NP clusters@Si microparticles (2F-2J), and Si NP clusters@Si@G microparticles are shown. The scale bars in images (2B, 2G, and 2L) are 2 μm. The scale bars in other images are 1 μm. The inset in image (2N) is an SEM image of a single Si NP cluster@Si@G microparticle showing the surface of the microparticle, with a scale bar of 500 nm. The inset in image (2O) is a high-resolution TEM image of the hierarchical structure of the graphene cage according to the present invention, with a scale bar of 20 nm.
[0021] Figures 3A-3MThe pressure resistance test is shown, including: (3A, 3E, 3I) schematic diagrams of uncoated (3A), Si NP clusters coated with 100 nm Si skin (3E) and 200 nm Si skin (3I) after calendering; (3B-3D) SEM images of uncoated Si NP clusters after pressing at (3B) 0 MPa, (3C) 3 MPa, (3D) 15 MPa. (3F-3H), SEM images of Si NP clusters coated with 100 nm Si skin after pressing at (3F) 0 MPa, (3G) 15 MPa, (3H) 60 MPa. jl, SEM images of Si NP clusters coated with 200 nm Si skin after pressing at (3J) 0 MPa, (3K) 60 MPa, (3L) 100 MPa. (The scale bars in 3B-3D, 3F-3H, and 3J-3L are 2 μm. (3M) The fraction of unruptured spheres after pressure application versus applied pressure according to the present invention.
[0022] Figures 4A-4I Electrochemical characterization is shown, which includes all specific capacities reported based on the total mass of active materials (Si and C in Si NP clusters@G and Si NP clusters@Si@G microparticles). (4A) First cycle voltage curve of a single cell with corresponding coulombic efficiency. (4B) AC impedance spectrum of the resulting Si microparticle film anode at the first cycle. To better evaluate the electrochemical performance of Si NP clusters@Si@G microparticles, the AC impedance spectrum at the 100th cycle was also tested. (4C) Half-cell delithiation capabilities of different products. For Si NP clusters@G and Si NP clusters@Si@G samples, no conductive additives were added. For the bare Si NP clusters@Si sample, super P was added as a conductive additive. The mass loading of active materials was about 0.6 mg cm -2 The first three cycles were performed at a rate of C / 20, and the later cycles were performed at a rate of C / 2 (1C = 4.2 A g -1 ). The Coulombic efficiency of Si NP clusters@Si@G is plotted on the secondary y-axis. (4D) Schematic diagram of the in situ TEM setup. (4E, 4F) Time-lapse images of the lithiation of (4E) Si NP clusters@Si microparticles (see also Supplementary Video 1) and (4F) Si NP clusters@Si@G microparticles (see also Supplementary Video 2). The scale bar for all time-lapse images is 1 μm. (4G, 4H) Cross-sectional SEM images of Si NP clusters@Si without (4G) and with (4H) graphene encapsulation. Electrodes before (left) and after (right) cycling testing. (4I) Full-cell delithiation capability of Si NP clusters@Si@G microparticles paired with a conventional lithium cobalt oxide cathode. According to the present invention, the Coulombic efficiency of Si NP clusters@Si@G microparticles is plotted on the secondary y-axis.
[0023] Figure 5A-5B The design of Si skin coating on mesoporous Si particles is shown, (5A) without Si skin coating, the electrolyte diffuses into the internal pores, resulting in excessive SEI formation inside and outside, and the initial Coulombic efficiency (ICE) is as low as 37.6%, and (5A) according to the present invention, after coating the Si skin, the electrolyte is prevented from diffusing into the internal space, thereby limiting SEI formation to the outer surface and greatly improving the ICE to 87.5%.
[0024] Figures 6A-6M The following fabrication processes and characterizations are shown: (6A) Schematic diagram of the fabrication process of Mp-Si@Si@G particles. SEM (6B-6E) and TEM (6F-6I) images of annealed SiO particles (6B, 6F), Mp-Si particles (6C, 6G), Mp-Si@Si particles (6D, 6H), and Mp-Si@Si@G particles (6E, 6I). The inset is a magnified SEM image showing the surface of the particles, with a scale bar of 500 nm. (6J) XRD pattern of annealed SiO particles before and after HF etching. (6K, 6J) FIB-SEM characterization of Mp-Si particles without (6K) and with (6I) silicon encapsulation. (6M) High-resolution TEM image of the hierarchical structure of graphene cages according to the present invention.
[0025] Figures 7A-7D In situ TEM characterization during lithiation is shown: (7A, 7C), schematic diagram of the in situ TEM setup, (7B, 7D) time-lapse images of lithiation of dense Si microparticles (see Supplementary Movie 1) and Mp-Si@Si@G microparticles (see Supplementary Movie 2), (7B) for dense Si microparticles, the Si structure is violently broken due to the huge volume expansion, and the broken fragments are randomly scattered and lose contact with each other, (7D) for Mp-Si@Si@G microparticles, the Si structure is well maintained because the internal pores can provide enough space to accommodate the expansion. According to the present invention, during the entire lithiation process, the Si microparticles stay in the mechanically strong graphene cage, which remains intact throughout the highly anisotropic process.
[0026] Figures 8A-8FElectrochemical characteristics are shown, where all specific capacities are reported based on the total mass of active materials (Si and C in Mp-Si@G and Mp-Si@Si@G), (8A) the first cycle voltage curve of a single cell with corresponding coulombic efficiency, (8B) the AC impedance spectrum of the produced Si microparticle electrode at the first cycle. In order to better evaluate the electrochemical performance of Mp-Si@Si@G microparticles, the AC impedance spectrum of the 100th cycle was also tested, (8C) the half-cell delithiation ability of Mp-Si after different surface engineering treatments. For Mp-Si@G and Mp-Si@Si@G samples, no conductive additives were added. For bare Mp-Si and Mp-Si@Si samples, Super P was added as a conductive additive. The mass loading of active materials is about 0.68 mgcm -2 The first three cycles were performed at a rate of C / 20, and the later cycles were performed at a rate of C / 2 (1C = 4.2 A g -2 ). The Coulombic efficiency of Mp-Si@Si@G is plotted on the secondary y-axis. (8D, 8E) Cross-sectional SEM images of Mp-Si@Si (8D) and Mp-Si@Si@G (8E) electrodes before (left) and after (right) cycling testing, (8F) Full-cell delithiation capability of Mp-Si@Si@G microparticles paired with a conventional lithium cobalt oxide cathode. The Coulombic efficiency of Mp-Si@Si@G microparticles is plotted on the secondary y-axis according to the present invention.
[0027] Detailed Description
[0028] In order to meet the needs of the art, the present invention provides a battery electrode material, which includes a porous silicon microstructure precursor, a silicon shell coating deposited on the silicon microstructure precursor, and a graphene coating deposited on the silicon shell coating, wherein the graphene coating encapsulates the silicon shell coating to form a porous silicon microstructure precursor battery electrode protected by a graphene-encapsulated silicon shell. According to one embodiment, a pressure-resistant silicon hollow structure is provided by depositing silicon onto a silicon porous structure (precursor). The silicon shell significantly improves mechanical stability, while the porous internal structure provides void space to overcome volume expansion during cycling. Such a hollow structure can withstand high pressure and remain good after the calendering process. In addition, the silicon shell also reduces the surface area, thereby greatly improving the initial Coulomb efficiency.
[0029] Some advantages of the high performance materials according to the present invention reduce the accessible surface area and minimize side reactions. The present invention increases the initial coulombic efficiency and increases the mechanical stability and further increases the tap density and volume capacity density, thereby enabling scalable and adaptable manufacturing. The present invention can be combined with standard equipment and procedures and can be used as a diffusion-controlled surface coating or compression coating. Other advantages of silicon anodes include silicon sealing so that silicon can be used as a rechargeable anode material in batteries, which has the following characteristics: compared with lithium metal, the theoretical capacity is more than 10 times higher than the low potential of graphite (gravity).
[0030] The technology can be extended to other anode materials, including graphite, tin, germanium and oxides. In addition to being sealed with silicon, the porous / hollow structure can also be coated with carbon, tin, germanium and oxides.
[0031] In one aspect of the present invention, a surface engineering strategy is provided, which deposits a dense silicon skin onto each mesoporous Si particle precursor structure and further encapsulates it with a conformal graphene cage. The Si skin reduces the accessible surface area and minimizes side reactions, resulting in an initial Coulombic efficiency that is more than twice that without the Si skin coating. The graphene encapsulation, combined with sufficient internal voids for Si expansion, ensures structural integrity and stable SEI formation, resulting in high late-cycle Coulombic efficiency (99.8-100% for late-cycles) and excellent cycle stability.
[0032] The coulombic efficiency provided by the devices currently known in the art is still unsatisfactory, and the constructed microstructures often suffer from poor mechanical stability and easily collapse during the calendering process, thereby limiting their application in the manufacture of high area capacity anodes. In the present invention, the porous silicon nanostructure is sealed with silicon through a CVD process, thereby forming a concentrated coating on the surface. Due to the porous internal structure, the structure overcomes the volume expansion during the cycle. Moreover, the concentrated coating reduces the surface area and minimizes side reactions, thereby improving the initial coulombic efficiency. The coating also improves mechanical stability and resists high pressures exceeding 100 MPa, and remains in good condition after the calendering process, which is crucial for anode production.
[0033] According to the present invention, a pressure-resistant silicon structure is provided by engineering a dense silicon shell coating onto secondary micron-sized particles, each of which has many silicon nanoparticles. The silicon skin acts as a strong outer shell that can significantly improve mechanical stability, while the internal porous structure provides void space to accommodate volume expansion. This structure can resist high pressures exceeding 100 MPa and holds up well after the calendering process, showing 2,041 mAh cm -3In addition, the dense silicon shell also reduces the surface area, thus greatly improving the initial Coulombic efficiency. The silicon hollow structure is further encapsulated with a graphene cage, allowing the silicon core to expand in the cage while maintaining electrical contact. The silicon hollow structure has a first cycle Coulombic efficiency of up to 90.4% in the full battery, and the later Coulombic efficiency quickly rises to >99.5%, with excellent stability.
[0034] Turning now to the fabrication of shell-protected secondary silicon nanostructures and their advantages, Figure 1A The process flow of how we synthesized this structure is shown. Micrometer-sized silicon clusters were synthesized from silicon nanoparticles using a bottom-up microemulsion approach. The outer surface of each silicon cluster was then sealed with a dense silicon shell by a chemical vapor deposition (CVD) method and further encapsulated with highly conformal graphene cages by chemical deposition of a Ni template and subsequent CVD growth of graphene. After etching away the Ni template, a silicon hollow structure protected by a graphene-encapsulated silicon shell was obtained.
[0035] This novel design has several advantages: (1) The silica shell significantly improves the mechanical stability, enabling the structure to withstand high pressures of 100 MPa and survive the calendering process ( Figure 1B-1C ), the electrical contact and capacity are improved after calendering; (2) the silicon shell also increases the tap density. After the nanoparticles are assembled into clusters, the tap density increases from 0.14 g cm -3 Increased to 0.47 gcm -3 , and the tap density further increased to 0.79 g cm after the silica shell coating was formed. -3 (3) The dense silica shell prevents the electrolyte from diffusing into the internal pores, thereby reducing side reactions and SEI formation, thereby improving the first and later cycle Coulombic efficiency ( Figure 1B-1C ); (4) the internal porous structure provides void space to accommodate large volume expansion, thereby achieving good cycling stability; (5) the graphene cage external coating has mechanical strength and flexibility, ensuring a stable interface layer with the electrolyte and maintaining structural integrity during cycling.
[0036] Regarding morphological and structural characterization, Figure 2A-2O The morphology and structure of the products obtained at different steps during the synthesis are shown in Figure 1. Silicon clusters composed of silicon nanoparticles (Si NP clusters) are highly spherical with diameters ranging from 1 to 5 µm ( Figure 2A-2E), and has many internal pores as clearly shown by focused ion beam (FIB) scanning electron microscopy (SEM) and transmission electron microscopy (TEM) images. A dense silicon shell was deposited onto each cluster by CVD treatment (SiNP clusters@Si). The well-defined silicon shell should be able to fully seal the silicon clusters while still maintaining internal void space. After a short coating time at low pressure, both the inside and outside of the clusters were partially coated, allowing the electrolyte to leak from the unsealed pores into the interior of the clusters, resulting in a low initial Coulombic efficiency (ICE). However, after long-term low-pressure coating, both the inside and outside of the clusters were completely sealed, with no void space to buffer the volume expansion, resulting in poor cycling stability. After coating at higher pressure for a suitable time, the surface of the clusters was completely covered, while the internal pores were barely sealed ( Fig.2I ), thereby preventing the infiltration of electrolyte while still allowing the internal pores to buffer the expansion of the structure during repeated charge / discharge cycles. The thickness of the outer silicon shell is ~200 nm, which only covers the outer layer of the particle while retaining the highly porous interior. In order to better improve the electrochemical performance, the Si NP clusters@Si particles are further encapsulated with graphene cages. Each Si NP cluster@Si particle is first covered with a layer of Ni, which not only catalyzes the growth of graphene at low temperature, but also serves as a sacrificial layer to provide void space. After the Ni is etched away by FeCl3 aqueous solution, graphene-encapsulated Si NP clusters@Si particles are obtained as the final product (Si NP clusters@Si@G) ( Figure 2K-2O ). To better verify the advantages of our Si NP clusters@Si@G microparticles, Si NP clusters without silicon shell coating and encapsulated only with graphene cages (Si NP clusters@G) were also prepared. The multilayer structure of the graphene cages can be clearly observed by high-resolution TEM (HRTEM) images (see Fig.2O ). Raman spectroscopy also revealed the highly graphitic nature of the carbon shell, where a distinct D band with a narrow bandwidth indicated the presence of sufficient defects to facilitate the migration of lithium ions into silicon. Thermogravimetric analysis (TGA) showed that the graphene cages accounted for only ~8% of the total mass of the Si NP clusters@Si@G composites (~11% for the Si NP clusters@G composites). Here, the lower carbon content compared to previous work is believed to minimize the irreversible trapping of lithium ions by the graphene structure and improve the Coulombic efficiency without sacrificing the specific capacity.
[0037] For the voltage resistance test, as mentioned above, the calendering process in the battery electrode manufacturing process is very important, which can increase the volume energy density, improve the electrical contact and increase the adhesion between the particles and the current collector. Unfortunately, most previous hollow nanostructures have poor mechanical stability and easily collapse during the calendering process, resulting in low volume energy density, electrical contact loss, poor cycle stability and limited practical applications. According to the present invention, by depositing a dense silicon shell on each silicon cluster, the mechanical properties of the particles are greatly improved ( Figure 3J-3M ). The uncoated Si NP clusters partially ruptured at a rather low pressure of 3 MPa (about 20% of the clusters ruptured, Figure 3C ), while it completely collapsed at 15 MPa ( Figure 3D In contrast, after coating with a 100 nm silica shell, the particles barely break at 15 MPa ( Figure 3G ), however, about 45% collapsed at 60 MPa ( Figure 3H Impressively, after coating with a 200 nm silica shell, the structure and shape of the particles remained almost unchanged even at a higher pressure of 100 MPa ( Fig. 3I ). In addition, this result holds true for the actual calendering process on both Si NP clusters@G microparticles and Si NP clusters@Si@G microparticles. After the calendering process, the structure of Si NP clusters@Si@G microparticles remains intact, while Si NP clusters@G microspheres completely collapse, which clearly demonstrates the voltage-resistance superiority of these shell-protected secondary silicon nanostructures and their applicability in the fabrication of high-capacity electrodes.
[0038] Regarding electrochemical properties, the shell-protected pressure-resistant silicon hollow structures of the present invention show remarkable electrochemical performance in both half-cell and full-cell configurations. 2032-type button cells were constructed for cycling tests from 0.01 to 1 V (half-cell) and 3.0 to 4.2 V (full-cell).
[0039] exist Figure 4A The voltage curves of the first cycle of Si NP clusters@Si@G, Si NP clusters@Si, and Si NP clusters@G microparticle electrodes were compared in Figure 2. They all showed typical electrochemical characteristics of silicon. Impressively, the initial Coulombic efficiency of the Si NP clusters@Si@G microparticle electrode was 90.4%, which was better than the other two electrodes. It is worth noting that Coulombic efficiency is one of the most important parameters for evaluating battery performance, especially for batteries in the early cycles, which is responsible for most of the lithium ion loss and electrolyte consumption. Surprisingly, compared with other high-performance nano-Si anodes that usually require many cycles to reach 99%, the Coulombic efficiency of SiNP clusters@Si@G microparticles exceeded 99% after only 8 cycles ( Figure 4C), and remained at a high level (99.5-100%) thereafter.
[0040] Two features of the pressure-tolerant Si hollow structure contribute to the improved early and late cycle Coulombic efficiency: the surface chemistry allows initial SEI formation without excessive lithium consumption, and the mechanically stable electrode / electrolyte interface prevents the formation of additional SEI. First, the Si shell greatly reduces the surface area accessible to the electrolyte, minimizing possible side reactions and irreversible lithium consumption. The specific surface area of Si NP clusters@Si is about five times lower than that of Si nanoparticles (5.6 vs 29.3 m 2 / g) (the actual contact area between the uncoated Si NP cluster electrode and the electrolyte is similar to that between Si nanoparticles and the electrolyte (considering that the uncoated Si NP clusters collapse into nanoparticles after the calendering process)), resulting in less SEI formation and higher ICE generation. Second, encapsulating the Si NP clusters@Si@G microparticles with mechanically strong graphene ensures a stable electrode / electrolyte interface and prevents additional SEI formation. In addition, the Si NP clusters@Si@G microparticles electrode exhibits much faster kinetics than the other electrodes and shows excellent stability even after 100 cycles ( Figure 4B , electrochemical impedance spectroscopy test), which indicates that the SEI layer remains stable during the entire cycle of the Si NP cluster@Si@G microparticle electrode, thereby achieving a high late-stage Coulombic efficiency.
[0041] Specific capacity and cycle stability are two other very important parameters for evaluating actual batteries. Figure 4C As shown, through the Si NP cluster@Si@G microparticle electrode, at a current density of C / 20 (1C = 4.2 A g -1 ) obtained about 3,096 mAh g -1 If not mentioned, all reported capacities are based on the total mass of Si and C in the composite. Considering that silicon accounts for 92% of the composite mass, the specific capacity relative to silicon is as high as 3,365 mAh g -1 The calculated capacity is 2,041 mAh cm -3 , is 600 mAh cm obtained with graphite anode -3 The high capacity indicates that the active materials are well electrically connected and fully participate in the electrochemical lithiation / delithiation process. In addition, after 300 consecutive cycles at a high C / 2 rate, about 1,388 mAh g -1 The specific capacity is still the theoretical capacity of commercial graphite anode (372 mAh g -1) more than three times that of Si NP clusters@Si (373 mAh g at the 50th cycle). -1 ) and Si NP clusters@G (689 mAh g at the 300th cycle -1 ).
[0042] The excellent electrochemical stability can be attributed to two advantages of the Si NP cluster@Si@G composite: (1) the porous internal structure provides void space to accommodate the volume expansion during cycling; (2) the graphene shell acts as a mechanically strong and flexible buffer layer during deep galvanostatic cycling, limiting the expansion of the particles mainly to the interior and maintaining electrical contact, thereby improving the cycling stability.
[0043] To verify the compatibility of our Si NP clusters@Si@G structures with the dramatic volume expansion of Si lithiation, in situ TEM studies were performed to compare Si NP clusters@Si and Si NP clusters@Si@G microparticles. Si NP clusters@Si microparticles expanded significantly inwards and outwards during lithiation, and the random and violent expansion eventually led to structural fracture. For Si NP clusters@Si@G microparticles, the mechanically strong graphene cages restricted the internal silicon particles to expand mainly inwards and ensured the structural integrity during the entire lithiation process, resulting in good cycling stability.
[0044] To further investigate the reasons for such good cycling stability, post-cycling cross-sectional SEM analysis was performed to examine the morphological changes of the silicon electrode after charge and discharge. Figure 4G and Figure 4H As shown in the inserted image, the spherical shape of Si NP clusters@Si particles becomes irregular after cycling, indicating strong volume expansion and structural rupture; in contrast, Si NP clusters@Si@G particles remain spherical and intact after cycling, indicating good stability. Moreover, the volume expansion of the Si NP clusters@Si@G particle electrode is calculated to be only 13.7% (~81.4% for Si NP clusters@Si particles).
[0045] In addition to half-cells, full cells with high mass loading and areal capacity were constructed to better characterize the voltage resistance and good cycling stability of the Si NP clusters@Si@G composites. The areal capacities of the Si anode and conventional lithium cobalt oxide (LCO) cathode were initially matched (Li matching). Fig. 4I As shown in Figure 2, the Si NP cluster@Si@G microparticle electrode has a conductivity of 1.4 mA cm -2 The results show stable cycling at a current density of 2.1 mAh cm-2 (2.1 mAh cm-2 retained after 100 cycles) -2 ) and high Coulombic efficiency (99.7% on average after the fifth cycle).
[0046] Demonstrated here is a multifunctional silicon shell coating on a secondary silicon nanostructure that not only significantly improves the mechanical stability of the silicon structure to withstand a high voltage of 100 MPa, but also achieves a high capacity of 2,041 mAh cm -3 Not only does the silicon shell wrap only the outer surface of the silicon structure, but it also reduces the accessible surface area and prevents excessive SEI formation to achieve higher initial Coulombic efficiency. In addition, the silicon shell only wraps the outer surface of the silicon structure, retaining the porous internal structure to provide void space for buffering volume expansion during cycling, thereby improving the cycling stability. After further encapsulation with graphene cages, which restrict the silicon microparticles to expand mainly inward and maintain electrical connections, these shell-protected silicon secondary nanostructures show high Coulombic efficiency and good stability even during full battery cycling. This extraordinary high capacity and cycling stability of micro-silicon anode materials demonstrates the broad application prospects of our shell-protected pressure-resistant silicon hollow structures in the lithium battery industry.
[0047] We now turn to the assembly of Si nanoparticles into clusters based on microemulsion. Here, 10 g of Si nanoparticles (SiNP, ~80 nm, MTI, Inc.) were first dispersed in 500 mL of water (~2 wt% of Si in water) by ultrasound. The obtained Si aqueous dispersion (25 mL) was mixed with 100 mL of 1-octadecene (ODE, Aldrich) solution containing 0.6 wt% of an emulsion stabilizer (amphiphilic block copolymer, Hypermer 2524, Croda USA) and homogenized at 7000 rpm for 1 min. The mixture was then heated at 95–98 °C for 4 h. After evaporation of the water, the Si nanoparticle clusters were collected by centrifugation and washed once with cyclohexane. The final powder was calcined at 800 °C for 2 h in argon to remove organic matter and stabilize the clusters.
[0048] Regarding the synthesis of silicon-sealed Si NP clusters (Si NP clusters @Si) microparticles, Si nanoparticle clusters (Si NP clusters) were sealed with silicon by chemical vapor deposition (CVD). In a typical process, the Si NP clusters were transferred to a tube furnace (ThermoElectron Corporation) and then purged with high-purity Ar gas. The tube was then heated to 550°C at a heating rate of 50°C / min. After that, pure Ar gas and silane gas were introduced into the tube at a total pressure of 40-100 Torr, and the partial pressure of silane was 0.3 Torr / jump. After reacting at 550°C for 15-60 minutes, the silane gas was cut off and the tube was cooled under an Ar atmosphere. Finally, the Si-sealed mesoporous silicon microparticles were collected after the temperature was below 50°C.
[0049] To synthesize graphene-encapsulated Si NP clusters@Si (Si NP clusters@Si@G) microparticles, to obtain a conformal Ni coating, the surface of the Si NP clusters@Si microparticles must be densely coated with nucleation seeds (Pd in this case). As a surface adhesion layer, (3-aminopropyl)triethoxysilane (APTES) was used to sensitize the Si surface with –NH2 groups, and then Pd metal seeds were reduced from solution onto Si.
[0050] 1 g of the prepared Si NP clusters @Si microparticles was dispersed in 100 ml of isopropanol and sonicated for about 15 min. 1 ml of APTES (99% purity, Sigma-Aldrich) and 100 ul of distilled water were added to the isopropanol solution in sequence and stirred at 70 °C for 1 h. After that, a very thin layer of –NH2 groups was formed on the surface of the silicon microparticles. The samples were collected by centrifugation and then washed three times with deionized water. The particles were then immersed in 30 ml of palladium chloride aqueous solution (0.5 g / L PdCl2; 2.5 ml / L concentrated HCl; Sigma-Aldrich) and stirred for 15 min. After washing three times with deionized water, activated Si NP clusters @Si microparticles were obtained.
[0051] Two electroless nickel plating solutions were prepared: a primary solution (20 g / L nickel sulfate hexahydrate; 10 g / L citric acid dihydrate; 5 g / L lactic acid) and a secondary solution with double the concentration of components (40 g / L nickel sulfate hexahydrate; 20 g / L sodium citrate dihydrate; 10 g / L lactic acid). The activated Si NP clusters@Si microparticles were sequentially immersed in these EN solutions.
[0052] Prior to the first chemical deposition, 2 g of dimethylamine borane (DMAB; Sigma-Aldrich) and 2 ml of ammonium hydroxide (NH3·H2O, Sigma-Aldrich, 28%) were added to 360 ml of the primary EN solution. pH-sensitive DMAB was used as a reducing agent during the electroless nickel plating process. Then 1 g of the activated Si NP clusters@Si microparticles was added to the primary EN solution and gently stirred for about 30 min. As the reaction proceeded, bubbles began to appear and the color of the green EN solution became lighter. After the deposition was completed, the Si NP clusters@Si@1xNi settled to the bottom. While holding the Si NP clusters Si@1xNi particles at the bottom of the container with a magnet, the exhausted EN plating solution was carefully poured out. In another container, 4 g of DMAB and 4 ml of ammonium hydroxide were added to 360 ml of the secondary EN solution. This was then immediately added to the wet particles (Si NP clusters@Si@1xNi) and stirred for another 30 min. The resulting Si NP clusters@Si@2xNi particles were washed twice with ethanol.
[0053] For graphene encapsulation, Si NP clusters@Si@2xNi particles were dispersed in 150 ml triethylene glycol (Santa Cruz Biotechnology) and 500 ml NaOH aqueous solution (50%, w / w). After stirring at 185 °C for 8 h, the carburized Si NP clusters@Si@2xNi particles were collected by centrifugation and washed with ethanol three times. The carburization process occurs when the organic solvent decomposes, allowing carbon atoms to diffuse into the Ni layer and adhere to the surface. This triggers low-temperature graphene growth on the Si NP clusters@Si@2xNi particles. The samples were then dried in a vacuum oven at 50 °C for 1 h. The dried particles were placed in a tube furnace with the following temperature profile: heating to 450 °C at a rate of 15 °C / min; keeping the temperature at 450 °C for 1 h. The Ar flow rate was maintained at 80 sccm throughout the annealing process. The dual-purpose Ni template was etched away by immersing the annealed particles in 1 M FeCl3 (2 h) aqueous solution. After washing with 1 M HCL aqueous solution and deionized water for three times and drying in a vacuum oven at 60 °C for 1 h, graphene-encapsulated Si NP clusters@Si microparticles were obtained.
[0054] Regarding material characterization, the weight percentages of Si and C in Si NP clusters@Si@G and Si NP clusters@G were determined from weight loss curves measured on a TG / DTA instrument (Netzsch STA 449) at a heating rate of 5 °C / min in a simulated air atmosphere (20% O2 + 80% Ar). Under these conditions, the mass gain is due to slight Si oxidation, while the oxidation of carbon to gaseous species results in mass loss. To separate these two processes, a bare Si control sample was measured under the same heating conditions and the mass gain was subtracted from the Si NP clusters@Si@G and Si NP clusters@G curves. Additional characterizations were performed using scanning electron microscopy (FEI Sirion, Nova NanoSEM), transmission electron microscopy (FEI Tecnai, Titan), X-ray photoelectron spectroscopy (SSI S-ProbeMonochromatized, Al Kα radiation at 1486 eV), electrochemical impedance spectroscopy (BioLogic VMP3), and Raman spectroscopy (Horiba JY).
[0055] For in situ TEM characterization, a piezoelectrically controlled electrically biased TEM-AFM holder (NanofactoryInstruments) was used to observe the lithiation process of Si NP clusters@Si@G and Si NP clusters@Si microparticles. Li metal and Si microparticles were dispersed on 0.25 mm W and Cu wires, respectively. They were then contacted by a piezoelectric controller. By applying a bias of -3 V, Li ions flowed through the native oxide / nitride of Li metal to form an alloy with Si on the working electrode. The graphene cage remained intact throughout the lithiation process.
[0056] In the electrochemical characterization, all working electrodes were prepared using a conventional slurry method. Si N clusters@Si@G powder and polyvinylidene fluoride (PVDF, Kynar HSV 900) binder in a mass ratio of 9:1 were dispersed in N-methyl-2-pyrrolidone (NMP) and stirred for 12 h. Control electrodes with bare Si NP clusters@G or Si NP clusters@Si were prepared using the same slurry method, except that the mass ratio of active material (Si NP clusters@G or Si NP clusters@Si), carbon black conductive additive (Super P, TIMCAL, Switzerland) and PVDF binder was 8:1:1. After casting it onto a copper foil with a thickness of 15 μm and drying it in a vacuum oven at 60 °C for 12 h, the samples were calendered and cut into pieces with a mass loading of 0.6–2.0 mg cm -2 1 cm 2 disk. In an argon-filled glove box, these working electrodes were assembled into 2032-type coin cells using a polymer separator (Celgard 2250) and metallic lithium (Alfa Aesar) as the counter / reference electrode (half-cell) or lithium cobalt oxide (LCO) as the cathode (full cell). 100 μl of 1.0 M LiPF6 in 89 vol% 1:1 w / w ethylene carbonate / diethyl carbonate (BASF Selectilyte LP40) with 10 vol% fluoroethylene carbonate and 1 vol% vinyl carbonate (Novolyte Technologies) was added as the electrolyte, with complete wetting of the working and counter electrode surfaces. The coin cells were loaded into a battery test (Land Instruments) and cycled between 0.01 and 1 V (half-cell) or 3.0 and 4.2 V (full cell). The Si anode in the full cell was prepared exactly as described in the half-cell experiments and was not subjected to any pre-cycling or pre-lithiation before use in the full cell. The total mass of the graphene-encapsulated Si NP clusters@Si composites was used to calculate the specific capacities of all cells. The theoretical capacity of silicon (4,200 mAh g -1 Si, calculate the charge / discharge rate. Using delithiation (C 去合金化) capacity and lithiation (C 合金化 ) Capacity ratio (C 去合金化 / C 合金化 × 100%). For ex situ SEM / TEM characterization of the working electrode, the coin cell was charged to 1 V and then disassembled. The working electrode was then gently rinsed in acetonitrile to remove the Li salt from the residual electrolyte.
[0057] Turning now to another embodiment of the present invention, it includes surface engineered Si mesoporous particles to greatly improve the Coulombic efficiency. The mesoporous Si particles are obtained by thermal disproportionation of SiO particles followed by removal of the SiO2 byproduct, each of which is first coated with a Si shell and then encapsulated with a graphene cage. This design has several attractive advantages: (1) The Si shell can prevent electrolyte diffusion into the interior and limit SEI formation to the outer surface ( Figure 5A-5B ), thus greatly improving the initial Coulombic efficiency (Table 1, 37.6% before Si skin coating and 87.5% after); (2) the non-filled Si shell retains internal void space to accommodate volume expansion, thus having good cycling stability; (3) the Si particles are endowed with an electrochemically active surface through the inherent high electronic conductivity and ion permeability of the defective graphene cages; (4) the SEI is expected to form mainly on the mechanically strong and soft graphene cages, thus inducing stable SEI formation and improving the Coulombic efficiency of the later cycles; and (5) SiO particles are commercially available and inexpensive, making the anode material cost-effective and scalable.
[0058] Table 1. Summary of specific surface area, total pore volume, and lithium-ion battery performance of different products. Specific surface area was calculated from 0.05 – 0.20 based on Brunauer–Emmett–Teller (BET) data.
[0059]
[0060] The system was analyzed using Quantum software.
[0061] Regarding the material fabrication and characterization of the current embodiments, Fig. 6AThe synthesis process of our surface-engineered mesoporous Si microparticles is shown. Commercially available SiO particles (~325 mesh) were first ball-milled to reduce the size to 1-6 um. These SiO particles were then annealed at 950 °C for 10 h under Ar atmosphere. During the annealing process, SiO underwent thermal disproportionation and subsequent phase separation to form interconnected Si NPs embedded in a SiO2 matrix. After removing the SiO2 matrix with HF solution, mesoporous Si (Mp-Si) microparticles were obtained. A dense Si skin was then deposited on each Mp-Si microparticle by a chemical vapor deposition (CVD) method to obtain Si skin-sealed mesoporous Si (Mp-Si@Si) microparticles. These Mp-Si@Si microparticles were further encapsulated with highly conformal graphene cages by chemical deposition of a Ni template followed by CVD growth of graphene. Ni served as both a catalyst for graphene growth and a sacrificial template layer to provide voids. After low-temperature (450°C) annealing, graphene grows on Ni-coated Mp-Si@Si microparticles via a dissolution-precipitation mechanism. Finally, the Ni catalyst is etched away using an aqueous FeCl3 solution to obtain graphene cage-encapsulated Si skin-sealed mesoporous Si (Mp-Si@Si@G) microparticles.
[0062] exist Figure 6B-6M Representative transmission electron microscopy (TEM) and scanning electron microscopy (SEM) images of the products obtained at different steps in the synthesis process are shown in FIG. As shown in the inset magnified SEM image ( Figure 6B ), the size of the heat-treated SiO particles is 1-6 um and the surface is smooth. From TEM ( Fig.6I ) and high-resolution TEM (HRTEM) images clearly show the interconnected features of Si NPs with a size of less than 10 nm embedded in the SiO2 matrix. The unique lattice fringes with a d-spacing of 3.2 Å (111) indicate the crystalline nature of the Si NPs, while the adjacent amorphous material is SiO2. X-ray diffraction (XRD) characterization further confirmed that the SiO2 particles were transformed into nanocrystalline Si (JCPDS Card No. 27-1402) with an average particle size of ~ 8 nm (estimated by the Debye-Scherrer equation) and amorphous SiO2 ( Figure 6J ), which is consistent with the HRTEM results. X-ray photoelectron spectroscopy (XPS) also shows the coexistence of Si and SiO2 in the annealed SiO particles: the peak observed at ~99 eV corresponds to the binding energy of Si(0), while the peak centered at ~103 eV indicates the presence of SiO2.
[0063] After removing SiO2 by HF etching, a crystalline Si skeleton was obtained (Figures 6c, 6J, 6K). The XRD spectrum shows a significant suppression of the broad SiO2 peak after HF etching, while the remaining weaker SiO2 protrusions in the XPS spectrum may be caused by natural oxidation in air. After etching, the surface roughness of the particles is greatly increased ( Figure 6C ), and by TEM ( Figure 6G ) and focused ion beam SEM (FIB-SEM) images ( Figure 6K ) A highly porous structure is clearly observed. After 100nm Si skin sealing, the particles become smooth again ( Fig.6D Impressively, the highly mesoporous internal structure is preserved, indicating that the Si skin only encapsulates the outer layer of the particle ( Figure 6L ).
[0064] In order to better improve the electrochemical performance, the Mp-Si@Si particles were further encapsulated with graphene cages ( Fig. 6E , 6I , 6M). In addition, Mp-Si particles without Si skin but encapsulating graphene cages (Mp-Si@G) were also prepared. Obviously, the graphene cages exhibit a wavy structure, which is caused by the conformal growth of graphene along the large grains of Ni deposited on the Si particles. The highly graphitized nature of the graphene cages is demonstrated by the clearly observed multilayer structure ( Figure 6M ), and further confirmed by Raman spectroscopy, where a distinct D band with a narrow bandwidth indicates the presence of sufficient defects to facilitate lithium ion transport to Si. Thermogravimetric analysis (TGA) shows that the graphene cages only account for about 8% of the total mass of the Mp-Si@Si@G composite (about 10% for the Mp-Si@G composite). It is assumed that the lower carbon content compared to previous work minimizes the irreversible capture of lithium ions by the graphene structure and improves the Coulombic efficiency without sacrificing specific capacity.
[0065] For the in situ lithiation of Mp-Si@Si@G microparticles, there must be sufficient internal void space to maintain the structural integrity of the Si anode. To verify the compatibility of our Mp-Si@Si@G structure with the dramatic volume expansion of the Si anode, an in situ TEM study of the lithiation of Mp-Si@Si@G microparticles was performed and compared with the lithiation of dense Si microparticles ( Figures 7A-7D ).exist Fig. 7A and Figure 7C The electrochemical cell used for in situ TEM studies is schematically shown in Figure 1. A series of images were taken at regular intervals from a movie recording the in situ lithiation process of the Si anode to monitor its structural changes. A significant volume expansion of the dense Si microparticles ( Figure 7B), cracks appeared after only 32 seconds and expanded with time. At 160s, the dense Si particles broke violently into smaller particles. In contrast, the structural integrity of the Mp-Si@Si@G particles was well maintained throughout the lithiation process ( Fig.7D ). At 0 s (before lithiation), the surrounding graphene shell is clearly observed outside the inner Si microparticle. The volume of the Si microparticle expands as lithium ions diffuse through the graphene shell and form an alloy with silicon. The complete lithiation of the Si microparticle is completed around 168 s, as shown by the slight TEM contrast change of the graphene shell after this point. Even after full lithiation, the entire structure remains intact, thanks to the sufficient pore space inside the Mp-Si@Si@G microparticle to accommodate the large volume expansion, and the mechanically strong graphene cage restricts the Si core to expand mainly inside. These results indicate that this well-designed mesoporous core@Si skin@graphite cage structure can effectively prevent the structural rupture of the Si anode during lithiation, thereby improving the cycle life of the battery.
[0066] Regarding electrochemical performance, the advantages of our Mp-Si@Si@G microparticles have been further confirmed by electrochemical testing in half-cell and full-cell configurations. 2032-type coin cells were constructed for deep galvanostatic cycling tests from 0.01 to 1 V (half-cell, 0.01 to 2.0 V for the first three activation cycles) and from 3.0 to 4.2 V (full cell). All reported capacities are based on the total mass of Si and C in the composite.
[0067] Coulombic efficiency is one of the most important parameters for evaluating battery performance, especially in the early cycles, which is responsible for most of the lithium ion losses and electrolyte consumption during SEI formation. Fig. 8A As shown in Table 1, the initial Coulombic efficiency of Mp-Si@Si@G particles is better than any other intermediates, reaching 88.7%. The poor ICE of mesoporous silica particles (37.6%) is due to their large specific surface area (229 m 2 / g, as shown in Table 1), which will cause many side reactions and a large amount of irreversible lithium consumption. After sealing with dense silicon skin, the specific surface area is reduced to only 1.9 m 2 / g, the ICE is greatly improved to 87.5%, which is due to the reduction of side reactions and reduced SEI formation. After further encapsulation with graphene cages, the ICE of Mp-Si@Si@G particles reaches 88.7%, which is more than twice the ICE of the initial Mp-Si particles. More interestingly, unlike other high-performance nano-Si anodes that usually require many cycles to reach more than 99%, the Coulombic efficiency of Mp-Si@Si@G particles reaches more than 99% after only 7 cycles ( Figure 8C ), and has remained at a high level (99.8%-100%) since then.
[0068] The improvement in early and late cycle Coulombic efficiency can be explained in two parts: the surface chemistry allows initial SEI formation without excessive Li consumption, and the mechanically stable electrode / electrolyte interface prevents additional SEI formation. First, the silicon skin greatly reduces the surface area accessible to the electrolyte, thereby minimizing possible side reactions and irreversible lithium consumption. This can be verified by the cyclic voltammetry results: for the Mp-Si sample, a clear reduction peak is observed at about 1.15 V, which corresponds to the Li formed during the slurry preparation process and the surface SiO X In contrast, no obvious cathodic peak of irreversible reaction was observed for the Mp-Si@Si sample. In addition, the voltage distribution attributed to SiO was only observed for the Mp-Si sample. X The plateau of lithiation is about 1.2 V ( Fig. 8A ), further indicating that the irreversible Li consumption is greatly reduced by surface Si sealing.
[0069] Second, encapsulation of Mp-Si@Si with elastic graphene cages ensures the formation of a stable electrode / electrolyte interface and prevents uncontrolled SEI formation. The Nyquist plots obtained from electrochemical impedance spectroscopy (EIS) tests ( Figure 8B ) show that the Mp-Si@Si@G microparticles have much faster kinetics and excellent stability even after 100 cycles. Together with the higher late cycle Coulombic efficiency ( Figure 8C , 99.8–100.0%), and the EIS data provided strong evidence for the stable SEI layer during cycling of Mp-Si@Si@G microparticles.
[0070] In addition to Coulombic efficiency, specific capacity and cycling stability are the other two most important parameters for practical batteries. Figure 8C The half-cell data in Figure 2 show that Mp-Si@Si@G particles can be used for the production of nanostructured carbon nanotubes at C / 20 (1C = 4.2 A g -1 ) reached a current density of about 2834 mAh g -1 Considering that the mass ratio of Si in the composite is 92%, the specific capacity relative to Si is as high as 3080 mAh g -1 The high capacity indicates that the active materials are well electrically connected and fully participate in the electrochemical lithiation and delithiation processes. Note that this is achieved without the use of any conductive additives, which indicates the excellent conductivity of the graphene cage. In addition, at higher C / 2 (~ 1.4 mA cm -2 After 300 cycles at a rate of 1,246 mAh g -1 This is still more than three times the theoretical capacity of commercial graphite anodes and far exceeds the capacity of Mp-Si (560 mAh g at the 10th cycle).-1 ), Mp-Si@G (792 mAh g at the 300th cycle -1 ) or Mp-Si@Si (1047 mAh g at the 100th cycle -1 , 534 mAh g at the 300th cycle -1 It is worth mentioning that the cycling stability of Mp-Si@Si particles is better than that of dense Si particles (less than 370 mAh g in 20 cycles). -1 ), which is much better than the internal pore space that buffers the volume expansion during lithiation. However, the SEI on the Mp-Si@Si surface is unstable, resulting in poor stability in later cycles.
[0071] The excellent electrochemical stability can be attributed to the well-designed micro / nanoscale structure of the Si-C composite electrode. The void spaces automatically generated during the thermal disproportionation and etching process retain the secondary particles and buffer the volume expansion. According to the chemical equation (1)
[0072] 2SiO → Si + SiO2 (1)
[0073] According to their densities (2.1, 2.3, and 2.6 g cm for SiO, Si, and SiO2, respectively) -3 ), after heat dispersion, per cm 3 The SiO will generate 0.30 cm 3 Si and 0.55 cm 3 This means that after removing SiO2, a larger void ratio of about 11:6 is achieved:Si. Such a large volume ratio allows the free volume of the Si material to expand without destroying the graphene shell.
[0074] To better understand the reason for such good cycling stability, post-cycling cross-sectional SEM analysis was performed to show the morphological changes of the Si-C composite electrode after charge / discharge. Fig.8D , 8E ), the volume expansion of the Mp-Si@Si@G microparticle electrode is only 13%, which is much smaller than the volume expansion of Mp-Si@Si microparticles (about 86%) and dense Si microparticles (more than 150%), indicating that the cycling stability is improved.
[0075] Mp-Si@Si@G microparticles simultaneously show high Coulombic efficiency and good cycling stability. Therefore, practical full cells with high mass loading and improved cycling performance can be constructed. In contrast to the almost unlimited lithium supply in the half-cell, the full cell has a limited lithium supply, so the Coulombic efficiency of the early cycles is low, which means that the large irreversible lithium consumption will definitely lead to severe battery degradation. As a result, achieving high early cycle Coulombic efficiency is crucial to the cycling stability of the full cell. In addition, it is quite challenging to achieve good cycling stability at high mass loading due to the more difficult charge transfer and large volume changes. In the case of the current embodiment, when the mass loading is as high as ~ 2.0 mgcm -2 When quenched, the Mp-Si@Si@G particles can still achieve good cycling stability, showing great promise for practical full battery applications.
[0076] like Figure 8F As shown, when paired with a conventional lithium cobalt oxide (LCO) cathode, Mp-Si@Si@G microparticles exhibited a high charge / discharge rate at 0.8 mA cm -2 The current density was maintained at 1.75 mAh cm after 100 cycles. -2 ) and high Coulombic efficiency. Moreover, the voltage curves at different cycle numbers show no obvious increase in overpotential, indicating that both the anode and cathode are stable during cycling. This excellent full-cell capacity and stability for micro-Si anode materials demonstrates the great promise of our surface engineering approach in addressing existing challenges in today’s LIB industry.
[0077] Now turn to the synthesis of mesoporous Si (Mp-Si) microparticles. In a typical thermal disproportionation process, commercially available SiO particles (325 mesh, Sigma-Aldrich) were heated to 950 °C at a heating rate of 5 °C / min and kept under Ar atmosphere for 10 h. To remove the SiO2 matrix, the annealed sample was taken out of the test tube at a temperature below 50 °C and immersed in a 10 wt% HF solution (H2O:isopropanol = 3:1, v / v) at room temperature for 2 h. The obtained mesoporous Si was collected by filtration and washed several times with distilled water and ethanol in sequence. The final product was dried in a vacuum oven at 60 °C for 2 h and then stored in a glove box for further use.
[0078] To synthesize silicon-sealed Mp-Si (Mp-Si@Si) microparticles, mesoporous Si microparticles were sealed with Si by a chemical vapor deposition (CVD) method. In a typical method, the mesoporous Si microparticles were transferred to a tube furnace (Thermo Electron Corporation) and then purged with high-purity Ar gas. The tube was then heated to 550°C at a heating rate of 50°C / min. Thereafter, pure Ar gas and silane gas were introduced into the tube at a total pressure of 200 Torr, and the partial pressure of silane was 100 Torr. After reacting at 550°C for 30 minutes, the silane gas was cut off, and the tube was cooled under an Ar atmosphere. Finally, the silicon-sealed mesoporous Si microparticles were collected after the temperature was below 50°C.
[0079] In order to obtain a conformal Ni coating when synthesizing graphene-encapsulated Mp-Si@Si microparticles, the surface of the Mp-Si@Si microparticles must be densely covered with nucleation seeds (Pd in this case). (3-Aminopropyl)triethoxysilane (APTES) was used as a surface adhesion layer to sensitize the Si surface with –NH2 groups, followed by the reduction of Pd metal seeds from solution onto Si.
[0080] 1 g of the prepared Mp-Si@Si microparticles was dispersed in 100 ml of isopropanol and sonicated for about 15 min. 1 ml of APTES (99% purity, Sigma-Aldrich) and 100 ul of distilled water were added to the isopropanol solution in sequence and stirred at 70 °C for 1 h. This formed a very thin layer of –NH2 groups on the surface of the silicon microparticles. The sample was then collected by centrifugation and washed three times with deionized water. Finally, the particles were immersed in 30 ml of an aqueous palladium chloride solution (0.5 g / L PdCl2; 2.5 ml / L concentrated HCL; Sigma-Aldrich) and stirred for 15 min. The activated Mp-Si@Si microparticles were obtained by washing three times with deionized water and collecting by centrifugation.
[0081] The thickness of the nickel coating can be adjusted by changing the concentration of the electroless nickel (EN) solution or controlling the number of deposition reactions. In one example, a combination of the two methods was used.
[0082] Two electroless nickel plating solutions were prepared: a primary solution (20 g / L nickel sulfate hexahydrate; 10 g / L citric acid dihydrate; 5 g / L lactic acid) and a secondary solution with double the concentration of the components (40 g / L nickel sulfate hexahydrate; 20 g / L sodium citrate dihydrate; 10 g / L lactic acid). The activated Mp-Si@Si microparticles were immersed in these EN solutions in sequence.
[0083] Prior to the first chemical deposition, 2 g of dimethylamine borane (DMAB; Sigma-Aldrich) and 2 ml of ammonium hydroxide (NH3·H2O, Sigma-Aldrich, 28%) were added to 360 ml of the primary EN solution. pH-sensitive DMAB was used as a reducing agent during the electroless nickel plating process. Then 1 g of the activated Mp-Si@Si microparticles was added to the primary EN solution and gently stirred for about 30 min. As the reaction proceeded, bubbles began to appear and the color of the green EN solution became lighter. After the deposition was completed, the Mp-Si@Si@1xNi settled to the bottom. While holding the Mp-Si@Si@1xNi particles at the bottom of the container with a magnet, the exhausted EN plating solution was carefully poured out. In another container, 4 g of DMAB and 4 ml of ammonium hydroxide were added to 360 ml of the secondary EN solution. This was then immediately added to the wet particles (Mp-Si@Si@1xNi) and stirred for another 30 min. The resulting Mp-Si@Si@2xNi was washed twice with ethanol.
[0084] For graphene encapsulation, Mp-Si@Si@2xNi particles were dispersed in 150 ml triethylene glycol (Santa Cruz Biotechnology) and 500 ml NaOH aqueous solution (50%, w / w). After stirring at 185 °C for 8 h, the carburized Mp-Si@Si@2xNi particles were collected by centrifugation and washed three times with ethanol. The carburization process occurs when the organic solvent decomposes, allowing carbon atoms to diffuse into the Ni layer and adhere to the surface. This triggers low-temperature graphene growth on the Mp-Si@Si@2xNi particles. The sample was then dried in a vacuum oven at 50 °C for 1 h. The dried particles were placed in a tube furnace with the following temperature profile: heating to 450 °C at a rate of 15 °C / min; keeping the temperature at 450 °C for 1 h. The Ar flow rate was maintained at 80 sccm throughout the annealing process. During the annealing process, Brij® 58 decomposes, allowing carbon atoms to diffuse into the Ni layer and adhere to the surface. This triggers low-temperature graphene growth on Mp-Si@Si@2xNi. The dual-purpose Ni template is etched away by immersing the annealed particles in 1 M FeCl3 aqueous solution (2 h).
[0085] After washing with 1 M HCl aqueous solution and deionized water three times and drying in a vacuum oven at 60 °C for 1 h, graphene-encapsulated Mp-Si@Si microparticles were obtained.
[0086] Turning now to the material characterization, the weight percentages of Si and C in Mp-Si@Si@G were determined from the weight loss curves measured on a TG / DTA instrument (Netzsch STA 449) at a heating rate of 5 °C / min in a simulated air atmosphere (20% O2 + 80% Ar, both ultra-pure grade gases from Airgas). Under these conditions, the mass gain is due to slight Si oxidation, while the mass loss is caused by the oxidation of carbon to gaseous species. To separate these two processes, a bare Si control sample was measured under the same heating conditions and the mass gain was subtracted from the graphene encapsulated Mp-Si@Si curve. Additional characterizations were performed using scanning electron microscopy (FEI Sirion, Nova NanoSEM), transmission electron microscopy (FEI Tecnai, Titan), X-ray photoelectron spectroscopy (SSI S-Probe Monochromatized, Al Kα radiation at 1486 eV), electrochemical impedance spectroscopy (BioLogic VMP3), and Raman spectroscopy (Horiba JY).
[0087] For in situ TEM characterization, a piezoelectrically controlled electrically biased TEM-AFM holder (NanofactoryInstruments) was used to observe the lithiation (delithiation) process of graphene-encapsulated Mp-Si@Si microparticles and measure the electrical and mechanical properties of the graphene cages. Li metal and Mp-Si@Si@G microparticles were dispersed on 0.25 mm W and Cu wires, respectively. They were then contacted by a piezoelectric controller. By applying a bias of -3 V, Li ions flowed through the native oxide / nitride of Li metal to form an alloy with Si on the working electrode. The graphene cage remained intact throughout the lithiation process.
[0088] Regarding electrochemical characterization, all working electrodes were prepared using a conventional slurry method. Mp-Si@Si@G powder and polyvinylidene fluoride (PVDF, Kynar HSV 900) binder in a mass ratio of 9:1 were dispersed in N-methyl-2-pyrrolidone (NMP) in the absence of any conductive additive and stirred for 12 h. Control electrodes with bare Mp-Si, Mp-Si@G, or Mp-Si@Si were prepared using the same slurry method, except that the mass ratio of active material (Mp-Si or Mp-Si@Si), carbon black conductive additive (Super P, TIMCAL, Switzerland), and PVDF binder was 8:1:1. After casting it onto a copper foil with a thickness of 15 μm and drying it in a vacuum oven at 60 °C for 12 h, the samples were calendered and cut into pieces with a mass loading of 0.6–2.0 mg cm -2 1 cm 2disk. In an argon-filled glove box, these working electrodes were assembled into 2032-type coin cells using a polymer separator (Celgard 2250) and metallic lithium (Alfa Aesar) as the counter / reference electrode (half-cell) or lithium cobalt oxide (LCO) as the cathode (full cell). 100 μl of 1.0 M LiPF6 in 89 vol% 1:1 w / w ethylene carbonate / diethyl carbonate (BASF Selectilyte LP40) with 10 vol% fluoroethylene carbonate and 1 vol% vinyl carbonate (Novolyte Technologies) was added as the electrolyte, with complete wetting of the working and counter electrode surfaces. The coin cells were loaded into a battery tester (Land Instruments) and cycled between 0.01 and 1 V (half-cell, 0.01 to 2.0 V for the first three activation cycles) or 3.0 to 4.2 V (full cell). In the full-cell configuration, the mass loading of the Mp-Si@Si@G electrode was approximately 2.0 mg cm -2 , when Li metal was used as the counter electrode, the concentration was 0.24 mg cm -2 gives about 4.7 mAhcm -2 The areal capacity of the LCO cathode tested with Li metal as the counter electrode is 0.3 mg cm -2 The lower one is about 4.1 mAh cm -2 , giving a theoretical N / P ratio of about 1.14. The Si anodes in the full cells were prepared exactly as described in the half-cell experiments and were not subjected to any pre-cycling or pre-lithiation before use in the full cells. The total mass of the graphene-encapsulated Mp-Si@Si composite was used to calculate the specific capacity of all cells. The theoretical capacity of silicon (4,200 mAh g -1 Si, calculate the charge / discharge rate. Using delithiation (C 去合金化 ) capacity and lithiation (C 合金化 ) Capacity ratio (C 去合金化 / C 合金化 ×100%). For ex situ SEM / TEM characterization of the working electrode, the coin cell was charged to 1 V and then disassembled. The working electrode was then gently rinsed in acetonitrile to remove the Li salt from the residual electrolyte.
[0089] The present invention has now been described in terms of several exemplary embodiments, which are intended to be illustrative in all respects and not restrictive. Thus, the present invention is capable of many variations in detailed implementation, which can be derived by one of ordinary skill in the art from the description contained herein. For example, the porous silicon microstructure can be composed of silicon nanoparticles, nanosheets, nanosheets or nanorods, etc.
[0090] All such variations are considered to be within the scope and spirit of the invention as defined by the appended claims and their legal equivalents.
Claims
1. A battery electrode, comprising: a) a porous silicon microstructure comprising Si mesoporous particles having pores disposed therein; b) depositing a silicon shell coating on the porous silicon microstructure, wherein the outer contour of the porous silicon microstructure is conformally covered by the silicon shell coating so that the pores remain in the porous silicon microstructure; as well as c) depositing a graphene coating on the silicon shell coating, wherein the graphene coating encapsulates the silicon shell coating to form a porous silicon microstructure battery electrode protected by a graphene-encapsulated silicon shell. 2 . The battery electrode according to claim 1 , wherein the density of the silicon shell coating is greater than the density of the porous silicon microstructure. The battery electrode according to claim 1 , wherein the silicon shell coating comprises a sealing structure. 4 . The battery electrode according to claim 3 , wherein the mechanical strength of the silicon shell coating is greater than the mechanical strength of the porous silicon microstructure.
5. The battery electrode according to claim 1, wherein the silicon shell coating has a thickness of about 200 nm.
6. A battery electrode, comprising: A porous silicon microstructure comprising Si nanoparticle clusters having pores disposed between the Si nanoparticles; a silicon shell coating deposited on the porous silicon microstructure, wherein the outer contour of the porous silicon microstructure is conformally covered by the silicon shell coating so that the pores remain in the porous silicon microstructure; as well as A graphene coating is deposited on the silicon shell coating, wherein the graphene coating encapsulates the silicon shell coating to form a porous silicon microstructure battery electrode protected by a graphene-encapsulated silicon shell. 7 . The battery electrode of claim 6 , wherein the density of the silicon shell coating is greater than the density of the porous silicon microstructure.
8. The battery electrode according to claim 6, wherein the silicon shell coating comprises a sealing structure. 9 . The battery electrode according to claim 8 , wherein the mechanical strength of the silicon shell coating is greater than the mechanical strength of the porous silicon microstructure.
10. The battery electrode according to claim 6, wherein the silicon shell coating has a thickness of about 200 nm. 11 . The battery electrode according to claim 6 , wherein the Si nanoparticle clusters have a diameter ranging from 1 μm to 5 μm.